Light-curable long-carbon-chain wax resin as well as synthesis method and application thereof

By introducing UV-curable groups into the wax chain segments of long-chain wax resin, the compatibility and mechanical properties of UV-curable 3D printing materials have been solved, achieving efficient and stable casting printing and casting effects.

CN118955765APending Publication Date: 2024-11-15GUANGZHOU YOUSU PLASTIC TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411032282.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Existing UV-curable 3D printing materials face challenges in the casting field, including poor compatibility of wax with other organic compounds, increased thixotropy, and decreased mechanical properties, making it difficult to meet the requirements for accurate replication and efficient casting of complex parts.

Method used

A method for synthesizing photocurable long-chain wax resin was adopted. By introducing UV-curable double bond groups into the wax chain segments, the compatibility was enhanced, and the cross-linking was carried out through chemical reactions, thus solving the problems of compatibility and mechanical properties.

Benefits of technology

It significantly improves the compatibility and stability of materials, ensures a smooth printing process, enhances the quality and aesthetics of castings, reduces combustion residues, and improves casting efficiency and overall casting quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955765A_ABST
    Figure CN118955765A_ABST
Patent Text Reader

Abstract

The invention relates to the field of 3D printing casting materials, in particular to light-curable long-carbon-chain wax resin and a synthesis method and application thereof. A synthesis method of light-curable long-carbon-chain wax resin comprises the following steps: step 1, mixing maleic acid, a polymerization inhibitor A, a catalyst A and a reactive diluent until the maleic acid is dissolved to obtain a first mixture; 2, mixing glycidyl methacrylate with the first mixture, carrying out a heat preservation reaction, and filtering to obtain MA-GMA; 3, mixing HTPB, a catalyst B, a polymerization inhibitor B and MA-GMA, controlling the vacuum degree, carrying out a heat preservation reaction, and filtering to obtain light-curable long-carbon-chain wax resin; the molar ratio of the HTPB to the MA-GMA is 1: (0.8-1). The light-curable long-carbon-chain wax resin provided by the invention is good in compatibility with a 3D printing material, strong in stability, not easy to separate out, capable of being added in a large amount without influencing mechanical properties, and sufficient in combustion, and has a good application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of 3D printing casting materials, and more specifically, to a photocurable long carbon chain wax resin and a synthesis method and application thereof. Background Art

[0002] In the field of metal casting, lost wax casting is a long-standing and widely used process. Its core is to use wax materials to make models of complex castings. This method first makes a fine casting model with wax, then wraps the wax model with plaster and dries it. The wax is melted and burned by heating and baking to form an empty shell that can be used for metal solution casting. However, this traditional method faces many challenges in practical applications: 1. Complexity limitation of wax molds: For some extremely complex or delicate casting models (such as hollow, multi-curved, irregular, etc.), traditional wax materials are difficult to achieve accurate replication due to their physical properties and processing methods, making it difficult to ensure the quality of castings.

[0003] 2. The fluidity and cleanliness of the wax model: After the wax model is heated and melted, it must be ensured that it flows out of the gypsum shell completely and cleanly to avoid residues that cause casting defects. However, in actual operations, it is often difficult to completely avoid these problems, which affects the quality of the casting.

[0004] 3. Casting efficiency and cost: The traditional lost wax casting process is cumbersome, time-consuming, and has high requirements for materials and equipment, resulting in low overall casting efficiency and increased costs.

[0005] With the advancement of science and technology, UV-curing 3D printing technology has gradually emerged in the manufacturing industry as an efficient and precise rapid prototyping process. This technology uses ultraviolet light to irradiate liquid photosensitive materials to solidify them layer by layer to build objects. It has significant advantages such as high precision, high material selectivity and flexible customization, and can be used to build complex or delicate casting models.

[0006] However, UV-curing 3D printing also faces some challenges when applied to the casting field: 1. Material selection: Traditional UV-curable materials often have difficulty achieving ideal fluidity and thermal stability in casting, especially when it is necessary to simulate the properties of traditional wax models.

[0007] 2. Compatibility and mechanical properties: When wax is directly added to UV-curable materials, due to the straight-chain alkane structure of the wax and the lack of photocurable groups, it leads to problems such as poor compatibility, increased thixotropy of the system, and decreased mechanical properties of the material.

[0008] In order to solve the above problems, the prior art attempts to directly blend different types of waxes (such as polyethylene wax, modified polyethylene wax slurry, polypropylene wax, etc.) into UV-curable materials by physical mixing. However, this method has the following shortcomings: 1. Compatibility issues: Wax has poor compatibility with other organic compounds and is prone to precipitation, which affects the stability of the material and the printing effect.

[0009] 2. Thixotropy increase: The addition of wax will cause the thixotropy of the system to increase significantly, increasing the difficulty of printing and even leading to printing failure. Therefore, it can only be added in small amounts, and most of the addition amounts in the existing technology are less than 30%.

[0010] 3. Decreased mechanical properties: Since wax only acts as a filler in the system and cannot participate in chemical reactions, the mechanical properties of the material are greatly reduced, making the material brittle.

[0011] In view of the above-mentioned deficiencies in the prior art, there is an urgent need to find a material suitable for UV-curing 3D printing. Summary of the invention

[0012] In view of the above-mentioned deficiencies in the prior art, the present invention aims to provide a photocurable long carbon chain wax resin and a synthesis method and application thereof.

[0013] In a first aspect, the present application provides a method for synthesizing a photocurable long carbon chain wax resin, using the following technical solution: A method for synthesizing a photocurable long carbon chain wax resin comprises the following steps: Step 1: mixing maleic acid, inhibitor A, catalyst A and active diluent at 90-100° C. until the maleic acid is dissolved to obtain a first mixture; the stirring speed is 300 r / min-500 r / min; Step 2: mixing glycidyl methacrylate with the first mixture, reacting at a temperature of 100 °C, and filtering to remove the catalyst A to obtain MA-GMA; The molar ratio of maleic acid to glycidyl methacrylate is (0.8-1.2):(0.8-1.2); Step 3: Mix HTPB, catalyst B, inhibitor B and MA-GMA at 110-120° C., control the vacuum degree to 0.5-1.0 MPa, keep the temperature for 4-5 hours, filter and remove the catalyst B to obtain a photocurable long carbon chain wax resin; the molar ratio of HTPB to MA-GMA is 1:(0.8-1).

[0014] The synthesis path is as follows: (1) Carboxyl-terminated intermediates: (2) Photocurable long carbon chain wax resin: The n value in HTPB is 22 to 28.

[0015] The photocurable long carbon chain wax resin prepared in the present application significantly enhances the compatibility between the wax resin and the UV-curable material by introducing UV-curable double bond groups, thus solving the problem that traditional wax materials are difficult to be compatible in UV-curable systems.

[0016] Due to its good compatibility in UV curing systems, its dosage can be greatly increased. The modified wax resin is no longer mixed into the system as a simple filler, but participates in cross-linking through chemical reactions. Adding a large amount into the system will not affect the mechanical properties of the material.

[0017] At the same time, good compatibility enables UV-curable 3D printing materials to be stored for a long time and not easy to delaminate. Not only that, printing large or complex models takes a long time. If the compatibility is not good, the wax in the UV-curable 3D printing material will gradually precipitate, affecting the printing effect. The photocurable long carbon chain wax resin of this application does not have the above problems and guarantees quality.

[0018] The photocurable long carbon chain wax resin provided in the present application retains the natural property of wax to be converted into a fluid when heated, and can leave a gap between the plaster and the resin model after heating. The existence of the gap provides a buffer space for the thermal expansion of the resin model, thereby preventing the thermal expansion of the resin model from causing cracking of the plaster.

[0019] The long carbon chain structure of the wax resin not only maintains its unique fluidity as a wax material, but also gives it the ability to burn completely during the combustion process, significantly reducing combustion residues. This environmentally friendly feature not only meets the requirements of modern green production, but also shows advantages in the subsequent processing of metal castings. Due to more thorough combustion, the surface of the metal casting is smoother, reducing the workload of subsequent grinding and processing, and directly improving the overall quality and aesthetics of the metal casting.

[0020] Preferably, the active diluent may be a mixture of one or more of polyethylene glycol (400) dimethacrylate, 1,4-butanediol dimethacrylate, triethylene glycol dimethacrylate, diethylene glycol dimethacrylate, and tripropylene glycol diacrylate.

[0021] Preferably, the molar ratio of HTPB to MA-GMA is 1:1.

[0022] Preferably, in step 3, the vacuum degree is controlled to be 0.6-0.8 MPa.

[0023] Preferably, in step 1, the amount of inhibitor A is 0.08-0.15% of the total amount of glycidyl methacrylate and maleic acid, and the amount of catalyst A is 0.15-0.25% of the total amount of glycidyl methacrylate and maleic acid.

[0024] Preferably, in step 3, the amount of inhibitor B is 0.08-0.15% of the total amount of HTPB and MA-GMA, and the amount of catalyst B is 0.25-0.35% of the total amount of HTPB and MA-GMA.

[0025] Preferably, the inhibitor A is a mixture of one or more of p-hydroxyanisole, hydroquinone, and 2,6-di-tert-butyl-p-cresol, and the inhibitor B is a mixture of one or more of p-hydroxyanisole, hydroquinone, and 2,6-di-tert-butyl-p-cresol. The inhibitor A and the inhibitor B may be the same or different.

[0026] Preferably, the catalyst A is a solid acid catalyst, the catalyst B is a solid acid catalyst, and the catalyst A and the catalyst B may be the same or different.

[0027] In a second aspect, the present application provides a photocurable long carbon chain wax resin.

[0028] The photocurable long carbon chain wax resin provided in this application has the following advantages: 1. The photocurable long carbon chain wax significantly improves its compatibility in UV-curable materials, effectively preventing the occurrence of precipitation problems and ensuring the stability and quality consistency of the material during storage. In addition, its excellent compatibility characteristics avoid a significant increase in the thixotropy of the system, thereby ensuring a smooth printing process and improving production efficiency and product quality stability.

[0029] 2. Unlike the traditional method of simply mixing into the system as a filler, the photocurable long carbon chain wax resin deeply participates in the cross-linking network of the material through chemical reaction. This transformation allows the photocurable long carbon chain wax resin to be added in large quantities in the system without worrying about negative impact on the mechanical properties of the material. On the contrary, it can also enhance the overall performance of the material to a certain extent and meet higher-end application requirements.

[0030] 3. During the dewaxing stage of the casting process, the light-curable long carbon chain wax can be pre-melted to create the necessary gaps between the gypsum and the resin model. These gaps serve as a buffer area for thermal expansion, effectively absorbing the expansion stress generated by the resin model during the heating process, thereby avoiding the risk of cracking of the gypsum due to extrusion. This not only improves the safety and success rate of the casting process, but also ensures the integrity and aesthetics of the final casting.

[0031] 4. The application of photocurable long carbon chain wax also brings about a significant reduction in combustion ash. This improvement directly improves the casting effect, making the surface of the casting smoother and more delicate, and reducing defects and flaws caused by residual ash. At the same time, it also improves the dimensional accuracy and overall quality level of the casting, meeting the requirements of more stringent and complex application scenarios.

[0032] In a third aspect, the present application provides an application of a photocurable long carbon chain wax resin in a photocurable 3D printing material.

[0033] Preferably, the amount of the photocurable long carbon chain wax resin added to the photocurable 3D printing material is 15-80%.

[0034] The present application overcomes the compatibility problem of the wax itself, avoids precipitation, reduction of mechanical properties, etc., and the photocurable long carbon chain wax resin participates in cross-linking by chemical reaction. Therefore, it can be added to UV-curable 3D printing materials in large quantities, and the added amount far exceeds 30% of the prior art.

[0035] In summary, the present invention has the following beneficial effects by introducing UV-curable groups into the wax segments: 1. Improve compatibility: Solve the compatibility problem of wax in UV-curing materials to avoid precipitation.

[0036] 2. Control thixotropy: Reduce the effect of wax addition on system thixotropy to ensure smooth 3D printing.

[0037] 3. Enhance mechanical properties: Make the wax resin participate in cross-linking through chemical reaction, so that it can be added to the system in large quantities without affecting the mechanical properties of the material.

[0038] 4. Retain thermal fluidity: Retain the characteristic of wax turning into fluid when heated, provide buffer space for thermal expansion of resin model and avoid plaster cracking. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 It is the photocurable long carbon chain wax resin prepared in Example 1 of the present application.

[0040] Figure 2 It is a product printed by a 3D printer using the light-curing 3D printing material of Application Example 1 of the present application.

[0041] Figure 3 It is a metal part cast using the light-curing 3D printing material of Application Example 1 of the present application.

[0042] Figure 4 This is the thermogravimetric analysis result of Application Example 1 in Test 4.

[0043] Figure 5This is the thermogravimetric analysis result of commercially available product 1 in test 4.

[0044] Figure 6 This is a graph showing the thermogravimetric analysis results of commercially available product 2 in test 4. DETAILED DESCRIPTION

[0045] The present application is further described in detail below with reference to the accompanying drawings and embodiments.

[0046] The raw materials used in the following examples and comparative examples are all commercially available products. Example

[0047] Example 1 A method for synthesizing a photocurable long carbon chain wax resin comprises the following steps: Step 1: Preheat the reactor to 90° C., add maleic acid, inhibitor A, catalyst A and active diluent into the reactor, and stir and mix at a speed of 400 r / min until the maleic acid is dissolved to obtain a first mixture.

[0048] Step 2: Control the temperature of the reactor at 90°C, then slowly drop glycidyl methacrylate (GMA) into the reaction system and keep the temperature for 3 hours.

[0049] Catalyst A was removed by filtration to obtain MA-GMA.

[0050] Step 3: Add HTPB, catalyst B and inhibitor B into a reactor, start stirring and heat the reactor to 110° C. to obtain a second mixture.

[0051] MA-GMA was slowly added dropwise to the second mixture, and the vacuum degree was controlled at 0.6 MPa. The mixture was kept warm for 4 h.

[0052] After filtering and removing the catalyst B, a white waxy photocurable long carbon chain wax resin can be obtained.

[0053] The active diluent can be a mixture of one or more of polyethylene glycol (400) dimethacrylate, 1,4-butylene glycol dimethacrylate, triethylene glycol dimethacrylate, diethylene glycol dimethacrylate, and tripropylene glycol diacrylate. In this embodiment, the active diluent is active diluent DPGDA (tripropylene glycol diacrylate).

[0054] Inhibitor A is a mixture of one or more of p-hydroxyanisole, hydroquinone, and 2,6-di-tert-butyl-p-cresol, and inhibitor B is a mixture of one or more of p-hydroxyanisole, hydroquinone, and 2,6-di-tert-butyl-p-cresol. Inhibitor A and inhibitor B may be the same or different. In the present embodiment, inhibitor A and inhibitor B are p-hydroxyanisole.

[0055] Catalyst A and Catalyst B are solid acid catalysts, specifically HND26 solid acid catalysts.

[0056] In the above reaction, the molar ratio of maleic acid to glycidyl methacrylate is 1:1, the amount of inhibitor A is 0.1% of the total amount of glycidyl methacrylate and maleic acid, the amount of catalyst A is 0.2% of the total amount of glycidyl methacrylate and maleic acid, and the amount of diluent DPGDA is 20% of the total amount of glycidyl methacrylate and maleic acid.

[0057] The molar ratio of HTPB to MA-GMA is 1:1, the dosage of inhibitor B is 0.092% of the total amount of HTPB and MA-GMA, and the dosage of catalyst B is 0.3% of the total amount of HTPB and MA-GMA.

[0058] That is, 116g of maleic acid, 0.258g of inhibitor A, 0.516g of catalyst A and 51.6g of active diluent DPGDA (tripropylene glycol diacrylate), 142g of glycidyl methacrylate; 3564g of HTPB, 11.623g of catalyst B and 3.564g of inhibitor B, 310.37g of MA-GMA.

[0059] The n value in HTPB is 22 to 28.

[0060] The prepared light-curable long carbon chain wax resin is referred to Figure 1 .

[0061] Example 2 A method for synthesizing a photocurable long carbon chain wax resin, which is different from that of Example 1, comprises the following steps: Step 1: Preheat the reactor to 90° C., add maleic acid, inhibitor A, catalyst A and active diluent DPGDA (tripropylene glycol diacrylate) into the reactor, stir and mix at a speed of 500 r / min until the maleic acid is dissolved to obtain a first mixture.

[0062] Step 2: Control the temperature of the reactor at 100° C., then slowly drop glycidyl methacrylate into the reaction system, and keep the temperature to react for 3 hours.

[0063] Catalyst A was removed by filtration to obtain MA-GMA.

[0064] Step 3: Add HTPB, catalyst B and inhibitor B into a reactor, start stirring and heat the reactor to 110° C. to obtain a second mixture.

[0065] MA-GMA was slowly added dropwise to the second mixture, and the vacuum degree was controlled at 0.8 MPa. The reaction was kept warm for 4 hours.

[0066] After filtering and removing the catalyst B, a white waxy photocurable long carbon chain wax resin can be obtained.

[0067] The inhibitor A and the inhibitor B are p-hydroxyanisole. The catalyst A and the catalyst B are solid acid catalysts, specifically HND26 solid acid catalysts.

[0068] In the above reaction, the molar ratio of maleic acid to glycidyl methacrylate is 0.8:1.2, the amount of inhibitor A used is 0.08% of the total amount of glycidyl methacrylate and maleic acid, the amount of catalyst A used is 0.15% of the total amount of glycidyl methacrylate and maleic acid, and the amount of diluent DPGDA used is 15% of the total amount of glycidyl methacrylate and maleic acid.

[0069] The molar ratio of HTPB to MA-GMA is 1:0.8, the dosage of inhibitor B is 0.08% of the total amount of HTPB and MA-GMA, and the dosage of catalyst B is 0.25% of the total amount of HTPB and MA-GMA.

[0070] That is, 92.8g maleic acid, 0.211g inhibitor A, 0.395g catalyst A and 39.48g active diluent DPGDA (tripropylene glycol diacrylate), 170.4g glycidyl methacrylate; 3564g HTPB, 9.668g catalyst B and 2.85g inhibitor B, 237.27g MA-GMA.

[0071] Example 3 A method for synthesizing a photocurable long carbon chain wax resin, which is different from that of Example 1, comprises the following steps: Step 1: Preheat the reactor to 90° C., add maleic acid, inhibitor A, catalyst A and active diluent DPGDA (tripropylene glycol diacrylate) into the reactor, stir and mix at a speed of 300 r / min until the maleic acid is dissolved to obtain a first mixture.

[0072] Step 2: Control the temperature of the reactor at 90°C, then slowly drop glycidyl methacrylate into the reaction system and keep the temperature for 3 hours.

[0073] Catalyst A was removed by filtration to obtain MA-GMA.

[0074] Step 3: Add HTPB, catalyst B and inhibitor B into a reactor, start stirring and heat the reactor to 120° C. to obtain a second mixture.

[0075] MA-GMA was slowly added dropwise to the second mixture, and the vacuum degree was controlled at 0.5 MPa. The reaction was kept warm for 5 h.

[0076] After filtering and removing the catalyst B, a white waxy photocurable long carbon chain wax resin can be obtained.

[0077] The inhibitor A and the inhibitor B are p-hydroxyanisole. The catalyst A and the catalyst B are solid acid catalysts, specifically HND26 solid acid catalysts.

[0078] In the above reaction, the molar ratio of maleic acid to glycidyl methacrylate is 1.2:0.8, the amount of inhibitor A is 0.15% of the total amount of glycidyl methacrylate and maleic acid, the amount of catalyst A is 0.25% of the total amount of glycidyl methacrylate and maleic acid, and the amount of diluent DPGDA is 25% of the total amount of glycidyl methacrylate and maleic acid.

[0079] The molar ratio of HTPB to MA-GMA is 1:1, the dosage of inhibitor B is 0.15% of the total amount of HTPB and MA-GMA, and the dosage of catalyst B is 0.35% of the total amount of HTPB and MA-GMA.

[0080] That is, 139.2g of maleic acid, 0.379g of inhibitor A, 0.632g of catalyst A and 63.2g of active diluent DPGDA (tripropylene glycol diacrylate), 113.6g of glycidyl methacrylate; 3564g of HTPB, 13.583g of catalyst B and 5.822g of inhibitor B, 317.01g of MA-GMA.

[0081] Comparative Example Comparative Example 1 A method for synthesizing a photocurable long carbon chain wax resin, which is different from Example 1 in that the molar ratio of HTPB to MA-GMA is 1:0.5.

[0082] That is, 116g of maleic acid, 0.258g of inhibitor A, 0.516g of catalyst A and 51.6g of active diluent DPGDA (tripropylene glycol diacrylate), 142g of glycidyl methacrylate; 3564g of HTPB, 11.157g of catalyst B and 3.719g of inhibitor B, 155.18g of MA-GMA.

[0083] Comparative Example 2 A method for synthesizing a photocurable long carbon chain wax resin, which is different from Example 1 in that the molar ratio of HTPB to MA-GMA is 1:2.

[0084] That is, 116g of maleic acid, 0.258g of inhibitor A, 0.516g of catalyst A and 51.6g of active diluent DPGDA (tripropylene glycol diacrylate), 142g of glycidyl methacrylate; 3564g of HTPB, 12.554g of catalyst B and 4.184g of inhibitor B, 620.74g of MA-GMA.

[0085] Comparative Example 3 A method for synthesizing a photocurable long carbon chain wax resin, which is different from Example 1 in that HTPB is replaced by PCDL2000 (polycarbonate diol with a molecular weight of 2000).

[0086] Application Examples Application Example 1 A photocurable 3D printing material comprises the following raw materials in parts by mass: 20 kg of photocurable long carbon chain wax resin, 80 kg of UV monomer, 1.5 kg of initiator TPO, and 10 g of yellow toner.

[0087] The photocurable long carbon chain wax resin is the photocurable long carbon chain wax resin of Example 1.

[0088] The UV monomer is 1,4-butanediol dimethacrylate.

[0089] The raw materials are stirred evenly at room temperature to obtain light-curing 3D printing materials.

[0090] Reference for products printed by 3D printers using light-curing 3D printing materials Figure 2 .

[0091] Application Example 2 A photocurable 3D printing material, which is different from Application Example 1 in that the photocurable long carbon chain wax resin adopts the photocurable long carbon chain wax resin of Example 2.

[0092] Application Example 3 A photocurable 3D printing material, which is different from Application Example 1 in that the photocurable long carbon chain wax resin adopts the photocurable long carbon chain wax resin of Example 3.

[0093] Application Example 4 A photocurable 3D printing material comprises the following raw materials in parts by mass: 80 kg of photocurable long carbon chain wax resin, 20 kg of UV monomer, 1.5 kg of initiator TPO, and 10 g of yellow toner.

[0094] The photocurable long carbon chain wax resin is the photocurable long carbon chain wax resin of Example 1.

[0095] The UV monomer is 1,4-butanediol dimethacrylate.

[0096] The raw materials are stirred evenly at room temperature to obtain light-curing 3D printing materials.

[0097] Comparative application example 1 A photocurable 3D printing material, which is different from Application Example 1 in that the photocurable long carbon chain wax resin adopts the photocurable long carbon chain wax resin of Comparative Example 1.

[0098] Comparative Application Example 2 A photocurable 3D printing material, which is different from Application Example 1 in that the photocurable long carbon chain wax resin adopts the photocurable long carbon chain wax resin of Comparative Example 2.

[0099] Comparative Application Example 3 A photocurable 3D printing material, which is different from Application Example 1 in that the photocurable long carbon chain wax resin adopts the photocurable long carbon chain wax resin of Comparative Example 3.

[0100] Comparative Application Example 4 A photocurable 3D printing material, which is different from Application Example 1 in that the photocurable long carbon chain wax resin is replaced by commercially available micro wax powder.

[0101] Comparative Application Example 5 A photocurable 3D printing material, which is different from Application Example 4 in that the photocurable long carbon chain wax resin is replaced by commercially available micro wax powder.

[0102] Performance testing Test 1: Mechanical properties test: The photocurable 3D printing materials of Application Examples 1-4 and Comparative Application Examples 1-5 were placed in a photocurable 3D printer to print mechanical property test specimens, and the tensile strength was tested with reference to GB / T 1040.2-2006 "Determination of tensile properties of plastics Part 2: Test conditions for molded and extruded plastics", and the tensile strength was recorded in Table 1.

[0103] 3D printer printing parameters: Table 1 CEILING HEIGHT Layer exposure time Bottom layer exposure time Release film 0.05mm 5.5s~6.5s 30s~40s NFEP Number of bottom layers Transition Layers Static time after lifting Rest time after return trip 6 10 2s 2s Lifting speed Return speed Distance from mold 65mm / min 150mm / min 8mm~10mm Device model: YOUSU-10.1-inch-i-Jewelry Pro all in one Test 2: Extraction test: The light-curable 3D printing materials of Application Examples 1-4 and Comparative Application Examples 1-5 were canned and sealed, and stored at 55° C. for 30 days. After being taken out, they were visually observed to see if there was stratification, and the observation results were recorded in Table 2.

[0104] Test 3: Casting product performance test: The 3D printer was set according to the 3D printing parameters of Test 1, and the photocurable 3D printing materials of Application Examples 1-4 and Comparative Application Examples 1-5 were placed in the photocurable 3D printer to print test samples. The metal parts were cast through a casting process, and the surface of the metal parts was visually observed to see whether they were smooth. The observation results are recorded in Table 2.

[0105] Test sample appearance: fan-shaped model with holes.

[0106] Casting process: 1. Pouring gypsum; 2. Gypsum dewaxing; 3. Metal casting.

[0107] 1. Pouring gypsum: (1) Dispersed gypsum: The ratio of gypsum powder to water is 1000:400. First, put all the water into the container, start stirring (speed is less than 700r / min), and then add the weighed gypsum powder into the water in batches. After the gypsum powder is added, keep stirring for 3 minutes.

[0108] (2) Gypsum degassing: Place the stirred gypsum slurry in a degassing machine. When the pressure reaches 0.85, start shaking the degassing machine platform and start timing. The degassing time is 2 minutes.

[0109] (3) Pour the degassed gypsum into a steel pot until the gypsum covers the casting (fan-shaped model with holes) by 1.5 to 2 cm. Then degasmate it again for 2 minutes and finally leave it for 2 to 3 hours to allow the gypsum to fully harden.

[0110] 2. Gypsum dewaxing: (1) Preheat the muffle furnace to 50°C and place the steel cup containing the test sample into the furnace.

[0111] (2) The first stage: 50℃~760℃, heating rate is about 2.33℃ / min.

[0112] (3) Second stage: 760℃ for 120min, and dewaxing is completed.

[0113] 3. Metal casting: (1) Prepare for casting, keep the steel pot at 740℃.

[0114] (2) Casting: Brass insulation temperature 1000℃.

[0115] (3) Pour the dissolved brass metal into a steel cup.

[0116] (4) Place the steel cup in water to clean the plaster and obtain the final metal part.

[0117] Reference for metal parts cast using light-curing 3D printing materials in Application Example 1 Figure 3 .

[0118] Test 4: Combustion degree detection: The 3D printer was set according to the 3D printing parameters of Test 1, and the photocurable 3D printing materials of Application Examples 1-4 and Comparative Application Examples 1-5 were placed in the photocurable 3D printer for printing to prepare test samples. The samples were then burned according to the following conditions to obtain thermogravimetric analysis results, and the residual mass was recorded in Table 2.

[0119] Thermogravimetric analysis test conditions: The sample weight is about 5 mg; 30℃ to 800℃, heating rate 20.0 (k / min); Atmosphere: nitrogen, 20.0 ml / min.

[0120] The above test data are summarized in Table 2.

[0121] Table 2 Category Test 1 (MPa) Test 2 Test Three Test 4 (%) Application Example 1 17.31 No stratification Very smooth 0.40 Application Example 2 21.24 No stratification Very smooth 0.45 Application Example 3 14.56 No stratification Very smooth 0.53 Application Example 4 16.92 No stratification Very smooth 0.48 Comparative application example 1 12.35 Layering smooth 0.85 Comparative Application Example 2 14.06 No stratification Rough 1.76 Comparative Application Example 3 23.00 No stratification Very rough 3.30 Comparative Application Example 4 9.16 Layering smooth 0.52 Comparative Application Example 5 Unable to print Unable to print Unable to print Unable to print Commercially available 1 / / / 2.72 Commercially available 2 / / / 1.64 Comparative Application Example 1-2 is based on Application Example 1, using a photocurable long carbon chain wax resin prepared by using a molar ratio of HTPB and MA-GMA that is not within a specific range. According to the data in Table 2, the photocurable 3D printing material prepared in Application Example 1 has significantly higher tensile strength than that of Comparative Application Example 1-2, and it does not precipitate or delaminate. The surface of the prepared casting product is very smooth and of good quality, and the ash content is very low. The performance in all aspects is very outstanding and excellent. The photocurable 3D printing material in Comparative Application Example 1 has poor curing effect, a significant decrease in mechanical properties, and is prone to precipitation and delamination. In the precipitation test, the photocurable 3D printing material in Comparative Application Example 2 showed no delamination results and acceptable mechanical properties, but the surface of the resulting casting product was rough and the effect was not good; and the ash content was also high, and it could not be burned cleanly. Comparative Application Examples 1-2 cannot achieve the effect of Application Example 1.

[0122] Comparative Application Example 3 is based on Application Example 1, using PCDL2000 instead of HTPB to prepare a photocurable long carbon chain wax resin. Although the photocurable 3D printing material prepared in Comparative Application Example 3 has good mechanical properties and does not precipitate stratification, the surface of the cast product prepared is very rough, the ash content is high, and the casting effect is not good.

[0123] In summary, it is necessary to strictly limit the raw materials and dosage relationship used in the preparation of photocurable long carbon chain wax resin in order to obtain photocurable long carbon chain wax resin with special structure and excellent performance.

[0124] Comparative Application Examples 4 and 5 are to directly mix wax into UV-curable materials, simulating the commonly used methods on the market.

[0125] A small amount of wax is added to comparative application example 4. According to the test data in Table 2, the mechanical properties of the light-cured 3D printing material in comparative application example 4 are poor, and stratification occurs, and the effect is not as good as that in application example 1.

[0126] Comparative Application Example 5 corresponds to the addition of a large amount of wax. According to the test data in Table 2, after increasing the amount of photocurable long carbon chain wax resin used in Application Example 4, it is still possible to prepare a photocurable 3D printing material with good performance, and the quality of the casting product is also excellent; while Comparative Application Example 5 cannot be printed.

[0127] It is explained that the photocurable long carbon chain wax resin provided in the present application is used in photocurable 3D printing materials, has good compatibility with other organic compounds, and will not cause a significant increase in the thixotropy of the system even if added in large quantities. It also participates in chemical reactions, which can ensure that the photocurable 3D printing materials have high mechanical properties, and is very suitable for application in the field of ultraviolet light curing.

[0128] In actual experiments, it was also found that when the molar ratio of maleic acid to glycidyl methacrylate was 1:0.5, half of the unreacted maleic acid would remain in the system, and HTPB would precipitate directly from the system, resulting in the formation of a mixture, which could not achieve the purpose of this application. When the molar ratio of maleic acid to glycidyl methacrylate was 1:2, subsequent reactions could not be carried out directly, and the purpose of this application could not be achieved. Therefore, the molar ratio of maleic acid to glycidyl methacrylate needs to be strictly limited.

[0129] Reference Figure 4 , is the thermogravimetric analysis result of Application Example 1 in Test 4.

[0130] Reference Figure 5 , are the thermogravimetric analysis results of commercially available product 1 in test 4.

[0131] Reference Figure 6 , are the thermogravimetric analysis results of commercially available product 2 in test 4.

[0132] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A method for synthesizing a photocurable long carbon chain wax resin, characterized in that: The following steps are involved: Step 1: mixing maleic acid, inhibitor A, catalyst A, and active diluent at 90-100° C. until the maleic acid is dissolved to obtain a first mixture; Step 2: mixing glycidyl methacrylate with the first mixture, reacting at a temperature of 100 °C, and filtering to remove the catalyst A to obtain MA-GMA; The molar ratio of maleic acid to glycidyl methacrylate is (0.8-1.2):(0.8-1.2); Step 3: Mix HTPB, catalyst B, inhibitor B, and MA-GMA at 110-120° C., control the vacuum degree to 0.5-1.0 MPa, keep the temperature for 4-5 hours, filter and remove the catalyst B to obtain a photocurable long carbon chain wax resin; The molar ratio of HTPB and MA-GMA is 1:(0.8-1).

2. The method for synthesizing a photocurable long carbon chain wax resin according to claim 1, characterized in that: The molar ratio of the HTPB to the MA-GMA is 1:

1.

3. The method for synthesizing a photocurable long carbon chain wax resin according to claim 1, characterized in that: In step 3, the vacuum degree is controlled to be 0.6-0.8 MPa.

4. The method for synthesizing a photocurable long carbon chain wax resin according to claim 1, characterized in that: In the step 1, the amount of the inhibitor A is 0.08-0.15% of the total amount of glycidyl methacrylate and maleic acid, and the amount of the catalyst A is 0.15-0.25% of the total amount of glycidyl methacrylate and maleic acid.

5. The method for synthesizing a photocurable long carbon chain wax resin according to claim 1, characterized in that: In the step 3, the amount of inhibitor B is 0.08-0.15% of the total amount of HTPB and MA-GMA, and the amount of catalyst B is 0.25-0.35% of the total amount of HTPB and MA-GMA.

6. The method for synthesizing a photocurable long carbon chain wax resin according to claim 1, characterized in that: The inhibitor A is a mixture of one or more of p-hydroxyanisole, hydroquinone, and 2,6-di-tert-butyl-p-cresol, and the inhibitor B is a mixture of one or more of p-hydroxyanisole, hydroquinone, and 2,6-di-tert-butyl-p-cresol. The inhibitor A and the inhibitor B can be the same or different.

7. The method for synthesizing a photocurable long carbon chain wax resin according to claim 1, characterized in that: The catalyst A is a solid acid catalyst, and the catalyst B is a solid acid catalyst. The catalyst A and the catalyst B may be the same or different.

8. A photocurable long carbon chain wax resin obtained by the synthesis method of the photocurable long carbon chain wax resin according to any one of claims 1 to 7.

9. A photocurable long carbon chain wax resin prepared by the synthesis method of the photocurable long carbon chain wax resin according to any one of claims 1 to 7 or a use of the photocurable long carbon chain wax resin according to claim 8 in photocurable 3D printing materials.

10. A use of a photocurable long carbon chain wax resin prepared by the synthesis method of a photocurable long carbon chain wax resin according to any one of claims 1 to 7 or a photocurable long carbon chain wax resin according to claim 8 in a photocurable 3D printing material, characterized in that: The amount of the photocurable long carbon chain wax resin added to the photocurable 3D printing material is 15-80%.