Black mixed oxide material and manufacturing method thereof

By developing black mixed oxide materials with La, Mn and Cu as main components, the problem of chromium and cobalt content in the prior art was solved, and a black pigment with high safety and economicality was achieved, suitable for a variety of non-magnetic and insulating Sexual application.

CN118955135APending Publication Date: 2024-11-15NAKASHIMA SANGYO CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411077073.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2018-02-08
Filing Date
2018-06-07
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Existing black pigments contain chromium and cobalt during the manufacturing process, which leads to environmental and human health risks, and it is difficult to completely remove hexavalent chromium, affecting the safety and scope of use of the product.

Method used

A black mixed oxide material with La, Mn and Cu as the main components was developed, and prepared by the crushing and firing process to ensure that the material does not contain chromium and cobalt, and has a perovskite phase and spinel structure, suitable for use as a Used for non-magnetic and insulating materials.

Benefits of technology

High safety, economy and good tone are achieved, avoiding the risk of chromium and cobalt use, expanding the application range of materials, and reducing manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955135A_ABST
    Figure CN118955135A_ABST
Patent Text Reader

Abstract

Provided are: a black mixed oxide material which does not contain chromium itself in the main component, does not contain cobalt in the main component, is highly safe, has a good color tone, and is economical, a method for producing the black mixed oxide material, and various products using the black mixed oxide material. The present invention relates to a mixed oxide which contains oxides having La, Mn and Cu as main components and does not contain Cr and Co as the main components, and wherein the contents of La, Mn and Cu in the mixed oxide satisfy the following proportions in terms of oxides in which the total weight of the following oxides is taken as 100% by weight: La is 35-70% by weight in terms of La2O3; in terms of MnO2, Mn accounts for 25-60 wt%; and in terms of CuO, Cu accounts for 0.5-10 wt%.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application for the invention patent application with application date of June 7, 2018, application number 201880036637.2, and invention name “Black mixed oxide material and its manufacturing method”. Technical Field

[0002] The present invention relates to a black pigment containing no chromium and cobalt as a main component, a method for producing the same, and a product using the black pigment. Background Art

[0003] Inorganic black pigments are used in various fields such as ceramics, coatings, resin coloring, and pigment components of glass pastes. For example, glass pastes using black pigments are used in ceramic pastes that form the coating film on the edge of automobile window glass (see Patent Document 1), insulating pastes for insulating barriers of plasma displays, etc. (see Patent Document 2). Most black pigments so far contain chromium (Cr) in their constituent components. Cr2O3, which contains chromium compounds in order to improve the heat resistance of the pigment and adjust the color tone, is widely used as one of the raw material oxides that are indispensable for the manufacture of black pigments.

[0004] However, currently, the "Directive of the European Parliament and of the Council on the restriction of the use of certain hazardous substances in electrical and electronic equipment" is being implemented in all stages of the production and distribution of electrical and electronic equipment in the EU with the aim of minimizing the risks to the environment and human health. This is usually referred to as the RoHS Directive (RoHS: Restriction of Hazardous Substances). The RoHS Directive prohibits the use of hazardous substances in principle, and the six substances specified are lead (Pb), mercury (Hg), cadmium (Cd), hexavalent chromium (Cr 6+ ), polybrominated biphenyls (PBB), polybrominated diphenyl ethers (PBDE).

[0005] When developing products that comply with the RoHS Directive, it is necessary to thoroughly manage the raw material components used in the parts and materials that make up the product so that the products do not contain the above six prohibited substances. The restrictions on hazardous chemical substances that take such environmental issues into consideration are spreading not only in the EU countries, but also in countries around the world.

[0006] Cr, which is generally contained as a raw material oxide of a pigment, is converted into highly toxic hexavalent chromium (Cr) by heating or the like. 6+). In the pigment manufacturing process, the hexavalent chromium is removed due to water washing and other treatments as needed. However, after a drying process at about 180°C, some of it may become hexavalent chromium again. Therefore, the black pigment itself as a product may become a problem. On top of this, depending on the purpose of the pigment, it may be heated or exposed to ultraviolet rays due to its use conditions. In this case, it cannot be completely denied that the Cr contained in the black pigment has changed from trivalent (Cr 3+ ) becomes hexavalent (Cr 6+ ) danger.

[0007] The current RoHS directive only restricts hexavalent chromium. However, in the case of discarding products that use black pigments containing chromium, safety issues associated with changes in valence have begun to receive attention. Finally, attention has been paid to black pigments that do not contain chromium itself (see Patent Document 3). The black pigment of Patent Document 3 uses strontium compounds and iron oxides as its main components. Since strontium is highly soluble in water, the actual manufacturing method is limited to non-aqueous liquids or ethanol. Therefore, the cost of pigment manufacturing increases, and the scope of use and purpose are also extremely limited.

[0008] Furthermore, the formulation and method used in the production of black pigments have been repeatedly improved, and new black pigments that do not contain chromium itself have been proposed (see Patent Documents 4 and 5). The black pigment of Patent Document 4 is a pigment containing oxides of Mn, Co, Ni and Fe as main components. The black pigment of Patent Document 5 is a pigment containing oxides of Mn, Fe, Cu and Co as main components. In particular, the black pigment of Patent Document 5 obtains a high-quality black color.

[0009] As mentioned above, with the necessity of managing harmful chemical substances contained in products, pigments of component classes that do not contain chromium are available. However, as shown in this main component, cobalt is contained as one of the main components. Cobalt is known to be a cause of allergic symptoms, and it is hoped that the composition of the main components will be reduced as much as possible. Therefore, on the premise of presenting the good black color required for black pigments, a new component class that does not contain chromium and cobalt as the main component is urgently desired from the perspective of environmental compliance.

[0010] Patent Document 1: Japanese Patent Laid-Open No. 6-340447

[0011] Patent Document 2: Japanese Patent Laid-Open No. 6-144871

[0012] Patent Document 3: Japanese Patent Laid-Open No. 2000-264639

[0013] Patent Document 4: Japanese Patent Laid-Open No. 2007-217544

[0014] Patent Document 5: Japanese Patent No. 5131664

[0015] Based on this experience, the inventors readjusted the main components of black pigments and conducted in-depth research. As a result, they finally developed a black pigment with a main component composition that does not contain chromium or cobalt as a main component. Furthermore, they confirmed that in addition to the performance expected as a black pigment, it also has other physical properties. Summary of the invention

[0016] In view of the above aspects, the present invention provides a black pigment which is independent of the valence of chromium, does not contain chromium itself as a main component, and does not contain cobalt as a main component, has high safety, good color tone and economic efficiency, and a method for producing the same, and also provides various products based on the physical properties of the black pigment.

[0017] First, a black mixed oxide material, characterized in that it is a mixed oxide containing oxides having La, Mn and Cu as main components and excluding Cr and Co as the main components.

[0018] Second, a black mixed oxide material, characterized in that the mixed oxide has a perovskite phase, and the perovskite phase shows a diffraction peak with maximum intensity in the range of 31° to 34° of the diffraction angle 2θ during X-ray diffraction measurement using CuKα rays as the X-ray source, and the mixed oxide contains Mn3O4 with a spinel structure as the oxide of Mn.

[0019] Third, a black mixed oxide material, characterized in that, based on the oxide conversion amount with the total weight of the following oxides being set to 100 weight %, the contents of La, Mn and Cu in the mixed oxide satisfy the following ratios: calculated as La2O3, La is 35-70 weight %; calculated as MnO2, Mn is 25-60 weight %; calculated as CuO, Cu is 0.5-10 weight %.

[0020] Fourth, a black mixed oxide material, characterized in that the mixed oxide further contains Mo oxide as the main component, La is calculated as La2O3, Mn is calculated as MnO2, Cu is calculated as CuO, and the total weight of these three oxides is set to 100 weight% of the oxide conversion amount, Mo is calculated as MoO3 relative to 100 weight% of the oxide conversion amount, and the mixed oxide contains Mo in a ratio of less than 5 weight%.

[0021] Fifth, a black mixed oxide material, characterized in that the mixed oxide contains, in addition to the main component, any one or more of Li, B, Na, Mg, Al, Si, P, K, Ca, Ti, V, Fe, Zn, Sr, Y, Zr, Nb, Sn, Sb, Ba, Ta, W, Bi, Ce, Pr, Nd or Er as a minor component, La is calculated as La2O3, Mn is calculated as MnO2, Cu is calculated as CuO, and the total weight of these three oxides is In the oxide conversion amount whose volume weight is set to 100 weight %, the auxiliary components are Li2O, B2O3, Na2O, MgO, Al2O3, SiO2, P2O5, K2O, CaO, TiO2, V2O5, Fe3O3, ZnO, SrO, Y2O3, ZrO2, Nb2O3, SnO2, Sb2O3, BaO, Ta2O5, WO3, Bi2O3, CeO2, Pr6O 11 , Nd2O5 or Er2O3, the mixed oxide contains the accessory components in a proportion of 20 weight % or less.

[0022] Sixth, a black mixed oxide material, characterized in that the mixed oxide is a black pigment.

[0023] Seventh, a black mixed oxide material, characterized in that the mixed oxide is a non-magnetic material.

[0024] Eighth, a black mixed oxide material, characterized in that the mixed oxide is an insulating material.

[0025] Ninth, a method for manufacturing a black mixed oxide material, characterized in that it comprises: a primary crushing step, mixing and crushing oxide raw materials of La, Mn and Cu to obtain a primary crushed product with an average particle size of less than 5 μm; a raw material sintering step, sintering the primary crushed product at 700-1200°C to obtain a raw material sintered product; and a secondary crushing step, pulverizing the raw material sintered product to an average particle size of less than 50 μm, thereby obtaining a mixed oxide.

[0026] 10. A method for producing a black mixed oxide material, characterized in that, based on the oxide conversion amount in which the total weight of the following oxides is set to 100 weight %, the contents of La, Mn and Cu in the mixed oxide satisfy the following ratios: in terms of La2O3, La is 35 to 70 weight %; in terms of MnO2, Mn is 25 to 60 weight %; in terms of CuO, Cu is 0.5 to 10 weight %.

[0027] 11. A method for manufacturing a black mixed oxide material, characterized in that the mixed oxide further contains Mo oxide as the main component, La is calculated as La2O3, Mn is calculated as MnO2, Cu is calculated as CuO, and the total weight of these three oxides is set to 100 weight% of the oxide conversion amount, Mo is calculated as MoO3 relative to 100 weight% of the oxide conversion amount, and the mixed oxide contains Mo in a ratio of less than 5 weight%.

[0028] 12. A method for manufacturing a black mixed oxide material, characterized in that it comprises: a first crushing step, mixing and crushing oxide raw materials of La, Mn and Cu to obtain a first crushed product with an average particle size of less than 5 μm; a first sintering step, sintering the first crushed product at 700-1200°C to obtain a first sintered product; a second crushing step, crushing the first sintered product to obtain a second crushed product with an average particle size of less than 50 μm; a second sintering step, sintering the second crushed product at 600-1100°C to obtain a second sintered product; and a third crushing step, crushing the second sintered product to an average particle size of less than 20 μm, thereby obtaining a mixed oxide.

[0029] Thirteenth, a method for manufacturing a black mixed oxide material, characterized in that, based on the oxide conversion amount in which the total weight of the following oxides is set to 100 weight %, the contents of La, Mn and Cu in the mixed oxide satisfy the following ratios: calculated as La2O3, La is 35-70 weight %; calculated as MnO2, Mn is 25-60 weight %; calculated as CuO, Cu is 0.5-10 weight %.

[0030] 14. A method for manufacturing a black mixed oxide material, characterized in that the mixed oxide further contains Mo oxide as the main component, La is calculated as La2O3, Mn is calculated as MnO2, Cu is calculated as CuO, and the total weight of these three oxides is set to 100 weight% of the oxide conversion amount, Mo is calculated as MoO3 relative to 100 weight% of the oxide conversion amount, and the mixed oxide contains Mo in a ratio of less than 5 weight%.

[0031] 15. An inorganic ceramic material characterized by containing a black mixed oxide material and a ceramic agent.

[0032] 16. An inorganic glass slurry, characterized in that it contains a black mixed oxide material and a glass agent.

[0033] 17. A fired product, characterized in that it is made by firing inorganic glass slurry on a glass part, a metal part, pottery or porcelain.

[0034] 18. A resin slurry characterized by containing a black mixed oxide material and a resin agent.

[0035] 19. A coated product, characterized in that it is formed by coating a resin slurry on a support.

[0036] 20. A coated product, characterized in that the support is glass, metal, pottery, porcelain, resin product or carbon material.

[0037] 21. A resin component characterized by comprising a black mixed oxide material and a resin agent.

[0038] According to the black mixed oxide material, since it is an oxide containing La, Mn and Cu as main components, and is a mixed oxide that does not contain Cr and Co as the main components, it is independent of the valence of chromium, does not contain chromium itself in the main components, and does not contain cobalt in the main components, and has high safety, good color tone and economy.

[0039] Since the mixed oxide has a perovskite phase, the perovskite phase shows a diffraction peak with maximum intensity in the range of 31° to 34° of the diffraction angle 2θ during X-ray diffraction measurement using CuKα rays as the X-ray source, and the mixed oxide contains Mn3O4 with a spinel structure as the oxide of Mn, and therefore is in the form of a sintered mixed oxide.

[0040] Since the contents of La, Mn and Cu in the mixed oxide satisfy the following proportions based on the oxide conversion amount with the total weight of the following oxides being set to 100 weight %: La is 35 to 70 weight % in terms of La2O3; Mn is 25 to 60 weight % in terms of MnO2; Cu is 0.5 to 10 weight % in terms of CuO, chromium itself is not contained in the main components, and cobalt is not contained in the main components, and a good black color is exhibited.

[0041] Since the mixed oxide further contains Mo oxide as the main component, La is calculated as La2O3, Mn is calculated as MnO2, Cu is calculated as CuO, and the total weight of these three oxides is set to 100 weight%. In the oxide conversion amount, Mo is calculated as MoO3 relative to 100 weight% of the oxide conversion amount. The mixed oxide contains Mo in a ratio of less than 5 weight%, and thus presents a higher quality black color.

[0042] Since the mixed oxide contains any one or more of Li, B, Na, Mg, Al, Si, P, K, Ca, Ti, V, Fe, Zn, Sr, Y, Zr, Nb, Sn, Sb, Ba, Ta, W, Bi, Ce, Pr, Nd or Er as a minor component in addition to the main component, La is calculated as La2O3, Mn is calculated as MnO2, and Cu is calculated as CuO, and the total weight of these three oxides is set to 100 weight %, the auxiliary components are Li2O, B2O3, Na2O, MgO, Al2O3, SiO2, P2O5, K2O, CaO, TiO2, V2O5, Fe3O3, ZnO, SrO, Y2O3, ZrO2, Nb2O3, SnO2, Sb2O3, BaO, Ta2O5, WO3, Bi2O3, CeO2, Pr6O 11 , Nd2O5 or Er2O3, the mixed oxide contains the accessory components in a proportion of less than 20 weight %, and therefore there is no need to use high-purity raw materials or use special manufacturing management and methods for avoiding the mixing of impurities, and the raw material and manufacturing costs can be relatively cheap.

[0043] Since the mixed oxide is a black pigment, a non-magnetic material or an insulating material, the black mixed oxide material has a wide range of uses.

[0044] According to the manufacturing method of the black mixed oxide material, since it comprises: a primary crushing step, mixing and crushing oxide raw materials of La, Mn and Cu to obtain a primary crushed product with an average particle size of less than 5 μm; a raw material sintering step, sintering the primary crushed product at 700-1200°C to obtain a raw material sintered product; and a secondary crushing step, pulverizing the raw material sintered product to an average particle size of less than 50 μm to obtain a mixed oxide, it is independent of the valence of chromium, does not contain chromium itself in the main component, and does not contain cobalt in the main component, and has high safety, good color tone and economy.

[0045] Since the contents of La, Mn and Cu in the mixed oxide satisfy the following proportions based on the oxide conversion amount with the total weight of the following oxides being set to 100 weight %: La is 35 to 70 weight % in terms of La2O3; Mn is 25 to 60 weight % in terms of MnO2; Cu is 0.5 to 10 weight % in terms of CuO, chromium itself is not contained in the main components, and cobalt is not contained in the main components, and a good black color is exhibited.

[0046] Since the mixed oxide further contains Mo oxide as the main component, La is calculated as La2O3, Mn is calculated as MnO2, Cu is calculated as CuO, and the total weight of these three oxides is set to 100 weight%. In the oxide conversion amount, Mo is calculated as MoO3 relative to 100 weight% of the oxide conversion amount. The mixed oxide contains Mo in a ratio of less than 5 weight%, and thus presents a higher quality black color.

[0047] According to the manufacturing method of the black mixed oxide material, it comprises: a first crushing step, mixing and crushing the oxide raw materials of La, Mn and Cu to obtain a first crushed product with an average particle size of less than 5 μm; a first sintering step, sintering the first crushed product at 700-1200°C to obtain a first sintered product; a second crushing step, crushing the first sintered product to obtain a second crushed product with an average particle size of less than 50 μm; a second sintering step, sintering the second crushed product at 600-1100°C to obtain a second sintered product; and a third crushing step, crushing the second sintered product to an average particle size of less than 20 μm to obtain a mixed oxide. Therefore, it is independent of the valence of chromium, does not contain chromium itself in the main component, and does not contain cobalt in the main component, and has high safety, good color tone and economy.

[0048] Since the contents of La, Mn and Cu in the mixed oxide satisfy the following proportions based on the oxide conversion amount with the total weight of the following oxides being set to 100 weight %: La is 35 to 70 weight % in terms of La2O3; Mn is 25 to 60 weight % in terms of MnO2; Cu is 0.5 to 10 weight % in terms of CuO, chromium itself is not contained in the main components, and cobalt is not contained in the main components, and a good black color is exhibited.

[0049] Since the mixed oxide further contains Mo oxide as the main component, La is calculated as La2O3, Mn is calculated as MnO2, Cu is calculated as CuO, and the total weight of these three oxides is set to 100 weight % of the oxide conversion amount. Relative to 100 weight % of the oxide conversion amount, Mo is calculated as MoO3. The mixed oxide contains Mo in a ratio of less than 5 weight %, thereby being able to obtain a better quality black color.

[0050] The black mixed oxide material can be used in a wide range of products by being applied to black inorganic ceramic materials, black inorganic glass pastes, black resin pastes, etc. Therefore, as a material containing neither chromium nor cobalt, it can replace existing materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] Figure 1 This is a schematic process diagram of the method for producing the black mixed oxide material according to the first embodiment.

[0052] Figure 2 This is a schematic process diagram of a method for producing a black mixed oxide material according to a second embodiment.

[0053] Figure 3 This is a triangular diagram when the main components in the black mixed oxide material are converted into oxides.

[0054] Figure 4 yes Figure 3 An enlarged view of the main part.

[0055] Figure 5 This is the X-ray diffraction pattern of Sample Preparation Example 29.

[0056] Figure 6 This is the X-ray diffraction pattern of Sample Preparation Example 35.

[0057] Figure 7 This is the X-ray diffraction pattern of Sample Preparation Example 51.

[0058] Figure 8 is a graph of the magnetization curve of Sample Preparation Example 51.

[0059] Fig. 9 It is partially enlarged Figure 8 of charts for graphs. DETAILED DESCRIPTION

[0060] The black mixed oxide material of the present invention refers to a black mixed oxide material of the component type that does not contain Cr itself as a main component and does not contain Co as a main component, regardless of the valence of Cr. That is, the black mixed oxide material has three main components, namely La, Mn and Cu. Among them, Cr and Co are not contained in the main components. And it is a mixed oxide of oxides of metal elements containing the three main components. Furthermore, the use of the black mixed oxide material as a black pigment, in order to improve the good color rendering, Mo is also mixed in the main components of the three metal elements and modulated into a mixed oxide. In addition, as shown in the embodiments described later, in addition to the performance as a pigment, it also has the properties of a non-magnetic material and an insulating material.

[0061] In the X-ray diffraction (XRD) measurement of the mixed oxide using CuKα rays as an X-ray source, for example, Figures 5 to 7 X-ray diffraction pattern. Figure 5 , 6, 7 correspond to the subsequent sample preparation examples 29, 35, and 51. As can be seen from the illustrated pattern, a unique peak is confirmed for the mixed oxide. There is a diffraction peak with maximum intensity in the range of 31° to 34° set as the diffraction angle 2θ. Considering the same peaks, etc., it is assumed that the mixed oxide has a perovskite phase. In addition, based on the blackened positions of the four corners in the illustrated pattern, it is also assumed that the mixed oxide contains Mn3O4 with a spinel structure as an oxide of Mn.

[0062] The raw material form of La, Mn and Cu that become main component is not particularly limited, except each metal oxide, can also use metal compound such as carbonate, hydroxide.Specifically, from La2O3, La(OH)3, La2(CO3)3, MnO2, Mn3O4, MnCO3, Mn(OH)2, natural manganese dioxide pulverized product (containing MnO2+Fe2O3), CuO, Cu2O3, CuCO2, Cu(OH)2 etc. appropriately select.In the composition containing Mo in main component, from MoO2, MoO3, Mo(CO)6 etc. appropriately select.In addition, these can be combined as needed.

[0063] The black mixed oxide material shows the peak of the X-ray diffraction pattern shown in the figure, and it is also confirmed that it is a sintered mixed oxide. Therefore, the coordination amount between the main components of the mixed oxide La, Mn and Cu can be expressed by the relative ratio of the oxide conversion amount of each metal element in the form of the following oxide.

[0064] In the oxide conversion amount, the mixing ratio of the oxides of La, Mn and Cu as the main components is determined from the following examples. Figure 3 The triangular diagram is derived. The triangular diagram shows the quantitative balance between the various oxides of the black pigment of the mixed oxide as a sample preparation example described later. Specifically, the oxide forms of La in La2O3, Mn in MnO2, and Cu in CuO are fully understood. And the total weight of these three oxides is converted to 100 weight%. On this basis, the proportions of La2O3 in the range of 35-70 weight%, MnO2 in the range of 25-60 weight%, and CuO in the range of 0.5-10 weight%. If the oxides of each metal element are controlled within the aforementioned range, a good black color is presented. Therefore, the pigment use of black mixed oxide materials is the most powerful.

[0065] The ratio of each main component metal element is a convenient calculated value as the type of the oxide. Therefore, in reality, the sum of the weight percentages of the oxides of the main components La, Mn and Cu may exceed 100 or be less than 100. This is because the purity of the raw materials as the main component elements, the mixing of the auxiliary components described later, the change of the oxidation number (number of oxygen elements) in the pigment, etc. are taken into consideration. By temporarily converting the main component metal elements into the weight of the oxide, it is easy to grasp the pass or fail of the black color and the balance of the coordination amount of each metal element. In addition, it is also easy to grasp the amount and proportion of other components when they are added.

[0066] The more La2O3 as La oxide is added, the higher the concentration is and the higher the blackness is. When the converted weight of La2O3 is less than 35 wt%, the desired blackness is reduced. When the converted weight of La2O3 exceeds 70 wt%, the amount of raw materials other than La2O3 is reduced, and the quality stability cannot be maintained by other components. Therefore, La2O3 is preferably added in a ratio of 35 to 70 wt%, and more preferably in a ratio of 40 to 70 wt%.

[0067] The more MnO2, which is an oxide of Mn, is added, the higher the concentration becomes, and the blackness as a black pigment increases. When the converted weight of MnO2 is less than 25% by weight, a good black color cannot be obtained as with La. When the converted weight of MnO2 exceeds 60% by weight, the amount of raw materials other than MnO2 is reduced, and the quality stability based on other components cannot be maintained. Therefore, MnO2 is preferably 25 to 60% by weight.

[0068] CuO, which is an oxide of Cu, can obtain a good black color together with the oxides of La and Mn. When the converted weight of CuO is less than 0.5 weight %, the color tone other than black increases, and the concentration of the pigment and the feeling of black are difficult to produce. When the converted weight of CuO exceeds 10 weight %, when the use of the black pigment is envisioned from the relationship with other components, the red color will increase and the concentration cannot be obtained. In addition, the melting temperature of the ceramic slurry containing the mixed oxide material rises. Furthermore, the acid resistance will also decrease. Therefore, Cu is added from the balance of various conditions, and CuO is preferably 0.5 to 10 weight %.

[0069] For mixed oxides of La, Mn and Cu (3 main components), and oxides containing Mo as one of the main components (4 main components). With the addition of Mo, the mixed oxide can become a higher quality black pigment. In the mixed oxides of the 4 main components, Mo is measured by the converted weight of MoO3, and relative to the oxide conversion amount of the three oxides La2O3, MnO2 and CuO (the sum of La2O3, MnO2 and CuO) set to 100 weight%, MoO3 is contained in a ratio of less than 5 weight%. When the converted weight of MoO3 exceeds 5 weight%, the concentration of black begins to decrease. Therefore, 5 weight% is the upper limit. The lower limit of the converted weight of MoO3 is not particularly limited. Among them, from the point of view of clarifying the effect of Mo addition, it is preferably 0.01 weight%.

[0070] In the black mixed oxide material having La, Mn and Cu as main components (3 main component groups), or the mixed oxide containing Mo among these (4 main component groups), in addition to the main components, it also selectively contains any one or more of Li, B, Na, Mg, Al, Si, P, K, Ca, Ti, V, Fe, Zn, Sr, Y, Zr, Nb, Sn, Sb, Ba, Ta, W, Bi, Ce, Pr, Nd or Er as subcomponents.

[0071] The contents of the listed accessory components are as follows, relative to the oxide conversion amount taking the total weight of the three oxides La2O3, MnO2 and CuO (the sum of La2O3, MnO2 and CuO) as 100 weight %, in the case of Li2O, B2O3, Na2O, MgO, Al2O3, SiO2, P2O5, K2O, CaO, TiO2, V2O5, Fe3O3, ZnO, SrO, Y2O3, ZrO2, Nb2O3, SnO2, Sb2O3, BaO, Ta2O5, WO3, Bi2O3, CeO2, Pr6O 11 , Nd2O5 or Er2O3 in terms of oxide conversion, is specified to be less than 20 weight %.

[0072] By containing these accessory ingredients, it is expected that the effect of promoting the crystal growth of the mixed oxide generated by the reaction of the oxide of the raw material can be expected. Furthermore, it is also helpful to adjust the sintering temperature, stabilize the color of the pigment, etc. Therefore, the use of extremely high-purity raw materials, special manufacturing management and methods for avoiding the mixing of impurities are also reduced. Therefore, the raw materials and manufacturing costs can be relatively cheap. The practical problem is that it is extremely difficult to exclude the mixing of accessory raw materials during mass production. When the accessory ingredients exceed 20% by weight, it is not preferred because the properties of the desired black pigment are reduced, and the content of the accessory ingredients is as little as possible. However, although the role of the contribution of the accessory ingredients is unclear, as clearly shown in the embodiments described later, there are also examples of improving performance by adding.

[0073] Therefore, using Figure 1 The schematic process diagram of the method for manufacturing the black mixed oxide material of the first embodiment is described. First, an oxide raw material M that satisfies the aforementioned oxide conversion amounts of La, Mn and Cu (which may also contain Mo) is prepared. The oxide raw material M is mixed and crushed to obtain a primary crushed product 11 having an average particle size of less than 5 μm (S11: primary crushing step). The primary crushed product 11 is calcined in an oxidizing atmosphere at 700 to 1200° C. to obtain a raw material calcined product 12 (S12: raw material calcining step). The raw material calcined product 12 is crushed again to an average particle size of less than 50 μm to prepare a mixed oxide P1 of the black mixed oxide material (S13: secondary crushing step).

[0074] Next, use Figure 2 The schematic process diagram of the manufacturing method of the black mixed oxide material of the second embodiment is described. Prepare an oxide raw material M that satisfies the above-mentioned oxide conversion amount of La, Mn and Cu (Mo may be included). The oxide raw material M is mixed and crushed to obtain a first crushed product 21 with an average particle size of less than 5 μm (S21: first crushing step). The first crushed product 21 is fired in an oxidizing atmosphere at 700 to 1200°C to obtain a first sintered product 22 (S22: first sintering step). The first sintered product 22 is crushed to an average particle size of less than 50 μm to obtain a second crushed product 23 (S23: second sintering step). The second crushed product 23 is fired in an oxidizing atmosphere at 60 to 1100°C to obtain a second sintered product 24 (S24: second sintering step). Thereafter, the second sintered product 24 is crushed to an average particle size of less than 5 μm to prepare a mixed oxide P2 of the black mixed oxide material (S25: third crushing step).

[0075] exist Figure 1 and Figure 2In the pulverization (S11, S13, S21, S23, S25) shown in the schematic process diagram, a pulverizing device such as a ball mill, a vibration mill, a grinder, a bead mill, a jet mill, a tube mill, a sprayer, a fine mill, a pulverizer, etc. is used. During pulverization, since mixed pulverization can be performed by wet or dry methods, the productivity is high and the processing cost is also advantageous. For example, the wet mixed pulverization method in a ball mill is described, and oxide raw materials, water, balls and pulverization aids (dispersants, defoamers, etc.) are put into a ball mill for mixed pulverization. Defoamers and dispersants as pulverization aids can be appropriately selected and used. Known substances can be used so that the raw oxides are mixed and pulverized uniformly. In addition, the amount of the oxide raw materials is adjusted according to the oxide raw materials.

[0076] The inner surface of the ball mill is paved with lining materials such as alumina, zirconia, rubber, polyurethane, nylon, and silica. Alumina and zirconia are preferred because they are harder than other lining materials and can reduce the mixing of lining materials into the pigment and shorten the pulverization time.

[0077] The crushing balls used are alumina balls, zirconia balls, porcelain balls, steel balls, etc. In addition, zirconia balls can also be used for polyurethane or nylon linings. Since polyurethane and nylon are carbonized and disappear during firing, there is less possibility of impurities being mixed in. In addition, the particle size of the crushing balls is appropriately changed according to the particle size of the raw material oxide.

[0078] The dispersant as one of the grinding aids is selected from sodium polycarboxylate, sulfonic acid polymer (sodium salt), etc. on the basis of polycarboxylic acid compounds and ammonium polyacrylate and sodium polyacrylate as polyacrylic acid compounds. By appropriately adding the grinding aid, the dispersibility in the raw oxide liquid becomes good, and it can be crushed into small pieces in a shorter time. It is known that the specific gravity of the raw oxide of each main component is different. Therefore, in order to prevent the deviation of the grinding, all components need to be evenly crushed. In particular, ammonium polyacrylate is almost decomposed by calcination, and there is no residual sodium component compared with other grinding aids, so it is preferably used.

[0079] In the pulverization (S11, S13), the average particle size of the raw oxide after pulverization is pulverized to less than 5 μm, further pulverized to less than 2 μm, preferably pulverized to less than 1 μm, and more preferably pulverized to less than 0.7 μm. This is to promote the sintered particle growth of the mixed oxide generated during firing by reducing the average particle size as much as possible. In addition, since the reactivity of the oxide raw material on the side with a smaller average particle size is improved, it is easy to obtain a mixed oxide with a preferred crystal structure. In addition, since the smaller the average particle size, the longer the pulverization time, the average particle size is specified in consideration of the performance required by the pigment, the firing time, etc.

[0080] The “average particle size” in this specification refers to a particle size at which the cumulative value is 50% (cumulative average size) in a particle size distribution determined by a laser diffraction / scattering particle size / particle size distribution measuring apparatus described in the following Examples by a laser diffraction / scattering method.

[0081] The pulverized material obtained by wet grinding is put into a slurry tank and dried by a spray dryer, a filter press (dehydration dryer), a decanter (centrifugal dehydration dryer), etc. The moisture content is 1.0% or less, preferably 0.5% or less. When a filter press, a decanter, etc. are used for drying, it is necessary to dry and grind again. For the convenience of the production method, a spray dryer is preferably used. In addition, the drying process may be omitted depending on the state of the moisture content after the mixed grinding.

[0082] In process Figure 1 , 2 In the pulverization after firing (S13, S23), it is pulverized to an average particle size of less than 50 μm. Of course, the particle size during pulverization can also be finer than 50 μm as needed. In the first embodiment, the pulverization of S13 is finally completed. Therefore, in the pulverization of S13, the average particle size is selected according to the purpose, etc. Figure 2 The pulverization ( S23 ) of the (second embodiment) is adjusted so as to intentionally increase the size of the mixed oxide crystals in consideration of heat exposure during the subsequent sintering.

[0083] In process Figure 2 In the pulverization after firing (S25), it is pulverized to an average particle size of less than 20 μm, and further pulverized to less than 5 to 10 μm, preferably pulverized to an average particle size of 0.5 to 2 μm, and more preferably pulverized to an average particle size of 0.8 to 1 μm. By the pulverization after firing, the average particle size of the black mixed oxide material becomes smaller. As a result, the specific surface area becomes larger, the concentration becomes thicker, and the color tone becomes more uniform, so that a pigment with good reproducibility can be manufactured. In the pulverization after firing, a pulverizing device is used by the same method as the pulverization described above. When ball mill pulverization is performed according to a wet method, drying can be performed by a spray dryer or the like as necessary. In the case where the pigment is agglomerated due to drying, an impact pulverizing device such as a jet mill, a vibration mill, or a hammer mill can be used for pulverization.

[0084] Process Figure 1 , 2The firing of S12, S22, and S24 in the above process is also called calcination. During the firing, the oxide raw material (crushed material) is placed in a box made of mullite, cordierite, alumina, etc. After firing, a mixed oxide is generated from the oxide raw material. Depending on the degree of crystal growth and densification of the mixed oxide, the color tone and concentration of the black mixed oxide material will change. In the case where the black mixed oxide material is a black pigment, the firing temperature and firing time are appropriately selected according to the raw oxides contained, with reference to its use and performance.

[0085] In addition, during the firing (S12, S22) in the manufacturing method of the black mixed oxide material of the first and second embodiments, larger firing devices such as tunnel kilns, roller kilns, rotary kilns, and shuttle kilns are also used for mass production. Generally, when a large firing device is used, the sintering of the oxide raw materials is prone to unevenness. Therefore, by introducing heated air, heated oxygen, etc. into each of the kilns, the firing stage can be placed in an oxidizing atmosphere. Therefore, it is very convenient to manufacture black pigments of a full range of qualities at a low price. In addition, when a rotary kiln is used, the mixed crushed material is directly put into the kiln. Although the firing varies depending on the scale of the firing device and the amount of raw oxides, it is carried out in a temperature range of 700 to 1200°C for 1 to 8 hours. The firing time is the maintenance time of the highest temperature. In order to complete the treatment by one firing, a temperature gradient can also be set in the firing device.

[0086] In the calcination (S24) of the raw material oxide in the manufacturing method of the black mixed oxide material of the second embodiment, an electric furnace is used in addition to a tunnel kiln or the like. Since the temperature control of an electric furnace is easier than that of the above-mentioned kilns, the amount of heat applied to the oxide raw material during calcination can be accurately controlled. For example, when the metal oxide of the raw material is sintered and the crystals of the mixed oxide are grown, it is convenient to adjust the thermal history (heating temperature, heating time) of the raw material. When an electric furnace is used, the oxide raw material and the like are heated in a static state. Therefore, the amount of contact between the raw material and oxygen may become uneven, so oxidation is fully achieved by repeating the calcination twice.

[0087] In the case where the black mixed oxide material is a black pigment, its quality is affected by the crystal structure that develops rapidly during sintering, so in the case of stabilization of the preferred properties, the manufacturing method of the second embodiment is preferably adopted. The first sintering process is carried out at a temperature range of 600 to 1200°C for 1 to 6 hours, and the second sintering process is carried out at a temperature range of 600 to 1100°C for 1 to 4 hours, considering the composition of the oxide raw material provided to the sintering, the sintering performance of the accompanying composition, etc. The time of the first sintering process and the second sintering process is the maintenance time of each highest temperature.

[0088] As can be understood from the description of the main components so far, black mixed oxide materials are independent of the valence of chromium and do not contain chromium itself in the main components. They are very economical and extremely safe. 6+ ), a water washing process is required, but this water washing process can be omitted. In addition, the accompanying drying and crushing processes can also be omitted. Therefore, the manufacturing time can be greatly shortened, and the manufacturing cost can also be greatly reduced. In addition, there is no need to use extremely high-purity and expensive raw materials for the raw material oxides. Since relatively cheap raw materials can be used, it is very beneficial to the raw material cost.

[0089] In addition, since the black mixed oxide material (black pigment) which does not contain chromium and cobalt as main components is a non-magnetic material and an insulating material, hexavalent chromium which is harmful to the environment of use will not be generated. In addition, the incidence of allergies caused by cobalt can be reduced. Examples of the use of this black mixed oxide material include resin pigments, paint pigments, ceramic coloring pigments (including ultraviolet absorption and reflection pigments for automobile window glass, etc.), heat radiation pigments, infrared reflection pigments, colored ceramics, and various other products.

[0090] Regarding the black mixed oxide material described in detail so far, when the black mixed oxide material is a black pigment, it is used as an inorganic glass slurry (black inorganic glass slurry) containing a black mixed oxide material (black pigment) and a glass agent. For example, the inorganic glass slurry is fired on the surface of a glass plate to form a glass plate product. As specific glass plate products, they include window glasses such as the front windshield, rear windshield, and sunroof glass of a car. The inorganic glass slurry is applied to the surface of these glasses. The inorganic glass slurry protects the adhesive and buffer resin body between the above-mentioned glass plate product and the car body from ultraviolet rays, and avoids aging of the adhesive and buffer resin body. Of course, in addition to automobiles, inorganic glass slurry is also used for glass windows (glass plate products) of various transportation machinery such as heavy machinery, ships, and airplanes, and is also used for glass plate products for display screens. In addition, it can also be used for painting and coating of metal surfaces. In addition, it is also possible to paint on pottery or porcelain products and process cloisonné.

[0091] Regarding the composition of the inorganic glass paste, as disclosed in the Japanese Patent Gazette No. 2002-20140 and the Patent Gazette No. 4035673, the main component is glass composed of SiO2, B2O3, ZnO, TiO2, Li2O, Na2O, K2O, ZrO2, etc. The glass is crushed to 0.1 to 30 μm in advance, preferably to an average particle size of 0.5 to 20 μm, and is finely processed into a powder. A thermally decomposable resin such as cellulose resin and acrylic resin, a high-boiling point solvent grease such as pine oil, the aforementioned black mixed oxide material (black pigment), and other inorganic fillers are added thereto, and the mixture is fully kneaded and finely processed into a slurry.

[0092] The generated inorganic glass slurry containing a black mixed oxide material (black pigment) is applied to, for example, the edge of a glass plate cut out in an appropriate shape. The inorganic glass slurry can be applied to the surface of the glass plate by screen printing, spray coating, roller coating, etc. Among them, screen printing is relatively simple. The glass plate coated with the inorganic glass slurry is fixed to the surface of the glass plate by firing after drying.

[0093] The molding of the window glass for automobiles adopts a method of bending the glass plate between molds in a furnace, and a method of vacuuming the glass plate to the mold in the furnace and bending it. The molding of the glass plate is connected by a tunnel kiln for preheating from room temperature to about 660°C and an intermittent furnace for bending molding at 640-720°C, and the processing is carried out in the process of passing through these two furnaces. The inorganic glass slurry is fired on the surface of the glass plate in the preheating stage. Therefore, in the molding from plate-shaped glass, a glass plate product coated with inorganic glass slurry on an aspherical surface such as window glass can be obtained.

[0094] Instead of the aforementioned glass agent, a black mixed oxide material can be added to the ceramic agent to obtain an inorganic ceramic material. As the ceramic agent, for example, known ceramic materials such as aluminum oxide, partially stabilized zirconium oxide, and stabilized zirconium oxide are used. The components contained in the partially stabilized zirconium oxide and stabilized zirconium oxide are calcium oxide, magnesium oxide, cesium oxide, aluminum oxide, or yttrium oxide. This results in a black ceramic material.

[0095] In addition, a resin agent can be added to the black mixed oxide material to prepare a resin slurry. This resin slurry is coated on the surface of a support such as glass, metal, pottery, porcelain, resin products or carbon materials. As a result, black colors and patterns can be drawn on the surface of the listed support. The usage is the same as that of general black pigments.

[0096] Furthermore, by mixing the black mixed oxide material and the resin agent, a resin containing a black mixed oxide material can also be prepared. This is so-called coloring of the resin. The degree of blackness of the resin product is adjusted according to the amount added. In addition, the color tone of the resin can also be controlled by adding a transparent resin. The resin used for the resin slurry and the resin containing a black mixed oxide material is a well-known resin such as a thermoplastic resin and a thermosetting resin, and is not particularly limited. It is appropriately selected in consideration of the purpose, place of use, durability, etc. of the product. The resin containing a black mixed oxide material is processed into particles and used as a raw material for molded products such as injection molding and extrusion molding. As described above, the black pigment of the present invention, as a mixed oxide material that contains neither chromium nor cobalt, can replace the existing black material.

[0097] It has been described so far that the mixed oxide further has the function of being a non-magnetic material. Therefore, the mixed oxide can be a black mixed oxide material with a non-magnetic function. The mixed oxide is preferably used for avoiding excitation and shielding magnetic forces by having non-magnetic properties. For example, it is envisioned to be used for the protection of electronic components and the like. In addition, the mixed oxide itself also exhibits black color, so the product application is also wide.

[0098] In addition, the mixed oxide further has the function of being an insulating material. Therefore, the mixed oxide can be used as a black mixed oxide material with an insulating function. The mixed oxide is expected to have an electrical shielding effect by having insulating properties. For example, it is envisioned to be used for the protection of electronic components, etc. In addition, the mixed oxide itself also presents black, so the product application is also wide.

[0099] Example

[0100] [Raw materials used]

[0101] In the preparation of the black mixed oxide material of each sample preparation example, "La2O3, Mn3O4, CuO" were used as raw materials for the three main components of La, Mn and Cu. "MoO3" was used for Mo. "FeOOH, MgO, Al2O3, SiO2, CaCO3, V2O5, ZnO, SrCO3, Y2O3, ZrO2, BaCO3, Ta2O5, Bi2O3, CeO2, Pr6O 11 , Nd2O5".

[0102] [Preparation of black mixed oxide material (I)]

[0103] according to Figure 2The manufacturing method of the second embodiment disclosed herein produces black pigments (three main component types) of Sample Preparation Examples 1 to 25 while changing the mixing ratio of La, Mn and Cu in the mixed oxide. The following Tables 1 to 5 show the relative weight ratio (weight %) of each component.

[0104] The raw materials prepared according to the formulation of each sample preparation example were placed in a ball mill and mixed / crushed. The formulation in the mixed crushing was 100 parts by weight of the total weight of each raw material oxide, 300 parts by weight of steel balls (diameter 2 to 5 mm), 150 parts by weight of water, and 0.5 to 2 parts by weight of a water reducing agent (ammonium polyacrylate, manufactured by Toagosei Co., Ltd.: "A-6114") relative to 100 parts by weight of the total weight of each raw material oxide. The mixed crushing was carried out in a ball mill for 15 to 20 hours to obtain a mixed crushed product.

[0105] After the mixed pulverized material is dried at a hot air temperature of 280°C by a spray dryer, it is calcined at about 1000°C for 2 to 3 hours (first calcination) through a tunnel kiln. After the first calcination, dry pulverization is performed using a sprayer to an average particle size of 20 to 30 μm. Next, it is calcined at about 900°C for 2 to 3 hours (second calcination) through a tunnel kiln, and dry pulverized using a fine grinder and steel balls (diameter 2 to 5 mm) to an average particle size of 1 to 1.2 μm. After a series of operations, the black mixed oxide material (i.e., equivalent to black pigment, non-magnetic material, insulating material) of each sample preparation example is obtained. When making the sample preparation examples, the average particle size is measured after each pulverization using a laser diffraction / scattering particle size distribution measuring device (manufactured by Horiba, Ltd.: "LA-920").

[0106] [Evaluation of blackness]

[0107] The black mixed oxide material of each sample preparation example produced by the aforementioned process was placed in an alumina ring with an inner diameter of 40 mm and a thickness of 5 mm and pressed. In addition, a flat cylindrical measuring block was obtained. A colorless and transparent glass plate was placed on the measuring block, and the glass plate was contacted with a colorimeter (manufactured by Konica Minolta, Inc.: "CR-3500d") to measure the blackness (L value) of the L*a*b* colorimetric system (according to JIS-Z-8729). The measurement was performed with regular reflection treatment (SEC method: removing regular reflected light). When evaluating whether the blackness is qualified or not, the sample preparation examples with an "L value" of less than 25.0 are qualified products and are evaluated as "A", and the sample preparation examples exceeding 25.0 are evaluated as insufficient "F".

[0108] Tables 1 to 5 record the weight % of "La2O3, Mn3O4 and CuO" of the three main components of La, Mn and Cu, "L value, a value and b value", the first sintering temperature and the second sintering temperature (°C), the final average particle size (μm), and the pass / fail evaluation (A or F).

[0109] [Table 1]

[0110] Sample Preparation Example No. Sample Preparation Example 1 Sample Preparation Example 2 Sample Preparation Example 3 Sample Preparation Example 4 Sample Preparation Example 5 <![CDATA[La2O3 (wt%)]]> 55 56 57 59 39 <![CDATA[Mn3O4 (wt%)]]> 42 41 40 38 60 CuO (wt%) 3 3 3 3 1 Total (weight %) 100 100 100 100 100 L value 19.31 19.77 20.66 19.67 18.70 a value -0.01 0.08 0.08 0.06 0.08 b-value -1.74 -1.22 -1.63 -1.83 0.32 First sintering temperature (℃) 1000 1000 1000 1000 1000 Second sintering temperature (℃) 900 900 900 900 900 Final average particle size (μm) 1.11 1.08 1.07 1.10 1.01 Pass or fail evaluation A A A A A

[0111] [Table 2]

[0112] Sample Preparation Example No. Sample Preparation Example 6 Sample Preparation Example 7 Sample Preparation Example 8 Sample Preparation Example 9 Sample Preparation Example 10 <![CDATA[La2O3 (wt%)]]> 36 40 45 52 59 <![CDATA[Mn3O4 (wt%)]]> 57 50 50 42 32 CuO (wt%) 7 10 5 6 9 Total (weight %) 100 100 100 100 100 L value 18.70 19.01 19.19 19.33 19.72 a value 0.72 0.18 0.03 -0.05 0.14 b-value 0.29 0.01 -0.13 -0.39 -1.33 First sintering temperature (℃) 1000 1000 1000 1000 1000 Second sintering temperature (℃) 900 900 900 900 900 Final average particle size (μm) 1.02 1.03 1.10 1.09 1.04 Pass or fail evaluation A A A A A

[0113] [Table 3]

[0114] Sample Preparation Example No. Sample Preparation Example 11 Sample Preparation Example 12 Sample Preparation Example 13 Sample Preparation Example 14 Sample Preparation Example 15 <![CDATA[La2O3 (wt%)]]> 65 63 67 68 36 <![CDATA[Mn3O4 (wt%)]]> 27 32 31 27 61 CuO (wt%) 8 5 2 5 3 Total (weight %) 100 100 100 100 100 L value 19.99 20.48 20.51 20.53 25.11 a value 0.22 0.77 0.75 0.03 0.82 b-value -1.11 -1.02 -1.63 0.50 0.33 First sintering temperature (℃) 1000 1000 1000 1000 1000 Second sintering temperature (℃) 900 900 900 900 900 Final average particle size (μm) 1.12 1.10 1.09 1.13 1.05 Pass or fail evaluation A A A A F

[0115] [Table 4]

[0116] Sample Preparation Example No. Sample Preparation Example 16 Sample Preparation Example 17 Sample Preparation Example 18 Sample Preparation Example 19 Sample Preparation Example 20 <![CDATA[La2O3 (wt%)]]> 34 36 43 46 53 <![CDATA[Mn3O4 (wt%)]]> 58 51 42 43 36 CuO (wt%) 8 13 15 11 11 Total (weight %) 100 100 100 100 100 L value 25.15 25.21 25.29 25.11 25.22 a value 0.84 0.80 0.73 0.42 0.33 b-value 0.42 0.21 0.52 0.36 0.52 First sintering temperature (℃) 1000 1000 1000 1000 1000 Second sintering temperature (℃) 900 900 900 900 900 Final average particle size (μm) 1.03 1.11 1.12 1.05 1.05 Pass or fail evaluation F F F F F

[0117] [Table 5]

[0118] Sample Preparation Example No. Sample Preparation Example 21 Sample Preparation Example 22 Sample Preparation Example 23 Sample Preparation Example 24 Sample Preparation Example 25 <![CDATA[La2O3 (wt%)]]> 58 67 72 47 63 <![CDATA[Mn3O4 (wt%)]]> 29 23 23 53 37 CuO (wt%) 13 10 5 0 0 Total (weight %) 100 100 100 100 100 L value 25.28 25.35 25.31 25.09 25.13 a value 0.24 0.21 0.21 0.81 0.82 b-value 0.54 0.52 0.51 0.03 0.05 First sintering temperature (℃) 1000 1000 1000 1000 1000 Second sintering temperature (℃) 900 900 900 900 900 Final average particle size (μm) 1.08 1.07 1.10 1.03 1.01 Pass or fail evaluation F F F F F

[0119] [Results and Investigation of Preparation of Black Mixed Oxide Material (I)]

[0120] The results of the black mixed oxide materials (three main components) of Sample Preparation Examples 1 to 25 prepared by changing the mixing ratio of La, Mn and Cu in the mixed oxide are shown in Tables 1 to 5. Sample Preparation Examples 1 to 14 are evaluated as good in blackness (A). Sample Preparation Examples 15 to 25 are evaluated as insufficient (F). In addition, the weight % of La2O3, Mn3O4 and CuO in Sample Preparation Examples 1 to 25 are plotted in a triangular graph. Figure 3 is the overall triangle diagram, Figure 4 is an enlarged view of the main part. The numbers enclosed in brackets in the triangle diagram are the numbers of the sample preparation examples. Figure 4 As described in detail in , the pass / fail evaluation of blackness was superimposed on the plot positions of the three main component groups of the sample preparation example. And the area surrounded by the blending ratio (weight %) based on the pass / fail evaluation was obtained.

[0121] Figure 4The gray part in is the preferred area of ​​the black mixed oxide material (3 main component classifications) of the mixed oxide of La, Mn and Cu. Specifically, with regard to La (La2O3), sample preparation example 16 is less, and sample preparation example 23 is more. With regard to Mn (MnO2), sample preparation examples 22 and 23 are less, and sample preparation example 15 is more. With regard to Cu (CuO), sample preparation examples 24 and 25 are less, and sample preparation examples 17 to 21 are more. The switching boundaries of these pass / fail evaluations can be considered as the limits of matching. Therefore, in the oxide conversion amount with the total weight set to 100 weight%, the area surrounded by the range of La2O3 set to 35 to 70 weight%, the range of MnO2 set to 25 to 60 weight%, and the range of CuO set to 0.5 to 10 weight% is derived as the best.

[0122] [Preparation of black mixed oxide materials (II)]

[0123] According to the preparation of the black mixed oxide material (I) described above, the appropriate proportion of each component in the three main component types of black mixed oxide materials was found. Secondly, Mo was added to the three main component types of black mixed oxide materials to prepare four main component types of black mixed oxide materials. At the same time, the pass / fail evaluation of the blackness was attempted. As the formulation of sample preparation examples 26 to 34 in Tables 6 and 7, the formulation of Mo was increased successively, and the blackness was measured. In order to easily grasp the formulation amount of Mo (MoO3), the total of the three components was taken as 100 weight%, and MoO3 was formulated based on the 100 weight%. The preparation method of the black mixed oxide materials of sample preparation examples 26 to 34 was carried out under the same conditions as the preparation of the black mixed oxide material (I) described above. In addition, the pass / fail evaluation of the blackness was also set to the same standard as the above preparation (I).

[0124] [Table 6]

[0125] Sample Preparation Example No. Sample Preparation Example 26 Sample Preparation Example 27 Sample Preparation Example 28 Sample Preparation Example 29 Sample Preparation Example 30 <![CDATA[La2O3 (wt%)]]> 57 57 57 57 56 <![CDATA[Mn3O4 (wt%)]]> 40 40 40 40 39 CuO (wt%) 3 3 3 3 3 Total of 3 ingredients (weight %) 100 100 100 100 100 <![CDATA[MoO3 (wt%)]]> 0.01 0.1 0.5 1 2 Total of 4 ingredients (weight %) 100.01 100.1 100.5 101 102 L value 25.00 23.93 22.07 20.77 20.75 a value 0.09 0.09 -0.06 -0.04 -0.03 b-value -1.63 -1.65 -1.67 -1.68 -1.67 First sintering temperature (℃) 1000 1000 1000 1000 1000 Second sintering temperature (℃) 900 900 900 900 900 Final average particle size (μm) 1.04 1.05 1.01 1.02 1.04 Pass or fail evaluation A A A A A

[0126] [Table 7]

[0127] Sample Preparation Example No. Sample Preparation Example 31 Sample Preparation Example 32 Sample Preparation Example 33 Sample Preparation Example 34 <![CDATA[La2O3 (wt%)]]> 55 54 54 53 <![CDATA[Mn3O4 (wt%)]]> 39 38 37 37 CuO (wt%) 3 3 3 3 Total of 3 ingredients (weight %) 100 100 100 100 <![CDATA[MoO3 (wt%)]]> 3 5 6 7 Total of 4 ingredients (weight %) 103 105 106 107 L value 20.75 20.71 25.20 25.97 a value -0.01 -0.01 0.31 0.39 b-value -1.65 -1.59 -1.56 0.49 First sintering temperature (℃) 1000 1000 1000 1000 Second sintering temperature (℃) 900 900 900 900 Final average particle size (μm) 1.10 1.06 1.07 1.03 Pass or fail evaluation A A F F

[0128] [Production of black mixed oxide material (II) Results and investigation]

[0129] Regarding sample preparation examples 26 to 34, the compositions of the three main component classes in the previous stage of adding Mo (MoO3) are the same as those of the aforementioned sample preparation example 3. The tendency of the blackness (L value) after sample preparation example 26 is that the blackness increases in proportion to the amount of Mo (MoO3) added. However, with sample preparation example 32 as the boundary, the reduction in blackness becomes significant after sample preparation example 33. Based on this result, it is concluded that when preparing the black mixed oxide material of the four main component classes, La is calculated as La2O3, Mn is calculated as MnO2, and Cu is calculated as CuO, and the total weight of these three oxides is set to 100 weight % of the oxide conversion amount. It is desirable to contain Mo in the form of MoO3 at a ratio of 5 weight % or less relative to 100 weight % of the oxide conversion amount. In addition, regarding the lower limit of the converted weight of Mo, 0.01 weight % is appropriate from the perspective of clarifying the effect of Mo addition.

[0130] [Preparation of black mixed oxide materials (III)]

[0131] Regarding the auxiliary components that can be incorporated into the mixed oxide of the black mixed oxide material and their incorporation ratio, sample preparation examples 35 to 58 were prepared, and the blackness was measured and verified. The preparation method of the black mixed oxide material of sample preparation examples 35 to 58 was carried out under the same conditions as the preparation (I) of the aforementioned black mixed oxide material. In addition, the pass or fail evaluation of the blackness was also set to the same standard as the above preparation (I). In order to easily grasp the amount of auxiliary components incorporated, the total of the three components was taken as 100 weight%, and the auxiliary components (the converted amount of the aforementioned oxides) were incorporated based on this 100 weight%. The results are shown in Tables 8 to 12.

[0132] [Table 8]

[0133]

[0134] [Table 9]

[0135]

[0136] [Table 10]

[0137]

[0138] [Table 11]

[0139]

[0140] [Table 12]

[0141]

[0142] [Production of black mixed oxide material (III) Results and investigation]

[0143] Regarding the types of auxiliary components, they can be matched according to the results of sample preparation examples 35 to 50 shown in the table. It was confirmed that although there are deviations for each type, they generally contribute to the reduction of blackness (L value). Even if the amount of auxiliary components in sample preparation examples 49 and 58 is expanded to 20% by weight, sufficient blackness can be obtained. Of course, the amount of auxiliary components (oxide conversion amount) can be further expanded to more than 20% by weight. However, there is a concern that excessive increase in the amount of auxiliary components will affect the color of blackness. In addition, the influence on the reduction of the purity of the mixed oxide, the crystal structure of the mixed oxide, and the stability of the black mixed oxide material when used as a black pigment cannot be ignored. Therefore, according to the results of the sample preparation example, as a preliminary benchmark, La is calculated as La2O3, Mn is calculated as MnO2, and Cu is calculated as CuO, and the total weight of these three oxides is set to 100% by weight. In the oxide conversion amount, relative to 100% by weight of the oxide conversion amount, the amount of auxiliary components (oxide conversion amount) is specified to be less than 20% by weight.

[0144] [Preparation of black mixed oxide materials (IV)]

[0145] Instead of the manufacturing method of the second embodiment described so far, according to a simpler Figure 1 The black mixed oxide materials of Sample Preparation Examples 59 to 63 were prepared by the production method of the first embodiment disclosed in , and the evaluation of the degree of blackness was attempted. Table 13 shows the relative weight ratios (weight %) of the components.

[0146] The raw materials prepared according to the formulation of each sample preparation example are put into a ball mill and mixed / crushed. Regarding the formulation in the mixed crushing, the total weight of each raw material oxide is 100 parts by weight, steel balls (diameter 2 to 5 mm) are 300 parts by weight, and water is 150 parts by weight. In addition, the water reducer (ammonium polyacrylate, manufactured by Toagosei Co., Ltd.: "A-6114") is set to 0.5 to 2 parts by weight relative to the total weight of 100 parts by weight of each raw material oxide. Mixed crushing is carried out in a ball mill for 15 to 20 hours to obtain a mixed crushed product. The mixed crushed product is dried at a hot air temperature of 280°C by a spray dryer, and then sintered at about 1000°C for 2 to 3 hours in a tunnel kiln. After sintering, dry crushing is carried out using a pulse laser to an average particle size of 8 to 20μm, and particles below 2μm are classified. From a series of operations, the black mixed oxide material of each sample preparation example is obtained.

[0147] [Table 13]

[0148] Sample Preparation Example No. Sample Preparation Example 59 Sample Preparation Example 60 Sample Preparation Example 61 Sample Preparation Example 62 Sample Preparation Example 63 <![CDATA[La2O3 (wt%)]]> 55 56 57 59 40 <![CDATA[Mn3O4 (wt%)]]> 42 41 40 38 50 CuO (wt%) 3 3 3 3 10 Total (weight %) 100 100 100 100 100 L value 19.02 19.51 20.03 19.15 18.07 a value 0.08 0.16 0.18 0.17 0.29 b-value -1.53 -0.83 -1.19 -1.23 0.36 Firing temperature (℃) 1000 1000 1000 1000 1000 Final average particle size (μm) 1.01 0.97 1.05 1.10 1.03 Pass or fail evaluation A A A A A

[0149] [Results and investigation of preparation of black mixed oxide material (IV)]

[0150] In each sample preparation example according to the manufacturing method of the first embodiment, sufficient blackness (L value) was also confirmed. Sample preparation examples 59, 60, 61, 62, and 63 have the same composition of the three main component classes as the aforementioned sample preparation examples 1, 2, 3, 4, and 7, and only the manufacturing method is changed. According to mutual comparison, it is found that the increase in the number of firings leads to a decrease in the L value and an increase in the blackness. Therefore, any one of the manufacturing methods can be selected from the combination of the quality required for the use when the black mixed oxide material is used as a black pigment and the manufacturing cost.

[0151] [Structural analysis of black mixed oxide materials]

[0152] X-ray diffraction (XRD) measurement was attempted for the black mixed oxide material of the sample preparation example. An X-ray diffraction device "X'Pert 3 Powder”, X-ray source: CuKα ray. Figure 5 It is sample preparation example 29 (4 main component categories), Figure 6 This is sample preparation example 35 (Mo and auxiliary components are combined), Figure 7 This is the X-ray diffraction pattern of the black mixed oxide material of Sample Preparation Example 51 (Mo and auxiliary components are combined). In the diffraction pattern of any figure, there is a diffraction peak with the maximum intensity in the range of 31° to 34° of the diffraction angle 2θ. In addition, it is speculated that the phase containing the perovskite structure having a rhombohedral crystal system (space group R3-c) is the main phase. In addition, based on the blackened positions of the four corners in the illustrated pattern, it is also assumed that the mixed oxide contains Mn3O4 having a spinel structure as the oxide of Mn.

[0153] The phase of the perovskite in the black mixed oxide material of the sample preparation example can be given a Miller index (Miller plane index) corresponding to a hexagonal unit lattice with a lattice constant of a=b<c. Specifically, it is (012) plane, (110) plane, (104) plane, (113) plane, (202) plane, (006) plane, (024) plane, (122) plane, (116) plane, (030) plane, (214) plane, (018) plane, etc. (see the figure). In addition, with respect to Figure 5 Sample preparation example 29, lattice constants a = 0.552nm, c = 1.33nm.

[0154] [Study on Firing Temperature]

[0155] The optimum sintering temperature for the preparation of the black mixed oxide material was tested while changing the temperature. Sample preparation examples 64 to 71 in Tables 14 and 15 were prepared according to the preparation method of the black mixed oxide material preparation (IV) described above (see Figure 1 The first embodiment of the present invention) was prepared based on the relative weight ratio (weight %) of each component in the table. After preparation, the L value and the like were measured.

[0156] [Table 14]

[0157] Sample Preparation Example No. Sample Preparation Example 64 Sample Preparation Example 65 Sample Preparation Example 66 Sample Preparation Example 67 <![CDATA[La2O3 (wt%)]]> 57 57 57 57 <![CDATA[Mn3O4 (wt%)]]> 40 40 40 40 CuO (wt%) 3 3 3 3 Total of 3 ingredients (weight %) 100 100 100 100 <![CDATA[MoO3 (wt%)]]> 1 1 1 1 Subcomponents (wt%) FeOOH 3 3 3 3 <![CDATA[SiO2]]> 1 1 1 1 Total of auxiliary components (weight %) 4 4 4 4 Total (weight %) 105 105 105 105 L value 38.22 24.89 23.11 22.67 a value 9.79 5.34 3.38 2.41 b-value 9.89 4.41 3.38 2.15 Firing temperature (℃) 650 700 800 900 Final average particle size (μm) 0.99 1.02 1.06 1.09 Pass or fail evaluation F A A A

[0158] [Table 15]

[0159] Sample Preparation Example No. Sample Preparation Example 68 Sample Preparation Example 69 Sample Preparation Example 70 Sample Preparation Example 71 <![CDATA[La2O3 (wt%)]]> 57 57 57 57 <![CDATA[Mn3O4 (wt%)]]> 40 40 40 40 CuO (wt%) 3 3 3 3 Total of 3 ingredients (weight %) 100 100 100 100 <![CDATA[MoO3 (wt%)]]> 1 1 1 1 Subcomponents (wt%) FeOOH 3 3 3 3 <![CDATA[SiO2]]> 1 1 1 1 Total of auxiliary components (weight %) 4 4 4 4 Total (weight %) 105 105 105 105 L value 22.06 22.47 23.96 25.36 a value 2.18 0.42 0.45 0.45 b-value -1.03 2.41 2.73 2.99 Firing temperature (℃) 1000 1100 1200 1250 Final average particle size (μm) 1.06 1.06 1.02 1.05 Pass or fail evaluation A A A F

[0160] From the results of Tables 14 and 15, it can be seen that at the firing temperature of 650°C in Sample Preparation Example 64, the L value was significantly poor. It can be considered that the sintering was insufficient and no crystal structure was produced. In contrast, at the firing temperature of 700°C in Sample Preparation Example 65, the L value improved significantly. Between the firing temperature of 1200°C in Sample Preparation Example 70 and the firing temperature of 1250°C in Sample Preparation Example 71, the L value increased. Therefore, when the conditions for obtaining good black (L value below 25) as the pigment use are divided, the firing temperature can be derived as a range of 700 to 1200°C.

[0161] Furthermore, according to the preparation of the black mixed oxide material containing the auxiliary component (III) (refer to Figure 2 According to the second embodiment of the present invention, black mixed oxide materials of sample preparation examples 72 to 79 in Tables 16 and 17 were prepared. After the preparation, the L value and the like were measured.

[0162] [Table 16]

[0163] Sample Preparation Example No. Sample Preparation Example 72 Sample Preparation Example 73 Sample Preparation Example 74 Sample Preparation Example 75 <![CDATA[La2O3 (wt%)]]> 57 57 57 57 <![CDATA[Mn3O4 (wt%)]]> 40 40 40 40 CuO (wt%) 3 3 3 3 Total of 3 ingredients (weight %) 100 100 100 100 <![CDATA[MoO3 (wt%)]]> 1 1 1 1 Subcomponents (wt%) FeOOH 3 3 3 3 <![CDATA[SiO2]]> 1 1 1 1 Total of auxiliary components (weight %) 4 4 4 4 Total (weight %) 105 105 105 105 L value 33.29 31.36 30.11 28.29 a value 9.62 0.36 5.27 3.20 b-value 9.78 9.71 5.04 3.20 First sintering temperature (℃) 650 650 650 650 Second sintering temperature (℃) 550 600 700 800 Final average particle size (μm) 0.98 0.99 0.97 1.01 Pass or fail evaluation F F F F

[0164] [Table 17]

[0165] Sample Preparation Example No. Sample Preparation Example 76 Sample Preparation Example 77 Sample Preparation Example 78 Sample Preparation Example 79 <![CDATA[La2O3 (wt%)]]> 57 57 57 57 <![CDATA[Mn3O4 (wt%)]]> 40 40 40 40 CuO (wt%) 3 3 3 3 Total of 3 ingredients (weight %) 100 100 100 100 <![CDATA[MoO3 (wt%)]]> 1 1 1 1 Subcomponents (wt%) FeOOH 3 3 3 3 <![CDATA[SiO2]]> 1 1 1 1 Total of auxiliary components (weight %) 4 4 4 4 Total (weight %) 105 105 105 105 L value 22.33 22.08 23.31 25.09 a value 0.06 0.03 0.08 0.02 b-value 1.07 0.03 0.01 -0.09 First sintering temperature (℃) 1100 1100 1100 1100 Second sintering temperature (℃) 700 800 1000 1150 Final average particle size (μm) 1.01 0.99 1.03 1.09 Pass or fail evaluation A A A F

[0166] As shown in Sample Preparation Examples 72 to 75, in the case where the first firing temperature was lower than 700°C, the L value was significantly poor. This tendency is the same as that of Sample Preparation Example 64. Next, according to Sample Preparation Example 79, even if the first and second firing temperatures were below 1200°C, when the second firing temperature was set to a higher temperature than the first firing temperature, an increase in the L value was confirmed. Therefore, in the manufacturing method of double firing according to the second embodiment, it can be said that it is desirable to set the initial first firing temperature to the range of 700 to 1200°C and the subsequent second firing temperature to the range of 600 to 1100°C.

[0167] [Application of black mixed oxide materials]

[0168] 〈1. Inorganic glass paste〉

[0169] A glass color composition powder is prepared by mixing 25 parts by weight of the black mixed oxide material (black pigment) of Sample Preparation Example 29 and 75 parts by weight of glass powder. 30 parts by weight of an additional oil component is added to 100 parts by weight of the glass color composition powder, and the mixture is kneaded and finished into a slurry state using a three-roll kneader. The additional oil component is composed of 93 parts by weight of pine oil, 4 parts by weight of ethyl cellulose (manufactured by The Dow Chemical Company), and 3 parts by weight of isobutyl methacrylate resin (manufactured by Lucite Japan Co., Ltd.: "ELVACITE#2045"). The composition (indicated by the amount of the mixture) of the aforementioned glass powder is shown below. The average particle size of the glass powder is 3.3 μm.

[0170] [Table 18]

[0171] Glass powder (relative proportion)

[0172] composition weight% <![CDATA[SiO2]]> 45 ZnO 28 <![CDATA[B2O3]]> 8 <![CDATA[Na2O]]> 4 <![CDATA[Li2O]]> 4 F 2 <![CDATA[TiO2]]> 6 <![CDATA[ZrO2]]> 3 total 100

[0173] The prepared black inorganic glass paste was screen-printed on a 37 mm × 50 mm glass plate using a 180 mesh polyester fiber cloth. After drying, it was placed in an electric furnace set at 680° C. and fired for 4 minutes. In this way, the inorganic glass paste (black inorganic glass paste) was fired on the surface of the support of the glass plate to obtain a sintered product.

[0174] 〈2. Resin slurry〉

[0175] 99 parts by weight of polypropylene were heated and melted to 160 degrees, and 4 parts by weight of the black mixed oxide material (black pigment) of Sample Preparation Example 36 were added thereto and kneaded until the whole became uniform, and the resin slurry (black resin slurry) was used. The resin slurry was coated on the surface of the support of the glass plate. A scraper coater was used for coating. Then, the resin was allowed to stand at room temperature to solidify, thereby obtaining a black resin and a coated product thereof.

[0176] 〈3. Inorganic ceramic materials〉

[0177] As a ceramic agent, 5 parts by weight of the black mixed oxide material (black pigment) of Sample Preparation Example 51 is added to 95 parts by weight of yttria partially stabilized zirconium oxide to make 100 parts by weight of an inorganic mixture. 100 parts by weight of the inorganic mixture, 300 parts by weight of zirconium oxide balls (diameter 3 to 10 mm), and 150 parts by weight of water are put into a ball mill for 20 hours of mixed pulverization to obtain a mixed pulverized product. An organic binder of acrylic resin is added to the mixed pulverized product, and the mixed pulverized product is dried by spraying. The dried mixed pulverized product is extruded into a molded body, and the molded body is moved into an electric furnace and fired at 1500°C for 2 hours to sinter the whole. After cooling, the molded body is taken out from the electric furnace, and ground and polished appropriately to obtain an inorganic ceramic material (black inorganic ceramic material) of a sintered body.

[0178] As shown in the application results of the black mixed oxide material, for the three types of black mixed oxide materials used as black pigments, various products showing good black can be obtained. In particular, the particle size is small, so the application range is wide. Therefore, it can be used in the same way as the existing black pigment. For example, inorganic glass slurry (black inorganic glass slurry) is used for coating window glass of vehicles, etc. Resin slurry (black resin slurry) can be used for all resin processed products that are colored in existing black. It is envisioned that various molded products that are currently widely manufactured. Furthermore, inorganic ceramic materials (black inorganic ceramic materials) can also be expanded, so it can be expected to manufacture ceramic processed products that show black other than glass.

[0179] [Non-magnetic measurements / results]

[0180] In order to further investigate the properties of the black mixed oxide material, the inventors attempted to measure the magnetism. Using the aforementioned black mixed oxide material "Sample Preparation Example 51", the saturation magnetization [Ms] (emu / g), residual magnetization [Mr] (emu / g), and holding force [Hc] (Oe) were measured to obtain the weight magnetic susceptibility (emu / (g·Oe)).

[0181] The measuring device used was a vibrating sample type magnetometer (manufactured by Toei Industry Co., Ltd., VSM-5 model), the measuring temperature was room temperature, the magnetic field range was 10 kOe, and the sample weight was 163.66 mg. When measuring the saturation magnetization, the applied magnetic field was set to a value in 10 kOe. Table 19 shows the results of each measurement value. In addition, Figure 8 , Fig. 9 Also shown is a graph of a magnetization curve with magnetic field (Oe) as the X-axis and magnetization (emu / g) as the Y-axis. Fig. 9 The chart is enlarged Figure 8 of charts.

[0182] [Table 19]

[0183] [Magnetic properties]

[0184] project unit result Saturation magnetization Ms emu / g 1.24 Residual magnetization Mr emu / g <![CDATA[3.9×10 -3 ]]> Holding force Hc Oe <![CDATA[3.6×10 1 ]]> Gravimetric susceptibility emu / (g·Oe) <![CDATA[1.24×10 -4 ]]>

[0185] According to Table 19, Figure 8 and Fig. 9 It is confirmed that the black mixed oxide material is not easy to be magnetic. Therefore, it can be considered that the black mixed oxide material is suitable for magnetic shielding purposes. For example, the coating of electronic components, etc. Considering the reduction of the influence of external magnetic fields on electronic substrates, processors, etc., it is effective to suppress malfunctions, etc.

[0186] [Measurement and results of insulation properties]

[0187] Next, the inventors attempted to measure the insulation properties as a property of the black mixed oxide material. An aluminum ring with an inner diameter of 31 mm, an outer diameter of 38 mm, and a thickness of 5 mm was prepared. 7 g of the aforementioned black mixed oxide material "Sample Preparation Example 51" was loaded inside the inner diameter of the above ring. It was punched from the top and bottom directions, and the sample was granulated and used as a test piece. Secondly, a silicone rubber plate with the same thickness as the aforementioned ring was prepared for the purpose of insulation. A hole with the same outer diameter of 38 mm as the aforementioned ring was opened on the silicone rubber plate, overlapping and covering the surroundings of the aluminum ring. In addition, two stainless steel plates were prepared, and the ring, test piece and silicone rubber plate were sandwiched between the two steel plates. The lower stainless steel plate is connected to the negative electrode, and the upper stainless steel plate is connected to the positive electrode and electricity is passed through.

[0188] That is, the evaluation of insulation is to measure the applied voltage at the moment when insulation breakdown occurs. The result of power-on is that the insulation breakdown is "8.8kV". Converting it to every 1mm is "1.76kV / mm". Based on this value, the insulation of the mixed oxide material is confirmed. Therefore, from the perspective of insulation performance, the black mixed oxide material is used, for example, as a coating or frame of electronic components. Considering the combination with the above-mentioned difficult magnetization property, it reduces the impact on electronic substrates, processors, etc., and effectively suppresses erroneous operations.

[0189] Based on a series of measurement processes, black mixed oxide materials have the performance of non-magnetic materials and insulating materials in terms of magnetic shielding and insulation performance in addition to their use as black pigments. In addition, black mixed oxide materials can be easily mixed into ceramic agents, glass agents, and resin agents, so they can flexibly respond to the expansion of various products.

[0190] Industrial Applicability

[0191] Since the black mixed oxide material of the present invention is independent of the valence of chromium, does not contain chromium itself in the main component, and does not contain cobalt in the main component, it has high safety, good color tone and economy, and also has non-magnetic and insulating properties. Therefore, it can replace the existing black pigment and also achieve magnetic shielding and insulation purposes. Moreover, whether it is inorganic or organic, it can be widely developed.

[0192] Description of Reference Numerals

[0193] M oxide raw material

[0194] P1, P2 mixed oxide (black mixed oxide material)

[0195] 11. Primary crushed material

[0196] 12 Raw material burnt material

[0197] 21First crushed material

[0198] 22First fired product

[0199] 23 Second crushed material

[0200] 24 Second fired product

Claims

1. A method for producing a black pigment, comprising an oxide containing La, Mn and Cu as main components and excluding Cr and Co as the main components, It is characterized in that The method for producing the black pigment comprises the following steps: In the first crushing process, Mn is 3 O 4 As raw materials, oxide raw materials of La, Mn and Cu are mixed and crushed to obtain a primary crushed product with an average particle size of less than 5 μm; a raw material calcining step of calcining the primary pulverized product at 700° C. to 1200° C. to obtain a raw material calcined product; and The secondary pulverizing step is to pulverize the raw material burnt product to an average particle size of less than 20 μm. The mixed oxides are obtained, The contents of La, Mn and Cu in the black pigment satisfy the following ratios, based on the oxide conversion amount with the total weight of the following oxides being 100 wt %: Take La 2 O 3 According to the formula, La is 35 wt% to 70 wt%; MnO 2 Mn is 25 wt% to 60 wt%; Cu is 0.5 wt% to 10 wt% based on CuO. The black pigment further contains an oxide of Mo as the main component, La to La 2 O 3 Mn is calculated as MnO 2 In the oxide conversion amount, Cu is calculated as CuO, and the total weight of these three oxides is set to 100 weight %, Mo is added as MoO with respect to 100 wt % of the oxide conversion amount. 3 The black pigment contains Mo in a ratio of 0.01 wt % to 5 wt % or less, The black pigment has an average particle size of 20 μm or less, The black pigment in the L*a*b* color system according to JIS-Z-8729 is black as follows: the blackness, i.e., the L value is 25.0 or less, the b value is a negative value, The black pigment has a perovskite phase, and the perovskite phase shows a diffraction peak with a maximum intensity in a range of 31° to 34° at a diffraction angle 2θ when measured by X-ray diffraction using CuKα rays as an X-ray source. Miller indices corresponding to a hexagonal unit lattice in which the lattice constant of the perovskite phase is a=b<c show (012) plane, (110) plane, (104) plane, (113) plane, (202) plane, (006) plane, (024) plane, (122) plane, (116) plane, (030) plane, (214) plane, (018) plane, The black pigment contains Mn having a spinel structure 3 O 4 As an oxide of Mn, and The black pigment is composed of the perovskite phase and the spinel structure.

2. The method for producing a black pigment according to claim 1, in, The black pigment contains Si or Fe, or Si and Fe as subcomponents in addition to the main component.

3. The method for producing a black pigment according to claim 1, in, The black pigment contains, in addition to the main component, any one or more of Li, B, Na, Mg, Al, Si, P, K, Ca, Ti, V, Fe, Zn, Sr, Y, Zr, Nb, Sn, Sb, Ba, Ta, W, Bi, Ce, Pr, Nd or Er as a secondary component, La to La 2 O 3 Mn is calculated as MnO 2 In the oxide conversion amount, Cu is calculated as CuO, and the total weight of these three oxides is set to 100 weight %, The auxiliary component is Li 2 O.B 2 O 3 、Na 2 O, MgO, Al 2 O 3 、SiO 2 , P 2 O 5 , K 2 O, CaO, TiO 2 、V 2 O 5 , Fe 3 O 3 、ZnO、SrO、Y 2 O 3 、ZrO 2 , Nb 2 O 3 SnO 2 , Sb 2 O 3 、BaO、Ta 2 O 5 , WO 3 、Bi 2 O 3 、CeO 2 , Pr 6 O 11 、Nd 2 O 5 or 2 O 3 The black pigment contains the auxiliary component in a ratio of 20 weight % or less.

4. The method for producing a black pigment according to claim 1, in, The black pigment is a non-magnetic material.

5. The method for producing a black pigment according to claim 1, in, The black pigment is an insulating material.

6. The method for producing a black pigment according to claim 1, in, The primary pulverization step is performed by wet pulverization.

7. The method for producing a black pigment according to claim 1, in, The primary pulverization step is performed by wet pulverization using water as a solvent.

8. The method for producing a black pigment according to claim 1, in, The primary pulverization step is performed by wet pulverization using a ball mill.