Solid oxide electrolytic cell, method for manufacturing solid oxide electrolytic cell, solid oxide electrolytic module, electrochemical device, and energy system

By designing multiple pores with an area of ​​more than 0.75 μm2 in the electrode layer of the solid oxide electrolytic cell and having micron- and nano-scale pore structures, combining metal support and anti-reaction layer, the electrode layer is solved under high pressure. The peeling problem improves the strength and performance of the electrolytic cell and reduces manufacturing costs.

CN118946688APending Publication Date: 2024-11-12OSAKA GAS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380030316.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-28
Filing Date
2023-03-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

When a solid oxide fuel cell is used in a solid oxide electrolytic cell, when a water vapor or carbon dioxide electrolytic reaction is applied at a voltage of about 1.3V, the electrode layer cannot withstand the generated oxygen pressure, resulting in the electrode layer peeling off and the cell breakage.

Method used

A first electrode layer with a plurality of holes with an area of ​​0.75 μm2 or more is designed, through which oxygen is released, the pressure rise in the electrode layer is suppressed, and the presence of micro- and nano-scale pores in the electrode layer is increased to promote the surface area. Electrochemical reactions, while using metal support and anti-reaction layer to reduce high temperature treatment and material damage.

Benefits of technology

The peeling of the electrode layer is effectively suppressed, the strength, durability and performance of the solid oxide electrolytic cell is improved, the cell damage is avoided, and the manufacturing cost is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118946688A_ABST
    Figure CN118946688A_ABST
Patent Text Reader

Abstract

Provided is a solid oxide electrolytic cell in which peeling of an electrode layer is suppressed, and which has excellent strength (reliability), durability and performance. The solid oxide electrolytic cell (E) has at least a first electrode layer (6), a second electrode layer (2), and an electrolyte layer (4) disposed between the first electrode layer (6) and the second electrode layer (2), and the first electrode layer (6) has at least a plurality of holes having an area of 0.75 [mu] m2 or more in a longitudinal cross section thereof.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a solid oxide electrolytic cell, a method for manufacturing the same, and a solid oxide electrolytic module, an electrochemical device, and an energy system equipped with the solid oxide electrolytic cell. Background Art

[0002] Non-Patent Document 1 discloses a solid oxide fuel cell (SOFC).

[0003] The solid oxide fuel cell disclosed in non-patent document 1 is manufactured as follows: First, an anode electrode layer is formed by firing on a porous metal support obtained by sintering Fe-Cr alloy powder. Next, an electrolyte layer composed of yttria-stabilized zirconia (YSZ) is formed on the anode electrode layer without heating using an aerosol deposition method (AD method). Then, PVDF (polyvinylidene fluoride) as a pore-forming material is mixed into the LSCF powder, and in this state, it is stacked on the electrolyte layer and fired to form a cathode electrode layer having a nano-sized porous structure.

[0004] Prior art literature

[0005] Non-patent literature

[0006] Non-patent document 1: Jong-Jin Choi and Dong-Soo Park, "Preparation of Metal-supported SOFC using Low Temperature Ceramic Coating Process", Proceedings of 11th European SOFC&SOE Forum, A1502, Chapter 09-Session B15-14 / 117-20 / 117 (1-4July 2014). Summary of the invention

[0007] Problems to be solved by the invention

[0008] The solid oxide fuel cell described above functions as a power generation cell by generating a power generation reaction in the element portion composed of an electrode layer and an electrolyte layer. On the other hand, the reverse reaction of the power generation reaction, i.e., an electrolysis reaction, can also be generated in the element portion, in which case it functions as a solid oxide electrolytic cell (SOEC).

[0009] Here, it is known that when electrolysis of water vapor is performed using a solid oxide electrolytic cell based on a solid oxide fuel cell, a reaction condition (thermal neutral point) in which the heat absorption caused by the electrolysis of water and the heat release caused by the ohmic loss of the cell are balanced is theoretically established when the cell voltage is 1.3 V. Therefore, a system using a solid oxide electrolytic cell is preferably capable of continuously operating near the thermal neutral point where heat does not need to be discharged to the outside or supplied from the outside, in other words, in a state where a voltage of about 1.3 V is applied.

[0010] However, solid oxide fuel cells have been optimized for power generation. Therefore, when used as solid oxide electrolytic cells, if a voltage of about 1.3V is applied to perform an electrolysis reaction of water vapor or carbon dioxide, a large amount of oxygen is generated in the electrode layer, and the electrode layer may not be able to withstand the pressure of the generated oxygen. Specifically, there is the following problem: when a large amount of oxygen is generated, the release of oxygen from the electrode layer cannot keep up, so that the pressure in the electrode layer increases, and the electrode layer peels off from the base layer such as the electrolyte layer, resulting in cell damage.

[0011] The present invention has been completed in view of the above-mentioned actual situation, and its purpose is to provide: a solid oxide electrolytic cell with suppressed electrode layer peeling, excellent strength (reliability) and durability, and excellent performance, a manufacturing method thereof, and a solid oxide electrolytic module, electrochemical device and energy system equipped with the solid oxide electrolytic cell.

[0012] Means of solving problems

[0013] The solid oxide electrolytic cell of the present invention for achieving the above-mentioned object is characterized in that:

[0014] The solid oxide electrolytic cell comprises at least a first electrode layer, a second electrode layer and an electrolyte layer disposed between the first electrode layer and the second electrode layer.

[0015] The first electrode layer has at least a plurality of electrodes with an area of ​​0.75 μm in its longitudinal section. 2 The hole above.

[0016] According to the above-mentioned characteristic configuration, for example, even when a large amount of oxygen is generated in the first electrode layer, by having a plurality of 2 The above holes also make it easy for oxygen to be released from the first electrode layer, which can suppress the increase in pressure in the first electrode layer, thereby suppressing the peeling of the first electrode layer. Therefore, the solid oxide electrolytic cell has excellent strength (reliability), durability and performance.

[0017] The solid oxide electrolytic cell of the present invention is further characterized in that:

[0018] The first electrode layer has at least three or more electrodes with an area of ​​0.75 μm in its longitudinal section. 2 The above holes have a 10 μm square area.

[0019] According to the above-mentioned characteristic configuration, the area present in the first electrode layer is 0.75 μm 2 The above number of holes is sufficient for supplying and releasing the gas involved in the electrolytic reaction, and can further suppress the peeling of the first electrode layer.

[0020] The solid oxide electrolytic cell of the present invention is further characterized in that:

[0021] The area in the first electrode layer is 0.75 μm 2 The above pores are pores having a diameter of 0.5 μm or more.

[0022] According to the above-mentioned characteristic configuration, oxygen is easily released from the first electrode layer, and the pressure increase in the first electrode layer can be suppressed, thereby suppressing the peeling of the first electrode layer. Therefore, the solid oxide electrolytic cell has excellent strength (reliability), durability and performance.

[0023] The solid oxide electrolytic cell of the present invention is further characterized in that:

[0024] The first electrode layer has at least an area of ​​0.04 μm in its longitudinal section. 2 The following hole.

[0025] According to the above-mentioned characteristic configuration, the presence of both micrometer-level pores and nanometer-level pores not only makes it easier for gas to be released from the first electrode layer, but also increases the surface area compared to the case of only having micrometer-level pores, thereby ensuring a large number of electrochemical reaction fields in the first electrode layer. That is, according to the above-mentioned characteristic configuration, the performance as an electrolytic cell can be improved while suppressing the peeling of the first electrode layer.

[0026] The solid oxide electrolytic cell of the present invention is further characterized in that:

[0027] The area in the first electrode layer is 0.04 μm 2 The following pores are pores having a diameter of 0.1 μm or less.

[0028] According to the above-mentioned characteristic configuration, as described above, by having both micron-sized pores and nano-sized pores, not only is it easy to release gas from the first electrode layer, but also the surface area is increased compared to the case of having only micron-sized pores, so that many electrochemical reaction fields can be ensured in the first electrode layer. That is, according to the above-mentioned characteristic configuration, the performance as an electrolytic cell can be improved, and the peeling of the first electrode layer can be suppressed.

[0029] The solid oxide electrolytic cell of the present invention is further characterized in that:

[0030] The first electrode layer has a surface area of ​​0.75 μm 2 The first porosity associated with the above pores is 5% or more and less than 20% of the longitudinal section.

[0031] According to the above-mentioned characteristic configuration, since there is a 0.75 μm 2 The first porosity of the above holes is an appropriate value of more than 5% and less than 20% in the longitudinal section, so the strength of the first electrode layer can be ensured, and the gas involved in the electrolytic reaction can be easily supplied and released from the first electrode layer, thereby easily suppressing the peeling of the first electrode layer.

[0032] The solid oxide electrolytic cell of the present invention is further characterized in that:

[0033] The first electrode layer has a surface area of ​​0.75 μm 2 The area of ​​the hole is 0.04 μm 2 The second porosity of the following pores is 10% or more and 40% or less in the longitudinal section.

[0034] According to the above-mentioned characteristic configuration, since there is a 0.75 μm 2 The pore area is 0.04 μm. 2 The second porosity associated with the following pores is an appropriate value of more than 10% and less than 40% in the longitudinal section, so the strength of the first electrode layer can be ensured, and the gas involved in the electrolytic reaction can be easily supplied and released from the first electrode layer, thereby suppressing the peeling of the first electrode layer.

[0035] The solid oxide electrolytic cell of the present invention is further characterized in that:

[0036] The first electrode layer contains at least a plurality of particles having a particle size of 0.1 μm or less.

[0037] According to the above-mentioned characteristic configuration, the first electrode layer has an area of ​​0.75 μm 2 In addition to the above pores, at least a plurality of particles having a particle size of 0.1 μm or less are contained, thereby suppressing an extreme decrease in the strength of the first electrode layer and ensuring a large number of electrochemical reaction fields, thereby realizing a high-performance solid oxide electrolytic cell.

[0038] The solid oxide electrolytic cell of the present invention is further characterized in that:

[0039] The first electrode layer is an oxygen generating electrode.

[0040] According to the above-mentioned characteristic configuration, if electrolysis is performed at a high voltage and a high current density, a large amount of oxygen is generated on the first electrode layer side due to the electrolysis reaction of water vapor or carbon dioxide, but the first electrode layer easily releases the gas (oxygen) generated in the electrolysis reaction. Therefore, the peeling of the first electrode layer from the base layer such as the electrolyte layer can be suppressed.

[0041] The solid oxide electrolytic cell of the present invention is further characterized in that:

[0042] An anti-reaction layer is disposed between the first electrode layer and the electrolyte layer.

[0043] According to the above-described characteristic configuration, it is possible to prevent the reaction between the components of the first electrode layer and the components of the electrolyte layer.

[0044] The solid oxide electrolytic cell of the present invention is further characterized in that:

[0045] The electrolyte layer contains an oxide ion conductor.

[0046] According to the above-described characteristic configuration, since the electrolyte layer contains an oxide ion conductor, a solid oxide electrolytic cell capable of exhibiting high electrochemical performance can be realized.

[0047] The solid oxide electrolytic cell of the present invention is further characterized in that:

[0048] With metal support.

[0049] According to the above-mentioned characteristic configuration, since the first electrode layer, the second electrode layer and the electrolyte layer can be supported by a cheap and strong metal support, the use amount of expensive ceramic materials can be reduced, and a solid oxide electrolytic cell with high strength, reliability and excellent durability can be obtained. In addition, since the processability is also excellent, the manufacturing cost can also be reduced.

[0050] In addition, in order to suppress damage to the metal support, the solid oxide electrolytic cell having a metal support needs to avoid processing in a high temperature region (e.g., a temperature region higher than 1100°C) during manufacturing. As a result, the adhesion strength between the first electrode layer and the layer serving as the base is easily reduced, and the first electrode layer is easily peeled off. However, in the solid oxide electrolytic cell having the above-mentioned characteristic configuration, the first electrode layer has an area of ​​0.75 μm 2 The above holes can suppress the peeling of the first electrode layer. Therefore, the solid oxide electrolytic cell with a metal support, which is prone to the problem of peeling of the first electrode layer, can be made into a product with excellent strength (reliability) and durability and performance, in which the peeling of the first electrode layer can be suppressed.

[0051] In addition, the method for manufacturing a solid oxide electrolytic cell according to the present invention is characterized in that:

[0052] It is a method for manufacturing the above-mentioned solid oxide electrolytic cell,

[0053] A pore-forming material is used in the step of forming the first electrode layer.

[0054] According to the above-mentioned characteristic configuration, since a pore-forming material is used when forming the first electrode layer, a pore-forming material with an area of ​​0.75 μm can be formed in the first electrode layer. 2 The hole above.

[0055] Other characteristic features of the method for manufacturing a solid oxide electrolytic cell according to the present invention are:

[0056] It is a method for manufacturing the above-mentioned solid oxide electrolytic cell,

[0057] The processing temperature in all steps is 1100° C. or less.

[0058] According to the above-described characteristic configuration, for example, even when the solid oxide electrolytic cell has a metal support, damage to the metal support can be suppressed.

[0059] The solid oxide electrolysis module of the present invention for achieving the above-mentioned object is characterized in that:

[0060] The solid oxide electrolytic cells are arranged in a state of being assembled in plurality.

[0061] According to the above-mentioned characteristic configuration, the solid oxide electrolytic cells are arranged in a state of being assembled in plurality, thereby suppressing material costs and processing costs, and realizing a compact and high-performance solid oxide electrolytic module having excellent strength and reliability.

[0062] The electrochemical device according to the present invention for achieving the above-mentioned object is characterized in that:

[0063] The present invention comprises at least the solid oxide electrolysis cell or the solid oxide electrolysis module and a fuel converter for converting a gas containing a reducing component generated in the solid oxide electrolysis cell or the solid oxide electrolysis module.

[0064] When the solid oxide electrolytic cell or the solid oxide electrolytic module is operated as an electrolytic cell, a gas containing water vapor or carbon dioxide is passed to the second electrode layer, and a voltage is applied between the second electrode layer and the first electrode layer. - Reacts with water H2O or carbon dioxide molecules CO2 to form hydrogen H2 or carbon monoxide CO and oxygen ions O 2- The oxygen ions O produced2- Then, in the first electrode layer, oxygen ions O 2- It releases electrons and becomes oxygen O2. Through the above reaction, when a gas containing water vapor is circulated, water H2O is decomposed into hydrogen H2 and oxygen O2, and when a gas containing carbon dioxide molecules CO2 is circulated, it is electrolyzed into carbon monoxide CO and oxygen O2.

[0065] Therefore, when a gas containing water vapor and carbon dioxide molecules CO2 is circulated, a fuel converter can be provided to synthesize various compounds such as hydrocarbons from hydrogen and carbon monoxide generated by the above electrolysis in a solid oxide electrolysis cell or a solid oxide electrolysis module. Thus, the hydrocarbons generated by the fuel converter can be circulated in the solid oxide electrolysis cell or the solid oxide electrolysis module, or taken out of the system / device and used as fuel or chemical raw materials.

[0066] The electrochemical device according to the present invention for achieving the above-mentioned object is characterized in that:

[0067] The invention comprises at least the solid oxide electrolytic cell or the solid oxide electrolytic module and a power converter for flowing electric power to the solid oxide electrolytic cell or the solid oxide electrolytic module.

[0068] According to the above-mentioned characteristic configuration, the power converter can allow electricity to flow into the solid oxide electrolytic cell or the solid oxide electrolytic module. Thus, as described above, the solid oxide electrolytic cell or the solid oxide electrolytic module functions as an electrolytic cell. Therefore, according to the above-mentioned characteristic configuration, an electrochemical device with improved efficiency in converting electrical energy into chemical energy such as fuel can be realized. It should be noted that, for example, when an inverter is used as a power converter, an electrochemical device can be constructed that can obtain direct current from an AC power supply and supply direct current power to the solid oxide electrolytic cell or the solid oxide electrolytic module when working as an electrolytic cell, so it is preferred.

[0069] The energy system of the present invention for achieving the above-mentioned object is characterized in that:

[0070] The invention comprises at least the electrochemical device described above and a waste heat utilization unit for reusing the heat exhausted from the electrochemical device.

[0071] According to the above-mentioned characteristic configuration, an energy system having excellent durability, reliability, and performance and also excellent energy efficiency can be realized. BRIEF DESCRIPTION OF THE DRAWINGS

[0072] [ Figure 1 ] A diagram showing a schematic structure of a solid oxide electrolytic cell according to one embodiment.

[0073] [ Figure 2 ] A diagram showing a schematic structure of a solid oxide electrolysis module involved in one embodiment.

[0074] [ Figure 3 ]A diagram showing a schematic structure of an electrochemical device and an energy system according to one embodiment.

[0075] [ Figure 4 ] represents a SEM image of a longitudinal section of the solid oxide electrolytic cell involved in the embodiment.

[0076] [ Figure 5 ] represents a SEM image of a longitudinal section of the solid oxide electrolytic cell involved in the embodiment.

[0077] [ Figure 6 ] represents a SEM image of a longitudinal section of a solid oxide electrolytic cell according to a comparative example.

[0078] [ Figure 7 ] is a diagram showing the schematic structure of a solid oxide electrolysis module involved in other embodiments. DETAILED DESCRIPTION

[0079] Hereinafter, the solid oxide electrolytic cell E, the manufacturing method thereof, the solid oxide electrolytic module M, the electrochemical device Y and the energy system Z according to the embodiment will be described. It should be noted that, when indicating the positional relationship of the layers, for example, when viewed from the electrolyte layer 4, the side of the electrode layer 6 (first electrode layer) is sometimes referred to as "upper" or "upper side", and the side of the electrode layer 2 (second electrode layer) is sometimes referred to as "lower" or "lower side". In addition, the surface of the metal support 1 on which the electrode layer 2 is formed is sometimes referred to as the "surface side surface", and the surface on the opposite side is sometimes referred to as the "back side surface".

[0080] (Solid Oxide Electrolytic Cell)

[0081] like Figure 1 As shown, the solid oxide type electrolytic cell E comprises a metal support 1, an electrode layer 2 (second electrode layer), a first reaction prevention layer 3 formed on the electrode layer 2, an electrolyte layer 4 formed on the first reaction prevention layer 3, a second reaction prevention layer 5 formed on the electrolyte layer 4, and a counter electrode layer 6 (first electrode layer) formed on the second reaction prevention layer 5. That is, the electrolyte layer 4 is arranged between the counter electrode layer 6 and the electrode layer 2, and the second reaction prevention layer 5 is arranged between the counter electrode layer 6 and the electrolyte layer 4.

[0082] (Metal support)

[0083] The metal support 1 supports the electrode layer 2, the first reaction preventing layer 3, the electrolyte layer 4, the second reaction preventing layer 5 and the counter electrode layer 6 to maintain the strength of the solid oxide electrolytic cell E. That is, the metal support 1 functions as a support for supporting the components of the electrolytic cell.

[0084] As the material of the metal support 1, a material with excellent electronic conductivity, heat resistance, oxidation resistance and corrosion resistance is used. For example, ferritic stainless steel, austenitic stainless steel, nickel-based alloy, etc. are used. It is particularly preferred to use an alloy containing chromium. In the present embodiment, the metal support 1 uses a Fe-Cr alloy containing 18% by mass or more and 25% by mass or less of Cr, and is particularly preferably a Fe-Cr alloy containing 0.05% by mass or more of Mn, a Fe-Cr alloy containing 0.15% by mass or more and 1.0% by mass or less of Ti, a Fe-Cr alloy containing 0.15% by mass or more and 1.0% by mass or less of Zr, a Fe-Cr alloy containing Ti and Zr and a total content of Ti and Zr of 0.15% by mass or more and 1.0% by mass or less of Cu, and a Fe-Cr alloy containing 0.10% by mass or more and 1.0% by mass or less of Cu.

[0085] It should be noted that if the metal support 1 is made of a ferritic stainless steel material, a low-cost and high-strength solid oxide electrolytic cell E can be realized, which is preferred.

[0086] The metal support 1 is plate-shaped as a whole. As long as the metal support 1 has sufficient strength to form a solid oxide electrolytic cell E as a support, from the viewpoint of ensuring strength, its thickness is, for example, preferably 0.1 mm or more, more preferably 0.15 mm or more, and further preferably 0.2 mm or more. In addition, from the viewpoint of suppressing costs, its thickness is, for example, preferably 2 mm or less, more preferably 1 mm or less, and further preferably 0.5 mm or less. Moreover, the metal support 1 has a plurality of through holes 1a that penetrate from the surface (the surface side) where the electrode layer 2 is provided to the back side. In the present embodiment, the metal support 1 is a metal plate provided with a plurality of through holes 1a to penetrate the surface side and the back side of the metal plate by mechanical, chemical or optical perforation processing (hole processing) such as punching processing or etching processing, laser processing, etc. Thus, a gas containing water vapor or carbon dioxide (hereinafter also referred to as "mixed gas") can be smoothly supplied from the back side of the metal support 1 facing the electrode layer 2, thereby realizing a high-performance solid oxide electrolytic cell E.

[0087] It should be noted that the plate-like metal support 1 may be bent and deformed into a shape such as a box or a cylinder for use.

[0088] A metal oxide layer 1b as a diffusion suppression layer is provided on the surface of the metal support 1. That is, a diffusion suppression layer is formed between the metal support 1 and the electrode layer 2 described later. The metal oxide layer 1b is provided not only on the surface of the metal support 1 exposed to the outside, but also on the contact surface (interface) with the electrode layer 2 and the surface inside the through hole 1a. The metal oxide layer 1b can inhibit the mutual diffusion of elements between the metal support 1 and the electrode layer 2. For example, in the case of using ferritic stainless steel containing chromium as the metal support 1, the metal oxide layer 1b is mainly chromium oxide. In this way, the metal oxide layer 1b with chromium oxide as the main component inhibits the diffusion of chromium atoms of the metal support 1 to the electrode layer 2 or the electrolyte layer 4. The thickness of the metal oxide layer 1b can be a thickness that can take into account both high diffusion prevention performance and low resistance. For example, it is preferably submicron-level, and specifically, the average thickness is more preferably about 0.3μm or more and about 0.7μm or less. In addition, the minimum thickness is more preferably about 0.1μm or more. In addition, the maximum thickness is preferably about 1.1μm or less.

[0089] It should be noted that the metal oxide layer 1b can be formed by various techniques, preferably by using a technique of oxidizing the surface of the metal support 1 to form a metal oxide. In addition, on the surface of the metal support 1, the metal oxide layer 1b can be formed by a PVD method such as a sputtering method or a PLD method, a CVD method, a spraying method (thermal spraying or aerosol deposition method, aerosol gas deposition method, powder spray deposition method, particle spray deposition method, cold spray method, etc.), or by plating and oxidation treatment. In addition, the metal oxide layer 1b may also contain a spinel phase with high conductivity.

[0090] (Electrode layer)

[0091] Electrode layer 2 Figure 1 As shown, it can be provided in a thin layer state on the surface of the metal support 1 to cover the area of ​​the metal support 1 where the through holes 1a are formed. In the case of making a thin layer, its thickness can be set to, for example, about 1μm to 100μm, preferably 5μm to 50μm. If it is set to such a thickness, the use of expensive electrode layer materials can be reduced to achieve cost reduction, while ensuring sufficient electrode performance. In addition, the area of ​​the metal support 1 where the through holes 1a are provided is covered by the electrode layer 2 as a whole. That is, the through holes 1a are formed on the inner side of the area of ​​the metal support 1 where the electrode layer 2 is formed. In other words, all the through holes 1a are provided facing the electrode layer 2.

[0092] As the material of the electrode layer 2, for example, a composite material such as NiO-GDC, Ni-GDC, NiO-YSZ, Ni-YSZ, CuO-CeO 2 , or Cu-CeO 2 can be used.

[0093] In these examples, GDC, YSZ, and CeO2 can be referred to as aggregates of the composite material.

[0094] It should be noted that the electrode layer 2 is preferably formed by a low-temperature sintering method (for example, a wet method using sintering in a low-temperature region instead of sintering in a high-temperature region higher than 1100°C) or a spraying method (thermal spraying or aerosol deposition method, aerosol gas deposition method, powder jet deposition method, particle jet deposition method, cold spray method, etc.), a PVD method (sputtering method or pulsed laser deposition method, etc.), a CVD method, etc. By these processes that can be used in a low-temperature region, for example, sintering in a high-temperature region higher than 1100°C is not used, a good electrode layer 2 can be obtained. Therefore, the metal support 1 can be not damaged, and the element diffusion between the metal support 1 and the electrode layer 2 can be suppressed, so a solid oxide electrolytic cell E with excellent durability can be realized, so it is preferred. In addition, if a low-temperature sintering method is used, the handling of the raw materials becomes easy, so it is more preferred.

[0095] The electrode layer 2 has a plurality of pores inside and on the surface thereof in order to have gas permeability. That is, the electrode layer 2 is formed as a porous layer. The electrode layer 2 is formed, for example, in a manner in which its density is greater than 30% and less than 80%. The size of the pores can be appropriately selected to be suitable for a smooth reaction during an electrochemical reaction. It should be noted that density refers to the proportion of the material constituting the layer in the space, which can be expressed as (1-porosity), and is also equal to the relative density.

[0096] (First anti-reaction layer)

[0097] The first anti-reaction layer 3 is Figure 1 As shown, the electrode layer 2 can be covered in a thin layer state on the electrode layer 2. In the case of a thin layer, the thickness can be set to about 1 μm to 100 μm, preferably about 2 μm to 50 μm, and more preferably about 4 μm to 25 μm. If the thickness is set to such a thickness, the amount of expensive anti-reaction layer material used can be reduced to achieve cost reduction, while ensuring sufficient performance.

[0098] As the material of the first reaction preventing layer 3, for example, YSZ (yttria stabilized zirconia), SSZ (scandium stabilized zirconia), GDC (gadolinium doped ceria), YDC (yttrium doped ceria), SDC (samarium doped ceria), etc. Ceria-based ceramics are particularly preferably used.

[0099] The first reaction prevention layer 3 is preferably formed by a low-temperature sintering method (for example, a wet method that uses sintering in a low-temperature region instead of 1100°C), a spraying method (thermal spraying, aerosol deposition, aerosol gas deposition, powder spray deposition, particle spray deposition, cold spray, etc.), a PVD method (sputtering, pulse laser deposition, etc.), a CVD method, etc. By these film-forming processes that can be used in a low-temperature region, for example, without using sintering in a high-temperature region higher than 1100°C, the first reaction prevention layer 3 can be obtained. Therefore, the mutual diffusion of elements between the metal support 1 and the electrode layer 2 can be suppressed without damaging the metal support 1, and a solid oxide electrolytic cell E with excellent durability can be realized. In addition, if a low-temperature sintering method is used, the handling of the raw materials becomes easy, so it is more preferred.

[0100] In this embodiment, the first reaction prevention layer 3 is more preferably a mixed conductor having conductivity of both oxygen ions (oxide ions) and electrons. The first reaction prevention layer 3 having such properties is suitable for use in the solid oxide electrolytic cell E.

[0101] (Electrolyte layer)

[0102] The electrolyte layer 4 is Figure 1 As shown, it is formed on the first reaction preventing layer 3 in a thin layer state.

[0103] Alternatively, it may be formed in a thin film state with a thickness of 10 μm or less. In the present embodiment, the electrolyte layer 4 is arranged across (spanning) the first reaction prevention layer 3 and the metal support 1. By configuring in this way and bonding the electrolyte layer 4 to the metal support 1, the overall firmness of the solid oxide electrolytic cell E can be excellent.

[0104] In addition, the electrolyte layer 4 can be provided in an area larger than the area where the through hole 1a is provided in the surface of the surface side of the metal support 1. That is, the through hole 1a is formed on the inner side of the area where the electrolyte layer 4 is formed on the metal support 1. Thus, around the electrolyte layer 4, gas leakage from the electrode layer 2 and the first reaction prevention layer 3 can be suppressed. If explained, when the solid oxide electrolytic cell E is working, the mixed gas is supplied to the electrode layer 2 from the back side of the metal support 1 through the through hole 1a. In the part where the electrolyte layer 4 contacts the metal support 1, other components such as gaskets can be not provided to suppress gas leakage. It should be noted that in the present embodiment, the surroundings of the electrode layer 2 are completely covered by the electrolyte layer 4, but it can also be configured to provide the electrolyte layer 4 on the upper part of the electrode layer 2 and the first reaction prevention layer 3, and to provide gaskets and the like around them.

[0105] As the material of the electrolyte layer 4, an electrolyte material (oxide ion conductor) that conducts oxygen ions such as YSZ (yttria stabilized zirconia), SSZ (scandium stabilized zirconia), GDC (gadolinium doped cerium oxide), YDC (yttrium doped cerium oxide), SDC (samarium doped cerium oxide), LSGM (strontium magnesium doped lanthanum gallate) can be used. In particular, zirconium oxide-based ceramics are preferably used. It should be noted that in the present embodiment, the electrolyte layer 4 contains stabilized zirconium oxide.

[0106] The electrolyte layer 4 is preferably formed by a low-temperature sintering method (for example, a wet method using sintering in a low-temperature region instead of sintering in a high-temperature region exceeding 1100°C) or a spraying method (thermal spraying or aerosol deposition method, aerosol gas deposition method, powder jet deposition method, particle jet deposition method, cold spray method, etc.), a PVD method (sputtering method, pulsed laser deposition method, etc.), a CVD method, etc. By these film-forming processes that can be used in a low-temperature region, for example, without using sintering in a high-temperature region exceeding 1100°C, a dense electrolyte layer 4 with high airtightness and gas barrier properties can be obtained. Therefore, damage to the metal support 1 can be suppressed, and element diffusion between the metal support 1 and the electrode layer 2 can be suppressed, so that a solid oxide electrolytic cell E with excellent performance / durability can be realized.

[0107] In particular, if a low-temperature sintering method or a spraying method is used, a low-cost element can be realized, so it is preferred. In addition, if a spraying method is used, it is easy to obtain a dense electrolyte layer 4 with high airtightness and gas barrier properties in a low temperature region, so it is more preferred.

[0108] The electrolyte layer 4 is densely constructed to shield the leakage of the mixed gas supplied to the electrode layer 2 and the oxygen generated in the counter electrode layer 6, and shows high ion conductivity. The density of the electrolyte layer 4 is preferably 90% or more, more preferably 95% or more, and further preferably 98% or more. In the case where the electrolyte layer 4 is a uniform layer, its density is preferably 95% or more, and more preferably 98% or more. In addition, in the case where the electrolyte layer 4 is constructed in multiple layers, it is preferred that at least a portion thereof contains a layer (dense electrolyte layer) with a density of 98% or more, and more preferably contains a layer (dense electrolyte layer) with a density of 99% or more. This is because, if such a dense electrolyte layer is included in a part of the electrolyte layer 4, even if the electrolyte layer 4 is constructed in multiple layers, it is easy to form a dense electrolyte layer 4 with high airtightness and gas barrier properties.

[0109] (Second anti-reaction layer)

[0110] The second reaction-preventing layer 5 can be formed in a thin layer state on the electrolyte layer 4. In the case of a thin layer, the thickness can be set to, for example, about 1 μm to 100 μm, preferably about 2 μm to 50 μm, and more preferably about 3 μm to 15 μm. If such a thickness is set, the amount of expensive reaction-preventing layer material used can be reduced to achieve cost reduction, while ensuring sufficient performance.

[0111] As the material of the second reaction prevention layer 5, any material that can prevent the reaction between the components of the electrolyte layer 4 and the components of the counter electrode layer 6 can be used, for example, cerium oxide-based materials, etc. In addition, as the material of the second reaction prevention layer 5, it is preferred to use a material containing at least one element selected from Sm, Gd and Y. It should be noted that it is preferable that the material contains at least one element selected from Sm, Gd and Y, and the total content of these elements is 1.0 mass% or more and 10 mass% or less. By introducing the second reaction prevention layer 5 between the electrolyte layer 4 and the counter electrode layer 6, the reaction between the constituent materials of the counter electrode layer 6 and the constituent materials of the electrolyte layer 4 can be effectively suppressed, thereby improving the long-term stability of the performance of the solid oxide electrolytic cell E.

[0112] The second reaction preventing layer 5 preferably has oxygen ion (oxide ion) conductivity. In addition, it is more preferably a mixed conductor having both oxygen ion (oxide ion) and electron conductivity. The second reaction preventing layer 5 having such properties is suitable for use in the solid oxide electrolytic cell E.

[0113] The second reaction-preventing layer 5 is preferably formed by appropriately using a method that can be formed at a treatment temperature of 1100°C or less, thereby suppressing damage to the metal support 1 and suppressing element diffusion between the metal support 1 and the electrode layer 2, thereby realizing a solid oxide electrolytic cell E with excellent performance / durability. For example, a low-temperature sintering method (for example, a wet method that uses sintering in a low-temperature region instead of sintering in a high-temperature region exceeding 1100°C), a spraying method (thermal spraying or aerosol deposition method, aerosol gas deposition method, powder spray deposition method, particle spray deposition method, cold spray method, etc.), a PVD method (sputtering method, pulsed laser deposition method, etc.), a CVD method, etc. can be appropriately used. In particular, if a low-temperature sintering method or a spraying method is used, a low-cost electrolytic cell can be realized, which is preferred. In addition, if a low-temperature sintering method is used, the handling of the raw materials becomes easy, which is more preferred.

[0114] (Counter Electrode Layer)

[0115] The counter electrode layer 6 can be formed in a thin layer state on the second reaction preventing layer 5. In the case of a thin layer, the thickness can be set to, for example, about 1 μm to 100 μm, preferably 5 μm to 50 μm. If such a thickness is set, the amount of expensive counter electrode layer material used can be reduced to achieve cost reduction, while ensuring sufficient electrode performance.

[0116] As the material of the counter electrode layer 6, for example, composite oxides such as LSCF and LSM, cerium oxide-based oxides, and mixtures thereof can be used. It is particularly preferred that the counter electrode layer 6 contains a perovskite-type oxide containing two or more elements selected from La, Sr, Sm, Mn, Co, and Fe. The counter electrode layer 6 composed of the above materials functions as an oxygen generating pole.

[0117] It should be noted that if the formation of the electrode layer 6 is appropriately performed using a method that can be formed at a processing temperature below 1100°C, damage to the metal support 1 can be suppressed, and element diffusion between the metal support 1 and the electrode layer 2 can be suppressed, so that a solid oxide electrolytic cell E with excellent performance / durability can be achieved, and therefore it is preferred. For example, a low-temperature sintering method (for example, a wet method using sintering treatment in a low-temperature region instead of sintering treatment in a high-temperature region exceeding 1100°C) can be appropriately used. In particular, if a low-temperature sintering method is used, a low-cost electrolytic cell can be achieved, so it is preferred. In addition, if a low-temperature sintering method is used, the handling of the raw materials becomes easy, so it is more preferred.

[0118] The counter electrode layer 6 of this embodiment has a longitudinal cross-sectional area of ​​0.75 μm 2 The above holes (see Figure 4 and Figure 5 ), preferably with an area of ​​0.75 μm 2 Above (preferably 3 μm 2 More preferably 12 μm 2 Above) and 55μm 2 In particular, there are 3 or more holes with an area of ​​0.75 μm in the longitudinal section. 2 Above (or area 0.75μm 2 Above (preferably 3 μm 2 More preferably 12 μm 2 Above) and 55μm 2 The 10 μm square area of ​​the hole ( Figure 4 Thus, by having a region R1 with an area of ​​0.75 μm in the counter electrode layer 6, 2The above holes can easily release oxygen generated on the counter electrode layer 6 side due to the electrolysis reaction of water vapor or carbon dioxide from the counter electrode layer 6, thereby suppressing the peeling of the counter electrode layer 6 from the second reaction prevention layer 5. It should be noted that if the area of ​​the holes in the counter electrode layer 6 is 0.75 μm 2 If the number of the above holes is small, the release of oxygen from the counter electrode layer 6 is insufficient, and as a result, there is a possibility that the peeling of the counter electrode layer 6 cannot be sufficiently suppressed.

[0119] However, in the solid oxide electrolytic cell E according to the present embodiment, as described above, the counter electrode layer 6 has three or more regions with an area of ​​0.75 μm in its longitudinal section. 2 The area of ​​the 10 μm square area of ​​the above holes in the counter electrode layer 6 is 0.75 μm. 2 The number of holes above this is sufficient for releasing the gas (oxygen) involved in the electrolytic reaction, and thus the peeling of the counter electrode layer 6 can be further suppressed. 2 The above holes are preferably holes with a diameter of 0.5 μm or more in the longitudinal section. In addition, the area in the longitudinal section is 0.75 μm 2 The shape of the above holes in the longitudinal section is Figure 4 The shape in the longitudinal section is generally circular, but the shape may be changed appropriately depending on the shape of the pore-forming material described later or the posture of the pores in the counter electrode layer 6, and may be a triangle, a quadrilateral, or an ellipse in addition to a circle.

[0120] In addition, the counter electrode layer 6 has at least a longitudinal cross-sectional area of ​​0.04 μm 2 The following holes (see Figure 4 and Figure 5 ). That is, the counter electrode layer 6 has both micron-sized pores and nano-sized pores as a whole. In this way, by having both micron-sized pores and nano-sized pores, it is not only easy to release oxygen from the counter electrode layer 6, but also the surface area is increased compared to the case of having only micron-sized pores, so that many electrochemical reaction fields can be ensured in the counter electrode layer 6, and the performance / strength as an electrolytic cell can be improved. It should be noted that the area is 0.04μm 2 The following pores are preferably pores having a diameter of 0.1 μm or less in a longitudinal section.

[0121] It should be noted that if the area of ​​the counter electrode layer 6 (first electrode layer) is 0.75 μm 2 If there are too many holes, the strength of the counter electrode layer 6 will be reduced, and it may be difficult to ensure the durability of the solid oxide electrolytic cell E. On the contrary, as mentioned above, if the area of ​​the holes in the counter electrode layer 6 is 0.75 μm 2If the number of the above holes is small, the release of oxygen from the counter electrode layer 6 is likely to be insufficient, and the peeling of the counter electrode layer 6 may not be sufficiently suppressed. Therefore, it is preferable that the counter electrode layer 6 has an area of ​​0.75 μm 2 Therefore, it is preferred that the counter electrode layer 6 has a hole with an area of ​​only 0.75 μm 2 Above (or area 0.75μm 2 Above (preferably 3 μm 2 More preferably 12 μm 2 Above) and 55μm 2 The proportion of pores (less than 10%), i.e., the first porosity, is greater than 5% and less than 20% of the longitudinal section. In this way, the strength of the electrode layer 6 can be ensured while suppressing the peeling of the electrode layer 6. It should be noted that the lower limit of the first porosity is more preferably greater than 8%, and more preferably greater than 10%. In addition, the upper limit of the first porosity is more preferably less than 15%, and more preferably less than 12%.

[0122] From the same viewpoint, the counter electrode layer 6 preferably has an area of ​​0.75 μm 2 The pore area is 0.04 μm. 2 The proportion of the following pores, i.e., the second porosity, is 10% or more and 40% or less in the longitudinal section. It should be noted that the lower limit of the second porosity is preferably 15% or more, more preferably 20% or more, and the upper limit of the second porosity is preferably 35% or less, more preferably 30% or less. In addition, it is preferred that only 0.04 μm in area exist in the electrode layer 6. 2 The third porosity of the following pores is 5% or more and 35% or less in the longitudinal section. It should be noted that the lower limit of the third porosity is preferably 7% or more, more preferably 10% or more, and the upper limit of the third porosity is preferably 20% or less, more preferably 18% or less. Even in this case, the strength of the electrode layer 6 can be ensured while suppressing the peeling of the electrode layer 6.

[0123] It should be noted that the area appearing on the longitudinal section is 0.75 μm 2 The above holes vary depending on the dispersion of the pore-forming material during production or the location of the cross section, but are assumed to be 0.75 μm in area. 2 When the above pores are uniformly dispersed in the entire counter electrode layer 6, the first porosity is equivalent to a pore size of only 0.75 μm 2 The porosity of the above pores is the volume ratio of the entire electrode layer 6. In addition, assuming that the area is 0.04 μm 2 When the following pores are also uniformly dispersed in the entire counter electrode layer 6, the second porosity is equivalent to an area of ​​0.75 μm 2 The pore area is 0.04 μm.2 The following porosity is the volume ratio of the pores in the entire counter electrode layer 6. The third porosity is equivalent to a porosity of 0.04 μm in area. 2 The following porosity is the volume ratio of the pores in the entire counter electrode layer 6. In addition, it is assumed that most of the pores existing in the counter electrode layer 6 are 0.75 μm in area on the longitudinal section. 2 Pores above 0.04 μm 2 The following holes occupy an area of ​​0.75 μm 2 The pore area is 0.04 μm. 2 When the following pores are uniformly dispersed throughout the counter electrode layer 6 , the second porosity may be regarded as the porosity of the counter electrode layer 6 .

[0124] In addition, the counter electrode layer 6 contains at least a plurality of particles having a particle size (average particle size) of 0.1 μm or less. In addition, the counter electrode layer 6 preferably has at least a region ( Figure 5 Thus, a large number of electrochemical reaction fields can be ensured, thereby obtaining a high-performance counter electrode layer 6.

[0125] In addition, an extreme decrease in the strength of the counter electrode layer 6 can also be suppressed.

[0126] When the solid oxide electrolytic cell E having the above-described structure is operated, for example, a mixed gas (water vapor or carbon dioxide) is flowed through the electrode layer 2, and a voltage is applied between the electrode layer 2 and the counter electrode layer 6. As a result, the electrons e in the electrode layer 2 are - Reacts with water H2O or carbon dioxide molecules CO2 to form reducing components such as hydrogen H2 or carbon monoxide CO and oxygen ions O 2- . Oxygen ion O 2- Move to the counter electrode layer 6 through the electrolyte layer 4. Then, the oxygen ions O in the counter electrode layer 6 2- It releases electrons and becomes oxygen O2. Through the above reaction, water H2O is electrolyzed into hydrogen H2 and oxygen O2. When a gas containing carbon dioxide molecules CO2 is passed through, it is electrolyzed into carbon monoxide CO and oxygen O2.

[0127] (Method for manufacturing solid oxide electrolytic cell)

[0128] Next, a method for manufacturing the solid oxide electrolytic cell E is described. The method for manufacturing the solid oxide electrolytic cell E according to the present embodiment includes an electrode layer forming step, a first reaction preventing layer forming step, an electrolyte layer forming step, a second reaction preventing layer forming step, and a counter electrode layer forming step.

[0129] It should be noted that the treatment temperature in all of these steps (all processes) is preferably 1100° C. or lower.

[0130] (Electrode layer forming step)

[0131] In the electrode layer forming step, the electrode layer 2 is formed in a thin film state on the metal support 1. The electrode layer 2 can be formed by the above-mentioned film forming method, but in order to suppress the degradation of the metal support 1, it is preferable to use a film forming method that can be used in a low temperature range of 1100°C or less.

[0132] In the case where the electrode layer forming step is performed by the low temperature firing method, it is specifically performed as in the following example.

[0133] First, the material powder of the electrode layer 2 and the solvent (dispersion medium) are mixed to prepare a material paste, which is applied to the surface of the surface side of the metal support 1. The electrode layer 2 is then compression molded (electrode layer smoothing process) and sintered at a temperature below 1100°C (electrode layer sintering process). The compression molding of the electrode layer 2 can be performed by, for example, CIP (Cold Isostatic Pressing: cold isostatic pressing) molding, roller press molding, RIP (Rubber Isostatic Pressing: rubber mold isostatic pressing) molding, etc. In addition, the sintering of the electrode layer 2 is preferably performed at a temperature above 800°C and below 1100°C. In addition, the order of the electrode layer smoothing process and the electrode layer sintering process may also be exchanged.

[0134] It should be noted that, in this embodiment, since the first reaction-preventing layer 3 is formed after the electrode layer 2 is formed, the electrode layer smoothing step and the electrode layer firing step can be omitted, or the electrode layer smoothing step and the electrode layer firing step can be included in the reaction-preventing layer smoothing step and the reaction-preventing layer firing step described later. In addition, the electrode layer smoothing step can also be performed by performing grinding molding or leveling treatment, surface cutting / polishing treatment, etc.

[0135] In addition, in the present embodiment, during the firing process in the electrode layer forming step, a metal oxide layer 1b (diffusion suppression layer) is formed on the surface of the metal support 1. That is, in the present embodiment, the firing process includes a firing process in which the firing atmosphere is set to an atmosphere condition with a low oxygen partial pressure. As a result, the mutual diffusion suppression effect of the elements is high, and a high-quality metal oxide layer 1b with a low resistance value is formed. It should be noted that, including the case where the electrolyte layer forming step is performed by a method without firing, a process of forming a diffusion suppression layer may be performed separately.

[0136] (First anti-reaction layer forming step)

[0137] In the first reaction preventing layer forming step, the first reaction preventing layer 3 is formed in a thin layer on the electrode layer 2 in the form of covering the electrode layer 2. The first reaction preventing layer 3 can be formed by the above-mentioned film forming method, but in order to suppress the degradation of the metal support 1, it is preferable to use a film forming method that can be used in a low temperature range of 1100° C. or less.

[0138] In the case where the first anti-reaction layer formation step is performed by a low-temperature sintering method, it is specifically performed as in the following example. First, the material powder of the first anti-reaction layer 3 and the solvent (dispersion medium) are mixed to prepare a material paste, which is applied to the surface of the surface side of the electrode layer 2. Then the first anti-reaction layer 3 is compression molded (first anti-reaction layer smoothing process) and sintered at a temperature below 1100°C (first anti-reaction layer sintering process). The compression molding of the first anti-reaction layer 3 can be performed by, for example, CIP molding, roller press molding, RIP molding, etc. In addition, the sintering of the first anti-reaction layer 3 is preferably performed at a temperature above 800°C and below 1100°C. This is because, if it is such a temperature, the damage / deterioration of the metal support 1 can be suppressed, and at the same time, the first anti-reaction layer 3 with high strength is formed. In addition, it is more preferred to sinter the first anti-reaction layer 3 at a temperature below 1050°C, and further preferably at a temperature below 1000°C. This is because, as the firing temperature of the first reaction prevention layer 3 is lowered, the damage / deterioration of the metal support 1 can be further suppressed, and the solid oxide type electrolytic cell E can be formed. It should be noted that the order of the first reaction prevention layer smoothing step and the first reaction prevention layer firing step can also be exchanged. In addition, the first reaction prevention layer smoothing step can also be performed by performing grinding molding or flattening treatment, surface cutting / polishing treatment, etc.

[0139] (Electrolyte layer forming step)

[0140] In the electrolyte layer forming step, the electrolyte layer 4 is formed on the first reaction prevention layer 3 in a thin layer state in a state of covering the electrode layer 2 and the first reaction prevention layer 3. The electrolyte layer 4 can be formed using the above-mentioned film forming method that can be used in a low temperature region, preferably using a spraying method. In particular, in terms of forming a high-quality electrolyte layer 4 that is dense and has high airtightness and gas barrier properties in a temperature range below 1100°C, it is more preferred to use any one of an aerosol deposition method, an aerosol gas deposition method, a powder spray deposition method, and a particle spray deposition method. In the present embodiment, the electrolyte layer 4 is formed using an aerosol deposition method. Specifically, the material powder of the aerosolized electrolyte layer 4 (in the present embodiment, a fine powder of stabilized zirconia such as YSZ or SSZ) is sprayed onto the first reaction prevention layer 3 on the metal support 1 to form the electrolyte layer 4.

[0141] (Second anti-reaction layer forming step)

[0142] In the second reaction preventing layer forming step, the second reaction preventing layer 5 is formed in a thin layer state on the electrolyte layer 4. The second reaction preventing layer 5 can be formed in the same manner as in the first reaction preventing layer forming step, and the above-mentioned film forming method can be used, but in order to suppress the degradation of the metal support 1, it is preferable to use a film forming method that can be used in a low temperature region of 1100° C. or less.

[0143] (Counter Electrode Layer Formation Step)

[0144] In the counter electrode layer forming step, the counter electrode layer 6 is formed as a thin layer on the second reaction preventing layer 5. The counter electrode layer 6 can be formed by the above-mentioned film forming method, but in order to suppress the degradation of the metal support 1, it is preferable to use a film forming method that can be used in a low temperature range of 1100°C or less.

[0145] In the case of performing the electrode layer formation step by a low-temperature sintering method, it is specifically carried out as in the following example. First, the material powder of the electrode layer 6, the pore-forming material and the solvent (dispersion medium) are mixed to prepare a material paste, which is applied to the surface of the surface side of the metal support 1. Then, the electrode layer 2 is compression molded (electrode layer smoothing process) and sintered at a temperature below 1100°C (electrode layer sintering process). Thus, the electrode layer 6 has an area of ​​0.75 μm in the longitudinal section. 2 It should be noted that as the pore-forming material, PMMA (polymethyl methacrylate) or PVDF (polyvinylidene fluoride) can be used. In addition, the mixing amount of the pore-forming material is as long as the area to be formed in the electrode layer 6 is 0.75 μm 2 The amount of the above pores can be appropriately determined. If the above-mentioned first porosity and second porosity are taken into consideration, the mixing ratio (mass basis) of the material powder relative to the counter electrode layer 6 is preferably 2% to 8%. In addition, the particle size (average particle size) of the pore-forming material can be appropriately determined according to the diameter of the pores to be formed in the counter electrode layer 6, for example, 0.5 μm or more and 4 μm or less, and in the present embodiment, 2 μm. It should be noted that the pore-forming material is not limited to a spherical shape, but can also be various shapes such as an ellipsoidal shape, a cylindrical shape, a prism shape, and a pellet shape.

[0146] As described above, it is possible to manufacture the solid oxide electrolytic cell E which has the counter electrode layer 6 which easily releases oxygen and can suppress the peeling of the counter electrode layer 6 .

[0147] (Solid Oxide Electrolysis Module)

[0148] Below, refer to Figure 2The solid oxide electrolysis module M is described. The solid oxide electrolysis module M includes a solid oxide electrolysis cell E in a state of a cylindrical support body formed by a metal support body 1 and a U-shaped member 9 mounted on the back of the metal support body 1. Moreover, the solid oxide electrolysis cell E is sandwiched by a plurality of stacked layers (a plurality of sets) of current collecting members 26 to constitute the solid oxide electrolysis module M. It should be noted that in the present embodiment, the current collecting member 26 is joined to the counter electrode layer 6 and the U-shaped member 9 of the solid oxide electrolysis cell E to electrically connect the two, but it can also be configured so that the counter electrode layer 6 and the U-shaped member 9 of the solid oxide electrolysis cell E are directly electrically connected.

[0149] In addition, the solid oxide electrolysis module M has a gas manifold 17, a terminal member, and a current lead-out portion. One open end of the cylindrical support of the plurality of stacked solid oxide electrolysis cells E is connected to the gas manifold 17, and gas (water vapor or carbon dioxide) is supplied from the gas manifold 17. The supplied gas flows through the inside of the cylindrical support and is supplied to the electrode layer 2 through the through hole 1a of the metal support 1.

[0150] (Electrochemical devices and energy systems)

[0151] Below, refer to Figure 3 , an electrochemical device Y and an energy system Z constructed using the above-mentioned solid oxide electrolysis module M are described.

[0152] like Figure 3 As shown, the energy system Z includes an electrochemical device Y and two heat exchangers 90 and 92 as waste heat utilization units for reusing heat flowing from the electrochemical device Y.

[0153] The electrochemical device Y includes a solid oxide electrolysis module M, a fuel converter 91 for synthesizing hydrocarbons based on hydrogen or the like generated in the solid oxide electrolysis module M, and a power converter 93 for allowing power to flow to the solid oxide electrolysis module M.

[0154] In the electrochemical device Y, the solid oxide electrolysis module M has a plurality of solid oxide electrolytic cells E and two gas manifolds 17, 171. The plurality of solid oxide electrolytic cells E are arranged in parallel in a state of being electrically connected to each other. One end (lower end) of the solid oxide electrolytic cell E is fixed to the gas manifold 17, and the other end (upper end) is fixed to the gas manifold 171. The gas manifold 17 at one end of the solid oxide electrolytic cell E receives the supply of water vapor and carbon dioxide. Then, the hydrogen and carbon monoxide generated by the above reaction in the solid oxide electrolytic cell E are collected by the gas manifold 171 connected to the other end.

[0155] In addition, in the electrochemical device Y, the power converter 93 allows power to flow to the solid oxide electrolytic cell E of the solid oxide electrolytic module M. Thus, in the solid oxide electrolytic cell E, water vapor and carbon dioxide supplied through the gas manifold 17 fixed to the lower end are electrolyzed, and hydrogen and carbon monoxide are converted into fuel through the gas manifold 171 fixed to the upper end via the heat exchanger 92, the fuel converter 91, and the heat exchanger 90. On the other hand, oxygen is released from the counter electrode layer 6 and discharged to the outside.

[0156] In the energy system Z, the heat exchanger 90 is operated as a waste heat utilization unit for exchanging heat between the reaction heat generated by the reaction in the fuel converter 91 and water to vaporize the water, and the heat exchanger 92 is operated as a waste heat utilization unit for exchanging heat between the waste heat generated by the solid oxide electrolytic cell E and water vapor and carbon dioxide to preheat the water vapor and carbon dioxide. By adopting such a configuration, energy efficiency is improved.

[0157] Example

[0158] First, a plurality of through holes 1a were formed in a region with a radius of 6 mm from the center of a circular ferritic stainless steel plate (metal plate) having a thickness of 0.3 mm and a diameter of 25 mm by laser processing to produce a metal support 1.

[0159] Next, 60% by mass of NiO powder and 40% by mass of GDC powder are mixed, and an organic binder and an organic solvent (dispersion medium) are added to make a paste. Using this paste, an electrode layer 2 is stacked in an area with a radius of 8 mm from the center of the metal support 1. It should be noted that the electrode layer 2 is formed using screen printing. Then, the metal support 1 stacked with the electrode layer 2 is sintered at 1000°C (electrode layer formation step).

[0160] Next, an organic binder and an organic solvent (dispersion medium) are added to the GDC powder to prepare a paste. The paste is used to laminate the first reaction prevention layer 3 by screen printing in a region with a radius of 10 mm from the center of the metal support 1 laminated with the electrode layer 2. Then, the metal support 1 laminated with the first reaction prevention layer 3 is CIP-molded at a pressure of 300 MPa and then sintered at 1000°C to form the first reaction prevention layer 3 with a flat surface (first reaction prevention layer formation step).

[0161] The electrode layer 2 obtained through the above steps has a thickness of about 25 μm, and the first reaction-preventing layer 3 has a thickness of about 10 μm.

[0162] Next, the electrolyte layer 4 is formed by aerosol deposition. Specifically, 8YSZ (yttria-stabilized zirconia) powder with a vibration shape of about 0.7 μm is aerosolized in dry air at a flow rate of 13 L / min. The aerosol is introduced into a chamber with a pressure set to 250 Pa, and for a metal support 1 stacked with an electrode layer 2 and a first reaction prevention layer 3, the first reaction prevention layer 3 is sprayed onto the entire surface of the metal support to form an electrolyte layer 4 (electrolyte layer formation step). It should be noted that at this time, the metal support 1 is not heated.

[0163] The thickness of the electrolyte layer 4 obtained by the above steps is about 3 to 4 μm. The He leakage of the metal support 1 in the state where the electrode layer 2, the first reaction prevention layer 3 and the electrolyte layer 4 are stacked was measured under a pressure of 0.2 MPa. The results showed that the He leakage was lower than the detection limit (1.0 mL / min·cm 2 ). That is, the He leakage in the state where the electrolyte layer 4 is stacked is significantly reduced and is below the detection limit compared to the He leakage in the state where the electrolyte layer 4 is stacked, and is below the detection limit. Therefore, it is confirmed that the formed electrolyte layer 4 is a dense and high-quality electrolyte layer with high gas barrier performance.

[0164] Next, an organic binder and an organic solvent (dispersion medium) are added to the GDC powder to prepare a paste. The paste is used to form a second reaction prevention layer 5 on the electrolyte layer 4 by screen printing. Then, the formed solid oxide electrolytic cell E is calcined at 1000° C. to form the second reaction prevention layer 5 (second reaction prevention layer formation step).

[0165] Next, as an example, GDC powder, LSCF powder and PMMA powder (particle size: 2 μm) as a pore-forming material are mixed (the mixing ratio (mass basis) of the pore-forming material to GDC powder + LSCF powder is 3.3%), and an organic binder and an organic solvent (dispersion medium) are added to prepare a paste. Using this paste, a counter electrode layer 6 is formed on the second reaction-proof layer 5 by screen printing. Finally, the solid oxide electrolytic cell E formed with the electrode layer 6 is fired at 900° C. to burn out the pore-forming material (counter electrode layer formation step).

[0166] In addition, as a comparative example, after forming the second reaction prevention layer 5 by the same procedure as above, GDC powder and LSCF powder were mixed, and an organic binder and an organic solvent (dispersion medium) were added to prepare a paste, and the paste was used to form a counter electrode layer 6 on the second reaction prevention layer 5 by screen printing. Then, the solid oxide type electrolytic cell E with the counter electrode layer 6 formed thereon was sintered at 900°C.

[0167] Figure 4 and Figure 5This is a SEM image obtained by photographing a longitudinal section of the solid oxide electrolytic cell E involved in the example. Figure 6 This is a SEM image obtained by photographing a longitudinal cross section of a solid oxide electrolytic cell according to a comparative example. Figures 4 to 6 It can be seen that by using a pore-forming material when forming the counter electrode layer 6, a pore-forming material with an area of ​​0.75 μm can be formed. 2 The first porosity, the second porosity, and the third porosity of the solid oxide electrolytic cell E according to the embodiment are 10.5%, 22.5%, and 12.0%, respectively. On the other hand, the first porosity, the second porosity, and the third porosity of the solid oxide electrolytic cell according to the comparative example are 0%, 15.2%, and 15.2%, respectively. It should be noted that each porosity is calculated by processing the above-mentioned SEM image.

[0168] Next, an electrolysis test was performed on the solid oxide electrolytic cells of the embodiment and the comparative example prepared as described above, with a voltage (1.3 V) applied near the thermal neutral point. As a result, in the solid oxide electrolytic cell of the embodiment, no peeling of the electrode layer 6 was found even when a voltage of 1.3 V was applied. In contrast, in the solid oxide electrolytic cell of the comparative example, the electrode layer 6 was peeled off by applying a voltage of 1.3 V. It can be confirmed that by making the electrode layer 6 have an area of ​​0.75 μm 2 The above-described holes can suppress the peeling of the counter electrode layer 6 even when a voltage near the thermal neutral point is applied.

[0169] [Other embodiments]

[0170] [1] In the above embodiment, the solid oxide type electrolytic cell E is provided with the first anti-reaction layer 3 and the second anti-reaction layer 5, but the present invention is not limited thereto and may be provided without the first anti-reaction layer 3 and / or the second anti-reaction layer 5. In this case, for example, the solid oxide type electrolytic cell E is in a state where the electrolyte layer 4 is formed on the electrode layer 2, or in a state where the counter electrode layer 6 is formed on the electrolyte layer 4.

[0171] [2] In the above embodiment, a method is adopted in which the metal support 1 is formed of a metal plate subjected to via processing, but the present invention is not limited to this. For example, a method without the metal support 1 or a method in which the metal support 1 is formed of a porous body obtained by sintering metal powder may also be adopted.

[0172] [3] In the above embodiment, a plurality of solid oxide electrolytic cells E are combined to form a solid oxide electrolytic module M, but the present invention is not limited thereto and a single solid oxide electrolytic cell E may be used.

[0173] [4] In the above embodiment, the energy system Z is provided with a waste heat utilization unit for reusing the heat exhausted from the electrochemical device Y. However, the present invention is not limited to this and may be provided without the waste heat utilization unit.

[0174] [5] In the above embodiment, the electrode layer 6 is an oxygen generating electrode, but the present invention is not limited thereto. Alternatively, the electrode layer 2 may be an oxygen generating electrode. In this case, the electrode layer 2 is formed to have an area of ​​0.75 μm in its longitudinal section. 2 The holes above the electrode layer 2 are formed, and water vapor or carbon dioxide is supplied to the counter electrode layer 6 side, and a voltage is applied between the electrode layer 2 and the counter electrode layer 6, thereby electrons e in the counter electrode layer 6 are - Reacts with water H2O or carbon dioxide molecules CO2 to form hydrogen H2 or carbon monoxide CO and oxygen ions O 2- Then, the oxygen ion O 2- Move through the electrolyte layer 4 to the electrode layer 2, and the oxygen ions O 2- The electrons are released to form oxygen O 2 , and the oxygen O 2 is released from the electrode layer 2 .

[0175] [6] In the above embodiment, the solid oxide electrolytic module M includes a solid oxide electrolytic cell E in a state where the solid oxide electrolytic module M includes a metal support 1 and a U-shaped member 9 mounted on the back of the metal support 1 to form a cylindrical support, but the present invention is not limited thereto. Figure 7 As shown, a solid oxide electrolytic cell E may be stacked with an inter-cell connecting member 71 therebetween to form a solid oxide electrolytic module M.

[0176] In this case, the inter-cell connection member 71 is a plate-shaped member having conductivity and no gas permeability, and has mutually orthogonal grooves 72 formed on the front and back surfaces. The inter-cell connection member 71 can be made of metal such as stainless steel or metal oxide.

[0177] Furthermore, when the solid oxide type electrolytic cells E are stacked with the inter-cell connecting member 71 therebetween, the gas can flow through the grooves 72, and the gas can be supplied to / recovered from the solid oxide type electrolytic cells E. Specifically, the grooves 72 formed on one surface become the first gas flow path 72a, which allows the oxygen released from the surface side of the solid oxide type electrolytic cell E, that is, from the counter electrode layer 6 to flow. In addition, the grooves 72 formed on the other surface become the second gas flow path 72b, which allows the water vapor or carbon dioxide supplied to the electrode layer 2 from the back side of the solid oxide type electrolytic cell E, that is, the back side of the metal support 1 through the through hole 1a to flow.

[0178] In the solid oxide electrolysis module M configured in this way, water vapor or carbon dioxide is supplied to the second gas flow path 72b, and a voltage is applied between the electrode layer 2 and the counter electrode layer 6 to perform an electrolysis reaction, thereby generating hydrogen or carbon monoxide on the electrode layer 2 side, and these generated gases flow through the second gas flow path 72b. In addition, oxygen is released from the counter electrode layer 6, and the released oxygen flows through the first gas flow path 72a.

[0179] It should be noted that, regarding the grooves 72 , the grooves formed on the front surface of the inter-cell connecting member 71 and the grooves formed on the back surface may be parallel to each other.

[0180] [7] In the above-mentioned embodiment, the solid oxide type electrolytic cell E is mainly a flat plate type or a cylindrical flat plate type, but it is not limited thereto. The solid oxide type electrolytic cell E may also be a cylindrical type.

[0181] [8] In the above embodiment, the electrochemical device Y includes a solid oxide electrolysis module M having a plurality of solid oxide electrolysis cells E, but the present invention is not limited thereto. For example, the electrochemical device may include one solid oxide electrolysis cell E.

[0182] It should be noted that the configuration disclosed in the above-mentioned embodiment (including other embodiments, the same below) can be combined with the configuration disclosed in other embodiments as long as no contradiction occurs. In addition, the embodiments disclosed in this specification are for illustration only, and the embodiments of the present invention are not limited thereto and can be appropriately changed within the scope of the purpose of the present invention.

[0183] Explanation of symbols

[0184] 1: Metal support,

[0185] 2: electrode layer (second electrode layer),

[0186] 3: The first anti-reaction layer,

[0187] 4: Electrolyte layer,

[0188] 5: The second anti-reaction layer,

[0189] 6: Counter electrode layer (first electrode layer),

[0190] E: solid oxide electrolytic cell,

[0191] M: solid oxide electrolysis module,

[0192] Y: electrochemical device,

[0193] Z: Energy system.

Claims

1. A solid oxide electrolytic cell comprising at least a first electrode layer, a second electrode layer and an electrolyte layer disposed between the first electrode layer and the second electrode layer, The first electrode layer has at least a plurality of electrodes with an area of ​​0.75 μm in its longitudinal section. 2 The hole above.

2. The solid oxide electrolytic cell according to claim 1, wherein: The first electrode layer has at least three or more electrodes with an area of ​​0.75 μm in its longitudinal section. 2 The above holes have a 10 μm square area.

3. The solid oxide electrolytic cell according to claim 1, wherein: The area in the first electrode layer is 0.75 μm 2 The above pores are pores having a diameter of 0.5 μm or more.

4. The solid oxide electrolytic cell according to claim 1, wherein: The first electrode layer has at least an area of ​​0.04 μm in its longitudinal section. 2 The following hole.

5. The solid oxide electrolytic cell according to claim 4, wherein: The area in the first electrode layer is 0.04 μm 2 The following pores are pores having a diameter of 0.1 μm or less.

6. The solid oxide electrolytic cell according to claim 1, wherein: The first electrode layer has a surface area of ​​0.75 μm 2 The first porosity associated with the above pores is 5% or more and less than 20% of the longitudinal section.

7. The solid oxide electrolytic cell according to claim 4, wherein: The first electrode layer has a surface area of ​​0.75 μm 2 The area of ​​the hole is 0.04 μm 2 The second porosity of the following pores is 10% or more and 40% or less in the longitudinal section.

8. The solid oxide electrolytic cell according to claim 1, wherein: The first electrode layer contains at least a plurality of particles having a particle size of 0.1 μm or less.

9. The solid oxide electrolytic cell according to claim 1, wherein: The first electrode layer is an oxygen generating electrode.

10. The solid oxide electrolytic cell according to claim 1, wherein: An anti-reaction layer is disposed between the first electrode layer and the electrolyte layer.

11. The solid oxide electrolytic cell according to claim 1, wherein: The electrolyte layer contains an oxide ion conductor.

12. The solid oxide electrolytic cell according to claim 1, comprising a metal support.

13. A method for producing a solid oxide electrolytic cell, which is the method for producing a solid oxide electrolytic cell according to any one of claims 1 to 12, wherein: A pore-forming material is used in the step of forming the first electrode layer.

14. A method for producing a solid oxide electrolytic cell, which is the method for producing a solid oxide electrolytic cell according to any one of claims 1 to 12, wherein: The processing temperature in all steps is 1100° C. or less.

15. A solid oxide electrolysis module, wherein: The solid oxide electrolytic cell according to any one of claims 1 to 12 is arranged in a state of being assembled in plurality.

16. An electrochemical device comprising at least the solid oxide electrolytic cell according to any one of claims 1 to 12 and a fuel converter for converting a gas containing a reducing component generated in the solid oxide electrolytic cell.

17. An electrochemical device comprising at least the solid oxide electrolysis module according to claim 15 and a fuel converter for converting a gas containing a reducing component generated in the solid oxide electrolysis module.

18. An electrochemical device comprising at least the solid oxide electrolytic cell according to any one of claims 1 to 12 and a power converter for flowing electric power into the solid oxide electrolytic cell.

19. An electrochemical device comprising at least the solid oxide electrolysis module according to claim 15 and a power converter for allowing electric power to flow into the solid oxide electrolysis module.

20. An energy system comprising at least the electrochemical device according to claim 16 and a waste heat utilization unit for reusing heat exhausted from the electrochemical device.