Membrane composition

By using acid copolymer and polyvinyl film composition in flexible packaging materials, combining high-density polyethylene and metal deposited layers, the problem of lack of barrier properties of polyethylene films in the prior art is solved, and high under low thickness is achieved The laminate with oxygen and water vapor barrier properties reduces costs and improves recycling.

CN118946626APending Publication Date: 2024-11-12HUHTAMAKI INDIA LIMITED
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280093584.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-01-31
Filing Date
2022-11-18
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

While existing flexible packaging materials achieve barrier protection, heat sealing capability and printing performance at low thickness, they are difficult to meet high barrier requirements. In addition, polyethylene film lacks barrier properties when used as a sealant, and need to be used with other additional barrier films. The thickness and complexity of the laminate are increased, resulting in increased costs.

Method used

Using highs containing 1 to 10% acid copolymer, 5 to 15% metallocene linear low density polyethylene, 5 to 10% low density polyethylene, 0.5 to 1% anti-blocking masterbatch, 20 to 50% high The film composition of density polyethylene, 5 to 30% plastic and 0.5 to 1% slip additives form a barrier film with a metal-based deposition layer, and the bond strength of the polymer carrier layer and the metal-based material is improved to achieve High oxygen and water vapor barrier properties.

Benefits of technology

The required barrier protection and heat sealing capabilities are achieved at lower thicknesses while reducing the overall thickness and weight of the laminate, reducing the amount and cost of plastics, and facilitates recycling when the film comes from the same polymer family .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118946626A_ABST
    Figure CN118946626A_ABST
Patent Text Reader

Abstract

The present invention relates to a film composition comprising 1 to 10% of an acidic copolymer, 5 to 15% of a metallocene linear low density polyethylene (LLDPE), 5 to 10% of a low density polyethylene (LDPE), 0.5 to 1% of an anti-blocking masterbatch, 20 to 50% of a high density polyethylene (HDPE), 5 to 30% of a plastomer, and 0.5 to 1% of a slip additive. The invention also relates to a film made from said film composition and to a laminate made from said film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a film composition. More specifically, the present invention relates to a film composition with excellent barrier properties widely used in packaging applications and a laminate made therefrom. The present application also relates to a barrier film, which is particularly suitable for forming packaging materials, such as a multilayer structure as a basis to form a flexible package. The present application also relates to a multilayer structure containing a barrier film, and a flexible package formed from the multilayer structure. Background Art

[0002] Flexible packaging solutions are used in beverages, food, consumer packaged goods, personal care products and other fields. With the continuous improvement of consumer needs and requirements, flexible packaging solutions are also constantly evolving. Flexible laminates used for packaging are usually customized according to the needs of the packaged products. Although barrier properties, durability, etc. are still the basic requirements of flexible packaging solutions, it is equally important to retain product characteristics (such as aroma, crispness, etc.). Different types of laminates are used in the industry depending on the product, its storage environment, geographical location of use, packaging size, etc.

[0003] Packaging materials are either monolayer films or made of at least two layers, where each layer requires inherent key properties to perform its role. Typically, laminates with barrier properties contain at least two or three layers / substrates, namely a printed substrate, a barrier substrate and / or a sealing substrate. Depending on the barrier requirements of the product to be packaged, the laminate can have a dedicated barrier layer or can contain a film with barrier properties sufficient to protect the product. The most commonly used barrier substrates in flexible packaging are metallized PET, metallized BOPP, aluminum foil, biaxially oriented polyamide (also known as BOPA, polyamide), metallized CPP, etc. Polyethylene films in flexible packaging are mainly used as sealing substrates, but there are some notable exceptions, such as when they contain EVOH, they are also used as barrier films for specific products (such as cheese, red meat, etc.). However, the use of polyethylene as a barrier is more of an exception than the norm.

[0004] Although the utility of polyethylene films as sealants has long been established, their lack of barrier properties is a disadvantage for packaging applications because they need to be used with other additional barrier films (as described above), thereby increasing the overall laminate thickness, complexity and, therefore, cost. In other words, high-barrier laminate designs in the industry are usually at least three layers (industry jargon is called "three ply"), where the polyethylene film is used as a sealant and the other films meet additional requirements such as printing and barrier. In a few cases, two-layer laminates can also be used as "low or medium" barrier laminates, which are usually composed of PET or BOPP films laminated to polyethylene films containing EVOH as printed films. There are other examples of two-layer laminates that are used to package low / medium barrier product requirements, such as BOPP / BOPP for biscuits, BOPP / MetBOPP for biscuits and candies, BOPP / METCPP for snacks, etc. However, all of these laminates are generally classified as low / medium barrier two-layer laminates, while the laminates required for key product applications (e.g., coffee, yeast, dry soup powder, infant formula, etc., to name a few) must be three-layer laminates containing specially designed barrier films (e.g., aluminum foil, metallized PET, metallized BOPP, etc.), as described above.

[0005] Barrier properties are essentially the ability of a material to restrict the passage of gases or vapors. The barrier requirements (higher or lower) of a laminate depend mainly on the nature of the packaged product, the size of the package and the expected shelf life after packaging. The more sensitive the product (hygroscopic, oxygen, moisture sensitivity), the higher the barrier requirements of the laminate and vice versa.

[0006] To determine barrier requirements and to determine barrier performance, two properties are typically used: Water Vapor Transmission Rate (MVTR), which is measured at 38°C and 90% RH and is expressed in grams / m 2 / day; and oxygen transmission rate (OTR), which is measured at 23°C and 0-50% RH in CC / m 2 / sky.

[0007] Material source reduction and recyclability are also ongoing goals for the flexible packaging industry. However, when the thickness of the laminate is reduced, the barrier properties and strength of the film are compromised.

[0008] Therefore, there is a need for a laminate that can achieve the desired barrier protection, heat seal ability and desired printing properties at a relatively low thickness, while being useful as packaging for different products having specific properties. Summary of the invention

[0009] In one aspect, the present invention provides a film composition comprising 1 to 10% of an acid copolymer, 5 to 15% of a metallocene linear low density polyethylene (LLDPE), 5 to 10% of a low density polyethylene (LDPE), 0.5 to 1% of an anti-blocking masterbatch, 20 to 50% of a high density polyethylene (HDPE), 5 to 30% of a plastomer, and 0.5 to 1% of a slip additive.

[0010] In another aspect, the present invention provides a film formed or prepared using the above film composition, wherein the film can be metallized or non-metallized.

[0011] In another aspect, the present invention provides a laminate comprising a first film; and a second film bonded to the first film, the second film comprising a metallized or non-metallized film, the film having a composition of the following ingredients: 1 to 10% of an acid copolymer, 5 to 15% of a metallocene linear low density polyethylene (LLDPE), 5 to 10% of a low density polyethylene (LDPE), 0.5 to 1% of an anti-blocking masterbatch, 20 to 50% of a high density polyethylene (HDPE), 5 to 30% of a plastomer, and 0.5 to 1% of a slip additive.

[0012] In other words, from a different perspective, the present application relates to a barrier film particularly suitable for forming a packaging material, for example as a base multilayer structure to form a flexible packaging body. The barrier film comprises a polymer carrier layer. The carrier layer carries a deposited layer of a metal-based material on at least one surface thereof. The polymer of the carrier layer contains a linear ethylene-based polymer.

[0013] Such barrier films with a polymeric carrier layer having a metal-based deposited layer deposited on at least one surface thereof are widely used in the packaging industry and can be found in many multilayer materials suitable and intended to form flexible packaging bodies such as bags, flow-wraps, etc.

[0014] A barrier film of the above general type as part of a multilayer structure is known, for example, from WO 2014 / 209411 A1. This document discloses an attempt to improve the otherwise generally poor bond strength between a polyethylene substrate or carrier layer and a metallized film applied to the substrate layer. WO 2014 / 209411 A1 teaches improving the bond strength by forming at least 50% by weight of an ethylene / α-interpolymer whose comonomer distribution constant is within a specific value range.

[0015] The carrier layer material of such a barrier film is rather difficult to synthesize.

[0016] The metal-based deposited layer significantly reduces the permeability of the barrier film to oxygen and water vapor (also commonly referred to as "moisture" in the prior art) compared to the carrier layer alone. Therefore, the metal-based deposited layer helps to a large extent to extend the shelf life of the packaged product, which would otherwise oxidize prematurely and / or accumulate moisture and soften, and eventually decay prematurely. Therefore, a universal type of barrier film is used for the packaging of food and other perishable products.

[0017] In addition to the focus of the present invention, namely oxygen and water vapor barrier properties, the metal-like deposited layer can also provide a metal-like appearance and enhance the aesthetics of the package when visible from the outside, depending on the respective deposited material.

[0018] Additionally, again depending on the respective deposited material, a metallic type deposited layer may render the deposited layer electrically conductive and thus provide a Faraday cage within the package, isolating the packaged objects from the electric fields outside the package.

[0019] Likewise, the conductive deposited layer exposed inside the flexible packaging body surrounding the packaging volume can serve to equalize the potential on the packaged product, thereby protecting sensitive electronic components contained within the packaging volume.

[0020] Before the increasing use of deposited metal-like materials on polymeric carrier layers, aluminum foil was laminated onto polymer films to provide layer structures with enhanced oxygen and water vapor barrier properties. However, aluminum foil is no longer preferred due to the high resource consumption of providing aluminum foil and the complex recycling process of laminates containing aluminum foil after use.

[0021] The deposited metal-based deposit layer is much thinner than the laminated aluminum foil. Typically, the aluminum foil in the flexible packaging laminate is 20 to 50 times thicker than the deposit layer used in the flexible packaging film.

[0022] This fragile deposit requires a polymer carrier layer deposited thereon to provide a reliable barrier effect, but is very susceptible to any adverse effects that may occur during or after the production of the barrier film.

[0023] It is therefore an object of the present invention to provide a barrier film of the generic type as set out at the beginning of the application, which has a reliable and durable metal-based deposit which provides the barrier film with strong oxygen and water vapor barrier properties over a long period of time.

[0024] The present invention achieves this object, wherein the polymer of the carrier layer comprises a mixture of low-density polyethylene, a linear vinyl polymer and at least one receptor component selected from the group consisting of:

[0025] i) a terpolymer of ethylene, acrylic acid and an acrylic ester, and

[0026] ii) Ethylene-based α-copolymers grafted with polar groups.

[0027] For example, the receptor component of the above type i) can be a polymer with the trade name "Nucrel™ AE", distributed by The Dow Chemical Company Global Dow Center, 2211 H.H. Dow Way, Midland, Michigan 48674 (US) and its affiliated companies. A possible receptor component of the above type ii) is a polymer with the trade name "Tafmer™ MA 9015", distributed by Mitsui Chemicals, Inc., Shiodome City Center, 5-2, Higashi-Shimbashi 1-chome, Minato-ku, Tokyo 105-7122 and its affiliated companies. Of course, corresponding receptor materials provided by other suppliers can also be used.

[0028] The inventors have shown in laboratory results that the combination of components forming the basic composition of the polymer carrier layer (mainly the polyethylene layer) greatly improves the bonding strength between the metal-based deposit layer and the carrier layer. The bonding strength between the metal-based deposit layer and the carrier layer reaches a peel strength of at least 2N per 15 mm as measured according to AIMCAL-TP-105-92.

[0029] The deposited layer can be produced by any known vapor deposition process, for example by physical vapor deposition or chemical vapor deposition. In order to avoid any unexpected and undesired chemical loading of the support layer, physical vapor deposition of the metal-based material is preferred.

[0030] The metal-based material can be any material containing a metal. Therefore, the metal-based material of the deposited layer includes at least one of a metal and a metal oxide. As the metal, aluminum is preferred, but any metal can be vapor deposited on the carrier layer, such as gold or silver or an alloy containing silver or aluminum. The deposition of the metal, i.e., metallization, can provide a shiny metallic appearance to the barrier film on one side of the deposited layer.

[0031] The barrier properties can also be significantly enhanced by depositing metal oxides on the surface of the support layer. Here, aluminum oxide (usually AlO x , especially Al2O3) or silicon oxide (usually SiO x ) is preferred. Such a deposited layer made of metal oxide is generally transparent and has little or no effect on the visual appearance of the barrier film when observing the deposited layer.

[0032] When the metal is deposited onto the support layer, it is preferably deposited to an optical density of at least 2.2, preferably at least 2.6, optionally even at least 2.8.

[0033] The linear vinyl polymer includes at least one of a linear low density polyethylene and a linear ethylene-octene copolymer, in particular an ethylene-1-octene copolymer. Experiments show that the maximum bonding strength between the metal deposition layer and the support layer can be achieved by using these linear vinyl polymers.

[0034] By using a metallocene linear ethylene polymer as a component of the linear ethylene polymer or as the linear ethylene polymer itself, the bonding strength between the deposited layer and the support layer can be further improved. Therefore, the linear ethylene polymer comprises a metallocene linear ethylene polymer or consists of a metallocene linear ethylene polymer.

[0035] As used in this application, the term "polymer" encompasses all possible types of polymeric materials, such as homopolymers, copolymers, terpolymers, etc., regardless of the number of different monomers used to form the polymer. In contrast, the term "copolymer" refers to a polymer of two different monomers, the term "terpolymer" refers to a polymer of three different monomers, and so on.

[0036] Regarding the proportions of the components that must be present in the carrier layer polymer,

[0037] i) the weight ratio of the receptor component in the total weight of the polymer carrier layer is 26 to 34% by weight,

[0038] ii) the weight ratio of the linear ethylene polymer in the total weight of the polymer carrier layer is 44 to 46 weight %, and

[0039] iii) The weight proportion of the low-density polyethylene in the total weight of the polymer carrier layer is 15 to 21 wt%.

[0040] The polymer of the polymeric support layer represents 100 wt%. This means that the sum of the weight percentages of the receptor component, linear vinyl polymer and low density polyethylene does not exceed 100, but can be less if other components contribute to the formation of the support layer polymer.

[0041] The mixture of the acceptor component, the linear vinyl polymer and the low density polyethylene is generally viscous and therefore may be difficult, but not impossible, to process on existing machinery. To facilitate mechanical processing of the polymer of the support layer, and thus facilitate mechanical processing of the support layer, the polymer of the support layer preferably comprises an anti-blocking agent. The anti-blocking agent increases the weight of the polymer of the polymer support layer.

[0042] Basically, the antiblocking agent can be any known and used antiblocking agent. Preferably, the useful antiblocking agent comprises or consists of mineral silica compounded in polyethylene. When compounded into polyethylene, the antiblocking agent is easily mixed into the remaining polymer of the carrier layer.

[0043] The proportion or weight ratio of the antiblocking agent in the total weight of the polymer carrier layer is preferably 1.4 to 2.6% by weight, so that it has an antiblocking effect without affecting other properties of the carrier layer.

[0044] Preferably, the polymer carrier layer is a blown film. It can be blown into the outermost exposed layer of a monolayer or multilayer film. Preferably, the entire multilayer film can be made into a blown film. Nevertheless, it can also be partially or completely made into an extrusion laminated multilayer film.

[0045] The polymer carrier layer may contain the above components and may contain other additional components, such as dyes or colored pigments, as required. Since the carrier layer in practical applications is only one of several polymer layers of the packaging multilayer film, the preferred embodiment of the polymer carrier is composed of the following mixture:

[0046] i) low density polyethylene;

[0047] ii) linear vinyl polymers;

[0048] iii) terpolymers of ethylene, acrylic acid and acrylic acid esters; and

[0049] iv) Anti-blocking agents, as described above.

[0050] The barrier film explained and detailed above is usually only a key component or one of several key components of the entire packaging multilayer film.

[0051] Therefore, the present invention also relates to a multilayer film comprising a barrier film as described and refined above and further comprising at least one additional layer selected from the group of layers comprising at least the following layer types:

[0052] a) Main layer,

[0053] b) a sealable layer,

[0054] c) oxygen barrier layer,

[0055] d) a water vapor barrier, and

[0056] e) an adhesive resin (tie) layer,

[0057] The multilayer film may include multiple layers of the same layer type. Therefore, if necessary, the multilayer film may include more than two main layers. Usually one sealable layer is sufficient, but it is not excluded that the multilayer film can be designed to be sealable on both of its exposed outermost surfaces. Additional barrier layers can further enhance the barrier properties of the entire laminate.

[0058] The multilayer film is preferably a blown multilayer film. However, it can be formed partially or completely by extrusion lamination.

[0059] An oxygen barrier layer in the sense of the present application refers to a material layer having an oxygen transmission rate that is particularly lower than the average level. The oxygen transmission rate of the present invention is measured according to ASTM D 3985, the test environment atmosphere is adjusted to 23° C. and 0% relative humidity, i.e. dry atmosphere. In order to determine the oxygen transfer rate under humid conditions with an ambient atmosphere of 23° C. and a relative humidity of 50%, the measurement is carried out according to ASTM F1927.

[0060] A layer is an oxygen barrier layer if its oxygen transmission rate is less than 75% of that of a LLDPE reference layer of equal thickness when measured according to the above measurement criteria.

[0061] A water vapor barrier layer within the meaning of the present application is a material layer having a particularly below average water vapor transmission rate. The water vapor transmission rate of the present invention is measured according to ASTM F1249 in a tropical test environment atmosphere adjusted to 38° C. and 90% relative humidity.

[0062] A layer is a water vapour barrier layer if its water vapour transmission rate is less than 75% of that of a LLDPE reference layer of equal thickness when measured according to the above measurement standard.

[0063] The oxygen barrier layer can be formed, for example, from a vinyl alcohol polymer, in particular from an ethylene vinyl alcohol copolymer or from polyvinyl alcohol, wherein ethylene vinyl alcohol copolymer is preferred because it is based on ethylene like the components of the carrier layer, which makes the carrier layer and the oxygen barrier layer formed from EVOH advantageously recyclable in a single recycling stream. The vinyl alcohol polymer oxygen barrier layer, whether it is based on ethylene or polyethylene, preferably accounts for 5 to 12% by weight, more preferably 6 to 10% by weight, particularly preferably 7.5 to 8.5% by weight of the total weight of the packaging multilayer film.

[0064] The bulk layer may be arranged next to the carrier layer on either side of the carrier layer, ie on one side of the deposition layer and on the opposite side, wherein preferably no deposition layer is deposited on the carrier layer.

[0065] Although the carrier layer may carry the deposition layer on both of its outermost surfaces, it is preferred that the deposition layer is deposited on only one surface of the carrier layer. Preferably, in a flexible package formed from a multilayer film comprising the barrier film explained and detailed above, the surface of the carrier layer on which the deposition layer is deposited is closer to the outside (i.e. towards a possible consumer).

[0066] The bulk layer may be formed of any suitable polymer, such as polyethylene terephthalate (PET), polyamide (PA), in particular axially oriented polyamide (BOPA), polypropylene (PP), in particular biaxially oriented polyethylene (BOPP), and polyethylene (PE), in particular machine direction oriented polyethylene (MDO-PE), particularly preferably medium density polyethylene (MDPE) or high density polyethylene (HDPE), in order to provide stability and structure to the multilayer film. A high density polyethylene layer is used as the bulk layer because HDPE not only provides mechanical stability, but also provides a large amount of oxygen and, to a lesser extent, water vapor barrier properties.

[0067] According to a preferred embodiment, the main body layer can be formed by a mixture of HDPE and linear low-density polyethylene (LLDPE) to enhance the bonding strength between the carrier layer and the main body layer. In this case, HDPE can account for at least 70% by weight of the total weight of the single main body layer, preferably at least 72.5% by weight, and even more preferably at least 75% by weight. The HDPE content may also reach at least 96% by weight or even 100% by weight.

[0068] On the other hand, the HDPE content may preferably not exceed 92 wt %, may more preferably not exceed 90 wt %, and may particularly preferably not exceed 88 wt % of the total weight of the single main body layer.

[0069] The LLDPE content of the single main layer may preferably account for at least 15% by weight, more preferably at least 16% by weight, and particularly preferably at least 18% by weight. The LLDPE content of the single main layer may preferably not exceed 26% by weight, more preferably not exceed 24% by weight, and particularly preferably not exceed 22% by weight. The sum of the percentages of HDPE and LLDPE in the single main layer cannot exceed 100%, but if there are other components involved in the formation of the main layer, it may be slightly less than 100%.

[0070] If a body layer is laminated onto the deposited layer, the body layer may comprise a printed layer either in a conventionally printed or reverse printed manner, whereby, in the latter case, the body layer itself protects the print from external influences.

[0071] Alternatively, the bulk layer may be formed from HDPE only.

[0072] If there is a vinyl alcohol barrier layer in the multilayer film, it is preferably present on the side of the main layer and the carrier layer that is bonded away from the barrier film. In order to ensure sufficient bonding strength between the main layer and the vinyl alcohol barrier layer, an adhesive resin layer can be provided between the main layer and the vinyl alcohol barrier layer.

[0073] The adhesive resin layer may preferably be a mixture of LLDPE and a vinyl maleic anhydride grafted polymer, but other adhesive resin layer materials may also be used. The grafted polymer is preferably polyethylene, and particularly preferably LLDPE.

[0074] The LLDPE content in the adhesive resin layer (which refers to ungrafted LLDPE) is preferably at least 65% by weight, more preferably at least 67.5% by weight, and particularly preferably at least 70% by weight. On the other hand, in order not to impair the improvement in adhesive strength brought about by the ethylene-based maleic anhydride grafted polymer, the LLDPE content may preferably be not more than 90% by weight, more preferably not more than 87.5% by weight, and particularly preferably not more than 85% by weight.

[0075] Neglecting inevitable impurities, the ethylene-based maleic anhydride grafted polymer forms the remaining component so that the content of the ungrafted LLDPE is made up to 100% by weight of the adhesive resin layer.

[0076] A further bonding resin layer may be applied on the side of the vinyl alcohol barrier layer facing away from the bulk layer in order to bond the other layers to the vinyl alcohol barrier layer. The bonding resin layer on the side of the vinyl alcohol barrier layer facing away from the bulk layer and the barrier film preferably corresponds to the first bonding resin layer on the side facing the multilayer and the carrier layer, or at least deviates from the first bonding resin layer in composition by no more than 5% of the ungrafted LLDPE and the vinyl maleic anhydride grafted polymer, respectively.

[0077] The ethylene-based maleic anhydride grafted polymer in the adhesive resin layer is preferably maleic anhydride grafted LLDPE.

[0078] The second bulk layer and / or sealant layer may be bonded (eg by coextrusion or by lamination) and disposed to the second bonding resin layer on the side of the vinyl alcohol barrier layer facing away from the barrier film and the first bulk layer.

[0079] When the second bulk layer is bonded to the vinyl alcohol barrier layer via the second adhesive resin layer, the second bulk layer preferably corresponds in composition and thickness to the first bulk layer.

[0080] If the sealant layer is bonded to the vinyl alcohol barrier layer or can also be bonded directly to the above-mentioned bulk layer, the sealant layer may comprise a bimodal terpolymer linear low density polyethylene as a main component. The bimodal terpolymer LLDPE is preferably mixed with LDPE.

[0081] The content of bimodal terpolymer LLDPE in the sealing layer polymer is preferably at least 60 wt%, more preferably at least 65 wt%. On the other hand, it is preferably not more than 88 wt%, more preferably not more than 76 wt%.

[0082] The LDPE content in the sealing layer is preferably not less than 8.5 wt %, more preferably not less than 8.8 wt %, particularly preferably not less than 9.0 wt %. On the other hand, the LDPE content is preferably not more than 11.5 wt %, more preferably not more than 11.1 wt %, particularly preferably not more than 10.7 wt %.

[0083] The sealing layer may also contain a vinyl plastomer, which may preferably be selected from ethylene / 1-octene or 1-octene family. The vinyl plastomer content in the sealing layer is preferably at least 15 wt %, more preferably at least 15.5 wt %, particularly preferably at least 15.9 wt %. On the other hand, the vinyl plastomer content in the sealing layer is preferably no more than 23 wt %, more preferably no more than 21.5 wt %, particularly preferably no more than 20 wt %.

[0084] The seal layer is essentially the outermost layer of the multilayer film and may also contain functional agents such as anti-blocking agents and / or friction reducing and slipping agents. The anti-blocking agent is preferably the same as that in the carrier layer. The slipping agent is preferably a non-migrating slip additive compounded in polyethylene.

[0085] In one embodiment, the content of antiblocking agent in the sealing layer polymer is preferably 2.3 to 2.8 wt%, or in another embodiment, it is preferably 0.9 to 1.1 wt%. Similarly, in one embodiment, the content of slip agent in the sealing layer polymer is preferably 1.3 to 1.6 wt%, and in another embodiment, the content of slip agent is preferably 0.9 to 1.1 wt%.

[0086] As described above, another layer of the at least one additional layer, in particular the main layer, is bonded to the deposited layer so that the deposited layer is located between the polymer carrier layer and the other layer. An adhesive resin layer may be present between the deposited layer and the other layer, depending on the material used to form the other layer.

[0087] In order to be able to form a closed package from the multilayer film, at least one additional layer comprises a sealable layer forming an exposed surface of the multilayer film.

[0088] The invention also relates to a packaging body, in particular a flexible packaging body, comprising a multilayer film as described and refined above. The packaging body encloses a packaging volume. The packaging volume is suitable and intended to contain the objects packaged at the time.

[0089] The package can be any type of flexible package. Possible flexible packages can be strip packs, bags (especially four-side sealed bags or three-side sealed bags), stand-up bags, flow packs, etc.

[0090] The barrier properties of the above-described multilayer films, in particular due to the barrier properties of the barrier films with the deposited layer, enable the packaging of chemically aggressive products such as coffee, soup powders, and even products that are loaded into the package in a hot state, such as ready-made instant foods.

[0091] Preferably, 90% by weight of the multilayer film consists of one material group, particularly preferably polymers with ethylene as monomer, so that the multilayer film can be easily recycled after use, preferably in a single recycling stream.

[0092] The designations "first", "second", "third", etc. used in this application are used only to distinguish similar or identically designated features. They are not used to indicate a certain order. Thus, the subject matter of the present invention may include first and third features of the same or similar type, but not the second feature. It may also include only the first feature, but not the second, third, or other substantially optional features of the same or similar type.

[0093] Based on the above description of the present invention from different perspectives, the following topics are particularly meaningful to the present invention, starting from Topic A:

[0094] A. A barrier film (12; 112), wherein the barrier film (12; 112) comprises a polymer carrier layer (14; 114), wherein the carrier layer (14; 114) carries a deposited layer (16; 116) of a metal-like material on at least one surface (14a; 114a) thereof, wherein the polymer of the carrier layer (14; 114) comprises a linear vinyl polymer,

[0095] Characterized in that the polymer of the carrier layer (14; 114) comprises a mixture of low-density polyethylene, a linear vinyl polymer and at least one receptor component selected from the following:

[0096] i) a terpolymer of ethylene, acrylic acid and an acrylic ester, and

[0097] ii) Ethylene-based α-copolymers grafted with polar groups.

[0098] B. The barrier film (12; 112) as described in subject A,

[0099] It is characterized in that the metal material of the deposited layer (16; 116) includes at least one of metal and metal oxide.

[0100] C. A barrier film (12; 112) as described in subject A or B,

[0101] Characterized in that the linear ethylene polymer includes at least one of a linear low-density polyethylene and a linear ethylene-octene copolymer.

[0102] D. A barrier film (12; 112) according to one of the preceding subjects,

[0103] Characterized in that the linear ethylene polymer includes a metallocene linear ethylene polymer or consists of a metallocene linear ethylene polymer.

[0104] E. A barrier film (12; 112) according to one of the preceding subjects,

[0105] It is characterized in that

[0106] i) the weight ratio of the receptor component in the total weight of the polymer carrier layer (14; 114) is 26 to 34 weight %,

[0107] ii) the weight ratio of the linear ethylene polymer in the total weight of the polymer carrier layer (14; 114) is 44 to 46 weight %, and

[0108] iii) the weight ratio of the low-density polyethylene in the total weight of the polymer carrier layer (14; 114) is 15 to 21% by weight,

[0109] The polymer of the polymer carrier layer (14; 114) represents 100% by weight.

[0110] F. A barrier film (12; 112) according to one of the preceding subjects,

[0111] It is characterized in that the polymer of the carrier layer (14; 114) contains an anti-adhesive agent.

[0112] G. The barrier film (12; 112) as described in subject F,

[0113] The invention is characterized in that the anti-blocking agent comprises or consists of mineral silicon dioxide compounded in polyethylene.

[0114] H. The barrier film (12; 112) as described in subject F or G,

[0115] It is characterized in that the weight proportion of the anti-adhesive agent in the total weight of the polymer carrier layer (14; 114) is 1.4 to 2.6 weight %.

[0116] I. A barrier film (12; 112) according to one of the preceding subjects,

[0117] It is characterized in that the polymer carrier layer (14; 114) is a blown film or is part of a blown multilayer film.

[0118] J. A barrier film (12; 112) according to one of the preceding subjects,

[0119] It is characterized in that the polymer of the carrier layer (14; 114) consists of a mixture of the following components:

[0120] i) low density polyethylene;

[0121] ii) linear vinyl polymers;

[0122] iii) terpolymers of ethylene, acrylic acid and acrylic acid esters; and

[0123] iv) Anti-blocking agents.

[0124] K. A multilayer film (10; 110) comprising a barrier film (12; 112) according to one of the preceding subjects and at least one additional layer selected from the group of layers comprising at least the following layer types:

[0125] a) Main layer (18, 22; 118, 122, 134),

[0126] b) a sealable layer (20; 120),

[0127] c) an oxygen barrier layer (128),

[0128] d) a water vapor barrier layer (134), and

[0129] e) an adhesive resin layer (130, 132),

[0130] The multilayer film (10; 110) may include multiple layers of the same layer type.

[0131] L. A multilayer film (10; 110) as described in subject L,

[0132] Characterized in that a further layer (22, 24, 26; 122, 124, 126) of at least one additional layer is bonded to the deposited layer (16; 116) such that the deposited layer (16; 116) is located between the polymer carrier layer (14; 114) and the further layer (22, 24, 26; 122, 124, 126).

[0133] M. A multilayer film (10; 110) as described in subject L or M,

[0134] Characterized in that the at least one additional layer comprises a sealable layer (20; 120) forming an exposed surface (10b; 110b) of the multilayer film (10; 110).

[0135] N. A packaging body (80) comprising a multilayer film (10; 110) as described in one of subjects L to N, wherein the packaging body (80) encloses a packaging volume (82), wherein the packaging volume (82) is suitable and intended to contain an object (86). BRIEF DESCRIPTION OF THE DRAWINGS

[0136] Reference will be made to embodiments of the present invention, examples of which may be illustrated in the accompanying drawings. These drawings are intended to be illustrative and not restrictive. Although the present invention is generally described in the context of these embodiments, it should be understood that it is not intended to limit the scope of the present invention to these specific embodiments.

[0137] Figure 1 A laminate according to an embodiment of the present invention is shown.

[0138] Figure 2 shows a schematic cross-sectional view of a second embodiment of a multilayer film according to the invention, comprising the barrier film described above,

[0139] Figure 3 A schematic cross-sectional view of a third embodiment of a multilayer film according to the present invention is shown, the multilayer film comprising the barrier film described above, and

[0140] Figure 4 Shown by Figure 2 or Figure 3 Illustrative examples of flexible packages formed from exemplary multilayer films. DETAILED DESCRIPTION

[0141] The present invention provides polyethylene films with excellent oxygen and moisture barrier properties while retaining other necessary properties such as heat sealability, machinability on packaging lines, product protection, etc. Laminates made using the films of the present invention provide barrier properties without the need to add a separate barrier layer while still maintaining heat sealability on the sealed side and heat resistance on the printed side. Eliminating the separate metallic or non-metallic barrier layers commonly used in laminates allows new laminate designs to be lower in thickness and weight, thereby reducing overall plastic usage and cost, and making them recyclable when the films used are from the same polymer family (single material).

[0142] In one aspect, the present invention provides a film composition comprising 1 to 10% of an acid copolymer, 5 to 15% of a metallocene LLDPE, 5 to 10% of a low density polyethylene (LDPE), 0.5 to 1% of an anti-blocking masterbatch, 20 to 50% of a high density polyethylene (HDPE), 5 to 30% of a plastomer, and 0.5 to 1% of a slip additive.

[0143] In one embodiment, the film composition further comprises 5 to 15% of medium density polyethylene (MDPE), 1 to 10% of an adhesive resin layer, and a maximum content of 7% of ethylene vinyl alcohol (EVOH, wherein the mol% content of ethylene is 27-40 mol%).

[0144] The acid copolymer in the film composition is selected from a terpolymer of ethylene, methacrylic acid and acrylate or an acid-modified olefin copolymer. The metallocene LLDPE includes a metallocene ethylene-octene copolymer. The LDPE includes a polyethylene with a minimum density of 0.910. The HDPE includes a polyethylene with a minimum density of 0.941. The adhesive resin layer includes a linear low-density polyethylene adhesive resin modified by maleic anhydride. The plastomer is selected from ethylene-1-octene or 1-octene. The slip additive is selected from erucamide, oleamide and / or stearamide compounded in polyethylene or a modified non-migrating polymer additive.

[0145] In one embodiment, the present invention provides a film formed using the composition as described above, wherein the film is further metallized and has an optical density equal to or greater than 2.2. In this regard, the film is metallized using a vacuum metallization process. During the metallization process, aluminum vapor is deposited on the film of the present invention using a vacuum coating machine. The aluminum metallization on the film of the present invention further improves the barrier level. In another embodiment, aluminum oxide (AlO) is deposited by a vacuum deposition process. x ) coating also improves the barrier properties of the film and has see-through characteristics. Therefore, the film has barrier properties embedded in the sealing layer.

[0146] In another embodiment, in order to further improve the barrier properties of the film, a water-based barrier coating may also be deposited / coated on both sides of the film before metallization.

[0147] As an alternative, instead of using EVOH as the resin in the film composition to improve barrier properties, a modified EVOH or PVOH coating may be applied in an off-line process.

[0148] In another aspect, the present invention provides a laminate. Figure 1A laminate 1000 according to an embodiment of the present invention is shown. The laminate comprises a first film 1010; and a second film 1020 bonded to the first film. The first film is preferably a printable film selected from the family of PET, BOPP, BOPE, MDO PE, BON, etc. The film may be reverse or surface printed. The second film is a film of the above invention, wherein the film is embedded in a sealing layer and has barrier properties. Therefore, the present invention eliminates the need for a separate barrier film. In one embodiment, the second film comprises a film composition of the following ingredients: 1 to 10% of an acid copolymer, 5 to 15% of a metallocene linear low density polyethylene (LLDPE), 5 to 10% of a low density polyethylene (LDPE), 0.5 to 1% of an anti-blocking masterbatch, 20 to 50% of a high density polyethylene (HDPE), 5 to 30% of a plastomer, and 0.5 to 1% of a slip additive. Furthermore, when the laminate of the present invention is designed with a PE film (MDO PE or BOPE or non-oriented PE, etc.) as the first film and the PE film of the present invention as the second film, the final laminate is more than 90% single material PE, so the recyclability level exceeds 90%.

[0149] In one embodiment, the film composition of the second film in the laminate further comprises 1 to 10% of an adhesive polymer, 5 to 15% of a medium density polyethylene (MDPE), and 0.1 to 7% of ethylene vinyl alcohol (EVOH), wherein the ethylene content of the EVOH is 27 to 40%.

[0150] The acid copolymer in the film composition of the laminate is selected from a terpolymer of ethylene, methacrylic acid and acrylate or an acid-modified olefin copolymer. The acid copolymer improves the adhesion of the plated metal to the base film and provides the best adhesion. The metallocene LLDPE includes a metallocene ethylene-octene copolymer and imparts mechanical strength to the film. LDPE includes polyethylene with a minimum density of 0.910 and plays an important role in the elongation of the film. Elongation is crucial for optimal processability. HDPE includes polyethylene with a minimum density of 0.941 and helps to improve the rigidity and barrier properties of the film. The adhesive resin layer includes a maleic anhydride-modified linear low-density polyethylene adhesive resin. The plastomer is selected from ethylene-1-octene or 1-octene and helps to reduce the sealing temperature of the composition, that is, provides an optimal sealing range and helps the convenience of processing. The slip additive is selected from erucamide, oleamide and / or stearamide compounded in polyethylene or a modified non-migrating polymer additive and helps to maintain the friction coefficient. Similarly, the adhesive resin layer enhances the adhesion between EVOH and the film component. MDPE provides rigidity and maintains a balance between density and mechanical strength. EVOH imparts barrier properties, more particularly oxygen barrier properties.

[0151] The laminates are suitable for forming packaging with barrier properties equivalent to or better than laminates using barrier films such as acrylic coated biaxially oriented polypropylene (BOPP), metallized BOPP, AlOx coated BOPP, SiOx coated BOPP, metallized cast polypropylene (CPP).

[0152] In another embodiment of the present invention, the laminate produced using the film of the present invention may additionally include a layer selected from the following (but not limited thereto): a printing / ink layer, an adhesive layer, a primer layer, an extrusion lamination layer, an extrusion coating, a (matte) paint layer, etc. In addition, depending on the functional requirements of the product to be packaged, the laminate produced using the film of the present invention may also include an additional barrier layer, a printing layer or a sealant layer, so that the final laminated composite material becomes a three-layer, four-layer, or five-layer laminate.

[0153] On the other hand, the present invention also relates to a method for manufacturing the film of the present invention using a blown film extrusion process, the method preferably comprising the following steps: melting a polymer resin in an extruder; extruding the polymer resin melt through a die and injecting air to radially expand the polymer into a hot capillary according to the desired film thickness and width; continuously cooling the hot capillary while moving upward through a high-speed air ring installed on the top of the die until it passes through a clamping roller; flattening the cooling tube that reaches the clamping roller to form a collapsed tube or a flat film; conveying the flat film to an extrusion tower via rollers; and winding the flat film onto a reel.

[0154] In a preferred embodiment of the process, air exchange occurs inside the bubbles as the flat film is on its way to the extrusion tower on a higher output line. This is called internal bubble cooling or IBC. Therefore, the process involves critical control of the internal bubble cooling (IBC) and OBC (external bubble cooling) temperature settings, typically maintained at 10°C to 30°C for both IBC and OBC, and a blow-up ratio equal to or greater than 2 is maintained.

[0155] Example

[0156] The following experimental examples are used to illustrate the present invention, but do not limit its scope:

[0157] Example 1

[0158] Membrane components % Ethylene-methacrylic acid and acrylic acid ester terpolymer 5.4 Ethylene-1-octene plastomer 6.6 Metallocene ethylene-octene copolymer 11.0 Low density polyethylene resin 3.96 Mineral silica anti-adhesive compounded in polyethylene 0.44 High-density polyethylene 44.6 Bimodal terpolymer linear low density polyethylene 24.5 Low density polyethylene 2.8 Mineral silica anti-adhesive compounded in polyethylene 0.35 Non-migrating slip additive compounded in polyethylene 0.35

[0159] The film prepared using the components of Example 1 was further metallized using a vacuum metallization process. During the metallization process, a vacuum coating machine was used to deposit the vapor of aluminum or aluminum oxide (ALOx) on the film layer. The aluminum layer on the film of Example 1 further improved the barrier properties.

[0160] The barrier value of the film of Example 1 of the present invention before and after metallization was tested, and the results obtained are as follows:

[0161]

[0162] From the results, it can be seen that the metallized film exhibits excellent barrier values.

[0163] Furthermore, from the results obtained it can be seen that the metallized film also exhibits excellent interlayer adhesion strength between the metal and the substrate PE film, which enables the highest quality packaging laminates to be achieved.

[0164] The non-metallized film prepared using the components of Example 1 is suitable for packaging products requiring a medium barrier level (e.g., cereals, cookies, crackers, etc.) when laminated to standard polyethylene terephthalate (PET) or biaxially oriented polypropylene (BOPP) films or biaxially oriented nylon (BOPA) or PE films (MDO or BOPE or non-oriented PE, etc.). The resulting laminate provides a barrier level equivalent to laminates in which barrier films such as metallized BOPP, metallized cast polypropylene (CPP), metallized PET layers, etc. are incorporated, respectively.

[0165] When laminated to standard polyethylene terephthalate (PET) or biaxially oriented polypropylene (BOPP), biaxially oriented nylon (BOPA) or PE film (MDO or BOPE or non-oriented PE, etc.), the film prepared in metallized form using the components of Example 1 provides a laminate suitable for packaging products requiring high barrier levels, such as shampoo, snacks, fabric conditioners, etc. The resulting laminate provides barrier properties comparable to laminates that specifically use high barrier metallized BOPP, metallized PET layers for barrier.

[0166] Example 2

[0167] Membrane components % Terpolymer of ethylene, methacrylic acid and acrylic ester 5.4 Metallocene ethylene-octene copolymer 8.64 Low density polyethylene resin 6.15 Mineral silica anti-adhesive compounded in polyethylene 0.7425 High Density Polyethylene 36 Medium density ethylene-1-octene copolymer 10.5 Maleic anhydride modified linear low density polyethylene adhesive resin 3.5 29 mol% ethylene-vinyl alcohol copolymer 6.5 Bimodal terpolymer linear low density polyethylene 17.085 Ethylene-1-octene plastomer 5.1 Non-migrating slip additives compounded into polyethylene 0.3825

[0168] The film prepared using the components of Example 2 was metallized using a vacuum metallization process. During the metallization process, aluminum vapor or aluminum oxide (ALOx) with a minimum optical density of 2.2 was deposited on the polyethylene layer using a vacuum metallizer. The aluminum layer on the film of Example 2 further improved the barrier level. The barrier values ​​of the film of Example 2 before and after metallization were tested, and the results are as follows:

[0169]

[0170] Furthermore, from the results obtained it can be seen that the metallized film also exhibits excellent interlayer adhesion strength between the metal and the substrate PE film, which enables the highest quality packaging laminates to be achieved.

[0171] When laminated to standard polyethylene terephthalate (PET) or biaxially oriented polypropylene (BOPP) or biaxially oriented nylon (BOPA) or PE film (MDO or BOPE or non-oriented PE, etc.), the film produced using the components of Example 2 in a non-metallized version provides a laminate suitable for packaging products requiring high barrier levels, such as seasoned cereals, extruded snacks, cookies, salad dressings, meats and cheeses, etc. The resulting laminate provides a barrier level comparable to that of a laminate using a barrier film such as metallized PET (optical density >= 2.2) or a transparent barrier film or metallized BOPP, aluminum foil or coated film.

[0172] The films produced using the metallized versions of the components of Example 2, when laminated to standard polyethylene terephthalate (PET) or biaxially oriented polypropylene (BOPP) films or biaxially oriented nylon (BOPA) or PE films (MDO or BOPE or non-oriented PE, etc.), provide laminates suitable for packaging products requiring very high / ultra-high barrier levels, such as coffee, ketchup, milk powder, malt beverages, infant formula, etc. The resulting laminates provide barrier levels comparable to laminates that specifically use high barrier metallized BOPP, aluminum foil layers for barrier.

[0173] Example 3 - A PVOH (polyvinyl alcohol) coating or a polyvinyl alcohol coating modified with nanoparticles was further applied / coated to the film prepared using the components in Example 1 in an off-line process using a standard coating machine available in the industry. The PVOH coating weight was 0.5-2 g / m2. The resulting film coated with the PVOH coating was tested for barrier value (with and without metallization), and the results obtained were as follows:

[0174]

[0175] In order to facilitate consumers to tear the finished product package easily, at least 10% of COC (cyclic olefin copolymer) can be added to the film composition provided in the examples.

[0176] Various laminates were prepared using the films obtained in Examples 1-3, and the OTR and MVTR values ​​obtained were as follows:

[0177]

[0178] Advantageously, the present invention provides a film composition having excellent barrier properties and a laminate comprising the film, wherein the laminate exhibits excellent barrier properties without the need for a separate barrier layer. The laminate can be used for packaging of various products in combination with BOPP, PET, BOPA and PE films (MDO or BOPE or non-oriented PE, etc.). In addition, the present invention provides a very economical laminate because a separate metal / barrier layer is eliminated, which significantly reduces costs. Advantageously, the film of the present invention exhibits a more excellent barrier value compared to standard polyethylene films or even laminates having a polyethylene layer and a separate barrier layer, and eliminates the need for a separate barrier film. When laminated to a standard polyethylene terephthalate (PET) or biaxially oriented polypropylene (BOPP) film or biaxially oriented nylon film (BOPA) or PE film (MDO or BOPE or non-oriented PE, etc.), the film of the present invention provides a laminate suitable for packaging various products requiring low to high barrier levels. The resulting laminate provides barrier levels comparable to laminates using barrier films specifically such as BOPP, metallized BOPP, metallized cast polypropylene (CPP), metallized PET, aluminum foil layers, etc. This means that a two-layer laminate made using the film of the present invention provides barrier levels comparable to the barrier performance of conventional three-layer laminates. Reducing one barrier film layer in the laminate can increase production, reduce plastic sources, and save costs. In addition, when the laminate is designed with a PE film (MDO PE or BOPE or non-oriented PE, etc.) as the first film and the PE film of the present invention as the second film, the final laminate is more than 90% single material PE, so the recyclability level is more than 90%.

[0179] Figures 2 to 4 Not drawn to scale.

[0180] exist Figure 2 In the drawings, a second embodiment of the multilayer film according to the invention is indicated as a whole by reference numeral 10. The multilayer film 10 comprises a barrier film 12 formed by a carrier layer 14, on one of the outermost surfaces of which a deposition layer 16 is deposited. The deposition layer 16 is deposited, for example, by physical vapor deposition (PVD) onto a packaging body formed by the multilayer film 10 (see Figure 4 On the outermost surface 14a of the carrier layer 14 in the packaging body 80 facing outward (ie away from the packaged product).

[0181] The carrier layer 14 in the illustrated embodiment is made of a polymer blend containing 5.9 to 7.3 weight percent of a terpolymer of ethylene, methacrylic acid, and acrylic acid esters, based on the total weight of the multilayer film 10. The polymer blend of the carrier layer 14 also contains 9.9 to 12.1 weight percent of a metallocene linear low density polyethylene, 3.6 to 4.4 weight percent of LDPE, and 0.4 to 0.48 weight percent of a mineral silica antiblocking agent compounded in polyethylene.

[0182] In one embodiment of the multilayer film 10 , the support layer 14 comprises approximately 22 weight percent of the total weight of the multilayer film 10 , wherein the surface 16 a of the deposited layer 16 is the exposed outermost layer 10 a of the multilayer film 10 .

[0183] The deposited layer 16 in the illustrated embodiment is a physical vapor deposited aluminum layer having an optical density of 2.8 or more.

[0184] Although it is possible for the carrier layer 14 to carry two deposited layers, one on each of the surfaces 14a and 14b, it is preferred that the carrier layer 14 has only one deposited layer 16, which is deposited on one of its surfaces, here the surface 14a.

[0185] A first bulk layer 18 is provided on the surface 14b facing the packaging volume and thus the packaging product of the flexible package formed by or with the participation of the multilayer film 10. The first bulk layer 18 in the illustrated embodiment is formed from a mixture of 36 to 44 wt. % of high density polyethylene (HDPE) based on the total weight of the multilayer film 10 and 9 to 11 wt. % of linear low density polyethylene based on the total weight of the multilayer film 10. The bulk layer 18 forms about 50 % of the total weight of the multilayer film 10.

[0186] A sealing layer 20 is disposed on the surface 18b of the main body layer 18. The sealing layer 20 is formed by a mixture of a bimodal terpolymer LDPE (weight proportion is 21.6 to 24.4 weight % of the weight of the entire multilayer film), LDPE (component ratio is 2.5 to 3.0 weight %), a silica antiblocking agent (component ratio is 0.63 to 0.77 weight %), and a non-migrating slip additive compounded in polyethylene (component ratio is 0.37 to 0.46 weight % of the weight of the entire multilayer film). The weight ratio of the sealing layer 20 in the illustrated embodiment is about 28 weight % of the weight of the multilayer film.

[0187] This is a basic embodiment of a possible multilayer film 10 according to the invention. The outermost surface of the deposited layer 16a forms the outermost surface 10a of the multilayer film 10. The exposed surface 20b of the sealing layer forms the opposite outermost surface 10b of the multilayer film 10.

[0188] As described so far, the multilayer film 10 is preferably a multilayer coextruded film, particularly preferably a multilayer coextruded blown film.

[0189] Optionally, the multilayer film 10 may have a second bulk layer 22, for example formed of HDPE, optionally formed of machine direction oriented HDPE, which is reverse printed with a print layer 24 and laminated to the deposited layer 16 via a suitable adhesive resin layer 26. If optional layers 22, 24 and 26 are present, the exposed surface 22a of the second bulk layer 22 forms the exposed outer surface 10a' of the multilayer film 10, rather than the surface 16a (which would subsequently become the inner interlayer surface of the multilayer film 10).

[0190] By adding optional further layers 22, 24 and 26 (in Figure 2 The multilayer film 10 is expanded by modifying the weight percentages of the various layers and their constituents given above, which are associated with the multilayer film 10 without the optional layers.

[0191] The multilayer film 10 without the optional layer achieves a thickness of less than 20 cm as measured according to the above standards. 3 / (d·m 2 ) and the oxygen transmission rate measured according to the above standard is less than 0.5g / (d·m 2 ) water vapor transmission rate.

[0192] As a comparison, the same multilayer film 10 without the deposited layer 16 has an oxygen transmission rate 20 times that of the multilayer film 10 with the deposited layer, and a water vapor transmission rate 6 times that of the multilayer film 10 with the deposited layer. The significant decrease in transmission rate is attributed to the terpolymer of ethylene, methacrylic acid and acrylate in the mixture of the carrier layer 14. The terpolymer improves the bonding strength between the deposited layer 16 and the carrier layer 14, and as the bonding strength increases, the barrier performance also increases significantly. The improvement in barrier performance corresponds to the decrease in transmission rate.

[0193] Figure 3 A third embodiment of a layer 110 according to the invention is shown. This layer 110 also has a barrier film 112 formed by a carrier layer 114 and a deposition layer 116 deposited on an outer surface 114a of the carrier layer 114.

[0194] exist Figure 3 In the third embodiment shown, Figure 2 Components and component parts that are structurally or functionally identical to those in the second embodiment shown are labeled with the same reference numerals as in the second embodiment, but with the addition of the number 100. Only the parts of the third embodiment that differ from the second embodiment will be described in detail later. For components and component parts in the third embodiment that are not explicitly described below, reference is made to the description of the second embodiment (which also applies to the third embodiment).

[0195] The third embodiment has an additional barrier layer, thus achieving better barrier properties, ie lower oxygen and water vapor transmission rates.

[0196] The multi-layer film 110 includes a second bulk layer 122 , a reverse printed print layer 124 , and an adhesive resin layer 126 to bond the second bulk layer 122 together with the print layer 124 to the deposition layer 116 .

[0197] Compared with the second embodiment, the first body layer 118 of the third embodiment is formed of only HDPE.

[0198] The third embodiment comprises an oxygen barrier layer 128, which in the example shown is formed of ethylene-vinyl alcohol copolymer (EVOH). It is bonded to the first bulk layer 118 by an adhesive resin layer 130, which is formed of a mixture of conventional ungrafted LLDPE and maleic anhydride grafted polyethylene (particularly maleic anhydride grafted LLDPE). It contains about 3.3 to 3.6 times more ungrafted LLDPE than maleic anhydride grafted polyethylene by weight.

[0199] On the surface 128b facing away from the barrier film 112, another adhesive resin layer 132 is applied to the oxygen barrier layer 128 in order to bond another bulk layer, in this case a third bulk layer 134, to the oxygen barrier layer 128. Preferably, the further bulk layer 134 is identical to the first bulk layer 118. The presence of two bulk layers 118 and 134, each made of pure HDPE, further improves the barrier properties of the multilayer film 110.

[0200] The sealing layer 120 (referred to as the sealing layer 20 in the second embodiment) is bonded to another main body layer 134 on a surface 134 b facing away from the oxygen barrier layer 128 .

[0201] According to the above standard, the oxygen transmission rate of the multilayer film 110 of the third embodiment is less than 0.5 cm 3 / (d·m 2 ), and according to the above standard, the water vapor transmission rate of the multilayer film 110 of the third embodiment is also less than 0.5 g / (d·m 2 ).

[0202] Again, as a comparison, the same multilayer film 110 without the deposited layer 116 has an oxygen transmission rate that is twice that of the multilayer film 110 with the deposited layer, and a water vapor transmission rate that is six times that of the multilayer film 110 with the deposited layer. The significant decrease in transmission rate is again attributed to the terpolymer of ethylene, methacrylic acid, and acrylate in the mixture of the carrier layer 14. The terpolymer improves the bonding strength between the deposited layer 116 and the carrier layer 114, and as the bonding strength improves, the barrier properties also improve significantly.

[0203] The multi-layer film 110 is also preferably a multi-layer co-extruded film 110 , and is particularly preferably a multi-layer co-extruded blown film 110 .

[0204] Figure 4 It is shown in Figure 2 Multilayer film 10 or Figure 3 A possible flexible package formed by the multilayer film 110. The flexible package is a four-side sealed bag 80, which can be used to package items, especially food and similar important commodities.

[0205] The front side of bag 80 (at Figure 4 ) and the back of the bag 80 are made from the same rectangular blank of multilayer film 10 or 110.

[0206] The bag 80 has a central packaging volume 82 which is sealed around a sealing area 84, wherein the sealing layers 20 or 120, respectively, are placed with their exposed surfaces 20b or 120b in contact with each other and then heat sealed to seal around the packaging volume 82. Thus, the object 86 can be safely contained in the packaging volume 82 for a relatively long period of time without loss of quality.

[0207] While the present invention has been described with respect to certain embodiments, it will be apparent to those skilled in the art that various changes and modifications may be made without departing from the scope of the invention as defined in the following claims.

Claims

1. A film composition comprising 1 to 10% of an acid copolymer, 5 to 15% of a metallocene linear low density polyethylene (LLDPE), 5 to 10% of a low density polyethylene (LDPE), 0.5 to 1% of an anti-blocking masterbatch, 20 to 50% of a high density polyethylene (HDPE), 5 to 30% of a plastomer and 0.5 to 1% of a slip additive.

2. The film composition of claim 1, further comprising 1 to 10% of an adhesive polymer, 5 to 15% of a medium density polyethylene (MDPE), and 0.1 to 7% of ethylene vinyl alcohol (EVOH), wherein the ethylene content in the EVOH is 27 to 40%.

3. The film composition of claim 1, wherein the acidic copolymer is a terpolymer of ethylene, methacrylic acid and acrylic ester, or an acid-modified olefin copolymer.

4. The film composition of claim 1, wherein the metallocene LLDPE comprises a metallocene ethylene-octene copolymer.

5. The film composition of claim 1, wherein the plastomer is selected from ethylene-1-octene or 1-octene and the slip additive is selected from erucamide, oleamide and / or stearamide compounded with polyethylene or a modified non-migrating additive.

6. A film formed from the film composition of any preceding claim.

7. The film of claim 6, wherein the film is further coated with a modified EVOH or PVOH coating or a PVOH coating with nanoparticles.

8. The film of claim 6, wherein the film is metallized or non-metallized.

9. A laminate comprising: a. The first film; and b. A second film bonded to the first film, the second film comprising a film composition of the following ingredients: 1 to 10% of an acid copolymer, 5 to 15% of a metallocene linear low density polyethylene (LLDPE), 5 to 10% of a low density polyethylene (LDPE), 0.5 to 1% of an anti-blocking masterbatch, 20 to 50% of a high density polyethylene (HDPE), 5 to 30% of a plastomer, and 0.5 to 1% of a slip additive.

10. The laminate of claim 9, wherein the film composition of the second film further comprises 1 to 10% of an adhesive polymer, 5 to 15% of a medium density polyethylene (MDPE), and 0.1 to 7% of ethylene vinyl alcohol (EVOH), wherein, The ethylene content in EVOH is 27 to 40%.

11. The laminate of claim 9, wherein the second film is coated with a modified EVOH or PVOH coating or a PVOH coating with nanoparticles.

12. The laminate according to claim 9, wherein the acid copolymer is a terpolymer of ethylene, methacrylic acid and acrylic acid ester, or an acid-modified olefin copolymer.

13. The laminate of claim 9, wherein the metallocene LLDPE comprises a metallocene ethylene-octene copolymer.

14. The laminate of claim 9, wherein the plastomer is selected from ethylene-1-octene or 1-octene and the slip additive is selected from erucamide, oleamide and / or stearamide compounded with polyethylene or a modified non-migrating additive.

15. The laminate of claim 9, wherein the second film is metallized or non-metallized.