Wide-temperature-range composite solid electrolyte membrane and preparation method thereof
By preparing a wide-temperature composite solid electrolyte membrane composed of specific components, the problem of poor high-temperature stability of polymer solid lithium ion electrolytes is solved, and the high-temperature stability and safety of lithium ion batteries in a wide-temperature domain are improved.
Patent Information
- Application Number
- CN202411339626.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-25
- Publication Date
- 2024-11-12
AI Technical Summary
Polymer solid lithium-ion electrolyte has disadvantages in terms of low room temperature ion conductivity, narrow electrochemical windows, and poor high temperature stability, which limits its application.
Using a wide temperature domain composite solid electrolyte membrane composed of polyethylene glycol, hexamethylene diisocyanate, ethylenediamine and other components, the preparation method of supporting the mixing and coating of polymer and electrolyte solution is formed to form a high temperature stability. and safety composite solid electrolyte membrane.
It realizes the high temperature stability and cycle stability of lithium-ion batteries in a wide temperature domain, improving the safety and performance of the batteries.
Smart Images

Figure CN118943481A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of solid-state lithium-ion batteries and relates to a wide-temperature composite solid-state electrolyte membrane and a preparation method thereof. Background Art
[0002] Since its commercial application, lithium-ion batteries have been widely used in portable devices such as mobile phones and computers, and new energy vehicles. With the rapid development of new energy vehicles, the industry has put forward higher requirements for the safety and stability of lithium-ion batteries. Compared with liquid electrolytes, solid electrolytes have great advantages in safety; among them, polymer solid electrolytes have attracted widespread attention for their good film-forming properties, certain ductility, and easy large-scale manufacturing. However, polymer solid electrolytes still have disadvantages such as low room temperature ionic conductivity, narrow electrochemical window, and poor high temperature stability, which limit their application. Summary of the invention
[0003] The purpose of the present invention is to provide a composite solid electrolyte membrane for lithium ions, which has the characteristics of a wide temperature range.
[0004] The present invention also provides a method for preparing the composite solid electrolyte membrane and a solid-state lithium ion battery using the composite solid electrolyte membrane.
[0005] The invention discloses a wide temperature range composite solid electrolyte membrane and a preparation method thereof, wherein the wide temperature range composite solid electrolyte membrane is composed of component A, component B, component C, component D and component E.
[0006] The component A is one or more of polyethylene glycol, polycarbonate diol, polypropylene carbonate diol, polyphthalic anhydride, ethylenediaminetetraacetic anhydride, and 4,4′-biphenyl ether anhydride;
[0007] The component B is one or more of hexamethylene diisocyanate, isophorone diisocyanate, 4,4-methylenebis(phenyl isocyanate), ethylenediamine, diamine oxalate, triethylamine, p-phenylenediamine, butanediol, dihydroxyacetone, and trimethylolpropane;
[0008] The component C is one or more of dibutyltin dilaurate, isoquinoline, and acetic anhydride;
[0009] The component D is one or more of polyethylene oxide, polyacrylonitrile, polyacrylic acid, polyvinylidene fluoride, poly(vinylidene fluoride-co-hexafluoropropylene), polycarbonate, polyurethane, polymethyl methacrylate, and polyacetimide;
[0010] The component E is one or more of lithium perchlorate, lithium tetrafluoroborate, lithium hexafluoroborate, lithium difluorooxalatoborate, lithium bis(trifluoromethanesulfonyl)imide, and lithium bis(trifluorosulfonyl)imide.
[0011] The method for preparing a wide temperature range composite solid electrolyte membrane of the present invention is carried out according to the following steps:
[0012] 1. Preparation of supporting polymer: Disperse component A, component B and component C in a solvent according to a certain ratio, heat to 30-120°C under air-tight conditions, and stir for 1-50 hours. Then add a certain amount of component B to the solution, heat to 30-120°C under air-tight conditions, and stir for 1-50 hours to obtain a solution containing supporting polymer;
[0013] The solvent is one or more of ethanol, ether, acetonitrile, acetone, dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone;
[0014] The mass ratio of the component A to the volume ratio of the solvent is (1-10 g):(1-500 mL);
[0015] The mass ratio of the component B to the volume ratio of the solvent is (1-10 g):(1-500 mL);
[0016] The mass ratio of the component C to the volume ratio of the solvent is (1-10 g):(1-5000 mL);
[0017] 2. Preparation of a mixed solution of component D and component E: dissolve component D and component E in a solvent, heat to 30-120° C. in an airtight condition, and stir for 1-50 hours to obtain a mixed solution;
[0018] The solvent is one or more of ethanol, ether, acetonitrile, acetone, dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone;
[0019] The mass ratio of the component D to the volume ratio of the solvent is (1-10 g):(1-500 mL);
[0020] The mass ratio of the component E to the volume ratio of the solvent is (1-10 g):(1-500 mL);
[0021] 3. Preparation of a wide temperature range composite solid electrolyte membrane: Mix the two solutions obtained in step 1 and step 2 in a certain ratio, heat to 30-120°C under air-tight conditions, and stir for 1-50 hours to mix the two solutions evenly; apply the mixed solution on polytetrafluoroethylene or polyethylene terephthalate with a thickness of 100-1000 μm, and after drying, obtain a composite solid electrolyte membrane;
[0022] The drying step is to initially volatilize the solvent at room temperature, and then dry in vacuum at 30-120°C;
[0023] The drying time at room temperature is 4 to 24 hours; the drying time under vacuum is 4 to 96 hours.
[0024] The solid-state lithium-ion battery of the present invention uses the composite solid-state electrolyte membrane prepared in the above step three, and has high-temperature stability, safety and cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 The cycling curve of the lithium iron phosphate half-cell at 90°C in Experiment 2
[0026] Figure 2 The cycle curve of the lithium iron phosphate half-cell at 0°C in Experiment 2 DETAILED DESCRIPTION
[0027] The present invention will be further described below with reference to embodiments and drawings, but the present invention is not limited to these embodiments.
[0028] Specific implementation method 1: A wide temperature range composite solid electrolyte membrane and a preparation method thereof of the present invention are characterized in that the wide temperature range composite solid electrolyte membrane is composed of component A, component B, component C, component D and component E.
[0029] The component A is one or more of polyethylene glycol, polycarbonate diol, polypropylene carbonate diol, polyphthalic anhydride, ethylenediaminetetraacetic anhydride, and 4,4′-biphenyl ether anhydride;
[0030] The component B is one or more of hexamethylene diisocyanate, isophorone diisocyanate, 4,4-methylenebis(phenyl isocyanate), ethylenediamine, diamine oxalate, triethylamine, p-phenylenediamine, butanediol, dihydroxyacetone, and trimethylolpropane;
[0031] The component C is one or more of dibutyltin dilaurate, isoquinoline, and acetic anhydride;
[0032] The component D is one or more of polyethylene oxide, polyacrylonitrile, polyacrylic acid, polyvinylidene fluoride, poly(vinylidene fluoride-co-hexafluoropropylene), polycarbonate, polyurethane, polymethyl methacrylate, and polyacetimide;
[0033] The component E is one or more of lithium perchlorate, lithium tetrafluoroborate, lithium hexafluoroborate, lithium difluorooxalatoborate, lithium bis(trifluoromethanesulfonyl)imide, and lithium bis(trifluorosulfonyl)imide.
[0034] Specific implementation method 2: This implementation method is a method for preparing a wide temperature range composite solid electrolyte membrane of specific implementation method 1, and the specific steps are as follows:
[0035] 1. Preparation of supporting polymer: Disperse component A, component B and component C in a solvent according to a certain ratio, heat to 30-120°C under air-tight conditions, and stir for 1-50 hours. Then add a certain amount of component B to the solution, heat to 30-120°C under air-tight conditions, and stir for 1-50 hours to obtain a solution containing supporting polymer.
[0036] The solvent is one or more of ethanol, ether, acetonitrile, acetone, dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone.
[0037] The mass ratio of the component A to the volume ratio of the solvent is (1-10 g):(1-500 mL);
[0038] The mass ratio of the component B to the volume ratio of the solvent is (1-10 g):(1-500 mL);
[0039] The mass ratio of the component C to the volume ratio of the solvent is (1-10 g):(1-5000 mL);
[0040] 2. Preparation of a mixed solution of component D and component E: dissolve component D and component E in a solvent, heat to 30-120° C. in an airtight condition, and stir for 1-50 hours to obtain a mixed solution;
[0041] The solvent is one or more of ethanol, ether, acetonitrile, acetone, dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone;
[0042] The mass ratio of the component D to the volume ratio of the solvent is (1-10 g):(1-500 mL);
[0043] The mass ratio of the component E to the volume ratio of the solvent is (1-10 g):(1-500 mL);
[0044] 3. Preparation of a wide temperature range composite solid electrolyte membrane: Mix the two solutions obtained in step 1 and step 2 in a certain ratio, heat to 30-120°C under air-tight conditions, and stir for 1-50 hours to mix the two solutions evenly; apply the mixed solution on polytetrafluoroethylene or polyethylene terephthalate with a thickness of 100-1000 μm, and after drying, obtain a composite solid electrolyte membrane;
[0045] The drying step is to initially volatilize the solvent at room temperature, and then dry in vacuum at 30-120°C;
[0046] The drying time at room temperature is 4 to 24 hours; the drying time under vacuum is 4 to 96 hours.
[0047] The solid-state lithium-ion battery of the present invention uses the composite solid-state electrolyte membrane prepared in the above step three, and has high-temperature stability, safety and cycle stability.
[0048] Specific implementation method three: This implementation method is different from specific implementation method two in that the mass ratio of component A in step one to the volume ratio of the solvent is (1-5 g): 100 mL; the rest is the same as specific implementation method two.
[0049] Specific implementation method 4: This implementation method is different from specific implementation method 2 in that the volume ratio of the mass of component B in step 1 to the solvent is (1-5 g): 200 mL; the rest is the same as specific implementation method 2.
[0050] Specific implementation mode five: This implementation mode is different from specific implementation mode two in that the volume ratio of the mass of component C in step one to the solvent is (1-5 g): 500 mL; the rest is the same as specific implementation mode two.
[0051] Specific implementation method six: This implementation method is different from specific implementation method two in that the volume ratio of the mass of component D in step two to the solvent is (1-5 g):100 mL; the rest is the same as specific implementation method two.
[0052] Specific implementation method seven: This implementation method is different from specific implementation method two in that the mass ratio of component E in step two to the volume ratio of the solvent is (1-5 g):100 mL; the rest is the same as specific implementation method two.
[0053] Specific implementation eight: This implementation differs from specific implementation two in that, in step three, the mixed solution of step one and step three is coated on the polyethylene diaphragm with a certain thickness; the rest is the same as specific implementation two.
[0054] The present invention is verified by the following tests:
[0055] Experiment 1: A method for preparing an electrolyte solution is carried out according to the following steps:
[0056] Dissolve polyvinylidene fluoride-co-hexafluoropropylene in N-methylpyrrolidone, and stir at 80° C. for 5 h; then add lithium bis(trifluoromethanesulfonyl)imide to the solution, and stir at 80° C. for 3 h to obtain an electrolyte solution.
[0057] The mass ratio of the polyvinylidene fluoride-co-hexafluoropropylene to N-methylpyrrolidone is 1g:8g
[0058] The mass ratio of lithium bis(trifluoromethanesulfonyl)imide to N-methylpyrrolidone is 1 g:8 g
[0059] Experiment 2: Use the electrolyte solution prepared in Experiment 1 to prepare lithium iron phosphate electrodes and assemble half-cells for testing. Follow the steps below:
[0060] 1. Lithium iron phosphate half-cell assembly:
[0061] Lithium iron phosphate, conductive carbon material, binder, and electrolyte solution were mixed in a mass ratio of 6:1:1:2, and added to N-methylpyrrolidone to form a uniform slurry. The slurry was applied to the current collector aluminum foil and dried in a vacuum oven at 80°C for 24 hours. The dried aluminum foil was then cut into discs and assembled with the diaphragm and lithium sheet. The polymer solid electrolyte precursor was then injected and packaged using a battery packaging machine to obtain a lithium iron phosphate half-cell for testing.
[0062] 2. Electrochemical performance test:
[0063] The constant current charge and discharge tester produced by Xinwei Company was used to carry out charge and discharge tests to measure the cycle performance curve of the solid-state lithium iron phosphate battery. The charge and discharge voltage range was 2.5V to 3.8V.
[0064] Figure 1 This is the cycle performance curve of the lithium iron phosphate half-cell at 90°C in Experiment 2. Figure 1 As shown, the assembled battery can be stably cycled 100 times at a high temperature of 90°C, with a discharge specific capacity of 147 mAh / g and a capacity retention rate of 97.4%.
[0065] Figure 2 This is the cycle performance curve of the lithium iron phosphate half-cell at 0°C in Experiment 2. Figure 2 As shown, the assembled battery can be stably cycled 50 times at a temperature of 0°C with a discharge specific capacity of 100 mAh / g.
[0066] It should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A wide temperature range composite solid electrolyte membrane and a preparation method thereof, characterized in that The wide temperature range solid electrolyte is composed of component A, component B, component C, component D and component E; The component A is one or more of polyethylene glycol, polycarbonate diol, polypropylene carbonate diol, polyphthalic anhydride, ethylenediaminetetraacetic anhydride, and 4,4′-biphenyl ether anhydride; The component B is one or more of hexamethylene diisocyanate, isophorone diisocyanate, 4,4-methylenebis(phenyl isocyanate), ethylenediamine, diamine oxalate, triethylamine, p-phenylenediamine, butanediol, dihydroxyacetone, and trimethylolpropane; The component C is one or more of dibutyltin dilaurate, isoquinoline, and acetic anhydride; The component D is one or more of polyethylene oxide, polyacrylonitrile, polyacrylic acid, polyvinylidene fluoride, poly(vinylidene fluoride-co-hexafluoropropylene), polycarbonate, polyurethane, polymethyl methacrylate, and polyacetimide; The component E is one or more of lithium perchlorate, lithium tetrafluoroborate, lithium hexafluoroborate, lithium difluorooxalatoborate, lithium bis(trifluoromethanesulfonyl)imide, and lithium bis(trifluorosulfonyl)imide.
2. A method for preparing a wide temperature range composite solid electrolyte membrane as claimed in claim 1, which is carried out according to the following steps:
1. Preparation of supporting polymer: Disperse component A, component B and component C in a solvent according to a certain ratio, heat to 30-120°C under air-tight conditions, and stir for 1-50 hours. Then add a certain amount of component B to the solution, heat to 30-120°C under air-tight conditions, and stir for 1-50 hours to obtain a solution containing supporting polymer; The solvent is one or more of ethanol, ether, acetonitrile, acetone, dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone; 2. Preparation of a mixed solution of component D and component E: dissolve component D and component E in a solvent, heat to 30-120° C. in an airtight condition, and stir for 1-50 hours to obtain a mixed solution; The solvent is one or more of ethanol, ether, acetonitrile, acetone, dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone; 3. Preparation of wide temperature range composite solid electrolyte membrane: Mix the two solutions obtained in step 1 and step 2 in a certain proportion, heat to 30-120°C under air-tight conditions, and stir for 1-50 hours to allow the two solutions to mix evenly; coat the mixed solution on polytetrafluoroethylene or polyethylene terephthalate with a thickness of 100-1000 μm, and after drying, obtain a composite solid electrolyte membrane.
3. The method for preparing a wide temperature range composite solid electrolyte membrane according to claim 2, characterized in that The mass ratio of component A to the volume ratio of the solvent in step 1 is (1-10 g):(1-500 mL).
4. The method for preparing a wide temperature range composite solid electrolyte membrane according to claim 2, characterized in that The mass ratio of component B to the volume ratio of the solvent in step 1 is (1-10 g): (1-500 mL).
5. The method for preparing a wide temperature range composite solid electrolyte membrane according to claim 2, characterized in that The mass ratio of component C to the volume ratio of the solvent in step 1 is (1-10 g):(1-5000 mL).
6. The method for preparing a wide temperature range composite solid electrolyte membrane according to claim 2, characterized in that The mass ratio of component D to the volume ratio of the solvent in step 2 is (1-10 g):(1-500 mL).
7. The method for preparing a wide temperature range composite solid electrolyte membrane according to claim 2, characterized in that The mass ratio of component E to the volume ratio of the solvent in step 2 is (1-10 g):(1-500 mL).
8. The method for preparing a wide temperature range composite solid electrolyte membrane according to claim 2, characterized in that The drying conditions in step 3 are to initially evaporate the solvent at room temperature and then dry it in vacuum at 30-120°C.
9. The method for preparing a wide temperature range composite solid electrolyte membrane according to claim 8, characterized in that The initial volatilization time of the solvent is 4 to 24 hours, and the drying time under vacuum is 4 to 96 hours.