Ion electronics power supply, preparation method thereof and energy management system

CN118943655AInactive Publication Date: 2024-11-12BEIJING INST OF NANOENERGY & NANOSYST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410977282.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Due to the influence of cellulose functional groups, whitening agents and complex surface morphology, existing paper-based energy sources are difficult to build breathable two-dimensional nano-limited ion channels on paper substrates, limiting the power and energy density of ionic electronic energy.

Method used

By constructing paper-based two-dimensional nanochannels with a humidity permeability of 500gm-2d-1-750gm-2d-1 on the paper base, a two-dimensional nanochannel layer was set on the paper base using 33%-98% of the two-dimensional nanomaterial. The proportion of two-dimensional nanomaterials is adjusted to improve the breathability and stability of the channel, and a positive electrode sheet and a negative electrode sheet are provided at both ends of the channel to achieve efficient ion transmission.

Benefits of technology

It realizes an ion electronic power supply with high power density and energy density, has good breathability and stability, and can reach 438.02mW·cm-3, with simple process and low cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943655A_ABST
    Figure CN118943655A_ABST
Patent Text Reader

Abstract

The invention discloses an ion electronics power supply, a preparation method thereof and an energy management system. The ion electronics power supply comprises a paper-based two-dimensional nano channel, the paper-based two-dimensional nano channel comprises a paper base and a two-dimensional nano channel layer arranged on at least one side surface of the paper base; the two-dimensional nano channel layer comprises a two-dimensional nano material, and the mass fraction of the two-dimensional nano material is 33%-98%; and the humidity permeability of the paper-based two-dimensional nano channel is 500-750g gm <-2 > d <-1 >. According to the ion electronics power supply, the paper-based two-dimensional nano channel with the humidity permeability of 500-750g gm <-2 > d <-1 > is constructed, so that ions can be efficiently transmitted in the two-dimensional nano channel layer, and the power and the energy density of the ion electronics power supply can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of energy storage devices, and in particular to an ion electronics power supply, a preparation method thereof, and an energy management system. Background Art

[0002] Traditional paper-based energy is based on the mechanism of ion-type batteries. Most of them use paper as the diaphragm of energy storage devices, so that particles are transmitted in the channels perpendicular to the paper, and form a sandwich structure with flexible electrodes, packaging materials, etc., which undoubtedly limits its permeability. Ion electronics energy, which uses the rapid transmission of ions in the nano-confined channels on the paper plane, realizes the efficient conversion of ion penetration energy to electrical energy and is a good energy storage unit. For ion electronics energy, constructing stable and breathable two-dimensional nano-confined channels on paper is the key to improving the power and energy density of ion electronics energy. However, due to the influence of cellulose functional groups on the surface of some paper substrates (such as hydroxyl and carboxyl groups on the surface of filter paper), whitening agents on the surface of paper substrates (such as calcium carbonate on the surface of A4 paper and photo paper) and the complex surface morphology of paper substrates, it is still a challenge to construct breathable two-dimensional nano-confined ion channels on paper substrates and use them in ion electronics energy systems. Summary of the invention

[0003] The present application discloses an ionic electronic power source and a preparation method and an energy management system thereof, which can construct a stable and breathable two-dimensional nanochannel on a paper substrate and can be used for an ionic electronic power source with high power density and energy density, simple process and low cost.

[0004] In order to achieve the above objectives, this application provides the following technical solutions:

[0005] In a first aspect, the present application provides an ionotronic power source, comprising a paper-based two-dimensional nanochannel;

[0006] The paper-based two-dimensional nanochannel comprises a paper base and a two-dimensional nanochannel layer disposed on at least one side of the paper base;

[0007] The two-dimensional nanochannel layer includes two-dimensional nanomaterials, and the mass fraction of the two-dimensional nanomaterials is 33%-98%;

[0008] The moisture permeability of the paper-based two-dimensional nanochannel is 500 gm -2 d -1 -750gm -2 d -1 .

[0009] The above iontronic power supply is constructed with a moisture permeability of 500gm -2 d -1 -750gm -2 d -1The paper-based two-dimensional nanochannel allows ions to be efficiently transmitted in the two-dimensional nanochannel layer, which is beneficial to improving the power and energy density of the ion electronics power supply. Specifically, the paper-based two-dimensional nanochannel includes a paper base and a two-dimensional nanochannel layer, wherein the two-dimensional nanochannel layer can be arranged on one side surface of the paper base, or can be arranged on both side surfaces of the paper base respectively. The two-dimensional nanochannel layer includes two-dimensional nanomaterials, which account for 33%-98% by mass. In the process of preparing the two-dimensional nanochannel layer, the proportion of two-dimensional nanomaterials is regulated according to the characteristics of the selected paper base itself, and then the matching degree of the two-dimensional nanochannel layer and the paper base can be regulated, so that the constructed two-dimensional nanochannel layer has good air permeability and stability. The humidity permeability of the paper-based two-dimensional nanochannel finally obtained (refers to the mass of water passing through the surface of the material per unit area per unit time) is 500gm -2 d -1 -750gm -2 d -1 , indicating that the paper-based two-dimensional nanochannel of the present application has good air permeability. When the paper-based two-dimensional nanochannel is applied to ion electronic power supply, ions can be smoothly transmitted within the planar nano-confinement of the two-dimensional nanochannel layer, which is conducive to improving the conversion efficiency of ion transmission energy to electrical energy, and the power density can reach 438.02mW·cm -3 .

[0010] In some embodiments, the paper base includes one or more of sulphate paper, kraft paper, A4 paper, filter paper and photo paper. By adjusting the proportion of two-dimensional nanomaterials in the two-dimensional nanochannel layer, a good match between the two-dimensional nanochannel layer and the selected paper base can be achieved, thereby improving the air permeability of the two-dimensional nanochannel layer and the stability on the paper base.

[0011] In some embodiments, the thickness of the two-dimensional nanochannel layer is 0.1 μm-1000 μm.

[0012] In some embodiments, the length of the two-dimensional nanochannel layer is 1 μm-1 m. The present application can improve the ion transmission efficiency by reasonably setting the thickness and length of the two-dimensional nanochannel layer, thereby improving the power and energy density of the ion electronics power supply.

[0013] In some embodiments, the ion electronics power supply further comprises a positive electrode sheet and a negative electrode sheet;

[0014] The positive electrode sheet is arranged at one end of the two-dimensional nanochannel layer, and the negative electrode sheet is arranged at the other end of the two-dimensional nanochannel layer;

[0015] The negative electrode sheet comprises a negative electrode active material layer and a negative electrode current collector, wherein the negative electrode active material layer is arranged between the two-dimensional nanochannel layer and the negative electrode current collector.

[0016] The present application prepares an ion electronic power supply by setting a positive electrode sheet and a negative electrode sheet at both ends of a two-dimensional nanochannel layer, so that ions in the ion electronic power supply can be transmitted through the two-dimensional nanochannel layer to achieve efficient conversion of ion transmission energy into electrical energy.

[0017] In a second aspect, the present application provides a method for preparing an ion electronics power supply, comprising:

[0018] Providing a paper base;

[0019] The two-dimensional nanochannel slurry is printed or coated on the paper base, and after drying, the paper-based two-dimensional nanochannel is obtained; the moisture permeability of the paper-based two-dimensional nanochannel is 500 gm -2 d -1 -750gm -2 d -1 ; The two-dimensional nanochannel slurry includes two-dimensional nanomaterials, surfactants and solvents, and the mass ratio of the two-dimensional nanomaterials, the surfactants and the solvent is 5-50:1-10:50-95.

[0020] The present application mixes a two-dimensional nanomaterial and a surfactant in a solvent to prepare a two-dimensional nanochannel slurry, and then prints or coats the two-dimensional nanochannel slurry on a paper base, and after drying, obtains a paper-based two-dimensional nanochannel. According to the characteristics of the selected paper base, the mass ratio of the two-dimensional nanomaterial, the surfactant, and the solvent needs to be adjusted so that the two-dimensional nanochannel slurry can be precisely printed or coated on the paper base, thereby improving the stability and air permeability of the paper-based two-dimensional nanochannel.

[0021] In some embodiments, in the two-dimensional nanochannel slurry, the concentration of the two-dimensional nanomaterial is 0.5 mg / mL-1000 mg / mL.

[0022] In some embodiments, in the two-dimensional nanochannel slurry, the concentration of the surfactant is 0.1 mg / mL-100 mg / mL.

[0023] In some embodiments, the preparation method further comprises:

[0024] Printing or coating the positive electrode slurry on the paper base and contacting it with one end of the two-dimensional nanochannel layer, and obtaining a positive electrode after drying;

[0025] Printing or coating a negative electrode active material on the paper base so as to contact the paper base with the other end of the two-dimensional nanochannel layer, and obtaining a negative electrode active material layer after drying;

[0026] The negative electrode current collector slurry is printed or coated on the paper base and is in contact with one end of the negative electrode active material layer away from the two-dimensional nanochannel layer, and the ion electronic power source is obtained after drying.

[0027] An ionic electronic power source is obtained by preparing a positive electrode sheet, a negative electrode active material layer and a negative electrode current collector at both ends of the two-dimensional nanochannel layer, so that ions in the negative electrode active material layer can be transmitted through the two-dimensional nanochannel layer to achieve efficient conversion of ion transmission energy into electrical energy.

[0028] In a third aspect, the present application provides an energy management system, comprising a friction nanogenerator and at least one iontronic power source as described in the first aspect;

[0029] The friction nanogenerator is electrically connected to the iontronic power supply.

[0030] The present application integrates a friction nanogenerator with at least one ionic electronic power source to obtain a paper-based energy management system, thereby realizing the parallel functions of energy capture and energy storage. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 A schematic diagram of the structure of an ion electronics power supply provided in an embodiment of the present application;

[0032] Figure 2 A schematic diagram of a process for preparing an ion electronics power supply provided in an embodiment of the present application;

[0033] Figure 3 A schematic diagram of a process for preparing an ion electronics power supply provided in an embodiment of the present application;

[0034] Figure 4 A schematic diagram of the structure of an energy management system provided in an embodiment of the present application;

[0035] Figure 5 A schematic diagram of the structure of a friction nanogenerator provided in an embodiment of the present application;

[0036] Figure 6 A scanning electron microscope image of graphene oxide provided in an embodiment of the present application;

[0037] Figure 7 A laser particle size test curve of graphene oxide provided in an embodiment of the present application;

[0038] Figure 8 A rheological property test curve of a two-dimensional nanochannel slurry provided in an embodiment of the present application;

[0039] Fig. 9 A photo of a precision test of printing a two-dimensional nanochannel slurry on different paper substrates provided in an embodiment of the present application;

[0040] Fig.10A scanning electron microscope image of a two-dimensional nanochannel slurry printed on a traditional plastic paper (left) and a sulfuric acid paper (right) provided in an embodiment of the present application;

[0041] Fig.11 A scanning electron microscope image of a paper-based two-dimensional nanochannel of a sulfuric acid paper provided in an embodiment of the present application;

[0042] Fig.12 A scanning electron microscope image of a bending test of a paper-based two-dimensional nanochannel of a sulfuric acid paper provided in an embodiment of the present application;

[0043] Fig.13 Photos of air permeability tests of sulfuric acid paper (left) and plastic paper (right) provided in the examples of the present application;

[0044] Fig.14 A scanning electron microscope image of silver nanoparticles provided in an embodiment of the present application;

[0045] Fig.15 A photo of an ion electronics energy source and an open circuit voltage test process provided in an embodiment of the present application;

[0046] Fig.16 The IV curve and power curve of an ion electronics power supply provided in an embodiment of the present application (left), and the discharge curve at 1 μA (right);

[0047] Fig.17 A photograph of a conductive layer (top) and a friction layer (bottom) of a triboelectric nanogenerator provided in an embodiment of the present application;

[0048] Fig.18 An output performance curve of a friction nanogenerator provided in an embodiment of the present application;

[0049] Fig.19 A photo of a paper-based energy management system provided in an embodiment of the present application;

[0050] Fig. 20 A discharge curve of an ion-electronic power supply at 1 μA after removing the friction nanogenerator from a paper-based energy management system provided in an embodiment of the present application;

[0051] Icons: 1. Paper base; 2. Two-dimensional nanochannel layer; 3. Positive electrode sheet; 4. Negative electrode sheet; 41. Negative electrode active material layer; 42. Negative electrode current collector; 100. Friction nanogenerator; 200. Ion electronics power supply; 300. Rectifier; 1001. Conductive layer; 1002. Friction layer; A. First conductive layer; B. Second conductive layer. DETAILED DESCRIPTION

[0052] First, let me introduce the application scenarios. With the rapid development of wearable devices and smart clothing, the demand for lightweight, flexible and efficient energy management systems is increasing. However, the existing energy management systems are bulky, heavy, lack flexibility and breathability, and are difficult to meet the needs of modern smart devices. In particular, when smart devices are used for a long time, their insufficient breathability will make users feel uncomfortable. Therefore, there is an urgent need for an innovative solution to overcome these technical difficulties.

[0053] Functionalized paper-based systems are naturally flexible and breathable, and are expected to be a low-cost solution. Using printing, writing, and through-hole technologies, functionalized paper-based systems can directly integrate electronic circuits and energy systems on an ultra-thin paper, achieving the parallel functions of energy storage and energy harvesting.

[0054] Traditional paper-based energy is based on the mechanism of ion batteries, and most of them use paper as the diaphragm of energy storage devices, allowing particles to be transmitted in channels vertical to the paper base and forming a sandwich structure with flexible electrodes, packaging materials, etc., which undoubtedly limits its air permeability.

[0055] Ion electronics energy, which utilizes the rapid transmission of ions in nano-confined channels on paper substrates, realizes the efficient conversion of ion penetration energy into electrical energy and is a good energy storage unit. For ion electronics energy, constructing stable and breathable two-dimensional nano-confined channels on paper substrates is the key to improving the power and energy density of ion electronics energy. However, due to the influence of cellulose functional groups on the surface of certain paper substrates (such as hydroxyl and carboxyl groups on the surface of filter paper), brighteners on the surface of paper substrates (such as calcium carbonate on the surface of A4 paper and photo paper), and the complex surface morphology of paper substrates, it is still a challenge to construct breathable two-dimensional nano-confined ion channels on paper substrates for ion electronics energy systems.

[0056] Based on the above problems, the embodiments of the present application provide an ionic electronic power supply, a preparation method thereof, and an energy management system, which can construct a stable and breathable two-dimensional nanochannel on a paper substrate, which can be used for an ionic electronic power supply for efficient energy storage, has high power and energy density, simple process, and low cost.

[0057] In a first aspect, an embodiment of the present application provides an ion electronics power supply. Figure 1 This is a schematic diagram of the structure of an ion electronics power supply provided in an embodiment of the present application. Figure 1 As shown, the ion electronics power source includes a paper-based two-dimensional nanochannel; the paper-based two-dimensional nanochannel includes a paper base 1 and a two-dimensional nanochannel layer 2 disposed on at least one side of the paper base 1; the two-dimensional nanochannel layer 2 includes a two-dimensional nanomaterial, and the mass fraction of the two-dimensional nanomaterial is 33%-98%; the humidity permeability of the paper-based two-dimensional nanochannel is 500gm -2 d -1-750gm -2 d -1 .

[0058] The above iontronic power supply is constructed with a moisture permeability of 500gm -2 d -1 -750gm -2 d -1 The paper-based two-dimensional nanochannel allows ions to be efficiently transmitted in the two-dimensional nanochannel layer 2, that is, a stable and breathable transmission channel is constructed for the ions, which is beneficial to improve the power and energy density of the ion electronics power supply. Specifically, the paper-based two-dimensional nanochannel includes a paper base 1 and a two-dimensional nanochannel layer 2, wherein the two-dimensional nanochannel layer 2 can be arranged on one side surface of the paper base 1, or can be arranged on both side surfaces of the paper base 1 respectively. The two-dimensional nanochannel layer 2 includes two-dimensional nanomaterials, which account for 33%-98% by mass. In the process of preparing the two-dimensional nanochannel layer 2, the proportion of two-dimensional nanomaterials is regulated according to the characteristics of the selected paper base itself, and then the matching degree of the two-dimensional nanochannel layer 2 and the paper base 1 can be regulated, so that the constructed two-dimensional nanochannel layer 2 has good air permeability and stability, and can allow ions to be transmitted in the planar two-dimensional nanochannel layer. The humidity permeability of the paper-based two-dimensional nanochannel finally obtained is 500gm -2 d -1 -750gm -2 d -1 , e.g. 500gm -2 d -1 , 550gm -2 d -1 , 600gm -2 d -1 、650gm -2 d -1 , 700gm -2 d -1 , 750gm -2 d -1 When the paper-based two-dimensional nanochannel is applied to ion electronic power source, ions can be smoothly transmitted in the planar nano-confinement of the two-dimensional nanochannel layer 2, which is beneficial to improve the conversion efficiency of ion transmission energy to electrical energy, and the power density can reach 438.02mW·cm -3 .

[0059] In some embodiments, reference Figure 1, the paper base 1 includes one or more of sulphate paper, kraft paper, A4 paper, filter paper and photo paper. By adjusting the proportion of two-dimensional nanomaterials in the two-dimensional nanochannel layer 2, a good match between the two-dimensional nanochannel layer 2 and the selected paper base 1 can be achieved to reduce the impact of the performance of the paper base 1 itself on the two-dimensional nanochannel layer 2, thereby improving the air permeability and stability of the two-dimensional nanochannel layer 2 on the paper base 1. For example, by adjusting the proportion of two-dimensional nanomaterials, the impact of cellulose functional groups (hydroxyl and carboxyl) on the surface of filter paper can be reduced, the impact of whitening agents (calcium carbonate) on the surfaces of A4 paper and photo paper can also be reduced, and the impact of the complex surface morphology of various paper bases 1 can also be reduced.

[0060] In some embodiments, reference Figure 1 , the thickness of the two-dimensional nanochannel layer 2 is 0.1 μm-1000 μm. Exemplarily, the thickness of the two-dimensional nanochannel layer 2 can be 0.1 μm, 0.2 μm, 0.5 μm, 1 μm, 2 μm, 5 μm, 10 μm, 20 μm, 50 μm, 100 μm, 120 μm, 150 μm, 200 μm, 300 μm, 400 μm, 500 μm, 600 μm, 700 μm, 800 μm, 900 μm, 1000 μm, etc., and the specific thickness value is not limited.

[0061] In some embodiments, reference Figure 1 , the length of the two-dimensional nanochannel layer 2 is 1 μm-1m. Exemplarily, the length of the two-dimensional nanochannel layer 2 can be 1 μm, 2 μm, 5 μm, 10 μm, 100 μm, 200 μm, 500 μm, 1000 μm, 2000 μm, 5000 μm, 0.01 m, 0.02 m, 0.05 m, 0.08 m, 0.1 m, 0.2 m, 0.5 m, 0.7 m, 0.9 m, 1 m. The specific thickness value is not limited.

[0062] The present application satisfies the air permeability requirements by reasonably setting the thickness and length of the two-dimensional nanochannel layer 2, thereby improving the transmission efficiency of ions in the ion electronics power supply, thereby improving the power and energy density of the ion electronics power supply.

[0063] In some embodiments, reference Figure 1 The ionic electronic power supply also includes a positive electrode sheet 3 and a negative electrode sheet 4; the positive electrode sheet 3 is arranged at one end of the two-dimensional nanochannel layer 2, and the negative electrode sheet 4 is arranged at the other end of the two-dimensional nanochannel layer 2; the negative electrode sheet 4 includes a negative electrode active material layer 41 and a negative electrode current collector 42, and the negative electrode active material layer 41 is arranged between the two-dimensional nanochannel layer 2 and the negative electrode current collector 42.

[0064] In the embodiment of the present application, a positive electrode sheet 3 and a negative electrode sheet 4 are arranged at both ends of the two-dimensional nanochannel layer 2 to obtain an ion electronic power supply. During the use of the ion electronic power supply, ions in the negative electrode active material layer 41 can be transmitted to the positive electrode through the planar nano-confinement of the two-dimensional nanochannel layer 2, so as to realize the efficient conversion of ion transmission energy into electrical energy, and the power density can reach 438.02mW·cm -3 .

[0065] In a second aspect, the present application provides a method for preparing an ion electronics power source. Figure 2 The following is a flow chart of a method for preparing an ion electronic power supply provided in an embodiment of the present application. Figure 2 As shown, the preparation method comprises the following steps:

[0066] S201, providing a paper base;

[0067] S202, printing or coating the two-dimensional nanochannel slurry onto a paper base, and drying to obtain a paper-based two-dimensional nanochannel; the humidity permeability of the paper-based two-dimensional nanochannel is 500 gm -2 d -1 -750gm -2 d -1 The two-dimensional nanochannel slurry includes two-dimensional nanomaterials, surfactants and solvents, and the mass ratio of the two-dimensional nanomaterials, surfactants and solvents is 5-50:1-10:50-95.

[0068] In the present embodiment, the two-dimensional nanomaterial and the surfactant are first mixed in a solvent to prepare a two-dimensional nanochannel slurry, and then the two-dimensional nanochannel slurry is printed or coated on a selected paper base, and dried to obtain a paper-based two-dimensional nanochannel. The humidity permeability of the paper-based two-dimensional nanochannel in the present embodiment is 500 gm -2 d -1 -750gm -2 d -1 , e.g. 500gm - 2 d -1 , 550gm -2 d -1 , 600gm -2 d -1 、650gm -2 d -1 , 700gm -2 d -1 , 750gm -2 d -1Etc., indicating that the paper-based two-dimensional nanochannel has good air permeability. According to the characteristics of the selected paper base itself, it is necessary to adjust the mass ratio of the two-dimensional nanomaterial, surfactant and solvent, and then adjust the viscosity and rheological properties of the two-dimensional nanochannel slurry, so that the two-dimensional nanochannel slurry matches the surface properties of the selected paper base, so that the two-dimensional nanochannel slurry can be precisely printed or coated on the paper base, and the stability and air permeability of the paper-based two-dimensional nanochannel are improved. It should be noted that after the two-dimensional nanochannel slurry is dried, the solvent is completely evaporated, and the two-dimensional nanochannel layer only includes two-dimensional nanomaterials and surfactants.

[0069] In some embodiments, in the two-dimensional nanochannel slurry, the concentration of the two-dimensional nanomaterial is 0.5mg / mL-1000mg / mL. Exemplary, in the two-dimensional nanochannel slurry, the concentration of the two-dimensional nanomaterial can be 0.5mg / mL, 1mg / mL, 2mg / mL, 5mg / mL, 10mg / mL, 15mg / mL, 20mg / mL, 30mg / mL, 50mg / mL, 65mg / mL, 80mg / mL, 120mg / mL, 150mg / mL, 300mg / mL, 460mg / mL, 500mg / mL, 600mg / mL, 700mg / mL, 800mg / mL, 900mg / mL, 1000mg / mL, etc. The two-dimensional nanomaterial includes one or more of nanostructured carbon, nanostructured silicon, graphene, graphene oxide, reduced graphene oxide, molybdenum disulfide, boron nitride, carbon nitride, covalent organic framework material, protein nanowire, cellulose, silk, montmorillonite and nanofiber composite material. The average particle size of the two-dimensional nanomaterial is 0.1 μm-1000 μm. Exemplarily, the average particle size of the two-dimensional nanomaterial can be 0.1 μm, 0.2 μm, 0.5 μm, 1 μm, 2 μm, 5 μm, 10 μm, 15 μm, 20 μm, 30 μm, 50 μm, 100 μm, 150 μm, 200 μm, 250 μm, 300 μm, 400 μm, 500 μm, 600 μm, 700 μm, 800 μm, 900 μm, 1000 μm, etc. The concentration, material type and average particle size of the specific two-dimensional nanomaterial need to be set according to the characteristics of the selected paper base.

[0070] In some embodiments, in the two-dimensional nanochannel slurry, the concentration of the surfactant is 0.1mg / mL-100mg / mL. Exemplarily, in the two-dimensional nanochannel slurry, the concentration of the surfactant can be 0.1mg / mL, 0.2mg / mL, 0.5mg / mL, 1mg / mL, 2mg / mL, 5mg / mL, 10mg / mL, 15mg / mL, 20mg / mL, 30mg / mL, 35mg / mL, 40mg / mL, 50mg / mL, 60mg / mL, 75mg / mL, 90mg / mL, 100mg / mL, etc., and the specific concentration needs to be set according to the characteristics of the selected paper base to adjust the viscosity, fluidity, leveling and other properties of the slurry. In some embodiments, the surfactant includes one or more of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, fatty alcohol polyoxyethylene ether and Nafion, and the specific material type needs to be set according to the characteristics of the selected paper base.

[0071] In some embodiments, the solvent includes one or more of deionized water, low-toxic organic solvents, ethanol, and ester compounds.

[0072] Figure 3 A schematic diagram of a method for preparing an ion electronic power supply provided in an embodiment of the present application. In some embodiments, Figure 3 As shown, the preparation method also includes the following steps:

[0073] S301, printing or coating a positive electrode slurry on a paper substrate and contacting the positive electrode slurry with one end of the two-dimensional nanochannel layer, and drying the positive electrode;

[0074] S302, printing or coating the negative electrode active material on the paper base and contacting it with the other end of the two-dimensional nanochannel layer, and obtaining the negative electrode active material layer after drying;

[0075] S303, printing or coating the negative electrode current collector slurry on a paper substrate, and contacting the negative electrode active material layer with one end away from the two-dimensional nanochannel layer, and obtaining an ion electronic power source after drying.

[0076] An ionic electronic power source is prepared by printing or coating a positive electrode sheet and a negative electrode sheet on a paper base, and drying the sheet. Specifically, the positive electrode sheet includes a positive electrode current collector, and the positive electrode current collector slurry is printed or coated on the paper base and in contact with one end of the two-dimensional nanochannel layer, and the positive electrode is obtained after drying. The negative electrode sheet includes a negative electrode active material layer and a negative electrode current collector, and the negative electrode active material is printed or coated on the paper base, and in contact with the other end of the two-dimensional nanochannel layer, and the negative electrode active material layer is obtained after drying; the negative electrode current collector slurry is printed or coated on the paper base, and in contact with one end of the negative electrode active material layer away from the two-dimensional nanochannel layer, and the ionic electronic power source is obtained after drying. The ionic electronic power source of the present application can transfer ions in the negative electrode active material layer from the negative electrode to the positive electrode with the help of the two-dimensional nanochannel layer, so as to achieve efficient conversion of ion transmission energy into electrical energy.

[0077] The preparation method of the positive electrode sheet slurry in the embodiment of the present application includes: preparing it through positive electrode collector powder. The positive electrode collector powder includes one or more of metal element powder, conductive carbon powder and conductive organic powder. The average particle size of the positive electrode collector powder is 0.1μm-1000μm. Exemplarily, the average particle size of the positive electrode collector powder can be 0.1μm, 0.2μm, 0.5μm, 1μm, 2μm, 5μm, 10μm, 15μm, 20μm, 30μm, 50μm, 100μm, 150μm, 200μm, 250μm, 300μm, 400μm, 500μm, 600μm, 700μm, 800μm, 900μm, 1000μm, etc. The specific material type and average particle size of the positive electrode collector need to be set according to the characteristics of the selected paper base.

[0078] The negative electrode active material includes one or more of reduced graphene oxide, metal elements, hydroxides, low-valent metal ions and their compounds, fluorides, chlorides, bromides, iodides, low-valent oxides, non-metal hydrides, low-valent salts, organic reducing agents, ferrocene, high-valent compounds containing variable-valence elements, and organic oxides. The average particle size of the negative electrode active material is 1 μm-1000 μm. Exemplarily, the average particle size of the negative electrode active material can be 1 μm, 2 μm, 5 μm, 10 μm, 15 μm, 20 μm, 30 μm, 50 μm, 100 μm, 150 μm, 200 μm, 250 μm, 300 μm, 400 μm, 500 μm, 600 μm, 700 μm, 800 μm, 900 μm, 1000 μm, etc. The specific material type and average particle size of the negative electrode active material need to be set according to the characteristics of the selected paper base.

[0079] The preparation method of the negative electrode current collector slurry includes: preparing it by negative electrode current collector powder. The negative electrode current collector powder includes one or more of metal element powder, conductive carbon powder and conductive organic powder. The average particle size of the negative electrode current collector powder is 1μm-1000μm. Exemplarily, the average particle size of the negative electrode current collector powder can be 1μm, 2μm, 5μm, 10μm, 15μm, 20μm, 30μm, 50μm, 100μm, 150μm, 200μm, 250μm, 300μm, 400μm, 500μm, 600μm, 700μm, 800μm, 900μm, 1000μm, etc. The specific material type and average particle size of the negative electrode current collector need to be set according to the characteristics of the selected paper base.

[0080] In a third aspect, an embodiment of the present application provides an energy management system. Figure 4 This is a schematic diagram of the structure of an energy management system provided in an embodiment of the present application. Figure 4 As shown, the energy management system includes a triboelectric nanogenerator 100 and at least one ionoelectronic power source 200 as in the first aspect; the triboelectric nanogenerator 100 is electrically connected to the ionoelectronic power source 200. The present application constructs a novel paper-based energy management system by combining the ionoelectronic power source 200 with the triboelectric nanogenerator 100, thereby improving the energy density of the ionoelectronic power source.

[0081] In one possible implementation, refer to Figure 4 The friction nanogenerator 100 includes a conductive layer 1001 and a friction layer 1002. When the conductive layer 1001 and the friction layer 1002 are in contact, electric charges are generated, and the electric charges are collected in the conductive layer 1001, thereby generating an alternating electronic current. The electronic current is transmitted along the wire to the rectifier 300, and the rectifier 300 converts the alternating electronic current into a direct current electronic current, and then the direct current electronic current continues to be transmitted along the wire to the ion electronic power supply 200. The electronic current is converted into an ionic current at the interface layer between the negative electrode current collector and the negative electrode active material layer of the ion electronic power supply 200, that is, the ions in the negative electrode active material layer are transmitted to the positive electrode current collector through the two-dimensional nanochannel layer, thereby realizing the charging of the ion electronic power supply 200. The present application integrates the friction nanogenerator 100 with at least one ion electronic power supply 200 to obtain a paper-based energy management system, which realizes the parallel functions of energy capture and energy storage. When the friction nanogenerator 100 is removed, the ion electronic power supply 200 can be discharged. The integrated method of the energy management system of the present application can extend the discharge time of the ion electronics power supply 200, that is, extend the use time.

[0082] In some embodiments, the conductive layer 1001 may be made of graphite, and the thickness of the conductive layer 1001 is 0.1 μm-100 μm. For example, the thickness of the conductive layer 1001 may be 0.1 μm, 0.2 μm, 0.5 μm, 1 μm, 2 μm, 5 μm, 10 μm, 15 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, etc., and the specific thickness is not limited. The friction layer 1002 may be made of polytetrafluoroethylene. The thickness of the friction layer 1002 is 10μm-1000μm. Exemplarily, the thickness of the friction layer 1002 can be 10μm, 15μm, 20μm, 30μm, 50μm, 100μm, 150μm, 200μm, 250μm, 300μm, 400μm, 500μm, 600μm, 700μm, 800μm, 900μm, 1000μm, etc., and the specific thickness is not limited.

[0083] Figure 5 A schematic diagram of the structure of a friction nanogenerator provided in an embodiment of the present application. In some embodiments, Figure 5 As shown, the conductive layer 1001 of the triboelectric nanogenerator includes a first conductive layer A and a second conductive layer B, and the friction layer 1002 is disposed between the first conductive layer A and the second conductive layer B; the first conductive layer A is electrically connected to the ion electronic power source 200, and the second conductive layer B is electrically connected to the ion electronic power source 200. When the first conductive layer A and the second conductive layer B are in contact with the friction layer 1002, electric charges are generated, and the electric charges are collected in the first conductive layer A and the second conductive layer B, thereby generating an alternating electronic current. Figure 4 , the electronic current is transmitted along the wire to the rectifier 300, and the rectifier 300 converts the alternating electronic current into a direct current electronic current, and then the direct current electronic current continues to be transmitted along the wire to the ion electronic power supply 200. The electronic current is converted into an ion current at the interface layer between the negative electrode current collector and the negative electrode active material layer of the ion electronic power supply 200, that is, the ions in the negative electrode active material layer are transmitted to the positive electrode current collector through the two-dimensional nanochannel layer, thereby realizing the charging of the ion electronic power supply 200.

[0084] In some embodiments, reference Figure 4 The energy management system includes a plurality of ion electronic power supplies 200, which are connected in series and parallel. Arranging a plurality of ion electronic power supplies 200 can realize the conversion of more electronic currents into ion currents, and improve the energy density of the energy management system.

[0085] In order to further illustrate the present application, an ionic electronic power supply, a preparation method thereof, and an energy management system provided by the present application are described in detail below in combination with specific embodiments.

[0086] Example 1

[0087] This embodiment is a method for preparing an energy management system, which specifically includes the following steps:

[0088] (1) A two-dimensional nanochannel slurry is prepared, wherein the two-dimensional nanomaterial is graphene oxide, the surfactant is Nafion, and the solvent is deionized water. The concentration of graphene oxide is 10 mg / mL, and the concentration of Nafion is 1 mg / mL.

[0089] (2) Printing the two-dimensional nanochannel slurry on various paper substrates by extrusion printing, the thickness of the two-dimensional nanochannel layer is 1 μm-2 μm, and after drying, the paper-based two-dimensional nanochannel is obtained.

[0090] (3) Select a two-dimensional nanochannel on a sulfuric acid paper, print the positive electrode current collector slurry (nanosilver paste) on the paper base, and contact it with one end of the paper base two-dimensional nanochannel. Print the negative electrode active material (reduced graphene oxide containing lithium iodide) on the paper base, and contact it with the other end of the paper base two-dimensional nanochannel. Print the negative electrode current collector slurry (nanosilver paste) on the paper base, and contact it with the end of the negative electrode active material away from the two-dimensional nanochannel layer, and obtain an ionic electronic power supply after drying.

[0091] (4) Graphite and polytetrafluoroethylene are written or covered on two arbitrary paper substrates, respectively, wherein the thickness of the graphite coating is 0.1 μm-100 μm, and the thickness of the polytetrafluoroethylene is 10 μm-1000 μm. The graphite and polytetrafluoroethylene are placed in relative contact and dried to obtain a friction nanogenerator.

[0092] (5) Integrate the friction nanogenerator with the ionic electronic power source in step (3) through wires to ultimately obtain a paper-based energy management system.

[0093] Figure 6 This is a scanning electron microscope image of graphene oxide provided in Example 1 of the present application.

[0094] Figure 7 This is a laser particle size test curve of graphene oxide provided in Example 1 of the present application. Figure 7 As shown, the particle size of graphene oxide powder is 0.1 μm-10 μm.

[0095] Figure 8 This is a rheological property test curve of a two-dimensional nanochannel slurry provided in Example 1 of the present application. Figure 8 As shown, the storage modulus (G′) and loss modulus (G″) vary with frequency, and the two-dimensional nanochannel slurry exhibits good rheological properties. In the range of 0.1-100 Hz, G′ is always better than G″, showing typical elastic solid properties and excellent stability.

[0096] Fig. 9 This is a photo of a precision test of printing a two-dimensional nanochannel slurry on different paper substrates provided in Example 1 of the present application. Fig.10 This is a scanning electron microscope image of a two-dimensional nanochannel slurry printed on traditional plastic paper (left) and sulfuric acid paper (right) provided in Example 1 of the present application. Fig. 9 and Fig.10 As shown, the printing accuracy of the two-dimensional nanochannel slurry is good.

[0097] Fig.11 This is a scanning electron microscope image of a paper-based two-dimensional nanochannel of the sulfate paper provided in Example 1 of the present application. Fig.12 This is a scanning electron microscope image of a bending test of a two-dimensional nanochannel of a sulfuric acid paper provided in Example 1 of the present application. Fig.12 As shown, the two-dimensional nanochannel still maintains good adhesion ability under bending conditions.

[0098] Fig.13 The following are photos of the air permeability test of a sulfuric acid paper (left) and a plastic paper (right) provided in Example 1 of the present application. Fig.13 As shown, a simple cupping test was used. Two glasses with a diameter of 10 cm were stacked with the sample to form a sandwich structure. The lower glass contained 95°C hot water. After two hours, water mist could be observed in the top glass of the sulfuric acid paper, while there was no obvious change in the top glass of the plastic paper. After 2 hours of humidity penetration, the mass change of the top glass was weighed to be 0.34g, and the humidity permeability (permeation mass / (permeation area*time)) was calculated to be 519.75gm -2 d -1 , which is comparable to 785g m -2 d -1 This shows that the sulfuric acid paper has good air permeability.

[0099] Fig.14 This is a scanning electron microscope image of silver nanoparticles provided in Example 1 of the present application. The average particle size of the silver nanoparticles is about 2 μm.

[0100] Fig.15 Photos of an ionic electronic energy source and open circuit voltage test process provided in Example 1 of the present application. Fig.16 The IV curve and power curve (left) of an ion electronics power supply provided in Example 1 of the present application, and the discharge curve at 1 μA (right). Fig.16 As shown in Figure 2, the paper-based iontronic power supply can maintain an open circuit voltage of about 0.95 V, a short circuit current of about 700 μA, and a power density of about 438.02 mW·cm-3 , and continued to discharge at 1uA for 14h.

[0101] Fig.17 This is a photograph of the conductive layer (top) and friction layer (bottom) of a friction nanogenerator provided in Example 1 of the present application. Fig.18 The output performance curves of a friction nanogenerator provided in Example 1 of the present application are: charge (left), open circuit voltage (middle), and short circuit current (right).

[0102] Fig.19 This is a photo of a paper-based energy management system provided in Example 1 of the present application. Fig. 20 The discharge curve of the iontronic power supply at 1 μA after the friction nanogenerator is removed from a paper-based energy management system provided in Example 1 of the present application. Fig. 20 As shown, after combining with a friction nanogenerator, the discharge time of the iontronic power supply can be extended to more than 20 hours.

[0103] In summary, the breathable, ultra-thin energy management system based on paper-based two-dimensional nanochannels provided in this application can realize the parallel functions of energy storage and energy capture, and has high-efficiency performance and broad application prospects. It is expected to become the energy source for the next generation of self-driven sensing and wearable smart devices. It is simple to prepare and low-cost.

[0104] Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application. In the description of the embodiments of this application, unless otherwise specified, " / " means or, for example, A / B can mean A or B; "and / or" in the text is only a description of the association relationship of associated objects, indicating that there can be three relationships, for example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. In addition, in the description of the embodiments of this application, "multiple" means two or more than two.

[0105] The terms "first" and "second" are used for descriptive purposes only and should not be understood as suggesting or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the embodiments of the present application, unless otherwise specified, "multiple" means two or more.

[0106] Obviously, those skilled in the art can make various changes and modifications to the present application without departing from the spirit and scope of the present application. Thus, if these modifications and variations of the present application fall within the scope of the claims of the present application and their equivalents, the present application is also intended to include these modifications and variations.

Claims

1. An ion electronics power supply, characterized in that: Includes paper-based two-dimensional nanochannels; The paper-based two-dimensional nanochannel comprises a paper base and a two-dimensional nanochannel layer disposed on at least one side of the paper base; The two-dimensional nanochannel layer includes two-dimensional nanomaterials, and the mass fraction of the two-dimensional nanomaterials is 33%-98%; The moisture permeability of the paper-based two-dimensional nanochannel is 500 gm -2 d -1 -750gm -2 d -1 .

2. The iontronic power supply according to claim 1, characterized in that: The paper base includes one or more of sulphate paper, kraft paper, A4 paper, filter paper and photographic paper.

3. The iontronic power supply according to claim 1, characterized in that: The thickness of the two-dimensional nanochannel layer is 0.1 μm-1000 μm.

4. The iontronic power supply according to claim 1, characterized in that: The length of the two-dimensional nanochannel layer is 1 μm-1 m.

5. The iontronic power supply according to claim 1, characterized in that: The ion electronics power supply also includes a positive electrode sheet and a negative electrode sheet; The positive electrode sheet is arranged at one end of the two-dimensional nanochannel layer, and the negative electrode sheet is arranged at the other end of the two-dimensional nanochannel layer; The negative electrode sheet comprises a negative electrode active material layer and a negative electrode current collector, wherein the negative electrode active material layer is arranged between the two-dimensional nanochannel layer and the negative electrode current collector.

6. A method for preparing an ion electronic power source, characterized in that: include: Providing a paper base; The two-dimensional nanochannel layer slurry is printed or coated on the paper base, and after drying, the paper-based two-dimensional nanochannel is obtained; the moisture permeability of the paper-based two-dimensional nanochannel is 500gm -2 d -1 -750gm -2 d -1 ; The two-dimensional nanochannel layer slurry includes two-dimensional nanomaterials, surfactants and solvents, and the mass ratio of the two-dimensional nanomaterials, the surfactants and the solvent is 5-50:1-10:50-95.

7. The preparation method according to claim 6, characterized in that: In the two-dimensional nanochannel layer slurry, the concentration of the two-dimensional nanomaterial is 0.5 mg / mL-1000 mg / mL.

8. The preparation method according to claim 6, characterized in that: In the two-dimensional nanochannel layer slurry, the concentration of the surfactant is 0.1 mg / mL-100 mg / mL.

9. The preparation method according to claim 6, characterized in that: The preparation method further comprises: Printing or coating the positive electrode slurry on the paper base and contacting it with one end of the two-dimensional nanochannel layer, and obtaining a positive electrode after drying; Printing or coating a negative electrode active material on the paper base so as to contact the paper base with the other end of the two-dimensional nanochannel layer, and obtaining a negative electrode active material layer after drying; The negative electrode current collector slurry is printed or coated on the paper base and is in contact with one end of the negative electrode active material layer away from the two-dimensional nanochannel layer, and the ion electronic power source is obtained after drying.

10. An energy management system, characterized in that: Comprising a triboelectric nanogenerator and at least one ionotronic power source as claimed in any one of claims 1 to 5; The friction nanogenerator is electrically connected to the iontronic power supply.