Preparation of POP-1 / TpPa-1-COF composite material and application of POP-1 / TpPa-1-COF composite material in hydrogen production through water photolysis
By combining POP-1 with TpPa-1-COF to form a composite material, the problem of low electron migration efficiency of COFs photocatalysts is solved, the efficiency of photolysis of hydrogen production is significantly improved, and more efficient photocatalytic decomposition of water and hydrogen production is achieved. .
Patent Information
- Application Number
- CN202410332194.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-21
- Publication Date
- 2024-11-15
AI Technical Summary
The existing covalent organic framework materials (COFs) photocatalysts have photogenerated electron-hole recombination problems in the process of photocatalytic decomposition of water to produce hydrogen, resulting in low electron migration efficiency and limiting the improvement of the catalyst activity.
Using the preparation method of POP-1/TpPa-1-COF composite, the heptazine polymer POP-1 and TpPa-1-COF are combined to form a Z-type heterojunction, and the synthesis is improved by sonication and solvent thermal method. The photocatalytic properties of the material.
The efficiency of photolysis of hydrogen production by photolysis was significantly improved, from the original 2.67mmol·h-1·g-1 to 14.19~25.87mmol·h-1·g-1, enhancing the electron migration efficiency of the photocatalyst.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] The invention relates to the preparation of a POP-1 / TpPa-1-COF composite material and its application in producing hydrogen by photolysis of water. Background Art
[0002] With the rapid economic development and the increasing population, energy and environmental issues are urgent problems that need to be solved. It is of great significance for us to cope with energy and environmental challenges by rationally utilizing resources and energy, handling the relationship between man and nature, and finding a clean energy. As a potential energy carrier, hydrogen energy has a combustion calorific value three times that of gasoline and has the advantages of being green, pollution-free, low in density and easy to transport. Therefore, the production of hydrogen by decomposing water through solar energy is undoubtedly an ideal conversion pathway. The development of efficient catalysts, the maximum use of visible light, and the improvement of electron-hole separation efficiency are still the key in this field.
[0003] Covalent organic frameworks (COFs) are porous crystalline materials formed by covalently connecting light elements such as C, B, O, N and Si. They have the advantages of light weight, low density, high specific surface area, regular structure, uniform pores, relatively stable structure, and easy functional modification. COFs have great potential for application in many fields such as gas storage and separation, catalysis, sensing, energy storage, and photoelectric conversion. However, single-component COFs photocatalysts have serious photogenerated electron-hole recombination problems, which limits the further improvement of COFs photocatalyst hydrogen production activity. Therefore, how to improve the electron transfer efficiency of the catalyst has become a research hotspot in the field of photocatalysis.
[0004] POP-1 is a heptazine-based porous organic polymer generated by the reaction of trichloroheptazine with anhydrous piperazine via nucleophilic substitution. 3 N is beneficial to improve the electron mobility of its π-conjugated structure, and heptazine itself is also an excellent photogenerated carrier redox active site. Therefore, the development and utilization of heptazine-based polymer materials with suitable energy bands is of great significance in the field of photocatalysis. Summary of the invention
[0005] The purpose of the present invention is to solve the problem that the efficiency of photocatalytic water decomposition to produce hydrogen is low in existing materials, and to provide a preparation method of a POP-1 / TpPa-1-COF composite material and its application in photocatalytic water decomposition to produce hydrogen.
[0006] The preparation method of a POP-1 / TpPa-1-COF composite material of the present invention is completed by the following steps: Preparation of POP-1 / TpPa-1-COF composite material: Heptazine polymer (POP-1), 1,4-diaminobenzene and 1,3,5-trialdehyde phloroglucinol were added into a heat-resistant glass tube, followed by a mixed solution of N,N-dimethylformamide (DMF) and acetic acid, and ultrasonically treated for 30 to 35 minutes at an ultrasonic frequency of 40 kHz, and degassed by three freeze-thaw cycles in a liquid nitrogen bath, and then sealed and heated at 120 to 150°C for 72 to 120 hours, filtered and washed with tetrahydrofuran several times, and dried to obtain the POP-1 / TpPa-1-COF composite material;
[0007] Furthermore, in the above preparation method, the mass of the POP-1 is 3.3 to 44.4 mg; In the above-mentioned preparation method, the mass ratio of 1,4-diaminobenzene to 1,3,5-trialdehyde phloroglucinol is 1:1.31; In the above preparation method, the volume ratio of N,N-dimethylformamide to acetic acid is 6:1; In the above preparation method, the concentration of acetic acid used is 3 mol·L -1 ; The above preparation method, wherein the sealing is followed by heating at 120° C. for 72 hours; In the above-mentioned preparation method, a Z-type heterojunction is formed between the POP-1 and TpPa-1-COF;
[0008] Application of the POP-1 / TpPa-1-COF composite material provided by the present invention in photocatalytic water decomposition to produce hydrogen: In order to investigate the effect of POP-1 / TpPa-1-COF material on catalytic decomposition of water to produce hydrogen, the visible light photocatalytic decomposition of water to produce hydrogen was tested according to the following method. The test process is as follows: POP-1 / TpPa-1-COF (10 mg) was used as a photocatalyst, sodium L-ascorbate (100 mg) was used as a sacrificial agent, H2PtCl6 6H2O (0.1 mL, 3 mg mL -1 ) as a co-catalyst, PBS buffer solution (50 mL, 0.1 mol·L -1 , pH = 7) as the reaction solution, ultrasonic for 30 min to form a uniform suspension and a xenon lamp (λ>420nm) as the light source for testing.
[0009] Beneficial effects of the present invention: The invention combines TpPa-1-COF with a polymer containing heptazine rings, POP-1, to synthesize a new photocatalytic material POP-1 / TpPa-1-COF, which effectively improves the performance of photocatalytic water splitting to produce hydrogen. Figure 1 As shown in Figure 2, the hydrogen production efficiency of TpPa-1-COF synthesized by the solvothermal method is 2.67 mmol·h-1 ·g -1 The efficiency of hydrogen production from photolysis of water by POP-1 / TpPa-1-COF composite material was increased to 14.19~25.87mmol·h -1 ·g -1 . BRIEF DESCRIPTION OF THE DRAWINGS
[0010] Figure 1 This is the performance diagram of the photocatalytic water decomposition and hydrogen production of POP-1 / TpPa-1-COF material.
[0011] Figure 2 is the X-ray powder diffraction pattern of POP-1 / TpPa-1-COF material;
[0012] Figure 3 Infrared spectra of POP-1 and TpPa-1-COF materials; DETAILED DESCRIPTION
[0013] The present invention is further described below with reference to examples. These examples are only used to illustrate the method of the present invention and have no limitation on the scope of application of the present invention.
[0014] Example 1: The preparation of a POP-1 / TpPa-1-COF material of this embodiment is completed by the following steps: 1. Preparation of trichloroheptylazine (C6N7Cl3): Melamine was placed in a crucible and calcined at 500°C in a muffle furnace for 8 hours to obtain a light yellow solid. The product was washed three times with ethanol and dried in a vacuum at 80°C to obtain g-C3N4 and heated and dissolved in a KOH aqueous solution. White crystals (potassium salt of cyanuric acid) were obtained after cooling. 2 g of the white crystals and 10 g of PCl5 were weighed and reacted under a nitrogen atmosphere for 5 hours to obtain a yellow-green solid. The yellow-green crystalline 2,5,8-trichloro-1,3,3a1,4,6,7,9-heptazobenzene (trichloroheptylazine) was obtained after washing and filtering with deionized water. 2. Preparation of POP-1: Weigh samples of anhydrous piperazine and trichloroheptazine (C6N7Cl3) (molar ratio = 2:3) and dissolve them in tetrahydrofuran solvent respectively. Add the tetrahydrofuran solution of piperazine to the solution of trichloroheptazine and stir until mixed evenly. Rapid formation of precipitate can be observed. After stirring for 3 hours, wash several times with water and tetrahydrofuran. Then Soxhlet extraction in tetrahydrofuran for 24 hours. After vacuum drying for 48 hours, the final product is obtained; 3. Preparation of POP-1 / TpPa-1-COF composite material: POP-1 (3.3 mg), 1,4-diaminobenzene (16 mg) and 1,3,5-trialdehyde phloroglucinol (21 mg) were added to a heat-resistant glass tube, followed by N,N-dimethylformamide (3 mL) and acetic acid (0.5 mL, 3 mol·L-1 ) was ultrasonically treated for 30 min at an ultrasonic frequency of 40 kHz, degassed by three freeze-thaw cycles in a liquid nitrogen bath, sealed, heated at 120 °C for 72 h, filtered, washed several times with tetrahydrofuran, and dried to obtain a POP-1 / TpPa-1-COF (mass ratio of 1:9) composite material.
[0015] Example 2: This embodiment differs from Example 1 in that the mass of POP-1 described in step 3 is 7.4 mg, and the other steps and parameters are the same as those in Example 1; a POP-1 / TpPa-1-COF (mass ratio is 2:8) composite material is obtained.
[0016] Example 3: This embodiment differs from Example 1 or 2 in that the mass of POP-1 described in step 3 is 12.7 mg, and the other steps and parameters are the same as those in Example 1 or 2; a POP-1 / TpPa-1-COF (mass ratio is 3:7) composite material is obtained.
[0017] Example 4: This embodiment differs from Examples 1 to 3 in that the mass of POP-1 described in step 3 is 19.7 mg, and the other steps and parameters are the same as those of Examples 1 to 3; a POP-1 / TpPa-1-COF (mass ratio of 4:6) composite material is obtained.
[0018] Example 5: This embodiment differs from Examples 1 to 4 in that the mass of POP-1 described in step 3 is 29.6 mg, and the other steps and parameters are the same as those of Examples 1 to 4; a POP-1 / TpPa-1-COF (mass ratio of 5:5) composite material is obtained.
[0019] Example 6: This embodiment differs from Examples 1 to 5 in that the mass of POP-1 described in step 3 is 44.4 mg, and the other steps and parameters are the same as those of Examples 1 to 4; a POP-1 / TpPa-1-COF (mass ratio is 6:4) composite material is obtained.
[0020] To verify the beneficial effects of the present invention, the following tests were performed: 1. X-ray diffraction (XRD) analysis: Use X-rays of sufficient energy to irradiate the sample. The substances in the sample are excited and produce secondary fluorescent X-rays. The position of the diffraction angle (peak position) is used to perform qualitative analysis of the compound. It has been determined that the crystal form of the POP-1 / TpPa-1-COF composite material provided by the present invention is consistent with the single crystal diffraction simulation and has the characteristic peaks of the monomer. 2. Infrared spectroscopy test: Determine the molecular structure of the compound through infrared spectroscopy, compare the spectrum of the standard, determine the characteristic functional groups, and assist in XRD testing to determine that the product has been successfully synthesized.
Claims
1. Preparation of a POP-1 / TpPa-1-COF composite material, characterized in that The method proceeds as follows:
1. Preparation of POP-1 / TpPa-1-COF composite material: Heptazine polymer (POP-1), 1,4-diaminobenzene and 1,3,5-trialdehyde phloroglucinol were added to a heat-resistant glass tube, followed by N,N-dimethylformamide (DMF), and ultrasonic treatment was performed at an ultrasonic frequency of 35 to 45 kHz for 30 to 35 min, followed by the addition of 3 mol·L -1 The acetic acid solution was cyclically frozen and degassed in liquid nitrogen three times, sealed, heated at 120°C for 72h, filtered and washed with tetrahydrofuran several times, and vacuum dried at 60°C to obtain a red powder, which is the POP-1 / TpPa-1-COF composite material.
2. The preparation of a POP-1 / TpPa-1-COF composite material according to claim 1, characterized in that Preparation of the Z-type heterojunction of POP-1 and TpPa-1-COF described in step 1.
3. The preparation of a POP-1 / TpPa-1-COF composite material according to claim 1, characterized in that The optimal performance-to-mass ratio of POP-1 to TpPa-1-COF described in step 1 is 4:6.