Wiring board
By adding nanosilicon dioxide particles and copper microcrystals to the conductor layer of the wiring substrate to control sintering and adhesion, the problem of insufficient conductivity at the interface of the conductor layer is solved, and high-frequency stable conductivity and low-cost production are achieved.
Patent Information
- Application Number
- CN202380028008.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-30
- Filing Date
- 2023-03-13
- Publication Date
- 2024-11-12
AI Technical Summary
The conventional wiring substrate has room for improvement in the interface conductivity of the conductor layer, and it is difficult to maintain efficient conductivity in high-frequency regions.
By adding nano-sized silica particles to the ceramic insulating layer and metal conductor layer, the sintering behavior and adhesion are controlled to ensure the compactness and flat surface of the conductor layer. The conductor layer is composed of microcrystals of metal materials such as copper and silver. , and set a specific profile ratio in the conductor layer (L1/L0 is 1.04-1.40) to improve the interface conductivity.
The interface conductivity of the conductor layer is significantly improved, the conductor stripping phenomenon is reduced, and stable conductivity is maintained in high-frequency areas, reducing manufacturing costs.
Smart Images

Figure CN118947228A_ABST
Abstract
Description
Technical Field
[0001] An embodiment of the present invention relates to a wiring substrate. Background Art
[0002] Conventionally, there is known a wiring substrate having an insulating layer mainly composed of ceramic and a conductive layer mainly composed of metal. The wiring substrate is obtained by, for example, simultaneously firing a conductive material having a metal oxide added to copper powder and a glass ceramic as a material for the insulating layer (for example, see Patent Document 1).
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2003-277852. Summary of the invention
[0006] The wiring substrate of the present invention comprises: an insulating layer, the insulating layer being composed of ceramic; and a conductor layer, the conductor layer extending in a planar direction inside the insulating layer. The conductor layer is composed of a sintered body of a plurality of microcrystals having a metal as a main component. When a specific range of the conductor layer is specified in a cross-sectional view, and the straight line length in the planar direction is set to L0, and the length of the outline of the conductor layer is set to L1, L1 / L0 is in the range of 1.04 to 1.40. BRIEF DESCRIPTION OF THE DRAWINGS
[0007] Figure 1 It is an enlarged cross-sectional view showing an example of the structure of the wiring substrate according to the embodiment.
[0008] Figure 2 yes Figure 1 An enlarged view of area A is shown.
[0009] Figure 3 This is a diagram showing a SEM observation photograph of the conductor layer of Example 1. DETAILED DESCRIPTION
[0010] Hereinafter, the embodiments of the wiring substrate disclosed in the present application will be described with reference to the accompanying drawings. In addition, the present invention is not limited to the embodiments shown below. In addition, each embodiment can be appropriately combined within the scope of not making the processing content contradictory. In addition, in each of the following embodiments, the same reference numeral is marked on the same part, and repeated description is omitted.
[0011] In the embodiments described below, the expression “parallel” may be used, but these expressions do not strictly require “parallel.” That is, the above expressions allow for variations in manufacturing accuracy, mounting accuracy, and the like.
[0012] Conventionally, there is known a wiring board having an insulating layer mainly composed of ceramic and a conductive layer mainly composed of metal. This wiring board is obtained by, for example, simultaneously firing a conductive material obtained by adding metal oxide to copper powder and glass ceramic as a material for the insulating layer.
[0013] However, in the prior art, there is still room for further improvement in improving the interface conductivity of the conductor layer. Therefore, it is desired to overcome the above problems and realize a technology that can improve the interface conductivity of the conductor layer in the wiring substrate.
[0014] Figure 1 is an enlarged cross-sectional view showing an example of a wiring substrate 1 according to the embodiment, Figure 2 yes Figure 1 The enlarged view of area A is shown. Figure 1 and Figure 2 As shown, the wiring board 1 of the embodiment includes an insulating layer 10 and a conductive layer 20 .
[0015] For example, a glass ceramic sintered body can be used as an example of the insulating layer 10. The glass ceramic sintered body may contain ceramics such as aluminum oxide, aluminum nitride, silicon carbide, silicon nitride, or mullite as a filler.
[0016] Insulating layer 10 may be made of glass ceramics, for example. Thus, wiring board 1 can be manufactured by simultaneously firing a green sheet as a raw material of insulating layer 10 and a conductive paste as a raw material of conductive layer 20. Therefore, according to the embodiment, the manufacturing cost of wiring board 1 can be reduced.
[0017] The insulating layer 10 may include a first layer 11 and a second layer 12 facing each other across the conductive layer 20. The first layer 11 and the second layer 12 are disposed, for example, so as to sandwich both surfaces of the conductive layer 20 in the thickness direction.
[0018] The conductor layer 20 has conductivity and is arranged inside the insulating layer 10 along the plane direction ( Figure 1 The conductor layer 20 is arranged between the first layer 11 and the second layer 12 in a predetermined pattern shape, for example. It should be noted that in the present invention, the conductor layer 20 may be arranged to be exposed on the surface of the wiring substrate 1.
[0019] like Figure 2 As shown, the conductor layer 20 is composed of a sintered body of a plurality of microcrystals 21. The microcrystals 21 are composed of a metal material such as copper, silver, palladium, gold, platinum, tungsten, molybdenum or manganese, or an alloy material or a mixed material having these metal materials as main components.
[0020] Here, the main component is a metal material or a metal (e.g., copper) means that the metal accounts for 70% or more by volume in the conductor layer 20. When the conductor layer 20 includes voids, the volume ratio of the metal when the voids are removed may be 80% or more. The upper limit of the volume ratio of the metal (e.g., copper) contained in the conductor layer 20 may also be 99%.
[0021] The upper limit of the volume ratio of the metal (e.g., copper) contained in the conductor layer 20 is set to 99% because the wiring substrate 1 of the present invention is formed by simultaneously sintering a ceramic insulating layer and a metal, and therefore, it is considered that the elements contained in the insulating layer inevitably enter the conductor layer 20 from the insulating layer 10.
[0022] The volume ratio of the metal in the conductor layer 20 is obtained, for example, by the following method. In this case, the area ratio of the metal obtained by the following method is used as the volume ratio. First, the wiring board 1 is cut or broken to expose the internal cross section.
[0023] Then, one conductor layer 20 observed in the cross section of the exposed wiring substrate 1 is selected. At this time, when the length of the conductor layer 20 is as long as the width of the wiring substrate 1, a specific length is designated.
[0024] The designated length is sufficient as long as the portion of the conductor layer 20 to be evaluated is within the range of one photograph or screen during observation and photography using a scanning electron microscope (SEM) described later. The length is preferably greater than the thickness of the conductor layer 20. As a reference for the length, it is preferably greater than 1 μm and less than 100 μm.
[0025] It should be noted that, in the cross section of the wiring substrate 1, the range of the conductor layer 20 as the object is preferably set to a range in which the outline can be seen when observed using a scanning electron microscope, for example. The outline of the conductor layer 20 is preferably obtained by using a reflected electron image, which is one of the analysis methods of a scanning electron microscope, or can be obtained by mapping analysis using an element analyzer attached to the scanning electron microscope.
[0026] Alternatively, the volume ratio of the metal may be measured using an electron backscatter diffraction (EBSD) method. By using the electron backscatter diffraction method, the volume ratio (area ratio) of the conductor layer 20 is determined and it can be confirmed that the metal constituting the conductor layer 20 is composed of a plurality of microcrystals.
[0027] When there are voids (including pores) in the conductor layer 20, the area of all voids included in the observed range may be removed from the area of the conductor layer 20. The void size used as the void count is based on a size having a maximum diameter of 0.1 μm or more.
[0028] Here, in this embodiment, a specific range (for example, region A) of the conductor layer 20 is specified in the cross-sectional view, and the plane direction ( Figure 2 When the length of a straight line (in the horizontal direction) is defined as L0 and the length of the outline 20a of the conductor layer 20 (that is, the interface length between the conductor layer 20 and the insulating layer 10) is defined as L1, L1 / L0 is in the range of 1.04 to 1.40.
[0029] Here, the specific range refers to a range in which the width of the conductor layer 20 in the longitudinal direction is greater than or equal to 10 μm and less than or equal to 100 μm. The width in the longitudinal direction within the specific range can be any width selected within the range of greater than or equal to 10 μm and less than or equal to 100 μm. The arbitrary width is determined in consideration of the thickness of the conductor layer 20, the size of the microcrystals 21 contained in the conductor layer 20, and the like.
[0030] For example, the specific range may be a range where one conductor layer 20 is sandwiched between the upper and lower insulating layers 10. The specific range may be specified at multiple locations in the photograph. As a specific area, as long as the area is within 100 μm 2 Above and 10000μm 2 The following range is sufficient.
[0031] As described above, in the present embodiment, the interface conductivity of the conductor layer 20 can be improved by making the irregularities of the contour 20 a of the conductor layer 20 smaller.
[0032] In this embodiment, the sintered body constituting the conductor layer 20 includes nano-sized silica particles 22 (see Figure 3 ), the silicon dioxide particles 22 may be located on the surface of the microcrystals 21. In other words, in the wiring substrate 1, silicon dioxide may be present on the surface of the conductor layer 20 in a particle state.
[0033] Here, "the surface of the conductor layer 20" refers to the vicinity of the interface between the insulating layer 10 and the conductor layer 20 when the conductor layer 20 is formed on the surface of the insulating layer 10. The "visiting the interface" includes a small width range from the surface of the conductor layer 20 to the inside of the conductor layer 20. The "small width" is, for example, a range from the surface of the conductor layer 20 to within 1 μm.
[0034] When the silica particles 22 are present on the surface of the conductive layer 20, the conductive layer 20 is in a state where there are no voids partially within 1 μm from the silica particles 22 and within 1 μm from the surface of the conductive layer 20. In this case, the voids refer to spaces having a size greater than or equal to the maximum diameter of the silica particles 22.
[0035] It is considered that the reason why the conductor layer 20 has a dense region around the silica particles 22 as described above is that, as described later, the silica particles 22 exist at the interface between the conductor layer 20 and the insulating layer 10, thereby reducing the diffusion of components from the insulating layer 10 into the copper powder and controlling the sintering behavior of the copper powder, resulting in slow sintering.
[0036] The silica particles 22 are present near the interface between the conductor layer 20 and the insulating layer 10, thereby partially reducing the diffusion of the glass component of the insulating layer 10 from the glass ceramic. Thus, during firing, the surface of the insulating layer 10 can maintain a gentle shape, and thus the surface shape of the conductor layer 20 can be kept flat. The silica particles 22 are less likely to react excessively with the insulating layer 10.
[0037] The conductor layer 20 has a microstructure formed of fine copper crystallites 21. In this case, the plurality of crystallites 21 include crystallites forming a polygonal shape including linear edges, and are connected with the edges as grain boundaries. The longest diameter of the crystallites 21 is preferably greater than 1 μm and less than 10 μm. The plurality of crystallites 21 preferably have more than 70% of the crystallites having more than 2 edges in terms of number ratio.
[0038] In this embodiment, the silica particles 22 are present on the surface of the conductor layer 20, so that the adhesion between the conductor layer 20 and the insulating layer 10 can be improved. It should be noted that the silica particles 22 may be present on the entire surface of the conductor layer 20 facing the insulating layer 10, or may be present only on a portion of the surface of the conductor layer 20. When a plurality of silica particles 22 are present on the surface of the conductor layer 20, these silica particles 22 may be isolated and exist as mutually independent particles.
[0039] The presence of silica particles 22 on the surface of the conductor layer 20 or near the interface between the insulating layer 10 and the conductor layer 20 may improve the adhesion between the insulating layer 10 and the conductor layer 20 because the shrinkage behavior of the metal material (e.g., copper) used for the conductor layer 20 during sintering is similar to that of the silica particles 22.
[0040] The main reason why the shrinkage behavior of the metal material used for the conductor layer 20 during firing is close to the shrinkage behavior of the silica particles 22 is that the size of the silica particles 22 is very small (nano size).
[0041] If the silica particles 22 larger than nanometer size are used, there is a wide particle size distribution due to the size and an increase in heat capacity due to the size. And these factors become the main factors for changing the sintering behavior and adhesion.
[0042] When glass powder of a composite oxide is used instead of the nano-sized silica particles 22 , the glass powder contains a plurality of components, and therefore the temperature range in which the glass powder becomes molten is wider than that of the nano-sized silica particles 22 .
[0043] For example, in glass powder, the melting temperature sometimes starts from a lower temperature than that of nano-sized silica particles 22. In addition, glass powder often has a wide particle size distribution. When glass powder having these properties is used, the glass powder is likely to cause agglomeration or migration during sintering in the printed pattern as the conductor layer 20.
[0044] As a result, when forming the conductor layer 20 , the metal particles are likely to undergo grain growth, and voids are likely to be generated in the conductor layer 20 . This is because the glass powder is likely to diffuse from the portion where the pattern is printed to the region to be the insulating layer 10 .
[0045] On the other hand, when nano-sized silica particles 22 are used, they have a single composition and therefore have a narrower temperature range for molten state than glass powder. As a result, the conductor layer 20 becomes denser and a gentle concave portion is easily formed along the surface of the insulating layer 10 .
[0046] The particle size of the silica particles 22 of the embodiment is preferably 1 nm to 50 nm. Here, the particle size refers to the diameter. The diameter refers to the maximum diameter obtained when observing the silica particles 22. Among them, the average particle size of the silica particles 22 is preferably 20 nm. Furthermore, the ratio of the cumulative amount of the silica particles 22 with a lower limit of 10 nm and an upper limit of 30 nm is preferably 70% or more.
[0047] In this embodiment, the area ratio of the silica particles 22 in the conductor layer 20 may be 0.002% to 0.067%. This can improve the interface conductivity of the conductor layer 20. The method for calculating the area ratio of the silica particles 22 in the conductor layer 20 will be described later.
[0048] In the present embodiment, the content of the silica particles 22 in the conductor layer 20 may be 0.099 wt% to 2.912 wt%. This can improve the interface conductivity of the conductor layer 20. Here, the content of the silica particles 22 refers to the ratio obtained by dividing the amount of the silica particles 22 added by the total amount of the copper powder and the silica particles 22.
[0049] In the present embodiment, the crystallites 21 are mainly composed of copper, and the content of copper in the conductor layer 20 may be 80 wt % to 99 wt %. This can further improve the interface conductivity of the conductor layer 20 .
[0050] In addition, in this embodiment, if Figure 2 As shown, the crystallites 21 may be polygonal. This can reduce the decrease in interface conductivity in a high frequency region (eg, 1 GHz to 49 GHz), and thus improve the interface conductivity of the conductor layer 20 in the high frequency region.
[0051] Example
[0052] It should be noted that, in the embodiments described below, a wiring board having an insulating layer made of glass ceramic and a conductor layer mainly composed of copper is shown, and the present invention is not limited to the following embodiments.
[0053] <Example 1>
[0054] First, as a material for the insulating layer, a mixture of 40 wt% of aluminum oxide particles and 60 wt% of borosilicate glass was prepared. This mixture was a glass ceramic raw material with a firing temperature of 900°C to 1000°C.
[0055] In addition, as an organic binder, 20 parts by mass of isobutyl methacrylate resin and dibutyl phthalate were used with respect to 100 parts by mass of the glass ceramic raw material, and a green sheet having a thickness of 100 μm was prepared by doctor blade molding.
[0056] In addition, as raw materials for the conductor layer, copper powder (purity 99.9wt%) with an average particle size of 2μm and silicon dioxide particles with an average particle size of 20nm were prepared. The cumulative amount of silicon dioxide particles with a lower limit of 10nm and an upper limit of 30nm was 70% or more. The amount of silicon dioxide particles added was 0.1 parts by mass relative to 100 parts by mass of copper powder.
[0057] In addition, as an organic binder, a mixed solvent of isobutyl methacrylate resin, butyl carbitol acetate and dibutyl phthalate was used. Furthermore, isobutyl methacrylate resin was added in a ratio of 5 parts by mass to 100 parts by mass of copper powder, and a mixed solvent of butyl carbitol acetate and dibutyl phthalate was added to prepare a conductor paste containing copper powder and silica particles.
[0058] Then, the conductor paste was printed on both surfaces of the prepared green sheet in a predetermined area and fired. The firing was performed in a reducing environment using a hydrogen-nitrogen mixed gas at a maximum temperature of 930° C. and a holding time of 2 hours. Multiple green sheets were stacked to a thickness of 500 μm. Thus, the wiring substrate 1 of Example 1 was obtained.
[0059] <Examples 2 to 7>
[0060] Wiring boards 1 of Examples 2 to 7 were obtained by the same method and conditions as in Example 1, except for the amount of silica particles added in the preparation step of the conductor paste.
[0061] In Examples 2 to 7, the amounts of the conductive pastes were 0.3, 0.5, 1, 1.5, 2, and 3 parts by mass, respectively, relative to 100 parts by mass of the copper powder.
[0062] <Example 8>
[0063] The wiring board 1 of Example 8 was obtained by the same method and conditions as in Example 1 except for the preparation process of the conductor paste. It should be noted that in Example 8, copper powder (purity 99.9 (wt%)) with an average particle size of 2 μm and borosilicate glass powder with an average particle size of 2 μm were prepared as raw materials for the conductor layer. The amount of glass powder added was 6 parts by mass relative to 100 parts by mass of the copper powder.
[0064] In addition, as an organic binder, a mixed solvent of isobutyl methacrylate resin, butyl carbitol acetate and dibutyl phthalate was used. The isobutyl methacrylate resin was added at a ratio of 5 parts by mass to 100 parts by mass of the copper powder, and the mixed solvent of butyl carbitol acetate and dibutyl phthalate was further added to prepare a conductor paste containing copper powder and glass powder.
[0065] <Various Reviews>
[0066] Then, the wiring substrates 1 of Examples 1 to 8 obtained above were cut, the cut surfaces were mirror-polished, and the cross sections were observed with a scanning electron microscope. Figure 3 This is a diagram showing a SEM observation photograph of the conductor layer 20 of Example 1.
[0067] like Figure 3 As shown, in this embodiment, silicon dioxide particles 22 are observed between adjacent copper crystallites 21 (i.e., on the surface of the crystallites 21). In all samples, the volume ratio of the metal (copper) contained in the conductor layer 20 of the manufactured wiring substrate 1 was 90% or more and 98% or less, except for the voids.
[0068] Furthermore, using the SEM observation photographs obtained above, the ratio L1 / L0 of the length L1 of the outline 20 a of the conductor layer 20 in each of Examples 1 to 8 to the straight line length L0 in the planar direction was measured.
[0069] Specifically, first, for the conductor layer 20 captured in the cross-sectional photograph, point A and point B are marked at both ends of a contour 20a, and a straight line is drawn between point A and point B, and the length of the straight line is defined as L0. Then, the length of the contour 20a from point A to point B is calculated using an image processing device, and the length is defined as L1. Finally, L1 / L0 is calculated as the ratio of the two lengths.
[0070] In addition, the area ratio of the silica particles 22 in Examples 1 to 8 was measured using the SEM observation photographs obtained above. Specifically, first, for the conductor layer 20 photographed in the cross-sectional photograph, a plurality of locations were specified for a square range with a length of 1 / 10 to 1 / 2 of the thickness thereof. For example, 8 to 10 locations were specified for the square range in a manner that they were continuously arranged in the direction in which the conductor layer 20 extended (in the plane direction).
[0071] Then, the area of the metal portion (corresponding to the crystallite 21) in the region divided by the square is defined as A0. Figure 3 The area of the black portion (corresponding to the silica particles 22 ) is represented by A1 .
[0072] The area ratio A1 / A0 of the two is taken as the area ratio of the silica particles 22 in one square region. Finally, the average of the area ratios of the silica particles 22 in a plurality of square regions is taken as the area ratio of the silica particles 22 of the sample.
[0073] In addition, the interface conductivity of the wiring substrates 1 of Examples 1 to 8 obtained above was measured. The interface conductivity was measured by the dielectric cylindrical resonator method described below. In addition, as the sample for measurement, a sample with a diameter of 50 mm and a conductor layer 20 formed on almost the entire surface of both surfaces was used.
[0074] The method for measuring the interface conductivity using the dielectric cylinder resonator method is a method in which an insulating layer having the above-mentioned conductor formed therein is mounted in a predetermined relationship on both end faces or one end face of a dielectric cylinder made of a dielectric material having known relative dielectric constant and dielectric loss to form a dielectric resonator, thereby measuring the conductivity at the interface between the conductor and the insulating layer, that is, the conductor interface.
[0075] The principle of this measurement method is that when an electromagnetic field resonator is constructed by arranging two end faces of a dielectric cylinder having a specified size ratio (height h / diameter d) in parallel and clamping a sufficiently large conductor plate (usually a conductor plate having a diameter D about three times the diameter d of the dielectric cylinder) to a degree that the edge effect can be ignored, the high-frequency current flowing through the conductor plate in the TEomn resonance mode (hereinafter referred to as the TEomn mode) is distributed only on the short-circuit surface, that is, the opposing surfaces of the dielectric and the conductor.
[0076] In a dielectric resonator, the high-frequency current flowing through the conductor in the TEomn mode (m=1, 2, 3..., n=1, 2, 3, ...) is distributed only at the interface of the dielectric substrate where the conductor contacts the dielectric cylinder, and the interface conductivity can be calculated from the measured resonance frequency f0 of the TEomn mode (m=1, 2, 3..., n=1, 2, 3, ...) and the no-load Q and Qu. The interface conductivity is measured under the condition of a frequency of 10 GHz.
[0077] Furthermore, the presence or absence of conductor peeling in the wiring boards 1 of Examples 1 to 8 obtained above was evaluated. As evaluation samples, samples in which the insulating layer 10 was overlapped on both sides of the conductive layer 20 with a side of 10 mm to 50 mm were used.
[0078] In addition, for the evaluation of conductor peeling, first, the evaluation sample was cut at a position of about 1 / 2 of the length in one direction, and both interfaces of the insulating layer 10 and the conductor layer 20 in the cross section were observed. Then, when peeling was observed at one place, it was judged as "peeling was observed", and when no peeling was observed at all interfaces, it was judged as "no peeling".
[0079] It should be noted that in the above determination, the state of "exfoliation is present" is when the length of the region where the insulating layer 10 and the conductive layer 20 are separated by 0.1 mm or more is 1 mm or more.
[0080] Here, for Examples 1 to 8, the addition amounts of silica particles and glass powder in the conductor layer 20, the value of L1 / L0 in the conductor layer 20, the area ratio of silica particles in the conductor layer 20, the measurement results of the interface conductivity under the condition of a frequency of 10 GHz, and the evaluation results of the presence or absence of conductor peeling are shown in Table 1. It should be noted that the measurement results of the interface conductivity under the condition of a frequency of 10 GHz are relative values when the interface conductivity in direct current is 100%.
[0081] Table 1
[0082]
[0083] As shown in Table 1, it is found that the interface conductivity of the conductor layer 20 can be improved by setting the value of L1 / L0 in the conductor layer 20 to a range of 1.04 to 1.40. It is also found that the interface conductivity of the conductor layer 20 can be further improved by setting the value of L1 / L0 in the conductor layer 20 to a range of 1.04 to 1.18.
[0084] In addition, it is found that by setting the value of L1 / L0 in the conductor layer 20 to a range of 1.04 to 1.14, the interface conductivity of the conductor layer 20 can be further improved. In addition, it is found that by setting the value of L1 / L0 in the conductor layer 20 to a range of 1.04 to 1.11, the interface conductivity of the conductor layer 20 can be further improved.
[0085] It should be noted that, although not shown in Table 1, in a wiring substrate (so-called printed circuit board) having an insulating layer made of a resin such as an epoxy resin and a conductive layer made of copper foil, since the adhesion between the resin (insulating layer) and the copper foil (conductive layer) is low, an anchoring effect is produced by increasing the unevenness of the contour of the conductive layer, thereby ultimately ensuring adhesion.
[0086] Therefore, in this printed circuit board, the value of L1 / L0 in the conductor layer is greater than or equal to 2. In addition, in this printed circuit board, since the contour of the conductor layer is greatly uneven, the interface conductivity of the conductor layer is reduced.
[0087] In addition, if the results of Table 1 are expressed in other expressions, it can be seen that according to the samples (Examples 1 to 7) made using the conductor paste in which the addition amount of the silica particles 22 is 0.1 to 3 parts by mass relative to 100 parts by mass of the copper powder, the interface conductivity of the conductor layer 20 can be improved. In addition, it can be seen that according to the samples (Examples 2 to 7) made using the conductor paste in which the addition amount of the silica particles 22 is 0.3 to 3 parts by mass, the conductor peeling of the conductor layer 20 can be reduced.
[0088] In addition, according to the samples made using the conductor paste in which the addition amount of silica particles 22 is 0.3 to 2 parts by mass relative to 100 parts by mass of copper powder (Examples 2 to 6), the interface conductivity of the conductor layer 20 can be further improved and the conductor peeling of the conductor layer 20 can be reduced.
[0089] In addition, according to the samples made using the conductor paste in which the addition amount of silica particles 22 is 0.3 to 1.5 parts by mass relative to 100 parts by mass of copper powder (Examples 2 to 5), the interface conductivity of the conductor layer 20 can be further improved and the conductor peeling of the conductor layer 20 can be reduced.
[0090] In addition, as shown in Table 1, it can be seen that by setting the area ratio of the silica particles 22 in the conductor layer 20 to the range of 0.002% to 0.067%, the interface conductivity of the conductor layer 20 can be improved. In addition, it can be seen that by setting the area ratio of the silica particles 22 in the conductor layer 20 to the range of 0.005% to 0.067%, the conductor peeling of the conductor layer 20 can be reduced.
[0091] Furthermore, it is found that by setting the area ratio of the silica particles 22 in the conductor layer 20 to a range of 0.005% to 0.042%, the interface conductivity of the conductor layer 20 can be further improved, and conductor peeling of the conductor layer 20 can be reduced.
[0092] Furthermore, it is found that by setting the area ratio of the silica particles 22 in the conductor layer 20 to a range of 0.005% to 0.033%, the interface conductivity of the conductor layer 20 can be further improved, and conductor peeling of the conductor layer 20 can be reduced.
[0093] The above is a description of the embodiment of the present invention, but the present invention is not limited to the above embodiment, and various changes can be made without departing from the scope of the main purpose. For example, in the above embodiment, an example of adding fine powder of silicon dioxide particles to the conductive paste as the raw material of the conductor layer 20 is shown, but the present invention is not limited to this example.
[0094] For example, ceramic fine powder other than silicon dioxide (for example, aluminum oxide fine powder, etc.) may be added to the conductive paste. In this way, the same effects as those of the above-mentioned embodiment can be obtained.
[0095] Those skilled in the art can easily derive more effects and other aspects. Therefore, the broader aspects of the present invention are not limited to the specific details and representative embodiments shown and described above. Therefore, various changes can be made without departing from the spirit or scope of the concept of the overall invention defined by the attached claims and their equivalents.
[0096] Description of Reference Numerals
[0097] 1: Wiring substrate.
[0098] 10: Insulation layer.
[0099] 20: Conductor layer.
[0100] 20a: Outline.
[0101] 21: Microcrystalline.
[0102] 22: Silica particles.
Claims
1. A wiring substrate, wherein: The wiring substrate comprises: an insulating layer, the insulating layer being made of ceramic; and a conductor layer, the conductor layer extending in a planar direction inside the insulating layer. The conductor layer is composed of a sintered body of a plurality of microcrystals having metal as a main component. When a specific range of the conductor layer is designated in a cross-sectional view, and the length of a straight line in the plane direction is defined as L0 and the length of the outline of the conductor layer is defined as L1, L1 / L0 is in the range of 1.04 to 1.
40.
2. The wiring substrate according to claim 1, wherein: The sintered body contains silicon dioxide particles with a diameter of 1 nm to 50 nm. The silicon dioxide particles are located on the surface of the crystallites.
3. The wiring substrate according to claim 2, wherein: The area ratio of the silicon dioxide particles in the conductive layer is 0.002% to 0.067%.
4. The wiring substrate according to claim 2 or 3, wherein: The content of the silicon dioxide particles in the conductor layer is 0.099 wt % to 2.912 wt %.
5. The wiring substrate according to any one of claims 1 to 4, wherein: The microcrystals are mainly composed of copper. The content of copper in the conductor layer is 80 wt % to 99 wt %.
6. The wiring substrate according to any one of claims 1 to 5, wherein: The crystallites are polygonal in shape.