By applying a waterproof and antibacterial coating on the down jacket fabric, and using modified multi-wall carbon nanotubes and water-absorbing and expansion agent components, the problem of insufficient waterproof and windproof performance of down jackets is solved, achieving higher waterproof, warmth and antibacterial effects.

CN118947983AInactive Publication Date: 2024-11-15DANDONG HAIHEGU GARMENT CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202411089946.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing down jackets are not capable of waterproofing and windproofing, especially when exposed to water, which can easily absorb water and become heavier, affecting the comfort and warmth of wearing.

Method used

The inner and outer lining fabrics are coated with waterproof and antibacterial coating. The coating consists of modified multi-wall carbon nanotubes, polyacrylonitrile fibers, water-absorbing expansion agent and antibacterial agent. The pores are expanded in the pores of the porous skeleton material through the water-absorbing expansion agent to close the pores. , carbon nanotubes improve hydrophobicity and wind resistance.

Benefits of technology

It significantly improves the waterproof, warm and antibacterial properties of down jackets, enhances the waterproof performance and wind resistance of the fabric, and enhances the overall use value and application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004986245670000141
    Figure BDA0004986245670000141
  • Figure BDA0004986245670000151
    Figure BDA0004986245670000151
Patent Text Reader

Abstract

The invention discloses an outdoor water-repellent wind-resistant warm-keeping down jacket, the down jacket is formed by wrapping white duck down with an inner lining fabric and an outer lining fabric, the inner surface of the inner lining fabric and the inner surface of the outer lining fabric are both coated with waterproof antibacterial coatings, and the inner lining fabric and the outer lining fabric are both formed by weaving polyester or nylon yarns; the waterproof antibacterial coating is prepared from the following raw materials in parts by weight: 5-10 parts of modified multi-walled carbon nanotubes, 30-50 parts of polyacrylonitrile fibers, 1-5 parts of a cross-linking agent, 30-50 parts of deionized water, 15-20 parts of a porous framework material and 3-8 parts of a water absorption expanding agent filled in pores of the porous framework material. The inner surfaces of the inner lining fabric and the outer lining fabric are coated with the waterproof and antibacterial coatings, the water absorption expanding agent filled in the pores of the porous framework material on the waterproof and antibacterial coatings absorbs water and expands after meeting water, so that the pores in the coatings are closed to achieve the waterproof effect, and meanwhile, the antibacterial agent is added into the water absorption expanding agent to obtain antibacterial water-absorbent resin, so that the antibacterial and antibacterial effects are achieved. Certain antibacterial and bacteriostatic effects can be achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of down jackets, in particular to an outdoor water-repellent, wind-resistant and warm down jacket. Background Art

[0002] A down jacket is a top filled with down. It has a large and round shape. Generally, duck down accounts for more than half of the down jacket, and it can be mixed with some small feathers. The duck down is cleaned, sterilized at high temperature, and then filled into clothes to make a down jacket. Down jackets have the best warmth retention properties and are mostly worn by people in cold areas. They are also commonly used by polar expedition personnel.

[0003] However, in order to achieve its waterproof effect, the existing down jacket fabric adopts a single waterproof layer during use, but the waterproof effect of the single waterproof layer can no longer meet the use in real life, resulting in a decrease in the waterproof effect of the down jacket fabric.

[0004] At present, the patent with announcement number CN202603658U discloses a down jacket with sleeves, which belongs to the technical field of technical improvement of down jackets. It includes a sleeve with a cuff section, and the sleeve is fixedly provided at the connection between the sleeve and the cuff section. The sleeve opening extends along the outer side of the sleeve toward the upper end of the sleeve to 1 / 3 to 1 / 2 of the length of the sleeve. At the same time, the sleeve opening and the sleeve are connected by a detachable structure.

[0005] The above technical solution has the following defects: the prepared down jacket does not have the function of water-repellent and windproof, and once it encounters water, the down jacket easily absorbs water and becomes heavy, while affecting the comfort of wearing. Therefore, the current down jacket still needs to be improved in meeting the basic needs of warmth. Summary of the invention

[0006] In order to solve the problems mentioned in the above background technology, the present invention provides an outdoor water-repellent, wind-resistant and warm down jacket.

[0007] In order to achieve the above object, the present invention adopts the following technical solutions:

[0008] An outdoor water-repellent, wind-resistant and warm down jacket, the down jacket comprising inner and outer lining fabrics wrapped with white duck down, the inner surfaces of the inner lining fabric and the outer lining fabric are both coated with a waterproof and antibacterial coating, and the inner lining fabric and the outer lining fabric are both woven from polyester or nylon yarns;

[0009] The waterproof and antibacterial coating is made of the following raw materials in parts by weight: 5-10 parts of modified multi-walled carbon nanotubes, 30-50 parts of polyacrylonitrile fibers, 1-5 parts of a crosslinking agent, 30-50 parts of deionized water, 15-20 parts of a porous skeleton material, and 3-8 parts of a water-absorbing swelling agent filled in the pores of the porous skeleton material.

[0010] The particle size of polyacrylonitrile fiber is 7-9mm and the molecular weight is 100,000-120,000.

[0011] Preferably, the porous framework material is made of waterborne polyurethane material, and the median pore diameter of the waterborne polyurethane material is 80-380 nm.

[0012] Preferably, the water-absorbing expansion agent is composed of α-type hemihydrate gypsum, starch-grafted acrylate and antibacterial agent in a mass ratio of 2-5:3-7:1.

[0013] The starch grafted acrylate can be ethyl acrylate, butyl acrylate, 2-hydroxyethyl acrylate, and the grafting rate is between 40-50% by mass.

[0014] Preferably, the antibacterial agent is a silver ion antibacterial agent, and the silver ion antibacterial agent is selected from at least one of zirconium phosphate-supported silver, glass-supported silver, titanium dioxide-supported silver, silicate-supported silver, zeolite-supported silver, and silver phosphate.

[0015] Preferably, the cross-linking agent is at least one of ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, polyethyleneimine and polyethyleneamine.

[0016] Preferably, the method for preparing the modified multi-walled carbon nanotubes specifically comprises the following steps:

[0017] S1, mixing multi-walled carbon nanotubes with a sulfuric acid aqueous solution, stirring evenly, standing and soaking for 25-30 hours, heating, condensing and refluxing, and centrifuging to obtain carboxylated carbon nanotubes;

[0018] S2, the carboxylated carbon nanotubes and thionyl chloride are stirred and refluxed, distilled at 85-90° C. for 3-4 hours, and dried to obtain chlorinated carbon nanotubes;

[0019] S3, dissolving the chlorinated carbon nanotubes and methyl methacrylate in N-methylpyrrolidone, controlling the temperature and reacting for a period of time, then distilling, and then washing and drying to obtain modified multi-walled carbon nanotubes.

[0020] Preferably, the multi-walled carbon nanotubes have a diameter of 6-12 nm, an inner diameter of 3-5 nm, a length of 1-3 μm, and a specific surface area of ​​>350 m 2 / g.

[0021] Preferably, the mass concentration of the aqueous sulfuric acid solution in S1 is 88-90wt%, and the mass ratio of the multi-walled carbon nanotubes to the aqueous sulfuric acid solution is 1:50-60.

[0022] Preferably, the carboxylated carbon nanotubes and thionyl chloride in S2 are stirred and refluxed at 65-70° C. for 20-24 h.

[0023] Preferably, the reaction conditions in S3 are reaction at 70-80° C. for 20-25 h, and then distillation at 80-85° C. for 3-5 h.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] 1. The present invention coats the inner surface of the inner and outer lining fabrics with a waterproof and antibacterial coating, wherein the water-absorbing and swelling agent filled in the pores of the porous skeleton material on the waterproof and antibacterial coating absorbs water and swells when it comes into contact with water, thereby sealing the pores in the coating to achieve a waterproof effect. At the same time, an antibacterial agent is added to the water-absorbing and swelling agent to obtain an antibacterial water-absorbing resin, which can have a certain antibacterial and antimicrobial effect.

[0026] 2. In the present invention, since carbon nanotubes can be combined with polyacrylonitrile fibers, polyacrylonitrile fibers are endowed with certain waterproof properties. Carbon nanotubes themselves have a relatively low surface energy. When they are combined with polyacrylonitrile fibers, the surface energy of the fiber membrane can be reduced, thereby improving its hydrophobicity. This hydrophobicity helps to reduce the adsorption and penetration of water molecules on the fiber surface, thereby enhancing the waterproof properties of the overall fabric. At the same time, due to the small size and nanostructure of carbon nanotubes, they can form a dense protective layer on the fiber surface to prevent the penetration of water molecules. In addition, the high aspect ratio and strong mechanical properties of carbon nanotubes also help to improve the strength and durability of the fiber membrane.

[0027] 3. The present invention modifies multi-walled carbon nanotubes by acidification and chlorination so that their surfaces have abundant functional groups, which can form good chemical or physical interactions with polymers. This interfacial interaction can increase the adhesion between the carbon nanotubes and the matrix, effectively transfer stress, and prevent local stress concentration, thereby improving the wind resistance of the overall material. The specific specific surface area of ​​the modified multi-walled carbon nanotubes of the present invention enables them to have good dispersibility in the system of the present invention, and at the same time form a barrier effect, which can inhibit the spread of cold air in cold winters and absorb heat, thereby improving the overall wind resistance and warmth retention effect of the down jacket, and has high social use value and application prospects. DETAILED DESCRIPTION

[0028] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] Unless otherwise specified, the raw materials used in the present invention are all conventional products purchased from the market. Among them, α-hemihydrate gypsum was purchased from Hebei Mingzhe Mineral Products Co., Ltd., model number MZ-0025;

[0030] Preparation Example 1

[0031] The preparation method of the modified multi-walled carbon nanotubes specifically comprises the following steps:

[0032] S1, 5g of multi-walled carbon nanotubes were mixed with 250g of 88wt% sulfuric acid aqueous solution, stirred evenly, allowed to stand for 25h, heated to condense and reflux, and centrifuged to obtain carboxylated carbon nanotubes;

[0033] S2, the carboxylated carbon nanotubes and 10 g of thionyl chloride were stirred and refluxed at 68° C. for 24 h, distilled at 90° C. for 4 h, and dried to obtain chlorinated carbon nanotubes;

[0034] S3, dissolving the chlorinated carbon nanotubes and 25g methyl methacrylate in 100g N-methylpyrrolidone, controlling the temperature to react at 80°C for 20h, then distilling at 85°C for 3-5h, and then washing and drying to obtain modified multi-walled carbon nanotubes;

[0035] The multi-walled carbon nanotubes have a diameter of 8 nm, an inner diameter of 3 nm, a length of 1 μm, and a specific surface area of ​​360 m 2 / g.

[0036] Preparation Example 2

[0037] The preparation method of the modified multi-walled carbon nanotubes specifically comprises the following steps:

[0038] S1, 10g of multi-walled carbon nanotubes were mixed with 500g of 90wt% sulfuric acid aqueous solution, stirred evenly, allowed to stand for 28h, heated to condense and reflux, and centrifuged to obtain carboxylated carbon nanotubes;

[0039] S2, the carboxylated carbon nanotubes and 25 g of thionyl chloride were stirred and refluxed at 70° C. for 24 h, distilled at 90° C. for 3.5 h, and dried to obtain chlorinated carbon nanotubes;

[0040] S3, dissolving the chlorinated carbon nanotubes and 55g methyl methacrylate in 220g N-methylpyrrolidone, reacting at 78°C for 24h, distilling at 85°C for 4h, washing with water and drying to obtain modified multi-walled carbon nanotubes;

[0041] The multi-walled carbon nanotubes have a diameter of 12 nm, an inner diameter of 5 nm, a length of 3 μm, and a specific surface area of ​​450 m 2 / g.

[0042] Preparation Example 3

[0043] The preparation method of the modified multi-walled carbon nanotubes specifically comprises the following steps:

[0044] S1, 15g of multi-walled carbon nanotubes were mixed with 800g of 90wt% sulfuric acid aqueous solution, stirred evenly, allowed to stand for 30h, heated to condense and reflux, and centrifuged to obtain carboxylated carbon nanotubes;

[0045] S2, the carboxylated carbon nanotubes and 35 g of thionyl chloride are stirred and refluxed at 65-70° C. for 20-24 h, distilled at 85-90° C. for 3-4 h, and dried to obtain chlorinated carbon nanotubes;

[0046] S3, dissolving the chlorinated carbon nanotubes and 80g methyl methacrylate in 320g N-methylpyrrolidone, reacting at 80°C for 25h, distilling at 82°C for 5h, washing with water and drying to obtain modified multi-walled carbon nanotubes;

[0047] The multi-walled carbon nanotubes have a diameter of 10 nm, an inner diameter of 4 nm, a length of 2 μm, and a specific surface area of ​​380 m 2 / g.

[0048] Example 1

[0049] An outdoor water-repellent, wind-resistant and warm down jacket, the down jacket comprising inner and outer lining fabrics wrapped with white duck down, the inner surfaces of the inner lining fabric and the outer lining fabric are both coated with a waterproof and antibacterial coating, and the inner lining fabric and the outer lining fabric are both woven from polyester yarns;

[0050] The preparation method of the waterproof and antibacterial coating comprises the following steps:

[0051] Mix 20g of water-based polyurethane material with a pore median diameter of 150nm and 8g of water-absorbing expansion agent evenly, then add 40g of polyacrylonitrile fiber with a particle size of 9mm and a molecular weight of 110,000, 8g of modified multi-walled carbon nanotubes prepared in Preparation Example 1, 3g of diethylenetriamine and 45g of deionized water, heat to 98°C and stir thoroughly, and then cool to room temperature to obtain a waterproof surface coating.

[0052] The water-absorbing expansion agent is composed of α-type semi-hydrated gypsum, starch-grafted ethyl acrylate with a grafting rate of 40%, and titanium dioxide-supported silver antibacterial agent in a mass ratio of 2:3:1.

[0053] Example 2

[0054] An outdoor water-repellent, wind-resistant and warm down jacket, the down jacket comprising inner and outer lining fabrics wrapped with white duck down, the inner surfaces of the inner lining fabric and the outer lining fabric are both coated with a waterproof and antibacterial coating, and the inner lining fabric and the outer lining fabric are both woven from polyester yarns;

[0055] The preparation method of the waterproof and antibacterial coating comprises the following steps:

[0056] 18g of water-based polyurethane material with a pore median diameter of 150nm and 7g of water-absorbing expansion agent are mixed evenly, and then 45g of polyacrylonitrile fiber with a particle size of 9mm and a molecular weight of 110,000, 10g of modified multi-walled carbon nanotubes prepared in Preparation Example 1, 4g of triethylenetetramine and 40g of deionized water are added, heated to 98°C and stirred thoroughly, and the waterproof surface coating is obtained after cooling to room temperature.

[0057] The water-absorbing expansion agent is composed of α-type semi-hydrated gypsum, starch grafted acrylate with a grafting rate of 45% and silicate silver-loaded antibacterial agent in a mass ratio of 3:4:1.

[0058] Example 3

[0059] An outdoor water-repellent, wind-resistant and warm down jacket, the down jacket comprising inner and outer lining fabrics wrapped with white duck down, the inner surfaces of the inner lining fabric and the outer lining fabric are both coated with a waterproof and antibacterial coating, and the inner lining fabric and the outer lining fabric are both woven from polyester yarns;

[0060] The preparation method of the waterproof and antibacterial coating comprises the following steps:

[0061] 200g of water-based polyurethane material with a pore median diameter of 150nm is mixed evenly with 80g of a water-absorbing expansion agent, and then 400g of polyacrylonitrile fiber with a particle size of 9mm and a molecular weight of 110,000, 80g of modified multi-walled carbon nanotubes prepared in Preparation Example 1, 30g of diethylenetriamine and 450g of deionized water are added, heated to 98°C and stirred thoroughly, and the waterproof surface coating is obtained after cooling to room temperature.

[0062] The water-absorbing expansion agent is composed of α-type semi-hydrated gypsum, starch grafted acrylate with a grafting rate of 50%, and titanium dioxide-supported silver antibacterial agent in a mass ratio of 5:7:1.

[0063] Example 4

[0064] An outdoor water-repellent, wind-resistant and warm down jacket, the down jacket comprising inner and outer lining fabrics wrapped with white duck down, the inner surfaces of the inner lining fabric and the outer lining fabric are both coated with a waterproof and antibacterial coating, and the inner lining fabric and the outer lining fabric are both woven from polyester yarns;

[0065] The preparation method of the waterproof and antibacterial coating comprises the following steps:

[0066] Mix 20g of water-based polyurethane material with a pore median diameter of 150nm and 8g of water-absorbing expansion agent evenly, then add 40g of polyacrylonitrile fiber with a particle size of 9mm and a molecular weight of 110,000, 8g of modified multi-walled carbon nanotubes prepared in Preparation Example 2, 3g of polyethyleneimine and 45g of deionized water, heat to 98°C and stir thoroughly, and then cool to room temperature to obtain a waterproof surface coating.

[0067] The water-absorbing expansion agent is composed of α-type semi-hydrated gypsum, starch-grafted butyl acrylate with a grafting rate of 40%, and zeolite-supported silver antibacterial agent in a mass ratio of 2:5:1.

[0068] Example 5

[0069] An outdoor water-repellent, wind-resistant and warm down jacket, the down jacket comprising inner and outer lining fabrics wrapped with white duck down, the inner surfaces of the inner lining fabric and the outer lining fabric are both coated with a waterproof and antibacterial coating, and the inner lining fabric and the outer lining fabric are both woven from polyester yarns;

[0070] The preparation method of the waterproof and antibacterial coating comprises the following steps:

[0071] 18g of water-based polyurethane material with a pore median diameter of 150nm and 7g of water-absorbing expansion agent are mixed evenly, and then 45g of polyacrylonitrile fiber with a particle size of 9mm and a molecular weight of 110,000, 10g of modified multi-walled carbon nanotubes prepared in Preparation Example 2, 4g of polyethylene amine and 40g of deionized water are added, heated to 98°C and stirred thoroughly, and the waterproof surface coating is obtained after cooling to room temperature.

[0072] The water-absorbing expansion agent is composed of α-type semi-hydrated gypsum, starch-grafted butyl acrylate with a grafting rate of 45%, and zirconium phosphate silver-loaded antibacterial agent in a mass ratio of 3:5:1.

[0073] Example 6

[0074] An outdoor water-repellent, wind-resistant and warm down jacket, the down jacket comprising inner and outer lining fabrics wrapped with white duck down, the inner surfaces of the inner lining fabric and the outer lining fabric are both coated with a waterproof and antibacterial coating, and the inner lining fabric and the outer lining fabric are both woven from polyester yarns;

[0075] The preparation method of the waterproof and antibacterial coating comprises the following steps:

[0076] 200g of water-based polyurethane material with a pore median diameter of 150nm is evenly mixed with 80g of a water-absorbing expansion agent, and then 400g of polyacrylonitrile fiber with a particle size of 9mm and a molecular weight of 110,000, 80g of modified multi-walled carbon nanotubes prepared in Preparation Example 2, 30g of polyethyleneimine and 450g of deionized water are added, heated to 98°C and stirred thoroughly, and the waterproof surface coating is obtained after cooling to room temperature.

[0077] The water-absorbing expansion agent is composed of α-type semi-hydrated gypsum, starch-grafted butyl acrylate with a grafting rate of 50%, and titanium dioxide-supported silver antibacterial agent in a mass ratio of 3:7:1.

[0078] Example 7

[0079] An outdoor water-repellent, wind-resistant and warm down jacket, the down jacket comprising inner and outer lining fabrics wrapped with white duck down, the inner surfaces of the inner lining fabric and the outer lining fabric are both coated with a waterproof and antibacterial coating, and the inner lining fabric and the outer lining fabric are both woven from polyester yarns;

[0080] The preparation method of the waterproof and antibacterial coating comprises the following steps:

[0081] Mix 20g of water-based polyurethane material with a pore median diameter of 150nm and 8g of water-absorbing expansion agent evenly, then add 40g of polyacrylonitrile fiber with a particle size of 9mm and a molecular weight of 110,000, 8g of modified multi-walled carbon nanotubes prepared in Preparation Example 3, 3g of tetraethylenepentamine and 45g of deionized water, heat to 98°C and stir thoroughly, and then cool to room temperature to obtain a waterproof surface coating.

[0082] The water-absorbing expansion agent is composed of α-type semi-hydrated gypsum, starch-grafted 2-hydroxyethyl acrylate with a grafting rate of 40%, and titanium dioxide-supported silver antibacterial agent in a mass ratio of 2:4:1.

[0083] Example 8

[0084] An outdoor water-repellent, wind-resistant and warm down jacket, the down jacket comprising inner and outer lining fabrics wrapped with white duck down, the inner surfaces of the inner lining fabric and the outer lining fabric are both coated with a waterproof and antibacterial coating, and the inner lining fabric and the outer lining fabric are both woven from polyester yarns;

[0085] The preparation method of the waterproof and antibacterial coating comprises the following steps:

[0086] 18g of water-based polyurethane material with a pore median diameter of 150nm and 7g of water-absorbing expansion agent are mixed evenly, and then 45g of polyacrylonitrile fiber with a particle size of 9mm and a molecular weight of 110,000, 10g of modified multi-walled carbon nanotubes prepared in Preparation Example 3, 4g of triethylenetetramine and 40g of deionized water are added, heated to 98°C and stirred thoroughly, and the waterproof surface coating is obtained after cooling to room temperature.

[0087] The water-absorbing expansion agent is composed of α-type semi-hydrated gypsum, starch-grafted 2-hydroxyethyl acrylate with a grafting rate of 45%, and a silicate silver-loaded antibacterial agent in a mass ratio of 3:5:1.

[0088] Example 9

[0089] An outdoor water-repellent, wind-resistant and warm down jacket, the down jacket comprising inner and outer lining fabrics wrapped with white duck down, the inner surfaces of the inner lining fabric and the outer lining fabric are both coated with a waterproof and antibacterial coating, and the inner lining fabric and the outer lining fabric are both woven from polyester yarns;

[0090] The preparation method of the waterproof and antibacterial coating comprises the following steps:

[0091] 200g of water-based polyurethane material with a pore median diameter of 150nm is evenly mixed with 80g of a water-absorbing expansion agent, and then 400g of polyacrylonitrile fiber with a particle size of 9mm and a molecular weight of 110,000, 80g of modified multi-walled carbon nanotubes prepared in Preparation Example 3, 30g of tetraethylenepentamine and 450g of deionized water are added, heated to 98°C and stirred thoroughly, and the waterproof surface coating is obtained after cooling to room temperature.

[0092] The water-absorbing expansion agent is composed of α-type semi-hydrated gypsum, starch-grafted 2-hydroxyethyl acrylate with a grafting rate of 50%, and titanium dioxide-supported silver antibacterial agent in a mass ratio of 4:7:1.

[0093] Comparative Example 1

[0094] The invention discloses an outdoor water-repellent, wind-resistant and warm down jacket, which is composed of white duck down wrapped with inner and outer lining fabrics, and the inner and outer lining fabrics are both woven from polyester yarns.

[0095] Comparative Example 2

[0096] An outdoor water-repellent, wind-resistant and warm down jacket, the down jacket comprising inner and outer lining fabrics wrapped with white duck down, the inner surfaces of the inner lining fabric and the outer lining fabric are both coated with a waterproof and antibacterial coating, and the inner lining fabric and the outer lining fabric are both woven from polyester yarns;

[0097] The preparation method of the waterproof and antibacterial coating comprises the following steps:

[0098] 20g of waterborne polyurethane material with a pore median diameter of 150nm and 8g of water-absorbing swelling agent were mixed evenly, and then 40g of polyacrylonitrile fiber with a particle size of 9mm and a molecular weight of 110,000, 8g of modified multi-walled carbon nanotubes prepared in Preparation Example 1, 3g of diethylenetriamine and 45g of deionized water were added, heated to 98°C and stirred thoroughly, and the waterproof surface coating was obtained after cooling to room temperature. The modified multi-walled carbon nanotubes prepared in Preparation Example 1 were replaced with a carbon nanotube dispersion purchased from Beijing Tanyang Technology Co., Ltd., model CNT-W-5.

[0099] The water-absorbing expansion agent is composed of α-type semi-hydrated gypsum, starch-grafted ethyl acrylate with a grafting rate of 40%, and titanium dioxide-supported silver antibacterial agent in a mass ratio of 2:3:1.

[0100] Comparative Example 3

[0101] An outdoor water-repellent, wind-resistant and warm down jacket, the down jacket comprising inner and outer lining fabrics wrapped with white duck down, the inner surfaces of the inner lining fabric and the outer lining fabric are both coated with a waterproof and antibacterial coating, and the inner lining fabric and the outer lining fabric are both woven from polyester yarns;

[0102] The preparation method of the waterproof and antibacterial coating comprises the following steps:

[0103] Mix 20g of water-based polyurethane material with a pore median diameter of 150nm and 8g of water-absorbing expansion agent evenly, then add 40g of polyacrylonitrile fiber with a particle size of 9mm and a molecular weight of 110,000, 3g of diethylenetriamine and 45g of deionized water, heat to 98°C and stir thoroughly, and then cool to room temperature to obtain a waterproof surface coating.

[0104] The water-absorbing expansion agent is composed of α-type semi-hydrated gypsum, starch-grafted ethyl acrylate with a grafting rate of 40%, and titanium dioxide-supported silver antibacterial agent in a mass ratio of 2:3:1.

[0105] Comparative Example 4

[0106] An outdoor water-repellent, wind-resistant and warm down jacket, the down jacket comprising inner and outer lining fabrics wrapped with white duck down, the inner surfaces of the inner lining fabric and the outer lining fabric are both coated with a waterproof and antibacterial coating, and the inner lining fabric and the outer lining fabric are both woven from polyester yarns;

[0107] The preparation method of the waterproof and antibacterial coating comprises the following steps:

[0108] Heat 20g of water-based polyurethane material with a pore median diameter of 150nm, 40g of polyacrylonitrile fiber with a particle size of 9mm and a molecular weight of 110,000, 8g of modified multi-walled carbon nanotubes prepared in Preparation Example 1, 3g of diethylenetriamine and 45g of deionized water to 98°C and stir thoroughly, and then cool to room temperature to obtain a waterproof surface coating.

[0109] Comparative Example 5

[0110] An outdoor water-repellent, wind-resistant and warm down jacket, the down jacket comprising inner and outer lining fabrics wrapped with white duck down, the inner surfaces of the inner lining fabric and the outer lining fabric are both coated with a waterproof and antibacterial coating, and the inner lining fabric and the outer lining fabric are both woven from polyester yarns;

[0111] The preparation method of the waterproof and antibacterial coating comprises the following steps:

[0112] Mix 20g of water-based polyurethane material with a pore median diameter of 150nm and 8g of water-absorbing expansion agent evenly, then add 40g of polyacrylonitrile fiber with a particle size of 9mm and a molecular weight of 110,000, 8g of modified multi-walled carbon nanotubes prepared in Preparation Example 1, 3g of diethylenetriamine and 45g of deionized water, heat to 98°C and stir thoroughly, and then cool to room temperature to obtain a waterproof surface coating.

[0113] The water-absorbing expansion agent is composed of α-type semi-hydrated gypsum and starch-grafted ethyl acrylate with a grafting rate of 40% in a mass ratio of 2:3.

[0114] Comparative Example 6

[0115] An outdoor water-repellent, wind-resistant and warm down jacket, the down jacket comprising inner and outer lining fabrics wrapped with white duck down, the inner surfaces of the inner lining fabric and the outer lining fabric are both coated with a waterproof and antibacterial coating, and the inner lining fabric and the outer lining fabric are both woven from polyester yarns;

[0116] The preparation method of the waterproof and antibacterial coating comprises the following steps:

[0117] Mix 20g of water-based polyurethane material with a pore median diameter of 150nm and 8g of water-absorbing expansion agent evenly, then add 40g of polyacrylonitrile fiber with a particle size of 9mm and a molecular weight of 110,000, 8g of modified multi-walled carbon nanotubes prepared in Preparation Example 1, 3g of diethylenetriamine and 45g of deionized water, heat to 98°C and stir thoroughly, and then cool to room temperature to obtain a waterproof surface coating.

[0118] The water-absorbing and expanding agent is α-type hemihydrate gypsum.

[0119] The down jackets prepared in the above-mentioned Examples 1-9 and Comparative Examples 1-6 were respectively subjected to the following tests, and the results are shown in Table 1:

[0120] Waterproof performance: The reference standard number is AATCC 35-2000, and the standard name is Waterproof Test: Rain Test. 1-5 levels, 1 is completely wet.

[0121] Thermal insulation performance: refer to GB / T 11048-1989 Test method for thermal insulation performance of textiles (Grades I-V, with Grade I having the best thermal insulation performance).

[0122] Antibacterial properties: refer to "GB / T 20944-2007 Evaluation of antibacterial properties of textiles" (Grades I-V, with Grade I having the best antibacterial performance).

[0123] Table 1

[0124]

[0125]

[0126] In summary, the water-absorbing self-heating substance in the waterproof fabric used in the down jacket prepared by the present invention has a significant effect on the thermal insulation of the fabric. It can be seen from Examples 1-9 and Comparative Example 1 that the inner surfaces of the lining fabric and the outer lining fabric are coated with a waterproof and antibacterial coating, which can greatly improve the waterproof, warm and antibacterial properties of the down jacket.

[0127] In Comparative Example 2, since the modified multi-walled carbon nanotubes prepared in Preparation Example 1 were replaced with ordinary commercially available carbon nanotube dispersion, the waterproof, warm-keeping and antibacterial properties of the prepared down jacket were inferior to those of the embodiment, especially the waterproofness of the down jacket was greatly reduced;

[0128] In Comparative Example 3, since no multi-walled carbon nanotubes were added, the waterproof, warm and antibacterial properties of the prepared down jacket were greatly reduced, and the performance was much worse than the down jackets prepared in Examples 1-9;

[0129] In Comparative Example 4, no water-absorbing swelling agent was added, so that the waterproof, warm-keeping and antibacterial properties of the prepared down jacket were not as good as those of the down jackets prepared in Examples 1-9;

[0130] In comparative example 5, no antibacterial agent was added to the water-absorbing swelling agent during the preparation process, so that the antibacterial property of the prepared down jacket was greatly reduced;

[0131] In Comparative Example 6, the water-absorbing and expanding agent is only α-type hemihydrate gypsum, which reduces the comprehensive performance of the prepared down jacket, and its waterproof, warm-keeping and antibacterial properties are all reduced to a certain extent.

[0132] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. An outdoor water-repellent, wind-resistant and warm down jacket, characterized in that: The down jacket is composed of white duck down wrapped in inner and outer lining fabrics, the inner surfaces of the inner lining fabric and the outer lining fabric are coated with waterproof and antibacterial coatings, and the inner lining fabric and the outer lining fabric are woven from polyester or nylon yarns; The waterproof and antibacterial coating is made of the following raw materials in parts by weight: 5-10 parts of modified multi-walled carbon nanotubes, 30-50 parts of polyacrylonitrile fibers, 1-5 parts of a crosslinking agent, 30-50 parts of deionized water, 15-20 parts of a porous skeleton material, and 3-8 parts of a water-absorbing swelling agent filled in the pores of the porous skeleton material.

2. The outdoor water-repellent, wind-resistant and warm down jacket according to claim 1, characterized in that: The porous skeleton material is made of waterborne polyurethane material, and the median pore diameter of the waterborne polyurethane material is 80-380nm.

3. The outdoor water-repellent, wind-resistant and warm down jacket according to claim 1, characterized in that: The water-absorbing expansion agent is composed of α-type semi-hydrated gypsum, starch-grafted acrylate and antibacterial agent in a mass ratio of 2-5:3-7:

1.

4. The outdoor water-repellent, wind-resistant and warm down jacket according to claim 3, characterized in that: The antibacterial agent is a silver ion antibacterial agent, and the silver ion antibacterial agent is selected from at least one of zirconium phosphate-supported silver, glass-supported silver, titanium dioxide-supported silver, silicate-supported silver, zeolite-supported silver, and silver phosphate.

5. The outdoor water-repellent, wind-resistant and warm down jacket according to claim 1, characterized in that: The cross-linking agent is at least one of ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, polyethyleneimine and polyethyleneamine.

6. The outdoor water-repellent, wind-resistant and warm down jacket according to claim 1, characterized in that: The preparation method of the modified multi-walled carbon nanotubes specifically comprises the following steps: S1, mixing multi-walled carbon nanotubes with a sulfuric acid aqueous solution, stirring evenly, standing and soaking for 25-30 hours, heating, condensing and refluxing, and centrifuging to obtain carboxylated carbon nanotubes; S2, stirring and reflux the carboxylated carbon nanotubes and thionyl chloride, distilling at 85-90° C. for 3-4 hours, and drying to obtain chlorinated carbon nanotubes; S3, dissolving the chlorinated carbon nanotubes and methyl methacrylate in N-methylpyrrolidone, controlling the temperature and reacting for a period of time, then distilling, and then washing and drying to obtain modified multi-walled carbon nanotubes.

7. The outdoor water-repellent, wind-resistant and warm down jacket according to claim 6, characterized in that: The multi-walled carbon nanotubes have a diameter of 6-12 nm, an inner diameter of 3-5 nm, a length of 1-3 μm, and a specific surface area of ​​>350 m 2 / g.

8. The outdoor water-repellent, wind-resistant and warm down jacket according to claim 6, characterized in that: The mass concentration of the sulfuric acid aqueous solution in S1 is 88-90wt%, and the mass ratio of the multi-walled carbon nanotubes to the sulfuric acid aqueous solution is 1:50-60.

9. The outdoor water-repellent, wind-resistant and warm down jacket according to claim 6, characterized in that: The carboxylated carbon nanotubes in S2 are stirred and refluxed with thionyl chloride at 65-70° C. for 20-24 h.

10. The outdoor water-repellent, wind-resistant and warm down jacket according to claim 6, characterized in that: The reaction conditions in S3 are 70-80°C for 20-25h, followed by distillation at 80-85°C for 3-5h.

Citation Information

Patent Citations

  • Method for preparing macromolecule modified carbon nano-tube and application thereof

    CN101104512A

  • Super-hydrophobic conductive nano knitted fabric and preparation method thereof

    CN112301521A

  • Carbon nanotube modified polymethyl methacrylate with high thermal stability and preparation method thereof

    CN112409739A

  • Waterproof spraying liquid for down jacket and preparation method of waterproof spraying liquid

    CN113481736A

  • Waterproof coating of outdoor down jacket and production method of waterproof coating

    CN115029938A