Magnesium phosphate cement composite material containing sulfur concentrate tailings and preparation method of magnesium phosphate cement composite material
By introducing sulfur fine tailings and retarders into magnesium phosphate cement, replacing refiring magnesium oxide, the problem of fast coagulation speed and high cost of magnesium phosphate cement is solved, extending the setting time, reducing the hydration heat, and improving the resistance The compressive strength achieves cost-effective hydration and hardening effect.
Patent Information
- Application Number
- CN202411059775.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-15
AI Technical Summary
Magnesium phosphate cement has a fast set rate and high cost that limits its wide application. Excessive amount of existing retarders will reduce strength, and the lack of effective mineral blending utilization will lead to excessive hydration reaction rate and heat. Impacts construction and economics.
Sulfur fine tailings are introduced as a high-performance concrete admixture, replacing refired magnesium oxide, combining ammonium dihydrogen phosphate and retarder, adjusting the composition of hydration products, extending the settling time, reducing the heat of hydration, and improving compressive strength.
It effectively extends the settling time of magnesium phosphate cement, reduces hydration heat, reduces costs, and increases compressive strength, meets construction needs and achieves good hydration hardening strength.
Smart Images

Figure CN118955085A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of magnesium phosphate cement composite materials, in particular to the technical field of preparation of magnesium phosphate cement composite materials containing sulfur concentrate tailings. Technical Background
[0002] Magnesium phosphate cement has the characteristics of early strength and fast hardening, and has been promoted and applied in the fields of rapid repair and reinforcement of airport runways, tunnels, and roads. However, magnesium phosphate cement has the problem of setting too fast, and its hydration reaction process is an acid-base neutralization reaction. A large amount of heat released during the reaction will accelerate the reaction, causing inconvenience to the construction. Excessive heat release can easily lead to cracking of the hardened cement. In addition, due to the high cost of raw materials, the overall price of magnesium phosphate cement is high, which limits its widespread application. In order to slow down the hydration reaction rate of magnesium phosphate cement, reduce the hydration heat, and reduce costs, the following measures are currently taken:
[0003] First, adding retarders to control the reaction rate of magnesium phosphate cement. Common retarders include borax, boric acid, sodium tripolyphosphate, etc. However, excessive dosage of retarders will cause the strength of magnesium phosphate cement to drop too much. Second, various mineral admixtures are introduced to replace high-temperature calcined dead-burned magnesium oxide, reduce production costs, reduce hydration heat, and improve cement properties. Current studies have shown that mineral admixtures such as metakaolin, steel slag, volcanic ash, fly ash, and other industrial solid wastes can be used to modify magnesium phosphate cement. Appropriate addition will not reduce strength, but can also improve water resistance and bond strength. Studies have shown that the "activity effect", "micro-aggregate effect" and "adsorption effect" of mineral admixtures have a positive effect on improving the strength of cement stone. However, there is also the problem that the excessive dosage of mineral admixtures will reduce the strength of magnesium phosphate cement. Therefore, it is particularly necessary to explore new mineral admixtures and industrial solid wastes for improving magnesium phosphate cement.
[0004] China has abundant pyrite reserves, with total reserves equivalent to 1.493 billion tons of sulfur, ranking second in the world. Sulfur concentrate is pyrite that has been carefully selected. Sulfur concentrate tailings are the waste residue left after sulfuric acid is prepared from sulfur concentrate. Because of its high volcanic ash activity, it can be used as a high-performance concrete admixture to effectively improve the compressive strength of concrete. However, most of the sulfur concentrate tailings are abandoned and not effectively utilized, and there are no reports on their application in magnesium phosphate cement. XRD analysis shows that sulfur concentrate tailings contain actinolite (Fe, Mg, Ca, Na, Mn) 7 (Si, Al) 8 O 22 (OH) 1.9 , calcium zeolite (CaO·Al 2 O 3 ·2SiO 2 ·4H 2 O), Fe2 O 3 , Al 2 O 3 , aluminum oxalate (C 6 Al 2 O 12 ), CaCO 3 , iron alum FeAl 2 (SO 4 ) 4 ·22H 2 O (PDF#39-1387) and other crystalline phases. Calcium zeolite belongs to the category of aluminosilicates and can react with ammonium dihydrogen phosphate at a certain temperature to form an amorphous silicoaluminophosphate gel. Based on this, we speculate that sulfur tailings may participate in the hydration reaction in magnesium phosphate cement, and will show "activity effect" and "micro-aggregate effect". The present invention proposes to modify magnesium phosphate cement with sulfur tailings, replace dead-burned magnesium oxide with it, prolong the setting time, reduce the hydration heat, and reduce the cost of magnesium phosphate cement without reducing the strength. At the same time, it also opens up a new way for the comprehensive utilization of sulfur tailings. Summary of the invention
[0005] In view of this, the object of the present invention is to provide a magnesium phosphate cement composite material of sulfur-containing fine tailings and a preparation method, to prolong the setting time of magnesium phosphate cement, to reduce the hydration heat, to reduce the content of dead-burned magnesium oxide in magnesium phosphate cement, to reduce the cost, to adjust the composition of the hydration products of magnesium phosphate cement, and to give magnesium phosphate cement good hydration hardening strength.
[0006] The present invention provides a magnesium phosphate cement composite material containing sulfur concentrate tailings, the main components of which are measured by weight:
[0007] 15-90 parts of sulfur concentrate tailings;
[0008] 285-210 parts of dead-burned magnesium oxide;
[0009] 100 parts of diammonium phosphate;
[0010] Retarder 15-30 parts
[0011] 60-70 parts water
[0012] The specific surface area of the sulfur concentrate tailings of the present invention is 1029m 2 / kg, sulfur concentrate tailings account for 5-30% of the total mass of sulfur concentrate tailings and dead-burned magnesium oxide;
[0013] The dead-burned magnesium oxide of the present invention is prepared by calcining magnesite at 1600-1700°C, wherein the MgO content of the obtained dead-burned magnesium oxide is 90-95%, the fineness is 100-200 mesh, and the specific surface area is 500-900m 2 / kg;
[0014] The retarder of the present invention is of industrial grade with a purity greater than 90%. It can be one of boric acid and borax, or a compound of one of boric acid and borax and sodium tripolyphosphate. The amount of the retarder accounts for 5-10% of the total mass of dead-burned magnesium oxide and diammonium phosphate, and the mass ratio of boric acid (or borax) to sodium tripolyphosphate is 1:(0.5-1).
[0015] A method for preparing magnesium phosphate cement containing sulfur concentrate tailings, specifically comprising the following steps:
[0016] The sulfur concentrate tailings, dead-burned magnesium oxide, ammonium dihydrogen phosphate and retarder were weighed according to the set ratio and added into the slurry mixer. The mixture was slowly dry-mixed for 1-2 minutes. Then water was added and the mixture was slowly mixed for 20-30 seconds and then quickly mixed for 1-2 minutes to obtain magnesium phosphate cement slurry. The fluidity and setting time were tested. In addition, test blocks were prepared using a 160*160*40mm mold according to the same preparation method for compressive strength test.
[0017] Compared with traditional magnesium phosphate cement, the present invention has the following beneficial effects:
[0018] The introduction of sulfur concentrate tailings reduces the content of dead-burned magnesium oxide in magnesium phosphate cement, reduces costs, prolongs the setting time of magnesium phosphate cement, and reduces the hydration heat. More importantly, the appropriate introduction of sulfur concentrate tailings can improve the compressive strength of magnesium phosphate cement, which may be because some components in the sulfur concentrate tailings participate in the hydration reaction to form new hydration products. At the same time, the sulfur concentrate tailings with a high specific surface area provide a micro-aggregate effect, fill the microstructure of the cement stone, and improve the strength. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 The compressive strength of the hydration products of different ages (1d, 7d, 28d) of each embodiment and comparative example is shown in FIG.
[0020] Figure 2 This is a scanning electron microscope photograph of the 28-day hydration product of Example 1.
[0021] Figure 3 The X-ray diffraction spectra of the 28-day hydration products of Example 1 and Comparative Example are shown in FIG. DETAILED DESCRIPTION
[0022] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other examples improved or modified by ordinary technicians in this field belong to the scope of protection of the present invention.
[0023] Example 1
[0024] A magnesium phosphate cement composite material containing sulfur concentrate tailings, wherein the components thereof are calculated by weight: 30 parts of sulfur concentrate tailings, 270 parts of dead-burned magnesium oxide, 100 parts of ammonium dihydrogen phosphate, 30 parts of retarder (30 parts of boric acid), and 68 parts of water; and the preparation process thereof comprises the following steps: adding sulfur concentrate tailings, dead-burned magnesium oxide, phosphate, and retarder to a pure slurry mixer according to a set ratio, slowly dry-stirring for 2 minutes, adding water, first slowly stirring for 30 seconds, and then rapidly stirring for 2 minutes to obtain magnesium phosphate cement slurry, testing fluidity and setting time, preparing magnesium phosphate cement slurry according to the same method, and preparing compressive strength test blocks.
[0025] Example 2
[0026] A magnesium phosphate cement composite material containing sulfur concentrate tailings, wherein the components thereof are calculated by weight: 60 parts of sulfur concentrate tailings, 240 parts of dead-burned magnesium oxide, 100 parts of ammonium dihydrogen phosphate, 20 parts of a retarder (10 parts of boric acid and 10 parts of sodium tripolyphosphate), and 65 parts of water; and the preparation process thereof comprises the following steps: adding sulfur concentrate tailings, dead-burned magnesium oxide, phosphate, and a retarder to a pure slurry mixer according to a set ratio, slowly dry-stirring for 1.5 minutes, then adding water, first slowly stirring for 20 seconds, and then rapidly stirring for 1 minute to obtain magnesium phosphate cement slurry, testing fluidity and setting time, preparing magnesium phosphate cement slurry according to the same method, and preparing a compressive strength test block.
[0027] Example 3
[0028] A magnesium phosphate cement composite material containing sulfur concentrate tailings, wherein the components thereof are calculated by weight: 15 parts of sulfur concentrate tailings, 285 parts of dead-burned magnesium oxide, 100 parts of ammonium dihydrogen phosphate, 30 parts of a retarder (15 parts of borax and 15 parts of sodium tripolyphosphate), and 60 parts of water; and the preparation process thereof comprises the following steps: weighing sulfur concentrate tailings, dead-burned magnesium oxide, phosphate, and a retarder according to a set ratio and adding them into a slurry mixer, slowly dry-stirring for 1 minute, then adding water, first slowly stirring for 30 seconds, and then rapidly stirring for 1.5 minutes, so as to obtain magnesium phosphate cement slurry, testing fluidity and setting time, preparing magnesium phosphate cement slurry according to the same method, and preparing a compressive strength test block.
[0029] Example 4
[0030] A magnesium phosphate cement composite material containing sulfur concentrate tailings, the components of which are calculated by mass: 90 parts of sulfur concentrate tailings, 210 parts of dead-burned magnesium oxide, 100 parts of ammonium dihydrogen phosphate, 15 parts of retarder (15 parts of boric acid), and 65 parts of water. The preparation process comprises the following steps: sulfur concentrate tailings, dead-burned magnesium oxide, phosphate, and retarder are weighed according to a set ratio and added into a pure slurry mixer, slowly dry-mixed for 2 minutes, then water is added, slowly mixed for 30 seconds, and then quickly mixed for 1 minute to obtain magnesium phosphate cement slurry, test fluidity and setting time, prepare magnesium phosphate cement slurry according to the same method, and prepare compressive strength test blocks.
[0031] Comparative Example 1
[0032] A magnesium phosphate cement without sulfur tailings, the components of which are calculated by mass: 300 parts of dead-burned magnesium oxide, 100 parts of ammonium dihydrogen phosphate, 30 parts of boric acid, and 68 parts of water. The preparation process comprises the following steps: weighing sulfur tailings, dead-burned magnesium oxide, phosphate, and retarder according to a set ratio and adding them into a pure slurry mixer, slowly dry stirring for 2 minutes, then adding water, first slowly stirring for 30 seconds, and then quickly stirring for 1.5 minutes, to obtain magnesium phosphate cement slurry, testing fluidity and setting time, preparing magnesium phosphate cement slurry according to the same method, and preparing compressive strength test blocks.
[0033] Performance Testing
[0034] According to the mass fractions of the components and the preparation method of the magnesium phosphate cement composite materials of Examples 1 to 4 and the comparative example, magnesium phosphate cement slurry was prepared, the fluidity and setting time were tested, and compressive strength test blocks were prepared. The compressive strength was measured after curing in air for 1 day, 7 days and 28 days. The relevant test results are shown in the table below.
[0035]
[0036] It can be seen from the above table that compared with the comparative example, the setting time of the sulfur-containing refined tailings magnesium phosphate cement prepared by the present invention is longer, the fluidity is larger, and it can meet the construction requirements. The sulfur-containing refined tailings magnesium phosphate cement prepared by the present invention can reach a maximum 28d compressive strength of 75MPa, a 7d compressive strength of 66MPa, and a 1d compressive strength of 37MPa, indicating that the appropriate introduction of sulfur refined tailings can improve the compressive strength of magnesium phosphate cement. There are two reasons for the improvement of compressive strength: first, an appropriate amount of sulfur refined tailings can play the role of micro-aggregate, thereby improving the strength of cement; second, the components in the sulfur refined tailings participate in the hydration reaction to form a new crystalline or gel-like hydration product, which fills the cement stone structure, thereby improving the strength.
[0037] The above description is only a preferred embodiment of the present invention. All equivalent changes and modifications made according to the scope of the patent application of the present invention should fall within the scope of the present invention.
Claims
1. A magnesium phosphate cement composite material containing sulfur concentrate tailings, characterized in that: The invention is composed of the following components: sulfur concentrate tailings, dead-burned magnesium oxide, ammonium dihydrogen phosphate, retarder and water, wherein the mass proportions of the sulfur concentrate tailings, dead-burned magnesium oxide, ammonium dihydrogen phosphate and retarder are in the range of 15-90 parts of sulfur concentrate tailings, 210-285 parts of dead-burned magnesium oxide, 100 parts of ammonium dihydrogen phosphate, 15-30 parts of retarder and 60-70 parts of water.
2. A magnesium phosphate cement composite material of sulfur-containing concentrate tailings according to claim 1, wherein the preparation method is as follows: weigh the sulfur concentrate tailings, dead-burned magnesium oxide, ammonium dihydrogen phosphate, and retarder according to a set ratio and add them to a slurry mixer, slowly dry-mix for 1-2 minutes, then add water, first slowly mix for 20-30 seconds, and then quickly mix for 1-2 minutes to obtain magnesium phosphate cement slurry.
3. The magnesium phosphate cement composite material of a sulfur-containing concentrate tailings according to claim 1, characterized in that: The sulfur concentrate tailings described in claim 1 account for 5-30% of the total mass of the sulfur concentrate tailings and the dead-burned magnesium oxide.
4. The magnesium phosphate cement composite material of a sulfur-containing concentrate tailings according to claim 1, characterized in that: The sulfur concentrate tailings described in claim 1 are residual waste materials from the flotation of sulfur concentrate (pyrite) to produce sulfur concentrate powder. It is a gray-green powder, and its X-ray fluorescence spectrum gives the following chemical composition expressed as oxides: SiO2 39.7%, Fe2O3 24.0%, CaO12.9%, Al2O3 8.45%, MgO 2.79%, CO2 3.23%, and SO3 5.04%.
5. The magnesium phosphate cement composite material of a sulfur-containing concentrate tailing according to claim 1, characterized in that: The specific surface area of the sulfur concentrate tailings described in claim 1 is 1029m 2 / kg.
6. The magnesium phosphate cement composite material of sulfur-containing concentrate tailings according to claim 1, characterized in that: The dead-burned magnesium oxide described in claim 1 is obtained by calcining magnesite at a high temperature of 1600-1700°C, wherein the MgO content in the obtained dead-burned magnesium oxide is 90-95%.
7. The magnesium phosphate cement composite material of sulfur-containing concentrate tailings according to claim 1, characterized in that: The dead-burned magnesium oxide described in claim 1 has a fineness of 100-200 mesh and a specific surface area of 500-900m 2 / kg.
8. The magnesium phosphate cement composite material of sulfur-containing concentrate tailings according to claim 1, characterized in that: The retarder described in claim 1 can be at least one of boric acid and borax, or a compound of boric acid (or borax) and sodium tripolyphosphate, the mass ratio of boric acid (or borax) to sodium tripolyphosphate is 1:(0.5-1), and the amount of retarder accounts for 5-10% of the total mass of dead-burned magnesium oxide and diammonium phosphate.