Smelting process of high-alloy ultra-pure steel

Through the combined smelting process of electric arc furnace, ladle refining furnace and vacuum refining furnace, the addition of high-quality scrap steel, aluminum wire and calcium wires is solved, and the problem of removing inclusions in smelting in high-alloy ultrapure steel is realized. High standard pure finished product.

CN118957390APending Publication Date: 2024-11-15NANJING IRON & STEEL CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410928489.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The prior art is difficult to effectively smelve high alloy ultrapure steel, especially in improving the fatigue life and performance of steel.

Method used

Using a smelting process combining electric arc furnace, ladle refining furnace and vacuum refining furnace, the ratio of calcium oxide to aluminum trioxide and vacuum refining furnace is controlled through the combination of high-quality scrap steel and water iron, the use of aluminum wire and refined lime, and the vacuum refining of calcium wires. Time to achieve effective removal of inclusions.

Benefits of technology

A high alloy ultrapure steel smelting process was successfully developed, so that the sum of the coarse and fine systems of Class A, B, C, and D inclusions of the finished product did not exceed 1.0, meeting the requirements of high standards of purity.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a smelting process of high-alloy ultra-pure steel, which relates to the technical field of metallurgy and comprises the following steps: smelting in an electric arc furnace: smelting by combining high-quality scrap steel and molten iron; smelting in a ladle refining furnace: deoxidizing by adopting aluminum, adding an aluminum wire and refining lime for refining; and smelting in a vacuum refining furnace: adding a calcium line for vacuum refining. The smelting route of the electric arc furnace, the ladle refining furnace and the vacuum refining furnace is adopted, the high-alloy ultra-pure steel smelting process is developed, and the finished product meets the requirement that the sum of the coarse series and the fine series of A, B, C and D type inclusions does not exceed 1.0 level.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metallurgy, in particular to a smelting process of high-alloy ultra-pure steel. Background Art

[0002] In the development of the high alloy steel market, on the one hand, the performance of high alloy steel is continuously improved by designing its chemical composition. On the other hand, due to the application requirements of high fatigue life, ultra-purity has become an important research direction for smelting production. Summary of the invention

[0003] The technical problem to be solved by the present invention is to overcome the disadvantages of the prior art and provide a smelting process for high-alloy ultra-pure steel.

[0004] In order to solve the above technical problems, the technical solution of the present invention is as follows: A smelting process for high-alloy ultra-pure steel, comprising: Electric arc furnace smelting: using high-quality scrap steel and molten iron for smelting; Ladle refining furnace smelting: aluminum is used for deoxidation, and aluminum wire and refining lime are added for refining; Vacuum refining furnace smelting: adding calcium wire for vacuum refining.

[0005] As a preferred solution of the smelting process of the high-alloy ultra-pure steel of the present invention, the ratio of molten iron in the combination of high-quality scrap steel and molten iron is 50%-80%.

[0006] As a preferred solution of the smelting process of the high-alloy ultra-pure steel of the present invention, in the smelting in the ladle refining furnace, the amount of aluminum wire added is 100-150m, and the amount of refining lime added is 200-300kg.

[0007] As a preferred solution of the smelting process of the high-alloy ultra-pure steel of the present invention, the ratio of calcium oxide to aluminum oxide in the refining slag during smelting in the ladle refining furnace is greater than or equal to 1.3.

[0008] As a preferred solution of the smelting process of the high-alloy ultra-pure steel of the present invention, the white slag retention time in the ladle refining furnace is greater than or equal to 30 minutes.

[0009] As a preferred solution of the smelting process of the high-alloy ultra-pure steel of the present invention, in the smelting process of the vacuum refining furnace, the amount of calcium wire added is 50-100m.

[0010] As a preferred solution of the smelting process of the high-alloy ultra-pure steel of the present invention, the ultimate vacuum time of the smelting process in the vacuum refining furnace is greater than or equal to 15 minutes, and the static stirring time is greater than or equal to 30 minutes.

[0011] The beneficial effects of the present invention are: The present invention develops a high-alloy ultra-pure steel smelting process by adopting an electric arc furnace + ladle refining furnace + vacuum refining furnace smelting route, and the finished product meets the requirement that the sum of coarse and fine inclusions of A, B, C, and D types does not exceed level 1.0. DETAILED DESCRIPTION

[0012] In order to make the content of the present invention more clearly understood, the present invention is further described in detail below according to specific implementation methods.

[0013] The embodiment of the present application provides a smelting process for high-alloy ultra-pure steel, which includes arc furnace smelting, ladle refining furnace smelting and vacuum refining furnace smelting in sequence. By adopting the smelting process, the high-alloy steel product meets the requirement that the sum of coarse and fine inclusions of A, B, C and D types does not exceed 1.0 level.

[0014] Specifically, for the EAF electric arc furnace smelting process, a combination of high-quality scrap steel and molten iron is used for smelting, and the proportion of molten iron is 50%-80%. The high proportion of molten iron is used to dilute the residual elements, providing the basic conditions for the smelting of ultra-pure steel.

[0015] For the LF ladle refining furnace smelting process, aluminum is used for deoxidation, aluminum wire and refining lime are added for refining, and the ratio of calcium oxide to aluminum oxide in the refining slag is controlled to be greater than or equal to 1.3, and the white slag retention time is ≥30 minutes to maintain the strong inclusion adsorption capacity of the refining slag and promote the removal of inclusions in the molten steel.

[0016] Among them, the addition amount of aluminum wire is 100-150m, and the addition amount of refined lime is 200-300kg.

[0017] For the smelting process of the vacuum refining furnace, calcium wire is added for vacuum refining, and the ultimate vacuum time is controlled to be ≥15min, and the static stirring time is ≥30min. Ca is used to denature the inclusions to generate low-melting calcium aluminate inclusions that are easy to float. Through argon blowing and stirring, the inclusions float to the top slag for adsorption and removal; at the same time, the ultimate vacuum and carbon-oxygen reduction reaction are used to further remove the oxide inclusions.

[0018] Among them, the amount of calcium wire added is 50-100m.

[0019] The above process is described below by means of specific embodiments: (1) EAF process: A combination of high-quality scrap steel and molten iron is used, with a molten iron ratio of 65%. A high proportion of molten iron is used to dilute the residual elements, providing basic conditions for the smelting of ultra-pure steel.

[0020] (2) LF process: Aluminum is used for deoxidation. 120 m of aluminum wire and 230 kg of refined lime are added. The refining slag CaO / Al2O3=1.4 is kept for 30 min. The strong adsorption capacity of the refining slag for inclusions is maintained to promote the removal of inclusions in the molten steel.

[0021] (3) VD process: add 60m of calcium wire, extreme vacuum time 15min, static stirring time 30min. Ca is used to denature inclusions to generate low-melting calcium aluminate inclusions that are easy to float. Through argon blowing and stirring, the inclusions float to the top slag for adsorption and removal; at the same time, extreme vacuum and carbon-oxygen reduction reaction are used to further remove oxide inclusions.

[0022] The above process was used to produce high alloy ultra-pure steel No. 1 to No. 10. The finished products were tested according to GB / T 10561 standard. The sum of the coarse inclusions of A, B, C, and D types was ≤0.5, and the sum of the fine inclusions was ≤1.0. All the tests were qualified. The results are shown in Table 1:

[0023] Table 1 It can be seen from Table 1 that for the above-mentioned high-alloy ultra-pure steels No. 1 to 10, the sum of the coarse inclusions of A, B, C, and D types is ≤0.5 level, and the sum of the fine inclusions is ≤1.0 level, and all of them have passed the test.

[0024] Therefore, the technical solution of the present application develops a high-alloy ultra-pure steel smelting process by adopting an electric arc furnace + ladle refining furnace + vacuum refining furnace smelting route, and the finished product meets the requirement that the sum of coarse and fine inclusions of types A, B, C, and D does not exceed level 1.0.

[0025] In addition to the above embodiments, the present invention may also have other implementation modes; any technical solutions formed by equivalent replacement or equivalent transformation shall fall within the protection scope required by the present invention.

Claims

1. A smelting process for high-alloy ultra-pure steel, characterized in that: include: Electric arc furnace smelting: using high-quality scrap steel and molten iron for smelting; Ladle refining furnace smelting: aluminum is used for deoxidation, and aluminum wire and refining lime are added for refining; Vacuum refining furnace smelting: adding calcium wire for vacuum refining.

2. The smelting process of high alloy ultra-clean steel according to claim 1, characterized in that: The ratio of molten iron in the combination of high-quality scrap steel and molten iron is 50%-80%.

3. The smelting process of high alloy ultra-clean steel according to claim 1, characterized in that: During the smelting in the ladle refining furnace, the amount of aluminum wire added is 100-150m, and the amount of refining lime added is 200-300kg.

4. The smelting process of high alloy ultra-pure steel according to claim 1, characterized in that: The ratio of calcium oxide to aluminum oxide in the refining slag during smelting in the ladle refining furnace is greater than or equal to 1.

3.

5. The smelting process of high alloy ultra-clean steel according to claim 1, characterized in that: The white slag retention time during smelting in the ladle refining furnace is greater than or equal to 30 minutes.

6. The smelting process of high alloy ultra-clean steel according to claim 1, characterized in that: In the vacuum refining furnace smelting process, the amount of calcium wire added is 50-100m.

7. The smelting process of high alloy ultra-clean steel according to claim 1, characterized in that: The ultimate vacuum time of the vacuum refining furnace smelting process is greater than or equal to 15 minutes, and the static stirring time is greater than or equal to 30 minutes.

Citation Information

Cited By

  • Deep purification smelting method for high-purity steel

    CN119663094A