High-temperature-resistant compression permanent non-deformation slow-rebound sponge
The sponge prepared by a specific formula and process has solved the problem of sponge deformation at high temperatures, and has achieved the effects of high temperature compression resistance without deformation and slow rebound.
Patent Information
- Application Number
- CN202410927707.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-15
AI Technical Summary
Existing sponges are prone to deformation under high temperatures and have difficulty maintaining their shape after compression.
Sponges are prepared using raw materials such as polyethylene oxide polyether polyol, modified slow-rebound polyether polyol, and foaming agent, combined with components such as silicone oil, foam leveling agent, cell opening agent, citric acid, modified nano silica sol, nano-grade ceramic powder, nano zinc oxide, aminoethyl heptadecanyl imidazoline, antibacterial agent, and flame retardant, through high-temperature mixing and foaming processes.
A slow-rebound sponge that is resistant to high-temperature compression and does not deform permanently has been prepared. It can maintain its shape at high temperatures and has excellent resilience.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of sponges, in particular to a high-temperature resistant compression permanent non-deformation slow-rebound sponge. Background Art
[0002] The commonly used sponges are made of wood cellulose fibers or foamed plastic polymers. In addition, there are also natural sponges made from sponge animals. Most natural sponges are used for body cleaning or painting. Sponge products have gradually become popular in people's lives, including seats, sofas, mattresses and other household items made of sponges. Polyether polyols are the main raw materials for the production of polyurethane sponges. The polyether polyols generally used in the production of existing polyurethane sponges usually use petroleum polyether polyols.
[0003] At present, high-PO polyether polyols and polymer polyols are used as raw materials. During the use of sponges, they are highly sensitive to temperature, are not resistant to high temperatures, and are prone to deformation after compression. Summary of the invention
[0004] The purpose of the present invention is to provide a high temperature resistant compression permanent non-deformation slow rebound sponge to solve the problems raised in the above background technology.
[0005] To achieve the above object, the present invention provides the following technical solution: a high temperature resistant compression permanent non-deformation slow rebound sponge, comprising the following raw materials in percentage by weight:
[0006] Polyethylene oxide polyether polyol 45-50%;
[0007] Modified slow rebound polyether polyol 10-25%;
[0008] Foaming agent 1-3%;
[0009] Silicone oil 0.5-1%;
[0010] Foaming agent 0.5-1%;
[0011] Cell opener 0.5-1%;
[0012] Citric acid 0.5-1%;
[0013] Modified nano silica sol 4-5%;
[0014] Nano-grade ceramic powder 0.5-1%;
[0015] Nano zinc oxide 0.5-1%;
[0016] Aminoethyl heptadecenyl imidazoline 1-2%;
[0017] Antimicrobial agent 0.5-1%;
[0018] Flame retardant 0.5-1%.
[0019] Preferably, 15-20% of the modified slow-rebound polyether polyol is 20-40 mass fractions of a polyether polyol with a molecular weight of 1000 or 20-40 mass fractions of a polyether polyol with a molecular weight of 700.
[0020] Preferably, the polyethylene oxide polyether polyol is a polyether polyol with a molecular weight of 4000.
[0021] Preferably, the pore opening agent is BDM-1.
[0022] Preferably, the silicone oil is silicone oil B8002.
[0023] Preferably, the antibacterial agent is prepared from nano silver powder and activated carbon powder.
[0024] Preferably, the flame retardant is prepared from phosphate ester, metal salt of organic phosphinate and polyphosphoamine.
[0025] Preferably, deionized water is added during the preparation process for high-temperature mixing.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] The invention provides a high-temperature resistant compression permanent non-deformation slow-rebound sponge. The high-temperature resistant compression permanent non-deformation slow-rebound sponge can be obtained by foaming polyethylene oxide polyether polyol, modified slow-rebound polyether polyol, and a foaming agent, and adding silicone oil, a uniform foaming agent, a pore opening agent, citric acid, modified nano-silica sol, nano-grade ceramic powder, nano-zinc oxide, aminoethyl heptadecenyl imidazoline, an antibacterial agent, and a flame retardant. DETAILED DESCRIPTION
[0028] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0029] Embodiment 1:
[0030] The present invention provides a technical solution: a high temperature resistant compression permanent non-deformation slow rebound sponge, comprising the following raw materials in percentage by weight:
[0031] Polyethylene oxide polyether polyol 50%;
[0032] Modified slow-rebound polyether polyol 25%;
[0033] Foaming agent 2%;
[0034] Silicone oil 1%;
[0035] Equalizing agent 1%;
[0036] Cell opener 1%;
[0037] Citric acid 1%;
[0038] Modified nano-silica sol 5%;
[0039] Nano-grade ceramic powder 1%;
[0040] Nano zinc oxide 1%;
[0041] Aminoethyl heptadecenyl imidazoline 2%;
[0042] Antimicrobial 1%;
[0043] Flame retardant 1%;
[0044] Deionized water 8%.
[0045] 15-20% of the modified slow-rebound polyether polyol is 20-40 parts by weight of a polyether polyol with a molecular weight of 1000 or 20-40 parts by weight of a polyether polyol with a molecular weight of 700, the polyethylene oxide polyether polyol is a polyether polyol with a molecular weight of 4000, the pore-opening agent is BDM-1, the silicone oil is silicone oil B8002, the antibacterial agent is prepared from nano silver powder and activated carbon powder, the flame retardant is prepared from phosphate ester, organic phosphinate metal salt and polyphosphoric acid amine, and deionized water is added during the preparation process for high-temperature mixing.
[0046] Pour polyethylene oxide polyether polyol, modified slow-rebound polyether polyol, foaming agent, silicone oil, uniform foaming agent, pore opening agent, citric acid, modified nano-silica sol, nano-ceramic powder, nano zinc oxide, aminoethyl heptadecenyl imidazoline, antibacterial agent, flame retardant and deionized water into a high-temperature mixing equipment for stirring and mixing. After the foaming is completed, pour it into the mold with a height of 50MM and perform high-temperature extrusion for 22 hours. The height is measured to be 25MM after half an hour.
[0047] Embodiment 2:
[0048] A high temperature resistant compression permanent non-deformation slow rebound sponge, comprising the following raw materials in percentage by weight:
[0049] Polyethylene oxide polyether polyol 45%;
[0050] Modified slow-rebound polyether polyol 15%;
[0051] Foaming agent 3%;
[0052] Silicone oil%1;
[0053] Equalizing agent 1%;
[0054] Cell opener 1%;
[0055] Citric acid 1%;
[0056] Modified nano-silica sol 5%;
[0057] Nano-grade ceramic powder 1%;
[0058] Nano zinc oxide 1%;
[0059] Aminoethyl heptadecenyl imidazoline 2%;
[0060] Antimicrobial 1%;
[0061] Flame retardant 1%;
[0062] Deionized water 22%.
[0063] 15-20% of the modified slow-rebound polyether polyol is 20-40 parts by weight of a polyether polyol with a molecular weight of 1000 or 20-40 parts by weight of a polyether polyol with a molecular weight of 700, the polyethylene oxide polyether polyol is a polyether polyol with a molecular weight of 4000, the pore-opening agent is BDM-1, the silicone oil is silicone oil B8002, the antibacterial agent is prepared from nano silver powder and activated carbon powder, the flame retardant is prepared from phosphate ester, organic phosphinate metal salt and polyphosphoric acid amine, and deionized water is added during the preparation process for high-temperature mixing.
[0064] Pour polyethylene oxide polyether polyol, modified slow-rebound polyether polyol, foaming agent, silicone oil, uniform foaming agent, pore opening agent, citric acid, modified nano-silica sol, nano-ceramic powder, nano zinc oxide, aminoethyl heptadecenyl imidazoline, antibacterial agent, flame retardant and deionized water into a high-temperature mixing equipment for stirring and mixing. After the foaming is completed, pour it into the mold with a height of 51MM and perform high-temperature extrusion for 22 hours. The height is measured to be 26MM after half an hour.
[0065] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A high temperature resistant compression permanent non-deformation slow rebound sponge, It is characterized in that The following raw materials are included in weight percentage: Polyethylene oxide polyether polyol 45-50%; Modified slow rebound polyether polyol 10-25%; Foaming agent 1-3%; Silicone oil 0.5-1%; Foaming agent 0.5-1%; Cell opener 0.5-1%; Citric acid 0.5-1%; Modified nano silica sol 4-5%; Nano-grade ceramic powder 0.5-1%; Nano zinc oxide 0.5-1%; Aminoethyl heptadecenyl imidazoline 1-2%; Antimicrobial agent 0.5-1%; Flame retardant 0.5-1%.
2. A high temperature resistant compression permanent non-deformation slow rebound sponge according to claim 1, Features: 15-20% of the modified slow-rebound polyether polyol is 20-40 mass fractions of a polyether polyol with a molecular weight of 1000 or 20-40 mass fractions of a polyether polyol with a molecular weight of 700.
3. A high temperature resistant compression permanent non-deformation slow rebound sponge according to claim 1, Features: The polyethylene oxide polyether polyol is a polyether polyol with a molecular weight of 4000.
4. The high temperature resistant compression permanent non-deformation slow rebound sponge according to claim 1, Features: The pore opening agent is BDM-1.
5. The high temperature resistant compression permanent non-deformation slow rebound sponge according to claim 1, Features: The silicone oil is silicone oil B8002.
6. The high temperature resistant compression permanent non-deformation slow rebound sponge according to claim 1, Features: The antibacterial agent is prepared from nano silver powder and activated carbon powder.
7. The high temperature resistant compression permanent non-deformation slow rebound sponge according to claim 1, Features: The flame retardant is prepared from phosphate ester, organic phosphinate metal salt and polyphosphoamine.
8. The high temperature resistant compression permanent non-deformation slow rebound sponge according to claim 1, Features: During the preparation process, deionized water is added for high temperature mixing.