Graphene / perfluorophthalocyanine copper-based synaptic transistor and preparation method thereof

By depositing perfluorocopper phthalocyanine on the surface of graphene films, graphene/perfluorocopper phthalocyanine synaptic transistors with p-type and n-type performance matching were fabricated. This solved the problem that existing technologies could not simulate synaptic plasticity mediated by multiple neurotransmitters, and enabled rapid switching between short-range and long-range plasticity, thus promoting the functional diversity of neuromorphic systems.

CN118946255APending Publication Date: 2024-11-12SHENZHEN RES INST OF NANKAI UNIV +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411008597.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing artificial synaptic devices cannot effectively simulate synaptic plasticity changes mediated by various neurotransmitters, especially the rapid switching between long-range and short-range plasticity.

Method used

By depositing n-type perfluorocopper phthalocyanine on the surface of a graphene film, a graphene/perfluorocopper phthalocyanine synaptic transistor with p-type and n-type performance was fabricated. The presynaptic pulse applied to the gate was used to stimulate the change of the carrier type in the channel, thereby achieving rapid switching of short-range/long-range plasticity.

Benefits of technology

It realizes the simulation of multiplexing different neurotransmitters, can simulate synaptic plasticity under positive and negative gate voltages, and can achieve rapid switching of short-range/long-range plasticity by switching the polarity of the gate pulse, thus promoting the construction of functionally diverse neuromorphic systems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118946255A_ABST
    Figure CN118946255A_ABST
Patent Text Reader

Abstract

The invention relates to a synaptic transistor based on graphene / perfluorophthalocyanine copper and a preparation method of the synaptic transistor. The synaptic transistor structurally comprises a substrate, a functional layer, a source electrode, a drain electrode and an ionic gel gate dielectric layer from bottom to top, the functional layer is a graphene / perfluorophthalocyanine copper film, and the thickness of the functional layer is 2.5-25 nm; wherein the thickness of the graphene film is 0.5-5 nm, and the thickness of the perfluorophthalocyanine copper film is 2-20 nm. According to the graphene / perfluorophthalocyanine copper synaptic transistor prepared by the invention, the positive and negative polarities stimulated by the pre-synaptic pulse applied by the grid electrode are switched to change the carrier type (electron or hole) transmitted in the channel, so that short-range / long-range plasticity rapid switching can be realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of semiconductor devices, and in particular relates to a graphene / perfluorophthalocyanine copper synaptic transistor with fast switchable long-range and short-range plasticity and a preparation method thereof. Background Art

[0002] Inspired by the human brain, the construction of highly connected, low-energy, and parallel information processing neuromorphic systems has received increasing attention. Among them, artificial synaptic devices that can simulate neural functions such as synaptic plasticity of biological synapses are the key to successfully building neuromorphic systems. To date, various materials have been widely studied for the development of artificial synaptic devices, but most devices only simulate synaptic plasticity changes caused by the release of a single type of neurotransmitter. In fact, the ventral tegmental area (VTA) neurons of the brain can transmit dopamine, glutamate or GABA, as well as combinations of these neurotransmitters. The term "multiplexed neurotransmitter transmission" is used to describe neurons that can use two or more neurotransmitters to send signals. Multiplexed neurotransmission transmission expands the range of synaptic plasticity of individual neurons and realizes the functional diversity of neurons. According to the patent "A method for preparing a dual-excitatory artificial synaptic device for simulating biological synaptic neurotransmitter multiplexing" (patent application number: CN202011073522.6), the artificial synaptic device based on the bipolar two-dimensional material palladium diselenide realizes the simulation of the release of two excitatory neurotransmitters from the same presynaptic membrane, but does not realize the simulation of the rapid switching of synaptic plasticity in multiplexed neural transmission. Therefore, an artificial synaptic device that can simulate synaptic plasticity mediated by multiple neurotransmitters and can achieve rapid switching of long-range and short-range plasticity is very necessary. Among them, graphene, as a typical two-dimensional material, can exhibit both p-type and n-type conductive properties by regulating the type and concentration of carriers in graphene, showing bipolar characteristics. The bipolar characteristics of graphene have the potential to achieve multiplexed neural transmission. However, during the preparation and transfer of graphene, water molecules and oxygen molecules will be adsorbed on the graphene surface, making the graphene exhibit p-type semiconductor properties, and unable to obtain bipolar properties that match p-type and n-type performance. Therefore, the transferred graphene film cannot achieve multiplexed neurotransmission and synaptic plasticity switching. Summary of the invention

[0003] The purpose of the present invention is to address the deficiencies of the prior art and propose a synaptic transistor based on graphene / perfluorophthalocyanine copper and a preparation method thereof. The composition of the transistor is to evaporate n-type semiconductor perfluorophthalocyanine copper on the surface of the transferred graphene with strong p and weak n, and obtain a graphene / perfluorophthalocyanine copper synaptic transistor with bipolar characteristics matching p-type and n-type performance; during the preparation, by depositing n-type perfluorophthalocyanine copper on the surface of the transferred graphene film, a graphene / perfluorophthalocyanine copper synaptic transistor is prepared, and the bipolar characteristics of strong p and weak n of the single graphene device are converted into bipolar characteristics matching p-type and n-type performance of graphene / perfluorophthalocyanine copper, providing a performance basis for the simulation of multiplexed neural transmission of different neurotransmitters. The graphene / perfluorophthalocyanine copper synaptic transistor prepared by the present invention can achieve rapid switching of short-range / long-range plasticity by switching the positive and negative polarity of the presynaptic pulse stimulation applied by the gate to change the type of carrier (electron or hole) transmitted in the channel.

[0004] The technical solution of the present invention is:

[0005] A synaptic transistor based on graphene / perfluorophthalocyanine copper, the structure of the synaptic transistor from bottom to top is a substrate, a functional layer, a source-drain electrode and an ion glue gate dielectric layer;

[0006] Among them, the substrate is glass, Si / SiO 2 , PEN or PET substrate;

[0007] The functional layer is a graphene / perfluorophthalocyanine copper film with a thickness of 2.5 to 25 nm; wherein the graphene film has a thickness of 0.5 to 5 nm.

[0008] The source and drain electrodes are evaporated metal electrodes, the metal is gold, copper or silver, and the thickness is 40 to 80 nm;

[0009] The material of the ion glue grid dielectric layer is [PVDF-HFP] [EMIM-TFSI], and the thickness is 100-500 μm.

[0010] The method for preparing the graphene / perfluorocopper phthalocyanine-based synaptic transistor comprises the following steps:

[0011] 1) The substrate was ultrasonically cleaned with deionized water, acetone, and isopropanol, and then nitrogen (N 2 ) Blow dry its surface for later use;

[0012] 2) spin coating a polymethyl methacrylate (PMMA) solution onto the front surface of the copper foil on which the graphene film is grown, to obtain a graphene / PMMA film attached to the surface of the copper foil;

[0013] The mass concentration of the PMMA solution is 2-10%, the solvent is chlorobenzene, the spin coating speed of the PMMA solution is 2000-4000 r / min, and the spin coating time is 40-80 s;

[0014] 3) transferring the copper foil with the graphene / PMMA film attached in step 2) to the surface of the etching solution, floating for 2 to 8 hours, etching away the copper foil substrate, and obtaining a polymer-supported graphene / PMMA film;

[0015] The etching solution is ammonium persulfate (NH 4 ) 2 S 2 O 8 ) solution, the concentration is 0.1~1mol / L;

[0016] 4) using the substrate obtained in step 1) to fish out the graphene / PMMA film obtained in step 3) and dry it to obtain a graphene / PMMA film attached to the substrate;

[0017] 5) placing the graphene / PMMA film attached to the substrate in acetone, a mixed organic solvent, and an isopropanol solution in turn to remove PMMA, thereby obtaining a single-layer graphene film attached to the substrate;

[0018] The mixed organic solvent consists of acetone and isopropanol, and the volume ratio of the two is 1:1;

[0019] 6) placing the perfluorophthalocyanine copper in an evaporation boat in a vacuum chamber of physical vapor deposition (PVD), and then fixing the substrate with the graphene film transferred on a substrate holder in the chamber, and starting to deposit the perfluorophthalocyanine copper after the chamber is evacuated to finally obtain a graphene / perfluorophthalocyanine copper film;

[0020] The chamber is evacuated to 1×10 -4 Pa~1×10 -3 Pa; the deposition rate of perfluorophthalocyanine copper is The deposition time is 2 to 20 minutes;

[0021] 7) using a mask, evaporating metal source and drain electrodes with a thickness of 40 to 80 nm and spaced apart on the surface of the graphene / perfluorophthalocyanine copper film obtained in step 6); wherein the metal is gold, aluminum, silver or the like;

[0022] 8) Mix and stir PVDF-HFP, EMIM-TFSI ionic liquid and acetone in a mass ratio of 1:3 to 5:7, and after fully dissolving, drop the mixed solution onto a glass slide, and dry to obtain an ion gel film with a thickness of 100 to 500 μm;

[0023] 9) attaching the ion glue gate dielectric layer to the graphene / perfluorocopper phthalocyanine film between the source and drain electrodes, and finally preparing the graphene / perfluorocopper phthalocyanine synaptic transistor.

[0024] The application of the graphene / perfluorocopper phthalocyanine based synaptic transistor is used to simulate synaptic plasticity mediated by different excitatory neurotransmitters.

[0025] The simulated different excitatory neurotransmitters are preferably dopamine and glutamate.

[0026] The essential features of the present invention are:

[0027] In current technologies, most artificial synaptic devices only simulate synaptic plasticity changes caused by the release of a single type of neurotransmitter, and cannot simulate multiplexed neurotransmitter transmission, and the functional diversity of the devices is limited;

[0028] The present invention utilizes the intrinsic bipolar characteristics of graphene and can exhibit both p-type and n-type conductive properties by regulating the type and concentration of carriers in graphene, which helps to achieve the simulation of multiplexed neural transmission.

[0029] In the device preparation method, the present invention constructs a graphene / perfluorocopper phthalocyanine synaptic transistor with bipolar characteristics matching p-type and n-type performances by depositing n-type perfluorocopper phthalocyanine on the transferred graphene surface with strong p and weak n. Based on the bipolar characteristics of the graphene / perfluorocopper phthalocyanine synaptic transistor with matching p-type and n-type performances, the simulation of multiplexed neural transmission of different neurotransmitters can be realized.

[0030] The beneficial effects of the present invention are:

[0031] 1. The graphene / perfluorophthalocyanine copper synaptic transistor prepared by the present invention has bipolar characteristics matching the p-type and n-type performances, and can simulate synaptic plasticity under both positive and negative gate voltages; and has different synaptic plasticity under positive and negative presynaptic pulse stimulations, and can respond to an EPSC of 83.64 μA under +4V presynaptic pulse stimulation, while the EPSC is 100.83 μA under -4V presynaptic pulse stimulation, which can simulate multiplexed neurotransmission of different neurotransmitters;

[0032] 2. The graphene / perfluorophthalocyanine copper synaptic transistor prepared by the present invention can achieve rapid switching of short-range / long-range plasticity by switching the positive and negative polarity of the presynaptic pulse stimulation applied by the gate and changing the type of carriers (electrons or holes) transmitted in the channel; the long-term plasticity of the synapse can be achieved under 30 consecutive pulse stimulations with an amplitude of -4V, and when 30 consecutive pulse stimulations with an amplitude of +4V are continued, the long-term plasticity of the synapse can be quickly switched to short-term plasticity, thereby achieving rapid switching of long-range and short-range plasticity; bipolar synaptic devices with matching p-type and n-type performance and rapid switching of short-range / long-range plasticity are helpful in building a neuromorphic system with diverse functions. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 It is a schematic diagram of the structure of the synaptic transistor based on graphene / perfluorocopper phthalocyanine in the present invention.

[0034] Figure 2 The transfer curve of the single graphene film synaptic transistor obtained by transfer in Example 2, the applied source-drain voltage is +0.01V.

[0035] Figure 3 This is the transfer curve of the graphene / perfluorophthalocyanine copper synaptic transistor obtained in Example 1, and the applied source-drain voltage is +0.01V.

[0036] Figure 4 Graph showing the postsynaptic current response of the graphene / perfluorophthalocyanine copper synaptic transistor obtained in Example 1 to gate voltage stimulation of different polarities, wherein: Figure 4 (a) is the postsynaptic current response diagram with the applied gate voltage of +4V and source-drain voltage of +0.01V; Figure 4 (b) is the postsynaptic current response diagram when the applied gate voltage is -4V and the source-drain voltage is +0.01V.

[0037] Figure 5 To simulate the rapid switching of short-range / long-range plasticity of the graphene / perfluorophthalocyanine copper synaptic transistor obtained in Example 1, the gate voltage applied was a sequence of 30 continuously switched +4V or -4V pulses, and the source-drain voltage was +0.01V. DETAILED DESCRIPTION

[0038] The present invention is described below in conjunction with examples, but the present invention is not limited to the scope of the examples.

[0039] The copper foil with graphene film grown on it was purchased from Hangzhou Hangdan Optoelectronics Technology Co., Ltd. The graphene film was grown on the surface of the copper foil by chemical vapor deposition (CVD) technology. The grown graphene was a single-layer graphene, and the thickness of the copper substrate was 30 to 50 μm.

[0040] The structure of the graphene / perfluorophthalocyanine copper synaptic transistor in the present invention is shown in FIG. Figure 1 As shown, from bottom to top, they are the substrate, bipolar graphene / perfluorophthalocyanine copper with matching p-type and n-type performance, the surface of the graphene / perfluorophthalocyanine copper film is a vapor-deposited parallel metal electrode, and the ion glue gate dielectric layer is between the source and drain electrodes;

[0041] Embodiment 1:

[0042] 1) 2×2cm Si / SiO 2 The substrate was ultrasonically cleaned with deionized water, acetone, and isopropanol, and then with N 2 Blow dry the surface for later use;

[0043] 2) Spin-coating the PMMA solution onto the front side of the copper foil on which the graphene film (about 1.6 nm) is grown, to obtain a graphene / PMMA film attached to the surface of the copper foil; the total thickness of the graphene / PMMA film is about 25 nm;

[0044] The mass concentration of the PMMA solution is 4%, the solvent is chlorobenzene, and the spin coating speed and time of the PMMA solution are 3000 r / min and 60 s;

[0045] 3) transferring the copper foil with the graphene / PMMA film attached in step 2) to the surface of the etching solution so that it floats on the surface of the solution, and etching the copper foil substrate with the graphene / PMMA film attached in step 3) by wet etching to obtain a polymer-supported graphene / PMMA film;

[0046] The etching time of copper foil is 4h, and the etching solution is (NH 4 ) 2 S 2 O 8 Solution, concentration 0.1mol / L;

[0047] 4) Using the Si / SiO obtained in step 1) 2 Substrate: fish out the graphene / PMMA film obtained in step 3) and dry it to obtain a graphene / PMMA film attached to the substrate;

[0048] 5) placing the graphene / PMMA film attached to the substrate in acetone, acetone:isopropanol=1:1, and isopropanol solution in turn to remove PMMA, thereby obtaining a single-layer graphene film attached to the substrate;

[0049] 6) Take 20 mg of perfluorophthalocyanine copper material and put it into the evaporation boat in the vacuum chamber of PVD, then fix the substrate with the graphene film transferred on the substrate holder in the chamber, and evacuate the chamber to Perfluorophthalocyanine copper was deposited at a deposition rate of , and finally a graphene / perfluorophthalocyanine copper film was obtained, and the film thickness was about 23.4nm;

[0050] The chamber was evacuated to 5×10 -4 Pa, the temperature of the evaporation boat is about 380℃;

[0051] 7) using a mask, evaporating 80 nm thick, spaced metal source and drain electrodes on the surface of the graphene / perfluorophthalocyanine copper film obtained in step 6); wherein the metal is gold, and the spacing between the source and drain electrodes is 100 μm;

[0052] 8) PVDF-HFP, EMIM-TFSI ionic liquid and acetone in a mass ratio of 1:3:7 were mixed and stirred, and after being fully dissolved, the mixed solution was drop-coated on a clean glass slide, and after drying, an ion gel film with a thickness of 200 μm was obtained;

[0053] 9) attaching the ion glue gate dielectric layer to the graphene / perfluoro copper phthalocyanine film between the source and drain electrodes, and finally preparing the graphene / perfluoro copper phthalocyanine synaptic transistor;

[0054] 10) The electrical properties of the graphene / perfluorophthalocyanine copper synaptic transistor are tested and analyzed using a semiconductor test analyzer.

[0055] Figure 1 The schematic diagram of the structure of the synaptic transistor based on graphene / perfluorophthalocyanine copper of the present invention is shown in FIG. A source-drain voltage of +0.01 V is applied to both ends of the source-drain electrode by a Keithley 4200A semiconductor analyzer, a presynaptic stimulus is applied to the ion-glued gate dielectric layer, and then the synaptic plasticity of the device is measured by adjusting the presynaptic stimulus.

[0056] Figure 2 For example 2, the Si / SiO 2 The transfer curve of the single graphene synaptic transistor on the substrate was obtained by testing with Keithley 4200A semiconductor analyzer, and the gate voltage scanning range was +5V to -5V. It can be found that the Dirac point of the single graphene synaptic transistor shifts toward the positive direction of the gate voltage. This is because during the transfer process of the graphene film, impurities such as water molecules and oxygen molecules in the air and PMMA in the polymer support layer will be adsorbed on the graphene surface, making the graphene transistor show a strong p and weak n bipolar characteristic.

[0057] Figure 3The transfer curve of the graphene / perfluorophthalocyanine copper synaptic transistor prepared in Example 1 was obtained by testing with a Keithley 4200A semiconductor analyzer, and the gate voltage scanning range was also +5 V to -5 V. By comparison, it can be found that after a layer of n-type semiconductor perfluorophthalocyanine copper is evaporated on the surface of the transferred graphene, the n-type semiconductor characteristics of the device are enhanced, and a bipolar synaptic transistor with matching n-type and p-type semiconductor performance is obtained.

[0058] Figure 4 The synaptic plasticity simulation of the graphene / perfluorophthalocyanine copper synaptic transistor prepared in Example 1 was performed using a Keithley 4200A semiconductor analyzer. Figure 4 In a, under the stimulation of +4V presynaptic pulse, EMIM cations in the ionic colloid moved to the interface between the ionic colloid and the graphene / perfluorophthalocyanine copper channel and accumulated at the interface, thereby inducing electron carriers in the graphene / perfluorophthalocyanine copper channel, forming an EPSC of 83.64μA; under the stimulation of -4V presynaptic pulse, TFSI anions in the ionic colloid accumulated at the interface of the graphene / perfluorophthalocyanine copper channel, causing the accumulation of hole carriers, resulting in an EPSC of 100.83μA ( Figure 4 b) Under positive and negative presynaptic pulse stimulation, the graphene / perfluorophthalocyanine copper synaptic transistor has different synaptic plasticity, which can simulate the multiplexed neurotransmission of different neurotransmitters.

[0059] Figure 5 This is a simulation of the rapid switching of long-range plasticity and short-range plasticity of the graphene / perfluorophthalocyanine copper synaptic transistor prepared in Example 1. The device was tested by a Keithley 4200A semiconductor analyzer, and the gate voltage pulse sequence applied consisted of 30 consecutive pulse stimuli with an amplitude periodically switched between -4V and +4V. Applying 30 consecutive pulse stimuli with an amplitude of -4V can achieve long-term plasticity of the synapse, and then applying 30 consecutive pulse stimuli with an amplitude of +4V can quickly switch the long-term plasticity of the synapse to short-term plasticity, thereby achieving rapid switching of long-range / short-range plasticity.

[0060] It can be seen from the above tests and spectra that the graphene / perfluorophthalocyanine copper synaptic transistor obtained by the present invention can be used to simulate synaptic plasticity mediated by two different excitatory neurotransmitters, such as dopamine and glutamate.

[0061] That is, when a presynaptic pulse with positive polarity is applied through the gate, electron carriers can be induced in the graphene / perfluorocopper phthalocyanine bipolar channel to form an excitatory postsynaptic current, which can simulate synaptic plasticity mediated by a neurotransmitter, such as glutamate neurotransmitter; under the presynaptic pulse stimulation with negative polarity, hole carriers can be induced in the graphene / perfluorocopper phthalocyanine bipolar channel, which can simulate synaptic plasticity mediated by another neurotransmitter, such as dopamine neurotransmitter; after 30 consecutive +4V presynaptic pulse stimulations, the EPSC retention rate is less than 50%, realizing the simulation of short-range plasticity, and after 30 consecutive -4V presynaptic pulse stimulations, the EPSC retention rate is greater than 50%, realizing the simulation of long-range plasticity, and further by switching the positive and negative polarity of the presynaptic pulse stimulation applied by the gate, the rapid switching of short-range / long-range plasticity can be realized.

[0062] Embodiment 2:

[0063] 1) 2×2cm Si / SiO 2 The substrate was ultrasonically cleaned with deionized water, acetone, and isopropanol, and then with N 2 Blow dry the surface for later use;

[0064] 2) spin coating the PMMA solution onto the front side of the copper foil on which the graphene film is grown, to obtain a graphene / PMMA film attached to the surface of the copper foil; wherein the thickness of the graphene film is about 1.6 nm, and the total thickness of the graphene / PMMA film is about 25 nm;

[0065] The mass concentration of the PMMA solution is 4%, the solvent is chlorobenzene, and the spin coating speed and time of the PMMA solution are 3000 r / min and 60 s;

[0066] 3) transferring the copper foil with the graphene / PMMA film attached in step 2) to the surface of the etching solution so that it floats on the surface of the solution, and etching the copper foil substrate with the graphene / PMMA film attached in step 3) by wet etching to obtain a polymer-supported graphene / PMMA film;

[0067] The etching time of copper foil is 4h, and the etching solution is (NH 4 ) 2 S 2 O 8 Solution, concentration 0.1mol / L;

[0068] 4) Using the Si / SiO obtained in step 1) 2 Substrate: fish out the graphene / PMMA film obtained in step 3) and dry it to obtain a graphene / PMMA film attached to the substrate;

[0069] 5) placing the graphene / PMMA film attached to the substrate in acetone, acetone:isopropanol=1:1, and isopropanol solution in turn to remove PMMA, thereby obtaining a single-layer graphene film attached to the substrate;

[0070] 6) using a mask, evaporating 80 nm thick metal source and drain electrodes spaced apart on the surface of the single-layer graphene film obtained in step 5); wherein the metal is gold, and the spacing between the source and drain electrodes is 100 μm;

[0071] 7) PVDF-HFP, EMIM-TFSI ionic liquid and acetone in a mass ratio of 1:3:7 were mixed and stirred, and after being fully dissolved, the mixed solution was drop-coated on a clean glass slide, and after drying, an ion gel film with a thickness of 200 μm was obtained;

[0072] 8) attaching the ion glue gate dielectric layer to the graphene / perfluoro copper phthalocyanine film between the source and drain electrodes, and finally preparing the graphene / perfluoro copper phthalocyanine synaptic transistor;

[0073] 9) The electrical properties of the graphene / perfluorophthalocyanine copper synaptic transistor are tested and analyzed using a semiconductor test analyzer.

[0074] It can be seen from the above embodiments that the present invention deposits n-type perfluorocopper phthalocyanine on the surface of the transferred graphene film with strong p and weak n, thereby preparing a graphene / perfluorocopper phthalocyanine synaptic transistor with bipolar characteristics matching p-type and n-type performance. The synaptic transistor can realize the simulation of multifunctional synaptic plasticity. Based on the bipolar characteristics of the graphene / perfluorocopper phthalocyanine synaptic transistor, by adjusting the positive and negative gate voltage and changing the working carriers, the simulation of multiplexed neural transmission of different neurotransmitters is realized, and the rapid switching of short-range / long-range plasticity mediated by different neurotransmitters is realized. The construction strategy of bipolar synaptic devices with matching p-type and n-type performance promotes the simulation of multi-channel neural transmission and has potential application prospects in the fields of bionics and bio-integrated electronics.

[0075] Matters not covered by the present invention are known technologies.

Claims

1. A synaptic transistor based on graphene / perfluorocopper phthalocyanine, characterized by The structure of the synaptic transistor from bottom to top is substrate, functional layer, source-drain electrode and ion glue gate dielectric layer. Wherein, the substrate is glass, Si / SiO2, PEN or PET substrate; The functional layer is a graphene / perfluorophthalocyanine copper film with a thickness of 2.5 to 25 nm; wherein the graphene film has a thickness of 0.5 to 5 nm; The source and drain electrodes are evaporated metal electrodes, the metal is gold, copper or silver, and the thickness is 40 to 80 nm; The material of the ion glue grid dielectric layer is [PVDF-HFP] [EMIM-TFSI], and the thickness is 100-500 μm.

2. The method for preparing a synaptic transistor based on graphene / perfluorophthalocyanine copper as claimed in claim 1, characterized in that The following steps are involved: 1) The substrate was ultrasonically cleaned with deionized water, acetone, and isopropanol, and then its surface was blown dry with nitrogen (N2) for standby use; 2) spin coating a polymethyl methacrylate (PMMA) solution onto the front surface of the copper foil on which the graphene film is grown, to obtain a graphene / PMMA film attached to the surface of the copper foil; The mass concentration of the PMMA solution is 2-10%, the solvent is chlorobenzene, the spin coating speed of the PMMA solution is 2000-4000 r / min, and the spin coating time is 40-80 s; 3) transferring the copper foil with the graphene / PMMA film attached in step 2) to the surface of the etching solution, floating for 2 to 8 hours, etching away the copper foil substrate, and obtaining a polymer-supported graphene / PMMA film; Wherein, the etching solution is an ammonium persulfate ((NH4)2S2O8) solution with a concentration of 0.1 to 1 mol / L; 4) using the substrate obtained in step 1) to fish out the graphene / PMMA film obtained in step 3) and dry it to obtain a graphene / PMMA film attached to the substrate; 5) placing the graphene / PMMA film attached to the substrate in acetone, a mixed organic solvent, and an isopropanol solution in turn to remove PMMA, thereby obtaining a single-layer graphene film attached to the substrate; The mixed organic solvent consists of acetone and isopropanol, and the volume ratio of the two is 1:1; 6) placing the perfluorophthalocyanine copper in an evaporation boat in a vacuum chamber of physical vapor deposition (PVD), and then fixing the substrate with the graphene film transferred on a substrate holder in the chamber, and starting to deposit the perfluorophthalocyanine copper after the chamber is evacuated to finally obtain a graphene / perfluorophthalocyanine copper film; The chamber is evacuated to 1×10 -4 Pa~1×10 -3 Pa; the deposition rate of perfluorophthalocyanine copper is The deposition time is 2 to 20 minutes; 7) using a mask, evaporating 40-80 nm thick and spaced metal source and drain electrodes on the surface of the graphene / perfluorophthalocyanine copper film obtained in step 6); 8) Mix and stir PVDF-HFP, EMIM-TFSI ionic liquid and acetone in a mass ratio of 1:3 to 5:7, and after fully dissolving, drop the mixed solution onto a glass slide, and dry to obtain an ion gel film with a thickness of 100 to 500 μm; 9) attaching the ion glue gate dielectric layer to the graphene / perfluorocopper phthalocyanine film between the source and drain electrodes, and finally preparing the graphene / perfluorocopper phthalocyanine synaptic transistor.

3. The application of the graphene / perfluorocopper phthalocyanine based synaptic transistor as claimed in claim 1, characterized in that it is used to simulate synaptic plasticity mediated by different excitatory neurotransmitters.

4. The application of the graphene / perfluorocopper phthalocyanine based synaptic transistor as claimed in claim 3, characterized in that the simulated different excitatory neurotransmitters are dopamine and glutamate.

Citation Information

Patent Citations

  • Preparation method of double-excitability artificial synaptic device for simulating multiplexing of biological synaptic neurotransmitter

    CN112201750A