Method for preparing nitrogen-hydrogen mixed gas through pressure leaching of ferronickel powder
Through the leaching reaction of nickel iron powder and sulfuric acid under pressurized conditions, nitrogen is used to prepare nitrogen and hydrogen mixed gas, which solves the problems of high cost and safety hazards in the prior art, and achieves efficient and safe production of nitrogen and hydrogen mixed gas , and the hydrogen content can be adjusted according to demand.
Patent Information
- Application Number
- CN202411080217.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-15
AI Technical Summary
The method of preparing nitrogen and hydrogen mixed gas in the prior art is costly and has safety risks, and it is not possible to effectively use nickel iron powder to directly prepare nitrogen and hydrogen mixed gas.
Using nickel iron powder and sulfuric acid to leach reaction under pressurized conditions, using nitrogen as a gas source and protective gas to control the pressure and temperature in the reactor, and after exhausting the gas through the autoclave, it will cool, dry and compress it to prepare a nitrogen and hydrogen mixed gas .
The preparation of nitrogen and hydrogen mixed gas with high comprehensive resource utilization rate, excellent safety performance, fast hydrogen generation rate and high purity has been achieved, and the hydrogen content can be adjusted according to the conditions to meet the needs of different uses.
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing nitrogen-hydrogen mixed gas by pressure leaching of nickel-iron powder, belonging to the field of material chemical industry. Background Art
[0002] Nitrogen-hydrogen mixed gas is widely used in the fields of electronic device production, semiconductor material processing, and high-purity metal material preparation. Conventional nitrogen-hydrogen mixed gas uses water electrolysis to produce hydrogen, which is then mixed with nitrogen to prepare a mixed gas (CN202210692161.6); ammonia decomposition to prepare nitrogen-hydrogen mixed gas is also a commonly used process technology (CN 92108638.5); in addition, some factories use liquid ammonia vaporization to obtain nitrogen-hydrogen mixed gas (CN 200710133638.2). Although there are many methods for preparing nitrogen-hydrogen mixed gas, there are also disadvantages such as high cost, the need for electrolysis to produce hydrogen, and great safety hazards.
[0003] Nickel iron powder is mainly produced by the smelting process of laterite nickel ore. There are currently two main smelting processes: one is that laterite nickel ore is dried in a drying kiln, roasted in a rotary kiln for pre-reduction, smelted in an electric furnace, and crushed to produce nickel iron powder; the other is that laterite nickel ore is mixed with limestone and pulverized coal, pressed into balls, and then calcined in a rotary kiln, quenched in water, ball milled, and magnetically separated to produce nickel iron powder. Nickel iron powder usually contains 8-15% nickel and can be used as a raw material for the production of nickel sulfate or for the production of nickel-containing stainless steel.
[0004] At present, there are many reports on the use of nickel-iron powder. For example, the patent with patent application number 201710553021.X provides a method for leaching low-nickel and high-iron alloy powder in nitric acid, which achieves a nickel-cobalt leaching rate of more than 98%. The patent with patent number 202211252938.3 provides a method for preparing nickel sulfate from nickel-iron alloy powder. The method uses concentrated sulfuric acid to mix with nickel-iron alloy powder, roast twice, grind, and leaching to obtain nickel sulfate solution and iron slag. The patent with patent number 202211252938.3 provides a method for preparing ferric chloride and nickel salt using nickel-iron alloy as raw material. The method prepares ferric chloride solution and nickel salt products through leaching, oxidation, extraction and other processes.
[0005] Although a variety of methods for producing nitrogen-hydrogen mixed gas have been reported, how to directly prepare nitrogen-hydrogen mixed gas using nickel-iron powder remains a technical challenge in the industry. Summary of the invention
[0006] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a method for preparing nitrogen-hydrogen mixed gas by pressure leaching of nickel-iron powder, which rapidly produces hydrogen through pressure leaching of nickel-iron powder with sulfuric acid, and simultaneously utilizes nitrogen as a gas source and protective gas to increase the pressure of the reaction system and improve the safety performance of the reaction, thereby finally preparing a nitrogen-hydrogen mixed gas.
[0007] In order to achieve the above object, the present invention adopts the following technical solutions:
[0008] The present invention provides a method for preparing nitrogen-hydrogen mixed gas by pressure leaching of nickel-iron powder, comprising the following steps:
[0009] (1) Using nitrogen as the gas source and protective gas, maintaining the pressure in the reactor at 0.15-0.6 MPa, and controlling the oxygen volume fraction in the reactor to be less than 0.1%;
[0010] (2) Pumping ore slurry containing nickel iron powder and sulfuric acid solution into the reactor in sequence, controlling the sulfuric acid concentration in the reactor to be 50-300 g / L and the reaction temperature to be 80-120° C.;
[0011] (3) The gas produced by the reaction is discharged from the pressure reducing valve at the top of the high-pressure reactor. The obtained gas is cooled, dehydrated, dried and compressed to obtain a nitrogen-hydrogen mixed gas.
[0012] According to the optimized solution, the mass concentration of the nickel-iron powder in the nickel-iron powder-containing slurry is 20-60%, and the rest is water.
[0013] Further preferably, the main components of the nickel-iron powder are as follows by mass percentage: iron is 70-90% and nickel is 10-30%.
[0014] Further preferably, the particle size of the nickel-iron powder is ≤220 μm.
[0015] In the optimized solution, the temperature of the gas cooling and dehydration is 0-10°C, and the gas residence time is 5-30 minutes.
[0016] In an optimized solution, the drying agent used in the drying is calcium oxide or anhydrous calcium chloride.
[0017] In an optimized solution, the volume fraction of hydrogen in the nitrogen-hydrogen mixed gas obtained by compression is 5% to 45%, and the rest is nitrogen.
[0018] Compared with the prior art, the beneficial technical effects of the present invention are:
[0019] (1) The method of the present invention directly prepares a nitrogen-hydrogen mixed gas by pressurizing nickel iron powder with sulfuric acid at high temperature and nitrogen pressurizing conditions, which has the characteristics of high comprehensive resource utilization, safety and high efficiency.
[0020] (2) The method of the present invention increases the reaction temperature and accelerates the hydrogen precipitation rate by a closed pressurized leaching method, and has the characteristics of fast hydrogen production rate, high purity, and high hydrogen content in the mixed gas.
[0021] (3) The method of the present invention can obtain nitrogen-hydrogen mixed gas with different hydrogen contents by adjusting the partial pressure of nitrogen in the autoclave, the reaction temperature and the sulfuric acid concentration, so as to meet the needs of different applications. DETAILED DESCRIPTION
[0022] The present invention will be further described below in conjunction with specific implementation modes.
[0023] Example 1
[0024] Take 10kg of nickel-iron powder containing 80% iron, 15% nickel, and the rest oxygen and carbon as raw material, the particle size of the nickel-iron powder is ≤220μm, use nitrogen as the booster gas, and use sulfuric acid solution and nickel-iron powder to pressurize and leach in a closed reactor to prepare nitrogen-hydrogen mixed gas. The specific operation steps are as follows:
[0025] (1) nitrogen was introduced into the reactor to exhaust the oxygen in the reactor, and the pressure in the reactor was maintained at 0.6 MPa, and the oxygen volume fraction in the reactor was controlled to be 0.1%;
[0026] (2) 10 kg of nickel iron powder was mixed with 20 L of water to prepare a slurry. The slurry was mechanically stirred and mixed evenly, and then the mixed slurry was pumped into the pressure reactor using a pressure pump. At the same time, 100 L of sulfuric acid solution with a sulfuric acid concentration of 300 g / L was slowly added using another pressure pump. The addition was completed within 60 min, and the reaction temperature was controlled to be 110-120 ° C. The pressure in the reactor did not exceed 0.6 MPa, and the reaction time was 8 h;
[0027] (3) The gas produced by the reaction is discharged from the pressure reducing valve on the top of the high-pressure reactor. The gas passes through a shell-and-tube heat exchanger and is cooled and dehydrated at 0°C. The residence time is 5 minutes. Most of the water in the mixed gas is condensed and removed. The mixed gas is then introduced into a dryer filled with calcium oxide for further drying and dehydration. After drying and dehydration, the gas is compressed to obtain a nitrogen-hydrogen mixed gas, in which the volume fraction of hydrogen is 10.1% and the volume fraction of nitrogen is 89.5%.
[0028] Example 2
[0029] Take 10kg of nickel-iron powder containing 85% iron, 10.5% nickel, and the rest oxygen and carbon as raw material, the particle size of the nickel-iron powder is ≤220μm, use nitrogen as the booster gas, and use sulfuric acid solution and nickel-iron powder to pressurize and leach in a closed reactor to prepare nitrogen-hydrogen mixed gas. The specific operation steps are as follows:
[0030] (1) nitrogen was introduced into the reactor to exhaust the oxygen in the reactor, the pressure in the reactor was maintained at 0.4 MPa, and the oxygen volume fraction in the reactor was controlled to be 0.1%;
[0031] (2) 10kg of nickel iron powder was mixed with 15L of water to prepare a slurry. The slurry was mechanically stirred and mixed evenly, and then the mixed slurry was pumped into the pressure reactor using a pressure pump. At the same time, 100L of sulfuric acid solution with a sulfuric acid concentration of 200g / L was added using another pressure pump. The reaction temperature was controlled to be 100-110°C, the pressure in the reactor did not exceed 0.4MPa, and the reaction time was 10h;
[0032] (3) The gas produced by the reaction is discharged from the pressure reducing valve on the top of the high-pressure reactor. The gas passes through a shell-and-tube heat exchanger and is cooled and dehydrated at 5°C. The residence time is 15 minutes. Most of the water in the mixed gas is condensed and removed. The mixed gas is then introduced into a dryer filled with calcium oxide for further drying and dehydration. After drying and dehydration, the gas is compressed to obtain a nitrogen-hydrogen mixed gas, in which the volume fraction of hydrogen is 30.2% and the volume fraction of nitrogen is 69.5%.
[0033] Example 3
[0034] Take 10kg of nickel-iron powder containing 78% iron, 18% nickel, and the rest oxygen and carbon as raw material, the particle size of the nickel-iron powder is ≤220μm, use nitrogen as the booster gas, use sulfuric acid solution and nickel-iron powder to pressurize and leach in a closed reactor to prepare nitrogen-hydrogen mixed gas, the specific operation steps are as follows:
[0035] (1) nitrogen was introduced into the reactor to exhaust the oxygen in the reactor, and the pressure in the reactor was maintained at 0.3 MPa, and the oxygen volume fraction in the reactor was controlled to be 0.1%;
[0036] (2) 10kg of nickel iron powder was mixed with 15L of water to prepare a slurry. The slurry was mechanically stirred and mixed evenly, and then the mixed slurry was pumped into the pressure reactor using a pressure pump. At the same time, 150L of sulfuric acid solution with a sulfuric acid concentration of 200g / L was added using another pressure pump. The reaction temperature was controlled to be 90-100°C, the pressure in the reactor did not exceed 0.3MPa, and the reaction time was 10h;
[0037] (3) The gas produced by the reaction is discharged from the pressure reducing valve on the top of the high-pressure reactor. The gas passes through a shell-and-tube heat exchanger and is cooled and dehydrated at 5°C. The residence time is 30 minutes. Most of the water in the mixed gas is condensed and removed. The mixed gas is then introduced into a dryer filled with anhydrous calcium chloride for further drying and dehydration. After drying and dehydration, the gas is compressed to obtain a nitrogen-hydrogen mixed gas, in which the volume fraction of hydrogen is 35.6% and the volume fraction of nitrogen is 64.1%.
[0038] Example 4
[0039] Take 10kg of nickel-iron powder containing 70.2% iron, 26.5% nickel, and the rest oxygen and carbon as raw material, the particle size of the nickel-iron powder is ≤220μm, use nitrogen as the booster gas, and use sulfuric acid solution and nickel-iron powder to pressurize and leach in a closed reactor to prepare nitrogen-hydrogen mixed gas. The specific operation steps are as follows:
[0040] (1) nitrogen was introduced into the reactor to exhaust the oxygen in the reactor, the pressure in the reactor was maintained at 0.25 MPa, and the oxygen volume fraction in the reactor was controlled to be 0.05%;
[0041] (2) 10 kg of nickel iron powder was mixed with 20 L of water to prepare a slurry. The slurry was mechanically stirred and mixed evenly, and then the mixed slurry was pumped into the pressure reactor using a pressure pump. At the same time, 150 L of sulfuric acid solution with a sulfuric acid concentration of 200 g / L was slowly added using another pressure pump. The addition was completed within 60 minutes, and the reaction temperature was controlled to be 115-120°C. The pressure in the reactor did not exceed 0.25 MPa, and the reaction time was 12 hours;
[0042] (3) The gas produced by the reaction is discharged from the pressure reducing valve on the top of the high-pressure reactor. The gas passes through a shell-and-tube heat exchanger and is cooled and dehydrated at 2°C. The residence time is 6 minutes. Most of the water in the mixed gas is condensed and removed. The mixed gas is then introduced into a dryer filled with calcium oxide for further drying and dehydration. After drying and dehydration, the gas is compressed to obtain a nitrogen-hydrogen mixed gas, in which the volume fraction of hydrogen is 40.2% and the volume fraction of nitrogen is 59.1%.
[0043] Example 5
[0044] Take 10kg of nickel-iron powder containing 78.5% iron, 12.4% nickel, and the rest oxygen and carbon as raw material, the particle size of the nickel-iron powder is ≤220μm, use nitrogen as the booster gas, and use sulfuric acid solution and nickel-iron powder to pressurize and leach in a closed reactor to prepare nitrogen-hydrogen mixed gas. The specific operation steps are as follows:
[0045] (1) nitrogen was introduced into the reactor to exhaust the oxygen in the reactor, the pressure in the reactor was maintained at 0.15 MPa, and the oxygen volume fraction in the reactor was controlled to be 0.05%;
[0046] (2) 10 kg of nickel iron powder was mixed with 20 L of water to prepare a slurry. The slurry was mechanically stirred and mixed evenly, and then the mixed slurry was pumped into the pressure reactor using a pressure pump. At the same time, 300 L of sulfuric acid solution with a sulfuric acid concentration of 50 g / L was slowly added using another pressure pump. The addition was completed within 60 minutes, and the reaction temperature was controlled to be 80-105°C. The pressure in the reactor did not exceed 0.15 MPa, and the reaction time was 20 hours;
[0047] (3) The gas produced by the reaction is discharged from the pressure reducing valve on the top of the high-pressure reactor. The gas passes through a shell-and-tube heat exchanger and is cooled and dehydrated at 5°C. The residence time is 20 minutes. Most of the water in the mixed gas is condensed and removed. The mixed gas is then introduced into a dryer filled with calcium oxide for further drying and dehydration. After drying and dehydration, the gas is compressed to obtain a nitrogen-hydrogen mixed gas, in which the volume fraction of hydrogen is 45.0% and the volume fraction of nitrogen is 54.6%.
[0048] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A method for preparing nitrogen-hydrogen mixed gas by pressurized leaching of nickel-iron powder, It is characterized in that The following steps are involved: (1) Using nitrogen as the gas source and protective gas, maintaining the pressure in the reactor at 0.15-0.6 MPa, and controlling the oxygen volume fraction in the reactor to be less than 0.1%; (2) Pumping ore slurry containing nickel iron powder and sulfuric acid solution into the reactor in sequence, controlling the sulfuric acid concentration in the reactor to be 50-300 g / L and the reaction temperature to be 80-120° C.; (3) The gas produced by the reaction is discharged from the pressure reducing valve at the top of the high-pressure reactor. The obtained gas is cooled, dehydrated, dried and compressed to obtain a nitrogen-hydrogen mixed gas.
2. A method for preparing nitrogen-hydrogen mixed gas by pressurized leaching of nickel-iron powder according to claim 1, It is characterized in that The mass concentration of the nickel-iron powder in the nickel-iron powder-containing ore slurry is 20-60%, and the rest is water.
3. A method for preparing nitrogen-hydrogen mixed gas by pressurized leaching of nickel-iron powder according to claim 2, It is characterized in that The main components of the nickel-iron powder are as follows by mass percentage: iron accounts for 70-90% and nickel accounts for 10-30%.
4. A method for preparing nitrogen-hydrogen mixed gas by pressurized leaching of nickel-iron powder according to claim 2, It is characterized in that The particle size of the nickel-iron powder is ≤220 μm.
5. A method for preparing nitrogen-hydrogen mixed gas by pressure leaching of nickel-iron powder according to claim 1, It is characterized in that The temperature of the gas cooling and dehydration is 0-10°C, and the gas residence time is 5-30 minutes.
6. A method for preparing nitrogen-hydrogen mixed gas by pressure leaching of nickel-iron powder according to claim 2, It is characterized in that The drying agent used in the drying is calcium oxide or anhydrous calcium chloride.
7. A method for preparing nitrogen-hydrogen mixed gas by pressure leaching of nickel-iron powder according to claim 2, It is characterized in that In the compressed nitrogen-hydrogen mixed gas, the volume fraction of hydrogen is 5% to 45%, and the rest is nitrogen.
Citation Information
Patent Citations
Method of producing nitrogen-hydrogen atmospheres for metals processing
CA2114206A1
Method for making hydrogen by activation of lithium hydride
CN101423189A
Method for high-pressure acid leaching and high-pressure iron removal of cobalt-iron alloy
CN113881845A