Lead-free perovskite hemispherical photoelectric detector, preparation method and application of lead-free perovskite hemispherical photoelectric detector in single-pixel lens-free color imaging
Through the design of lead-free perovskite hemispherical photodetector, the problem of poor imaging quality of the photodetector in complex environments is solved, efficient color imaging is achieved, and stability is maintained under high temperature conditions, avoiding lead pollution and Costs increase.
Patent Information
- Application Number
- CN202411018614.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-29
AI Technical Summary
Existing photodetectors have poor imaging quality in complex environments, especially in high temperature and low light conditions, and traditional plane detectors have limitations in wide angle detection and optical signal collection efficiency, and the toxicity of lead-containing materials limits their application. .
The lead-free perovskite hemispherical photodetector is adopted, and the structure is composed of a chromium electrode layer, an electron transport layer, a perovskite layer, a hole transport layer and a metal electrode layer. It is prepared by spraying method, using CsBi3I10 and guanidine thiocyanate material. Achieve efficient color imaging.
Achieve high-quality and high-resolution lens-free color imaging in complex environments, improving the efficiency of light signal collection, avoiding lead contamination, and maintaining stability under high temperature conditions, reducing imaging costs.
Smart Images

Figure CN118946223A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of image processing, and in particular relates to a lead-free perovskite hemispherical photodetector, a preparation method and application thereof in single-pixel lens-free color imaging. Background Art
[0002] With the rapid development of the Internet of Things and artificial intelligence technologies, the way information is acquired and processed is undergoing profound changes. In this context, optical information processing technology, especially photodetector technology, has become particularly important due to its wide application in optical imaging, biological detection, optical communications, and military security. Photodetectors can convert optical signals into electrical signals and are the primary link in information acquisition. Their performance directly affects the accuracy and efficiency of subsequent information processing.
[0003] Traditional optical imaging technology relies on complex filter systems and multi-pixel arrays. This complexity not only increases the cost and maintenance difficulty of the system, but also limits its flexibility and efficiency in specific application scenarios. In particular, in applications that require fast response and high-resolution imaging, such as nighttime monitoring and biomedical imaging, existing technologies are difficult to meet the requirements. In addition, the integration of multi-pixel arrays also increases the size and energy consumption of the system, which is not conducive to its application in portable devices.
[0004] The performance of existing photodetectors often suffers significant effects in extreme environments such as low light and high temperature. In particular, the imaging quality of silicon photomultipliers (SiPMs) can degrade dramatically under these harsh conditions, which greatly limits their potential for use in a wider range of application scenarios. The main reason is that at high temperatures, the thermal noise of semiconductor materials increases significantly. This increase in noise not only leads to an increase in the noise of the device itself, but also causes fluctuations in the dark current. These factors work together to ultimately affect the clarity and reliability of imaging. Therefore, improving the performance of photodetectors in complex environments has become a technical problem that needs to be solved urgently to ensure that they can operate stably and reliably under various conditions.
[0005] In recent years, perovskite photodetectors have attracted much attention due to their excellent performance. These detectors not only have the characteristics of high sensitivity, wide spectral response range, fast response rate, low noise, but also have the advantages of simple preparation process, low cost, strong environmental adaptability, scalability and versatility. These characteristics make perovskite photodetectors show great application potential in the field of photoelectric imaging. However, many high-performance photodetectors currently rely on lead-containing perovskite materials. Although these materials have excellent photoelectric performance, the toxicity of lead limits their use in certain application scenarios. In addition, traditional planar photodetectors also have certain limitations in wide-angle detection and light signal collection efficiency. When receiving scattered light, the detector with a planar structure is limited by its receiving area and angle, and it is difficult to effectively capture light signals from different directions, thereby reducing the collection efficiency of light signals. In view of this, it is particularly urgent to develop a new type of lead-free perovskite hemispherical photodetector. This detector can achieve color imaging in complex environments, which not only solves the problem of lead pollution, but also improves the collection efficiency of light signals and broadens the application range of photodetectors. Summary of the invention
[0006] In view of the above problems and shortcomings, the present invention provides a lead-free perovskite hemispherical photodetector, a preparation method and its application in single-pixel lensless color imaging. The present invention breaks through the limitations of existing photodetectors in imaging technology and provides a solution for high-quality, high-resolution lensless color imaging in complex environments.
[0007] The present invention provides a lead-free perovskite hemispherical photodetector, which is composed of a chromium electrode layer, an electron transport layer, a perovskite layer, a hole transport layer and a metal electrode layer from the inside to the outside on the spherical surface of a hemispherical transparent substrate (such as glass);
[0008] The electron transport layer material is tin dioxide;
[0009] The perovskite layer material is CsBi containing guanidine thiocyanate. 3 I 10 ;
[0010] The hole transport layer material is poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine];
[0011] The metal electrode layer materials are chromium and gold.
[0012] Preferably, the thickness ratio of the chromium electrode layer, the electron transport layer, the perovskite layer, the hole transport layer and the metal electrode layer is 100-200 nm: 100-200 nm: 1000-1500 nm: 25-30 nm: 10-20 nm.
[0013] The present invention also provides a method for preparing the lead-free perovskite hemispherical photodetector, the steps of which are as follows:
[0014] (1) A chromium electrode layer is deposited by vacuum thermal evaporation on the spherical surface of a hemispherical glass substrate that has been treated with ultraviolet ozone for 15 to 30 minutes. The rate of vacuum thermal evaporation deposition is
[0015] (2) treating the hemispherical glass substrate obtained in step (1) with ultraviolet ozone for 15 to 30 minutes, and then transferring it to a plasma treatment chamber for treatment for 3 to 8 minutes; heating the treated substrate to 90 to 110° C., and then spraying an electron transport layer solution on the surface of the chromium electrode layer, and annealing at 140 to 160° C. for 20 to 40 minutes after the spraying, to obtain an electron transport layer on the surface of the chromium electrode layer; the electron transport layer solution is a tin dioxide aqueous solution with a concentration of 1.0 to 2.0 wt %;
[0016] (3) heating the hemispherical glass substrate obtained in step (2) to 90-110° C., and then spraying a perovskite precursor solution on the surface of the electron transport layer. After spraying, annealing is performed at 115-135° C. for 20-40 minutes to obtain a perovskite layer on the surface of the electron transport layer; the perovskite precursor solution is CsBi 3 I 10 An aqueous solution mixed with guanidine thiocyanate, CsBi 3 I 10 The concentration of is 0.2~0.4mol / L, and the concentration of guanidine thiocyanate is 0.5~3mol%;
[0017] (4) heating the hemispherical glass substrate obtained in step (3) to 80-100° C., and then spraying a hole transport layer solution on the surface of the perovskite layer. After spraying, annealing is performed at 100-120° C. for 8-15 minutes to obtain a hole transport layer on the surface of the perovskite layer; the hole transport layer solution is a toluene solution of poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine], and the concentration is 0.3-0.8 mg / mL;
[0018] (5) depositing a metal electrode layer by vacuum thermal evaporation on the surface of the hole transport layer obtained in step (4), thereby obtaining the lead-free perovskite hemispherical photodetector; the thermal evaporation deposition rate of the metal electrode layer is The metal electrode materials are chromium and gold.
[0019] The spraying equipment described in step (2) to step (4) is a spray gun, the nozzle diameter of the spray gun is 0.2 mm, the pressure of the spray gun is 1 to 1.1 bar, and the spraying distance is 3 to 4 cm.
[0020] The present invention also provides a process for color imaging of the lead-free perovskite hemispherical photodetector. A colored Fourier base pattern is generated by using a digital projector and the target imaging object is illuminated. The colored Fourier base pattern is generated by a computer, and the projector is controlled to project the pattern onto the target object. The reflected light obtained by the object under the illumination of the structured light pattern is collected by the perovskite hemispherical photodetector and converted into an electrical signal. The amplified electrical signal is collected by a power meter as a digital signal and transmitted to a computer for numerical calculation.
[0021] The perovskite obtained by the present invention has lead-free and excellent stability, and has outstanding charge carrier transmission ability, high collection efficiency, and strong weak light sensing ability. The present invention uses perovskite for color imaging, directly converts optical signals into electrical signals, has high sensitivity, and exhibits excellent performance with a linear dynamic response range of 146dB, and also has advantages such as uniform response ability and uniform thickness. In addition, the halide perovskite used in the present invention has low cost, short preparation time, and does not contain the toxic element lead, which increases the application range of the perovskite detector and reduces the manufacturing cost and time cost of the perovskite detector.
[0022] The lead-free perovskite hemispherical detector described in the present invention can maintain excellent stability in complex environments, such as high temperature conditions.
[0023] The present invention utilizes semiconductor materials to perform single-pixel lens-free color imaging, avoiding the complex pixel array structure and multiple lens devices required by common imaging methods, and greatly reducing the imaging cost.
[0024] The invention obtains a perovskite layer with large grains and uniform thickness by spraying, so that the hemispherical photodetector has good stability and excellent uniformity. The preparation method provided by the invention has simple steps, high efficiency and time saving, good operability, and has the prospect of large-scale production.
[0025] The present invention also provides a method for lensless hemispherical color imaging. The core part of the imaging scheme provided by the present invention is a hemispherical perovskite photodetector. The hemispherical photodetector of the present invention is a single-pixel photodetector, which is responsible for receiving diffusely reflected light signals and converting them into readable electrical signals. The present invention uses a Fourier basis combined with a Bayer template to obtain a colored Fourier basis pattern. The computer-generated colored Fourier basis pattern is projected onto the surface of the object to be imaged using a projector, and a data acquisition device is used to record the current value converted from the light intensity of the diffusely reflected light of the imaging object. By calculating the current value obtained by the perovskite hemispherical photodetector, the Fourier coefficients of the target object image can be obtained. Then, using the inverse Fourier transform, these spectral coefficients can be converted back to the spatial domain, thereby reconstructing the grayscale image of the object. Finally, using the traditional de-mosaicing algorithm for color restoration in color imaging, the color image of the object is reconstructed from the grayscale image, thereby realizing the application of the lead-free perovskite hemispherical photodetector in single-pixel lensless color imaging.
[0026] Therefore, the present invention applies lead-free perovskite to perovskite single-pixel color imaging, fully utilizes the performance of perovskite, and produces a high-performance single-pixel perovskite hemispherical photodetector capable of lens-free color imaging.
[0027] The perovskite hemispherical photodetector provided by the present invention is sensitive to slight changes in light and has excellent weak light imaging capabilities. The perovskite hemispherical photodetector provided by the present invention has uniform thickness, uniform response capability, high linearity, and good stability, so that the instrument provided by the present invention can accurately capture and represent the current values of different Fourier bases, which is crucial for color imaging.
[0028] The perovskite hemispherical photodetector provided by the present invention can receive diffusely reflected light at different angles and has excellent imaging capabilities at multiple angles. The color imaging effect of the perovskite hemispherical photodetector of the present invention is significantly improved compared with the planar photodetector at different angles.
[0029] The perovskite hemispherical photodetector of the present invention can maintain good photoelectric efficiency at high temperatures, and the current can maintain good stability at 100°C. It can achieve color imaging at 25°C to 100°C, and the imaging effect at high temperatures is better than that of traditional silicon photomultiplier tubes. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0031] Figure 1 This is a schematic diagram of the structure of the perovskite hemispherical photodetector prepared in Example 1 of the present invention;
[0032] Figure 2 A schematic diagram of color imaging performed by the perovskite hemispherical photodetector prepared in Example 1 of the present invention;
[0033] Figure 3 XRD spectra of the perovskite layers prepared in Examples 1 to 4 of the present invention;
[0034] Figure 4 This is a cross-sectional SEM image of the perovskite layer of the perovskite hemispherical photodetector prepared in Example 1 of the present invention;
[0035] Figure 5 This is a linear dynamic diagram of the perovskite photodetector prepared in Example 1 of the present invention;
[0036] Figure 6 This is a diagram of the responsivity and detectivity of the perovskite photodetector prepared in Example 1 of the present invention;
[0037] Figure 7 This is a long-term stability diagram of the perovskite hemispherical photodetector prepared in Example 1 of the present invention;
[0038] Figure 8 XRD patterns of the perovskite layer prepared in Example 1 of the present invention at different temperatures;
[0039] Fig. 9 This is a diagram of high temperature current stability of the perovskite photodetector prepared in Example 1 of the present invention;
[0040] Fig.10 A high-resolution color imaging diagram of the perovskite hemispherical photodetector prepared in Example 1 of the present invention;
[0041] Fig.11 This is a color imaging image of the perovskite hemispherical photodetector prepared in Example 1 of the present invention under weak light.
[0042] Fig.12 This is a color imaging diagram of the perovskite hemispherical photodetector prepared in Example 1 of the present invention at high temperature. DETAILED DESCRIPTION
[0043] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0044] Example 1
[0045] The preparation and color imaging of lead-free perovskite hemispherical photodetector are as follows:
[0046] (a) Preparation of CsBi 3 I 10 -Guanidine thiocyanate perovskite precursor solution: Cesium iodide and bismuth iodide powders were dissolved in a mixed solvent of N,N-dimethylformamide (DMF) and dimethyl sulfoxide (DMSO) at a molar ratio of 1:3 (the volume ratio of DMF and DMSO was 9:1), and 1 mol% of guanidine thiocyanate (GTC) was added to form CsBi 3 I 10 -Guanidine thiocyanate perovskite precursor solution (CsBi 3 I 10 -GTC-1).
[0047] (b) Fabrication of hemispherical devices: First, a hemispherical glass substrate with a radius of 5 mm was treated with UV ozone for 20 minutes, and then a 100 nm thick chromium electrode layer was deposited on the spherical surface by vacuum thermal evaporation at a rate of After the deposition of the chromium electrode layer was completed, the substrate was treated with ultraviolet ozone for 20 minutes and then transferred to a plasma treatment chamber (RF power 200W, working gas nitrogen) for 5 minutes. Next, the treated hemispherical glass substrate was fixed on a stainless steel plate and heated to 100°C. At the same time, the tin dioxide solution was dissolved in deionized water at a volume ratio of 1:12 to obtain a 1.5wt% tin dioxide aqueous solution and was evenly sprayed on the heated hemispherical substrate using a spray gun with a nozzle diameter of 2mm. The thickness of the resulting electron transport layer was 100nm. After spraying the tin dioxide aqueous solution, the chromium / tin dioxide substrate was thermally annealed at 150°C for 30 minutes. Then, the treated substrate was re-fixed and heated to 100°C, and the CsBi 3 I 10 -Guanidine thiocyanate perovskite precursor solution was uniformly sprayed on the treated chromium / tin dioxide substrate, and the thickness of the obtained perovskite layer was 1.5 μm. After spraying, the entire device was thermally annealed at 125°C for 30 minutes. Then, the hemispherical glass substrate obtained in step (2) was heated to 100°C, and poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine] was dissolved in toluene, and the concentration of poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine] was 0.5 mg mL -1 , it was uniformly sprayed on the heated substrate using a spray gun with a nozzle diameter of 2 mm and thermally annealed at 110°C for 10 minutes. The resulting hole transport layer had a thickness of 30 nm. Finally, 10 nm of chromium and 10 nm of gold were directly deposited on the device by vacuum thermal evaporation. The rate of vacuum thermal evaporation deposition was The schematic diagram of the obtained lead-free perovskite hemispherical photodetector is shown in Figure 1 shown.
[0048] (c) Perform color imaging and detection of target objects: The process of color imaging is as follows: Figure 2 As shown. First, a digital projector is used to generate a colored Fourier basis pattern and illuminate the target imaging object. The colored Fourier basis pattern is generated by a computer and controls the projector to project the pattern onto the target object. The intensity of the diffuse reflected light is about 30 μW cm -2 The reflected light from the object under the illumination of the structured light pattern is collected by the perovskite hemispherical photodetector and converted into an electrical signal. The converted electrical signal is collected by the power meter as a digital signal and transmitted to the computer for storage and recording.
[0049] (d) Calculation and processing to obtain a color image of the target object: The core of Fourier single-pixel imaging is to decompose the image information of the target object into the frequency domain through Fourier transform, that is, to obtain the Fourier spectrum of the image. This process is usually achieved by projecting a series of Fourier basis patterns onto the target object, and using a single-pixel detector to measure the light intensity values reflected by these patterns on the object and convert them into current values and record them. Through the recorded current values, the coefficients of the image in the Fourier domain, that is, the Fourier spectrum, can be calculated. By calculating the current value obtained by the perovskite hemispherical photodetector in step (c), the Fourier coefficients of the target object image can be obtained. Then, using the inverse Fourier transform, these spectrum coefficients can be converted back to the spatial domain to reconstruct the grayscale image of the object. Since the colorful Fourier basis pattern is used for illumination, the reconstructed object image is the same as the original pattern captured by the monochrome image sensor in traditional color imaging. Therefore, the traditional de-mosaicing algorithm used for color restoration in color imaging can also be used to reconstruct the color image of the object from the grayscale image.
[0050] Example 2
[0051] The preparation and color imaging of lead-free perovskite hemispherical photodetector are as follows:
[0052] (a) Preparation of CsBi 3 I 10 Perovskite precursor solution: Cesium iodide and bismuth iodide powders were dissolved in a mixed solvent of N,N-dimethylformamide (DMF) and dimethyl sulfoxide (DMSO) at a molar ratio of 1:3 (the volume ratio of DMF to DMSO was 9:1) to form CsBi 3 I 10 Perovskite precursor solution (CsBi 3 I 10 -GTC-0).
[0053] (b) Manufacturing of hemispherical devices: First, a hemispherical glass substrate with a radius of 5 mm was treated with ultraviolet ozone for 20 minutes, and then a 100 nm chromium electrode was deposited on the spherical surface of the hemispherical glass substrate by vacuum thermal evaporation. After the chromium electrode deposition was completed, the substrate was treated with ultraviolet ozone for 20 minutes, and then transferred to a plasma treatment chamber (RF power 200 W, working gas nitrogen) for 5 minutes. Next, the treated hemispherical glass substrate was fixed on a stainless steel plate and heated to 100°C. At the same time, a tin dioxide solution was dissolved in deionized water at a volume ratio of 1:12 to obtain a tin dioxide aqueous solution with a mass ratio of 1.5wt% and was evenly sprayed on the heated hemispherical substrate using a spray gun with a nozzle diameter of 2mm. The thickness of the resulting electron transport layer was 100nm. After spraying the tin dioxide aqueous solution, the chromium / tin dioxide substrate was thermally annealed at 150°C for 30 minutes. Then, the treated substrate was re-fixed and heated to 100°C. Then, a spray gun with a nozzle diameter of 2mm was used to spray CsBi 3 I 10 Perovskite precursor (CsBi 3 I 10 -GTC-0) solution was uniformly sprayed on the treated chromium / tin dioxide substrate, and the thickness of the obtained perovskite layer was 1.5 μm. After spraying, the entire device was thermally annealed at 125°C for 30 minutes. Then, the hemispherical glass substrate obtained in step (2) was heated to 100°C, and poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine] was dissolved in toluene, and the concentration of poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine] was 0.5 mg mL -1 , it was uniformly sprayed on the heated substrate using a spray gun with a nozzle diameter of 2 mm and thermally annealed at 110°C for 10 minutes. The resulting hole transport layer had a thickness of 30 nm. Finally, 10 nm of chromium and 10 nm of gold were directly deposited on the device by vacuum thermal evaporation. The rate of vacuum thermal evaporation deposition was The schematic diagram of the obtained lead-free perovskite hemispherical photodetector is shown in Figure 1 shown.
[0054] (c) Perform color imaging and detection of target objects: The process of color imaging is as follows: Figure 2 As shown. First, a digital projector is used to generate a colored Fourier basis pattern and illuminate the target imaging object. The colored Fourier basis pattern is generated by a computer and controls the projector to project the pattern onto the target object. The intensity of the diffuse reflected light is about 30 μW cm -2 The reflected light from the object under the illumination of the structured light pattern is collected by the perovskite hemispherical photodetector and converted into an electrical signal. The converted electrical signal is collected by the power meter as a digital signal and transmitted to the computer for storage and recording.
[0055] (d) Calculation and processing to obtain a color image of the target object: The core of Fourier single-pixel imaging is to decompose the image information of the target object into the frequency domain through Fourier transform, that is, to obtain the Fourier spectrum of the image. This process is usually achieved by projecting a series of Fourier basis patterns onto the target object, and using a single-pixel detector to measure the light intensity values reflected by these patterns on the object and convert them into current values and record them. Through the recorded current values, the coefficients of the image in the Fourier domain, that is, the Fourier spectrum, can be calculated. By calculating the current value obtained by the perovskite hemispherical photodetector in step (c), the Fourier coefficients of the target object image can be obtained. Then, using the inverse Fourier transform, these spectrum coefficients can be converted back to the spatial domain to reconstruct the grayscale image of the object. Since the colorful Fourier basis pattern is used for illumination, the reconstructed object image is the same as the original pattern captured by the monochrome image sensor in traditional color imaging. Therefore, the traditional de-mosaicing algorithm used for color restoration in color imaging can also be used to reconstruct the color image of the object from the grayscale image.
[0056] Example 3
[0057] The preparation and color imaging of lead-free perovskite hemispherical photodetector are as follows:
[0058] (a) Preparation of CsBi 3 I 10 -Guanidine thiocyanate perovskite precursor solution: Cesium iodide and bismuth iodide powders were dissolved in a mixed solvent of N,N-dimethylformamide (DMF) and dimethyl sulfoxide (DMSO) at a molar ratio of 1:3 (the volume ratio of DMF to DMSO was 9:1), and 0.5 mol% of guanidine thiocyanate (GTC) was added to form CsBi 3 I 10 -Guanidine thiocyanate perovskite precursor solution (CsBi 3 I 10 -GTC-0.5).
[0059] (b) Manufacturing of hemispherical devices: First, a hemispherical glass substrate with a radius of 5 mm was treated with ultraviolet ozone for 20 minutes, and then a 100 nm chromium electrode was deposited on the spherical surface of the hemispherical glass substrate by vacuum thermal evaporation. After the chromium electrode deposition was completed, the substrate was treated with ultraviolet ozone for 20 minutes, and then transferred to a plasma treatment chamber (RF power 200 W, working gas nitrogen) for 5 minutes. Next, the treated hemispherical glass substrate was fixed on a stainless steel plate and heated to 100°C. At the same time, a tin dioxide solution was dissolved in deionized water at a volume ratio of 1:12 to obtain a tin dioxide aqueous solution with a mass ratio of 1.5wt% and was evenly sprayed on the heated hemispherical substrate using a spray gun with a nozzle diameter of 2mm. The thickness of the resulting electron transport layer was 100nm. After spraying the tin dioxide aqueous solution, the chromium / tin dioxide substrate was thermally annealed at 150°C for 30 minutes. Then, the treated substrate was re-fixed and heated to 100°C. Then, a spray gun with a nozzle diameter of 2mm was used to spray CsBi 3 I 10 -Guanidine thiocyanate perovskite precursor (CsBi 3 I 10 -GTC-0.5) solution was uniformly sprayed on the treated chromium / tin dioxide substrate, and the thickness of the obtained perovskite layer was 1.5 μm. After spraying, the entire device was thermally annealed at 125°C for 30 minutes. Then, the hemispherical glass substrate obtained in step (2) was heated to 100°C, and poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine] was dissolved in toluene, and the concentration of poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine] was 0.5 mg mL -1 , it was uniformly sprayed on the heated substrate using a spray gun with a nozzle diameter of 2 mm and thermally annealed at 110°C for 10 minutes. The resulting hole transport layer had a thickness of 30 nm. Finally, 10 nm of chromium and 10 nm of gold were directly deposited on the device by vacuum thermal evaporation. The rate of vacuum thermal evaporation deposition was The schematic diagram of the obtained lead-free perovskite hemispherical photodetector is shown in Figure 1 shown.
[0060] (c) Perform color imaging and detection of target objects: The process of color imaging is as follows: Figure 2 As shown. First, a digital projector is used to generate a colored Fourier basis pattern and illuminate the target imaging object. The colored Fourier basis pattern is generated by a computer and controls the projector to project the pattern onto the target object. The intensity of the diffuse reflected light is about 30 μW cm -2 The reflected light from the object under the illumination of the structured light pattern is collected by the perovskite hemispherical photodetector and converted into an electrical signal. The converted electrical signal is collected by the power meter as a digital signal and transmitted to the computer for storage and recording.
[0061] (d) Calculation and processing to obtain a color image of the target object: The core of Fourier single-pixel imaging is to decompose the image information of the target object into the frequency domain through Fourier transform, that is, to obtain the Fourier spectrum of the image. This process is usually achieved by projecting a series of Fourier basis patterns onto the target object, and using a single-pixel detector to measure the light intensity values reflected by these patterns on the object and convert them into current values and record them. Through the recorded current values, the coefficients of the image in the Fourier domain, that is, the Fourier spectrum, can be calculated. By calculating the current value obtained by the perovskite hemispherical photodetector in step (c), the Fourier coefficients of the target object image can be obtained. Then, using the inverse Fourier transform, these spectrum coefficients can be converted back to the spatial domain to reconstruct the grayscale image of the object. Since the colorful Fourier basis pattern is used for illumination, the reconstructed object image is the same as the original pattern captured by the monochrome image sensor in traditional color imaging. Therefore, the traditional de-mosaicing algorithm used for color restoration in color imaging can also be used to reconstruct the color image of the object from the grayscale image.
[0062] Example 4
[0063] The preparation and color imaging of lead-free perovskite hemispherical photodetector are as follows:
[0064] (a) Preparation of CsBi 3 I 10 -Guanidine thiocyanate perovskite precursor solution: Cesium iodide and bismuth iodide powders were dissolved in a mixed solvent of N,N-dimethylformamide (DMF) and dimethyl sulfoxide (DMSO) at a molar ratio of 1:3 (the volume ratio of DMF to DMSO was 9:1), and 3 mol% of guanidine thiocyanate (GTC) was added to form CsBi 3 I 10 -Guanidine thiocyanate perovskite precursor solution (CsBi 3 I 10 -GTC-3).
[0065] (b) Manufacturing of hemispherical devices: First, a hemispherical glass substrate with a radius of 5 mm was treated with ultraviolet ozone for 20 minutes, and then a 100 nm chromium electrode was deposited on the spherical surface of the hemispherical glass substrate by vacuum thermal evaporation. After the chromium electrode deposition was completed, the substrate was treated with ultraviolet ozone for 20 minutes, and then transferred to a plasma treatment chamber (RF power 200 W, working gas nitrogen) for 5 minutes. Next, the treated hemispherical glass substrate was fixed on a stainless steel plate and heated to 100°C. At the same time, a tin dioxide solution was dissolved in deionized water at a volume ratio of 1:12 to obtain a tin dioxide aqueous solution with a mass ratio of 1.5wt% and was evenly sprayed on the heated hemispherical substrate using a spray gun with a nozzle diameter of 2mm. The thickness of the resulting electron transport layer was 100nm. After spraying the tin dioxide aqueous solution, the chromium / tin dioxide substrate was thermally annealed at 150°C for 30 minutes. Then, the treated substrate was re-fixed and heated to 100°C. Then, a spray gun with a nozzle diameter of 2mm was used to spray CsBi 3 I 10 -Guanidine thiocyanate perovskite precursor (CsBi 3 I 10 -GTC-3) solution was uniformly sprayed on the treated chromium / tin dioxide substrate, and the thickness of the obtained perovskite layer was 1.5μm. After spraying, the entire device was thermally annealed at 125°C for 30 minutes. Then, the hemispherical glass substrate obtained in step (2) was heated to 100°C, and poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine] was dissolved in toluene, and the concentration of poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine] was 0.5mg mL -1 , it was uniformly sprayed on the heated substrate using a spray gun with a nozzle diameter of 2 mm and thermally annealed at 110°C for 10 minutes. The resulting hole transport layer had a thickness of 30 nm. Finally, 10 nm of chromium and 10 nm of gold were directly deposited on the device by vacuum thermal evaporation. The rate of vacuum thermal evaporation deposition was The schematic diagram of the obtained lead-free perovskite hemispherical photodetector is shown in Figure 1 shown.
[0066] (c) Perform color imaging and detection of target objects: The process of color imaging is as follows: Figure 2 As shown. First, a digital projector is used to generate a colored Fourier basis pattern and illuminate the target imaging object. The colored Fourier basis pattern is generated by a computer and controls the projector to project the pattern onto the target object. The intensity of the diffuse reflected light is about 30 μW cm -2 The reflected light from the object under the illumination of the structured light pattern is collected by the perovskite hemispherical photodetector and converted into an electrical signal. The converted electrical signal is collected by the power meter as a digital signal and transmitted to the computer for storage and recording.
[0067] (d) Calculation and processing to obtain a color image of the target object: The core of Fourier single-pixel imaging is to decompose the image information of the target object into the frequency domain through Fourier transform, that is, to obtain the Fourier spectrum of the image. This process is usually achieved by projecting a series of Fourier basis patterns onto the target object, and using a single-pixel detector to measure the light intensity values reflected by these patterns on the object and convert them into current values and record them. Through the recorded current values, the coefficients of the image in the Fourier domain, that is, the Fourier spectrum, can be calculated. By calculating the current value obtained by the perovskite hemispherical photodetector in step (c), the Fourier coefficients of the target object image can be obtained. Then, using the inverse Fourier transform, these spectrum coefficients can be converted back to the spatial domain to reconstruct the grayscale image of the object. Since the colorful Fourier basis pattern is used for illumination, the reconstructed object image is the same as the original pattern captured by the monochrome image sensor in traditional color imaging. Therefore, the traditional de-mosaicing algorithm used for color restoration in color imaging can also be used to reconstruct the color image of the object from the grayscale image.
[0068] Test Example 1
[0069] Crystal structure: This invention is based on CsBi 3 I 10 Guanidine thiocyanate (GTC) is introduced into the perovskite layer as an additive, where the guanidine cation can passivate the cation vacancy defects and Bi-I antisite defects on the bottom surface of the perovskite layer through hydrogen bonds and electrostatic interactions between the amino groups in guanidine. - Similar chemical behavior (SCN - Ionic radius (217 pm) and I - (220m) equivalent) The lone electron pair in the linear structure can react with Bi 3+ Coordination, thereby controlling CsBi 3 I 10 It can form hydrogen bonds with cations in the material and anchor at the grain boundaries, enhancing the structural stability of the perovskite layer.
[0070] The perovskite materials prepared in Examples 1-4 and added with different concentrations of guanidine thiocyanate (GTC) were characterized by XRD. The characterization results are as follows: Figure 3 As shown in the XRD test. Figure 3 The horizontal axis is twice the incident angle of the X-ray, usually represented by the symbol "2θ", and the vertical axis is the intensity after diffraction. 3 I 10 Perovskites work differently. Figure 3 It can be seen that when guanidine thiocyanate (GTC) concentration is 1 mol% (CsBi3 I 10 -GTC-1), the effect is the best. 3 I 10 -Guanidine thiocyanate perovskite layer shows significantly suppressed (006) peak intensity and enhanced (003) peak intensity, indicating that the phase purity and crystallinity are significantly improved. This shows that the perovskite material obtained in Example 1 is the best.
[0071] Test Example 2
[0072] Appearance: The cross-sectional morphology of the perovskite layer was observed by SEM. The present invention adopts the spraying method to prepare the perovskite layer. The uniformity of thickness is very important for the performance of the device. The cross-sectional SEM result of the hemispherical perovskite layer prepared in Example 1 is as follows: Figure 4 As shown. Figure 4 It can be seen that the thickness of the perovskite layer is uniform and dense, indicating that the perovskite layer prepared by spraying has a good effect. The above test shows that the hemispherical perovskite photodetector prepared by the present invention has excellent crystallinity and uniform thickness.
[0073] Test Example 3
[0074] Photoelectric performance of hemispherical photodetector: The linear dynamic range, responsivity and specific detection rate of the lead-free perovskite hemispherical photodetector prepared in Example 1 were tested. Figure 5 and Figure 6 As shown. For diffuse reflection imaging, linear dynamic range is a key parameter. The linear dynamic range is used to describe the linear response capability of the detector to different light intensity ranges. The linear dynamic range is obtained by fitting the linear relationship between light intensity and photocurrent density. The current density of the hemispherical photodetector under different light intensities is recorded by using a current source meter. The intensity change of light is provided by a nanosecond laser. Figure 5 The horizontal axis represents the light intensity, and the vertical axis represents the photocurrent density. Figure 5 It can be seen that the linear dynamic range is 146dB, indicating that the hemispherical photodetector performs well in weak light detection. The responsivity and specific detectivity of the lead-free perovskite hemispherical photodetector are tested. Figure 6 shown. Figure 6 The horizontal axis represents the light intensity, the left vertical axis represents the responsivity, and the right vertical axis represents the specific detection rate. The responsivity (R) is defined as the ratio of the device's photocurrent to the light irradiation intensity. It is used to describe the magnitude of the current generated by light. The specific detection rate (D*) is a parameter for comprehensively evaluating the device's responsiveness, which is defined by the noise current and the responsivity. Its specific detection rate (D*) and responsivity (R) are 1.47×10 13 Jones and 188.6mAW -1This once again demonstrates that hemispherical photodetectors excel in low-light detection, which is crucial for color imaging in low-light conditions.
[0075] Test Example 4
[0076] Stability of hemispherical photodetector: CsBi prepared in Example 1 3 I 10 The long-term stability of the CsBi-guanidine thiocyanate perovskite layer was tested. The stability of the photodetector is very important for color imaging because it is directly related to the accuracy of the Fourier coefficients obtained in the reconstructed image. 3 I 10 - The absorption intensity curve of the device at different wavelengths after the guanidine thiocyanate perovskite layer was exposed to air (50% relative humidity (RH), 25°C) for 30 days. Figure 7 shown. Figure 7 The horizontal axis is the wavelength of light, and the vertical axis is the absorption intensity of light by the material. Figure 7 According to the light absorption curve, around 30 days, CsBi 3 I 10 -The absorption curves of the guanidine thiocyanate perovskite layer are almost the same, indicating that CsBi 3 I 10 -Guanidine thiocyanate perovskite layer has good stability.
[0077] The CsBi prepared in Example 1 3 I 10 -Guanidine thiocyanate perovskite layer was tested for high temperature stability. 3 I 10 -XRD test of guanidine thiocyanate perovskite layer Figure 8 When the temperature is 150℃, CsBi 3 I 10 -The characteristic peak (003) intensity of the guanidine thiocyanate perovskite layer does not change much. 3 I 10 -Guanidine thiocyanate perovskite layer has no significant changes in its lattice and structure at high temperature. 3 I 10 -Guanidine thiocyanate perovskite layer is suitable for the preparation of lead-free perovskite hemispherical photodetectors for application at high temperatures.
[0078] The CsBi prepared in Example 1 3 I 10 -The high temperature stability test of the guanidine thiocyanate perovskite photodetector was carried out by using a current source meter to record the current change curve of the lead-free perovskite photodetector when it was placed on a hot temperature table at 100°C. The results are as follows Fig. 9 shown. Fig. 9 The horizontal axis represents time, and the vertical axis represents current intensity. 3 I 10 - The photocurrent change of the guanidine thiocyanate perovskite photodetector is very small within 3600 seconds, which verifies the CsBi 3 I 10 -The devices made of guanidine thiocyanate perovskite material have good thermal stability. 3 I 10 -Guanidine thiocyanate perovskite photodetectors can meet the imaging needs at high temperatures.
[0079] Test Example 5
[0080] Color imaging: The lead-free perovskite hemispherical photodetector prepared in Example 1 was used for color imaging. Fig.10 As shown in the figure, a hemispherical perovskite photodetector is used to record the intensity of diffuse reflected light generated by Fourier base projection onto the surface of an object. The hemispherical photodetector converts the light signal into an electrical signal and records it, and then generates a color image through Fourier inverse transform calculation and demosaicing algorithm.
[0081] The lead-free perovskite hemispherical photodetector prepared in Example 1 was used to perform color imaging under weak light, and the results are as follows: Fig.11 At 5.5 μW cm -2 Under weak light conditions, a hemispherical perovskite photodetector is used to record the intensity of diffuse reflected light generated by the Fourier base projection onto the object. The hemispherical photodetector converts the optical signal into an electrical signal and records it. Fig.11 The imaging results show that even in low light conditions, CsBi 3 I 10 -Guanidine thiocyanate perovskite hemispherical photodetector can still perform color imaging (with slightly less pixels) Fig.10 ), which is conducive to expanding the application range of lead-free perovskite hemispherical photodetector imaging.
[0082] The lead-free perovskite hemispherical photodetector prepared in Example 1 was used to perform color imaging at high temperature. The results are as follows: Fig.12 As shown. Under high temperature conditions of 100°C, a hemispherical perovskite photodetector is used to record the intensity of diffuse reflected light generated by Fourier base projection onto an object. The hemispherical photodetector converts the optical signal into an electrical signal and records it. Fig.12 The imaging results show that even at a high temperature of 100°C, CsBi 3 I 10-Guanidine thiocyanate perovskite hemispherical photodetector can still perform color imaging, which shows that lead-free perovskite hemispherical photodetector can perform color imaging in complex environments from 25°C to 100°C.
[0083] As can be seen from the above embodiments, the present invention provides a hemispherical single-pixel photodetector based on a sprayed lead-free perovskite layer, which can achieve filter-free single-pixel color imaging in complex environments. The detector has excellent stability, outstanding low-light response capability, and a hemispherical device structure, which enables it to collect more diffusely reflected light, thereby improving imaging quality. This simple design not only saves the space and cost required to build a complex detector array, but also promotes the development of filter-free color imaging technology.
[0084] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A method for preparing a lead-free perovskite hemispherical photodetector, the steps of which are as follows: (1) depositing a chromium electrode layer by vacuum thermal evaporation on the spherical surface of a hemispherical glass substrate that has been treated with ultraviolet ozone for 15 to 30 minutes; (2) treating the hemispherical glass substrate obtained in step (1) with ultraviolet ozone for 15 to 30 minutes, and then transferring it to a plasma treatment chamber for treatment for 3 to 8 minutes; heating the treated substrate to 90 to 110° C., and then spraying an electron transport layer solution on the surface of the chromium electrode layer, and annealing at 140 to 160° C. for 20 to 40 minutes after the spraying, to obtain an electron transport layer on the surface of the chromium electrode layer; (3) heating the hemispherical glass substrate obtained in step (2) to 90-110° C., and then spraying a perovskite precursor solution on the surface of the electron transport layer. After spraying, annealing is performed at 115-135° C. for 20-40 minutes to obtain a perovskite layer on the surface of the electron transport layer; (4) heating the hemispherical glass substrate obtained in step (3) to 80-100° C., and then spraying a hole transport layer solution on the surface of the perovskite layer. After spraying, annealing is performed at 100-120° C. for 8-15 minutes to obtain a hole transport layer on the surface of the perovskite layer. (5) Vacuum thermal evaporation is performed on the surface of the hole transport layer obtained in step (4) to deposit a metal electrode layer, thereby obtaining the lead-free perovskite hemispherical photodetector.
2. The method for preparing a lead-free perovskite hemispherical photodetector according to claim 1, characterized in that: In step (2), the electron transport layer solution is a tin dioxide aqueous solution with a concentration of 1.0 to 2.0 wt%.
3. The method for preparing a lead-free perovskite hemispherical photodetector according to claim 1, characterized in that: The perovskite precursor solution in step (3) is CsBi3I 10 An aqueous solution mixed with guanidine thiocyanate, CsBi3I 10 The concentration of is 0.2~0.4mol / L, and the concentration of guanidine thiocyanate is 0.5~3mol%.
4. The method for preparing a lead-free perovskite hemispherical photodetector according to claim 1, characterized in that: In step (4), the hole transport layer solution is a toluene solution of poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine] with a concentration of 0.3 to 0.8 mg / mL.
5. The method for preparing a lead-free perovskite hemispherical photodetector according to claim 1, characterized in that: The thermal evaporation deposition rate of the metal electrode layer in step (5) is The metal electrode materials are chromium and gold.
6. The method for preparing a lead-free perovskite hemispherical photodetector according to claim 1, characterized in that: The spraying equipment described in step (2) to step (4) is a spray gun, the nozzle diameter of the spray gun is 0.2 mm, the pressure of the spray gun is 1 to 1.1 bar, and the spraying distance is 3 to 4 cm.
7. The method for preparing a lead-free perovskite hemispherical photodetector according to claim 1, characterized in that: In step (1) and step (5), the rate of vacuum thermal evaporation deposition is 8. A lead-free perovskite hemispherical photodetector, characterized in that: The method is prepared by any one of claims 1 to 7.
9. The lead-free perovskite hemispherical photodetector according to claim 8, characterized in that: The thickness ratio of the chromium electrode layer, the electron transport layer, the perovskite layer, the hole transport layer and the metal electrode layer is 100-200 nm: 100-200 nm: 1000-1500 nm: 25-30 nm: 10-20 nm.
10. Application of the lead-free perovskite hemispherical photodetector according to claim 8 or 9 in single-pixel lens-free color imaging.
Citation Information
Patent Citations
Hemi-spherical shape and spherical two-photon response semiconductor photoelectric detector
CN101013049A
Ultraviolet photoelectric detector of lead-free perovskite single crystal and preparation method of ultraviolet photoelectric detector
CN111725406A
Flexible lead-free tin-based perovskite device optical detector and preparation method thereof
CN118102822A
Hemispherical detector
US6534768B1
Infrared imaging device, fabrication method therefor, and simulation infrared spherical camera
WO2019153322A1