Spring steel machining method, steel plate spring and automobile

By using composite microalloying and process optimization of specific elements in the steel spring materials, the problem that existing spring steel materials cannot meet the requirements of high tensile strength and yield strength is solved, and the comprehensive performance and fatigue life of the steel spring are significantly improved.

CN118957453APending Publication Date: 2024-11-15DONGFENG COMML VEHICLE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410990184.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing spring steel materials cannot meet the requirements of steel leaf springs for high tensile strength, yield strength and toughness, which affects the performance of steel leaf springs.

Method used

Use spring steel materials of specific components, including composite microalloying of elements such as C, Si, Mn, Cr, Ni, Mo, V, Nb, Ti, Al and N, and refine the grains through quenching and tempering. Improve the tensile strength, yield strength and toughness of the material, and optimize the comprehensive mechanical properties of the material through blind holes, phosphorus removal and shot peening processes.

Benefits of technology

The high tensile strength of the steel spring is 1950-2100MPa, the yield strength of 1700-1850MPa, the elongation after breaking ≥9%, and the cross-section shrinkage rate is ≥30%, and the fatigue life is significantly improved to ≥200,000 times, improving the product's Quality and load carrying capacity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957453A_ABST
    Figure CN118957453A_ABST
Patent Text Reader

Abstract

The invention discloses a machining method of spring steel, a steel plate spring and an automobile, and relates to the technical field of vehicles. The raw materials comprise the following components in percentage by mass: 0.57%-0.62% of C; si: 1.22% to 1.38%; 0.70% to 1.10% of Mn; 0.90% to 1.20% of Cr; 0.20% to 2.00% of Ni; 0.08% to 0.10% of Mo; v: 0.15% to 0.25%; 0.02% to 0.04% of Nb; 0.010% to 0.018% of Ti; 0.010% to 0.040% of Al; n: 0.0040% to 0.0080%; less than or equal to 0.020% of P; less than or equal to 0.020% of S, and the balance Fe and inevitable impurity elements; the machining method of the spring steel comprises the following steps that raw materials of the spring steel are subjected to blanking, drilling, rolling, quenching and tempering treatment, and the spring steel is obtained; wherein the quenching temperature ranges from 850 DEG C to 930 DEG C. And the reeds with the thickness of less than 50mm can be completely quenched, so that the heat treatment quality of the high-use-stress steel plate spring is ensured, the obdurability and tensile strength of the material are improved, and the fatigue life of the material is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of automobile technology, and in particular to a spring steel processing method, a leaf spring and an automobile. Background Art

[0002] Leaf spring is an elastic element widely used in automobile suspension systems. It is composed of multiple or single alloy spring leaves to form an elastic beam of approximately equal strength. It not only enables it to withstand a large weight, but also has a certain shock-absorbing effect due to the friction between the leaves.

[0003] Leaf springs are widely used in non-independent suspension systems, especially in heavy-duty vehicles such as trucks and large buses. Due to its simple structure and high load-bearing capacity, it has become the preferred component for these heavy vehicles.

[0004] Leaf springs require materials to have high tensile strength and yield strength as well as high toughness, but existing spring steel materials cannot meet the requirements at the same time, which affects the use of leaf springs. Summary of the invention

[0005] The present application provides a spring steel processing method, a leaf spring and an automobile, so as to solve the problem that the existing spring steel materials cannot meet the requirements at the same time, thus affecting the use of the leaf spring.

[0006] In a first aspect, the present application provides a method for processing spring steel, wherein the raw materials thereof include, by mass fraction, the following: C: 0.57%-0.62%; Si: 1.22%-1.38%; Mn: 0.70%-1.10%; Cr: 0.90%-1.20%; Ni: 0.20-2.00%; Mo: 0.08%-0.10%; V: 0.15%-0.25%; Nb: 0.02%-0.04%|; Ti: 0.010%-0.018%; Al: 0.010%-0.040%; N: 0.0040%-0.0080%; P: ≤0.020%; S: ≤0.020%, and the remainder is Fe and unavoidable impurity elements;

[0007] The processing method of the spring steel comprises the following steps:

[0008] The raw materials of spring steel are cut, drilled, rolled, quenched and tempered to obtain spring steel;

[0009] Among them: the quenching temperature is 850~930℃.

[0010] In this application, the high-stress steel leaf spring is used under high stress conditions, and its sensitivity to defects is enhanced, which requires the material to have high tensile strength and yield strength while having high toughness. Grain refinement is an effective way to improve the strength and toughness of the material. Through composite microalloying of elements such as V, Nb, Ti, Als and N, the material has fine grains with a grain size ≥10 levels. The comprehensive mechanical properties of the material are improved. The material with a thickness of less than 50mm can be fully hardened, ensuring the heat treatment quality of the high-stress steel leaf spring. The strength and toughness of the material are improved, with a tensile strength of 1950-2100MPa and a yield strength of 1700-1850MPa; the elongation after fracture is ≥9%, and the cross-sectional shrinkage is ≥30%. The fatigue performance of high-stress steel leaf spring products is improved, and the fatigue life of the steel leaf spring (test stress 850±550MPa) is ≥200,000 times, which improves the product quality and bearing capacity.

[0011] C is the main strengthening element in steel and the element that contributes most to the strength of steel. In order to ensure that the tensile strength of the material is greater than 1950MPa and has high tempering stability, the C mass fraction must be no less than 0.57%. However, as the C mass fraction increases, the plasticity and toughness of the steel will decrease. In order to ensure that the material has good comprehensive mechanical properties, the C mass fraction should be no more than 0.62%.

[0012] Si is the main alloying element in spring steel. It has a solid solution strengthening effect and can significantly improve the elastic limit, yield strength and tensile strength of steel. Si can change the number, size and shape of carbides precipitated during tempering and improve the tempering stability of steel. At the same time, too high Si mass fraction will significantly increase the decarburization tendency. In order to ensure that the material has better comprehensive mechanical properties and less surface decarburization, the Si mass fraction is 1.22-1.38%.

[0013] Mn is the most effective alloying element for improving the hardenability of steel. It dissolves into ferrite to play a solid solution strengthening role. However, too high a Mn content will significantly reduce toughness and also produce a large amount of residual austenite. Therefore, the mass fraction of Mn is 0.70% to 1.10%.

[0014] Cr can significantly improve the hardenability of steel, and the effect is better when used together with Mn. Cr can reduce the activity of C in steel, and is also a carbide-forming element, which increases the activation energy of C diffusion in steel and reduces the decarburization tendency of steel. When the Cr content is high, the tempering structure will be uneven, reducing the spring steel's anti-elasticity and toughness. Therefore, the mass fraction of Cr in the material of the present invention is 0.90% to 1.20%.

[0015] Ni can stabilize austenite, enhance the hardenability of steel, and significantly improve the toughness and corrosion resistance of the material. Too much Ni will form a large amount of residual austenite during quenching. At the same time, Ni is costly, so it is not advisable to add a high amount of Ni to steel. The mass fraction of Ni is 0.20-2.00%.

[0016] Mo can improve the hardenability of steel, prevent temper brittleness, improve the fatigue performance of leaf springs, and inhibit surface decarburization of steel. However, Mo is expensive, so the mass fraction of Mo is 0.08% to 0.10%.

[0017] V and Nb are both strong carbide-forming elements. The fine and dispersed MC-type carbides precipitated in the solid state have a strong precipitation strengthening effect, which can improve the strength and hardness of steel. At the same time, V and Nb can prevent grain growth and play a role in grain refinement. However, when the V and Nb content is too high, the grain refinement effect is significantly reduced, and the material cost is increased. The mass fraction of V is 0.15% to 0.25%, and the mass fraction of Nb is 0.02% to 0.04%.

[0018] Ti has a strong affinity with N, O, and C. It is a good deoxidizing and degassing agent and an effective element for fixing N and C. Ti can make the internal structure dense and improve the strength of steel. TiC particles can prevent the growth of steel grains. Too high Ti content will lead to the precipitation of a large amount of carbonitrides at high temperatures, and its size will be large and the cross-sectional shrinkage will decrease. Therefore, the mass fraction of Ti in the material of the present invention is 0.010% to 0.018%.

[0019] Al is a deoxidizing and nitrogenating agent during steelmaking. Al is an impurity element in steel, and N is also a harmful element to steel. Al has a great affinity for N, but the combination of an appropriate amount of Al and N can generate an appropriate amount of fine AlN particles, which can improve the steel's anti-elasticity and durability. At the same time, AlN can refine the grains and improve toughness and plastic deformation ability. Therefore, the mass fraction of Al is 0.010% to 0.040%, and the mass fraction of N is 0.0040% to 0.0080%.

[0020] In some embodiments, the central positioning hole of the drilled hole is a blind hole, wherein: the depth of the central positioning hole is h, and the thickness of the spring steel is d:

[0021] 1 / 3≤h / d≤1 / 2. In order to reduce stress concentration, avoid the breakage of the leaf spring from the center hole during use, and increase the fatigue life of the leaf spring with high use stress, blind holes can be used to meet the positioning requirements and improve the processing accuracy.

[0022] In some embodiments, a dephosphorization treatment is further performed after the drilling and before the rolling, wherein:

[0023] The water pressure of dephosphorization treatment is 15-25MPa. Dephosphorization treatment can effectively remove the oxide scale produced during rolling and heating, and improve the surface quality of leaf springs.

[0024] In some embodiments, a heat preservation cooling process is further included after the rolling and before the quenching, and the termination temperature of the heat preservation cooling is less than or equal to 200° C. The material has high hardenability, and a slow cooling process, i.e., heat preservation cooling process, is used after rolling to eliminate the internal thermal stress of rolling and avoid cracks in the material during the cooling process.

[0025] In some embodiments, the quenching time is 30 to 200 minutes; and / or,

[0026] The initial temperature of the parts during quenching is 780-850°C.

[0027] Decarburization on the material surface will reduce the surface strength and thus reduce fatigue life. Due to the high Si content, there is a strong tendency for decarburization, so anti-decarburization coating needs to be applied before quenching heating to reduce surface decarburization generated during quenching heating.

[0028] In some embodiments, a cooling process is further included after the quenching and before the tempering, wherein:

[0029] The cooling rate of the cooling treatment is greater than or equal to 1°C / s, which can improve the mechanical properties of the material and increase the tensile strength and yield strength of the material.

[0030] In some embodiments, the tempering temperature is 380-450° C., which can improve the mechanical properties of the material and improve the tensile strength and yield strength of the material; and / or,

[0031] The tempering time is 30 to 300 minutes, which can improve the mechanical properties of the material and improve the tensile strength and yield strength of the material.

[0032] In some embodiments, the tempering treatment further includes shot peening treatment, wherein the shot peening treatment includes a first shot peening treatment and a second shot peening treatment:

[0033] The diameter of the steel shot in the first shot peening treatment is 1.0 to 1.4 mm; and / or,

[0034] The first shot peening treatment lasts for 60 to 180 seconds; and / or,

[0035] The diameter of the steel shot in the second shot peening treatment is 0.3 to 0.8 mm; and / or,

[0036] The first shot peening treatment takes 60 to 180 seconds.

[0037] First, coarser steel shot (diameter 1.0 ~ 1.4mm) is used for shot peening to form a higher residual compressive stress (≥500Mpa) on the material surface; then finer steel shot (diameter 0.3 ~ 0.8mm) is used for shot peening to improve the surface quality of the material and reduce the surface roughness of the reed.

[0038] In a second aspect, the present application provides a leaf spring, comprising spring steel produced by the spring steel processing method of the first aspect.

[0039] In a third aspect, the present application provides a vehicle comprising the leaf spring of the second aspect. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0041] Figure 1 This is the hardenability curve of the leaf spring in the spring steel processing method of Example 1 of the present application.

[0042] Figure 2 This is the grain growth curve of the leaf spring in the spring steel processing method of Example 1 of the present application.

[0043] Figure 3 This is the tempering stability curve of the leaf spring in the spring steel processing method of Example 1 of the present application.

[0044] Figure 4 This is a metallographic structure diagram of a leaf spring in the spring steel processing method of Example 1 of the present application.

[0045] Figure 5 This is a grain size diagram of the leaf spring in the spring steel processing method of Example 1 of the present application. DETAILED DESCRIPTION

[0046] In order to make the purpose, technical solution and advantages of the present application clearer, the technical solution of the present application will be clearly and completely described below in combination with the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present application.

[0047] Leaf spring is an elastic element widely used in automobile suspension systems. It is composed of multiple or single alloy spring leaves to form an elastic beam of approximately equal strength. It not only enables it to withstand a large weight, but also has a certain shock-absorbing effect due to the friction between the leaves.

[0048] Leaf springs are widely used in non-independent suspension systems, especially in heavy-duty vehicles such as trucks and large buses. Due to its simple structure and high load-bearing capacity, it has become the preferred component for these heavy vehicles.

[0049] Leaf springs require materials to have high tensile strength and yield strength as well as high toughness, but existing spring steel materials cannot meet the requirements at the same time, which affects the use of leaf springs.

[0050] 60Si2CrV is the material with the highest tensile strength in the national standard GB / T133164.1 "Spring Steel for Automobile Suspension System Part 1: Hot-rolled Flat Steel", with a tensile strength of not less than 1860MPa. However, 60Si2CrV has low toughness, with an elongation of 6-7% after fracture and a cross-sectional shrinkage of 20-25%. If used in high-stress leaf springs, it is prone to early fracture. 60Si2CrV has low hardenability, with J15 being 56HRC, and can only be used for leaf springs with a thickness of less than 24mm, which cannot fully meet the needs of high-stress leaf springs.

[0051] In view of this, the present application provides a spring steel processing method, a leaf spring and an automobile to solve the problem that the existing spring steel materials cannot meet the requirements at the same time, thus affecting the use of the leaf spring.

[0052] In a first aspect, the present application provides a method for processing spring steel, wherein the raw materials thereof include, by mass fraction, the following: C: 0.57%-0.62%; Si: 1.22%-1.38%; Mn: 0.70%-1.10%; Cr: 0.90%-1.20%; Ni: 0.20-2.00%; Mo: 0.08%-0.10%; V: 0.15%-0.25%; Nb: 0.02%-0.04%|; Ti: 0.010%-0.018%; Al: 0.010%-0.040%; N: 0.0040%-0.0080%; P: ≤0.020%; S: ≤0.020%, and the remainder is Fe and unavoidable impurity elements;

[0053] The processing method of the spring steel comprises the following steps:

[0054] The raw materials of spring steel are cut, drilled, rolled, quenched and tempered to obtain spring steel;

[0055] Among them: the quenching temperature is 850~930℃.

[0056] In this application, the high-stress steel leaf spring is used under high stress conditions, and its sensitivity to defects is enhanced, which requires the material to have high tensile strength and yield strength while having high toughness. Grain refinement is an effective way to improve the strength and toughness of the material. Through composite microalloying of elements such as V, Nb, Ti, Als and N, the material has fine grains with a grain size ≥10 levels. The comprehensive mechanical properties of the material are improved. The material with a thickness of less than 50mm can be fully hardened, ensuring the heat treatment quality of the high-stress steel leaf spring. The strength and toughness of the material are improved, with a tensile strength of 1950-2100MPa and a yield strength of 1700-1850MPa; the elongation after fracture is ≥9%, and the cross-sectional shrinkage is ≥30%. The fatigue performance of high-stress steel leaf spring products is improved, and the fatigue life of the steel leaf spring (test stress 850±550MPa) is ≥200,000 times, which improves the product quality and bearing capacity.

[0057] C is the main strengthening element in steel and the element that contributes most to the strength of steel. In order to ensure that the tensile strength of the material is greater than 1950MPa and has high tempering stability, the C mass fraction must be no less than 0.57%. However, as the C mass fraction increases, the plasticity and toughness of the steel will decrease. In order to ensure that the material has good comprehensive mechanical properties, the C mass fraction should be no more than 0.62%.

[0058] Si is the main alloying element in spring steel. It has a solid solution strengthening effect and can significantly improve the elastic limit, yield strength and tensile strength of steel. Si can change the number, size and shape of carbides precipitated during tempering and improve the tempering stability of steel. At the same time, too high Si mass fraction will significantly increase the decarburization tendency. In order to ensure that the material has better comprehensive mechanical properties and less surface decarburization, the Si mass fraction is 1.22-1.38%.

[0059] Mn is the most effective alloying element for improving the hardenability of steel. It dissolves into ferrite to play a solid solution strengthening role. However, too high a Mn content will significantly reduce toughness and also produce a large amount of residual austenite. Therefore, the mass fraction of Mn is 0.70% to 1.10%.

[0060] Cr can significantly improve the hardenability of steel, and the effect is better when used together with Mn. Cr can reduce the activity of C in steel, and is also a carbide-forming element, which increases the activation energy of C diffusion in steel and reduces the decarburization tendency of steel. When the Cr content is high, the tempering structure will be uneven, reducing the spring steel's anti-elasticity and toughness. Therefore, the mass fraction of Cr in the material of the present invention is 0.90% to 1.20%.

[0061] Ni can stabilize austenite, enhance the hardenability of steel, and significantly improve the toughness and corrosion resistance of the material. Too much Ni will form a large amount of residual austenite during quenching. At the same time, Ni is costly, so it is not advisable to add a high amount of Ni to steel. The mass fraction of Ni is 0.20-2.00%.

[0062] Mo can improve the hardenability of steel, prevent temper brittleness, improve the fatigue performance of leaf springs, and inhibit surface decarburization of steel. However, Mo is expensive, so the mass fraction of Mo is 0.08% to 0.10%.

[0063] V and Nb are both strong carbide-forming elements. The fine and dispersed MC-type carbides precipitated in the solid state have a strong precipitation strengthening effect, which can improve the strength and hardness of steel. At the same time, V and Nb can prevent grain growth and play a role in grain refinement. However, when the V and Nb content is too high, the grain refinement effect is significantly reduced, and the material cost is increased. The mass fraction of V is 0.15% to 0.25%, and the mass fraction of Nb is 0.02% to 0.04%.

[0064] Ti has a strong affinity with N, O, and C. It is a good deoxidizing and degassing agent and an effective element for fixing N and C. Ti can make the internal structure dense and improve the strength of steel. TiC particles can prevent the growth of steel grains. Too high Ti content will lead to the precipitation of a large amount of carbonitrides at high temperatures, and its size will be large and the cross-sectional shrinkage will decrease. Therefore, the mass fraction of Ti in the material of the present invention is 0.010% to 0.018%.

[0065] Al is a deoxidizing and nitrogenating agent during steelmaking. Al is an impurity element in steel, and N is also a harmful element to steel. Al has a great affinity for N, but the combination of an appropriate amount of Al and N can generate an appropriate amount of fine AlN particles, which can improve the steel's anti-elasticity and durability. At the same time, AlN can refine the grains and improve toughness and plastic deformation ability. Therefore, the mass fraction of Al is 0.010% to 0.040%, and the mass fraction of N is 0.0040% to 0.0080%.

[0066] In combination with the first aspect, in some embodiments provided in the present application, the central positioning hole of the drilled hole is a blind hole, wherein: the depth of the central positioning hole is h, and the thickness of the spring steel is d: 1 / 3≤h / d≤1 / 2. In order to reduce stress concentration, avoid the leaf spring from breaking from the central hole during use, and improve the fatigue life of the stress leaf spring, a blind hole can be used to meet the positioning requirements and improve the processing accuracy.

[0067] In combination with the first aspect, in some embodiments provided in the present application, a dephosphorization treatment is further included after the drilling and before the rolling, wherein: the water pressure of the dephosphorization treatment is 15-25 MPa. The dephosphorization treatment can effectively remove the oxide scale generated during the rolling and heating process and improve the surface quality of the leaf spring.

[0068] In combination with the first aspect, in some embodiments provided in the present application, a heat preservation cooling treatment is further included after the rolling and before the quenching, and the termination temperature of the heat preservation cooling is less than or equal to 200° C. The material has high hardenability, and a slow cooling process, i.e., heat preservation cooling treatment, is used after rolling to eliminate the internal thermal stress of rolling and avoid cracks in the material during the cooling process.

[0069] In combination with the first aspect, in some embodiments provided in the present application, the quenching time is 30 to 200 minutes.

[0070] In combination with the first aspect, in some embodiments provided in the present application, the initial temperature of the part during quenching is 780-850°C.

[0071] Decarburization on the material surface will reduce the surface strength and thus reduce fatigue life. Due to the high Si content, there is a strong tendency for decarburization, so anti-decarburization coating needs to be applied before quenching heating to reduce surface decarburization generated during quenching heating.

[0072] In combination with the first aspect, in some embodiments provided in the present application, a cooling treatment is also included after the quenching and before the tempering, wherein: the cooling rate of the cooling treatment is greater than or equal to 1°C / s, which can improve the mechanical properties of the material and improve the tensile strength and yield strength of the material.

[0073] In combination with the first aspect, in some embodiments provided in the present application, the tempering temperature is 380-450° C., which can improve the mechanical properties of the material and improve the tensile strength and yield strength of the material.

[0074] In combination with the first aspect, in some embodiments provided in the present application, the tempering time is 30 to 300 minutes, which can improve the mechanical properties of the material and improve the tensile strength and yield strength of the material.

[0075] In combination with the first aspect, in some embodiments provided in the present application, the tempering treatment further includes shot peening treatment, wherein the shot peening treatment includes a first shot peening treatment and a second shot peening treatment, and the diameter of the steel shot in the first shot peening treatment is 1.0 to 1.4 mm.

[0076] In combination with the first aspect, in some embodiments provided in the present application, the tempering treatment further includes shot peening treatment, wherein the shot peening treatment includes a first shot peening treatment and a second shot peening treatment, and the time of the first shot peening treatment is 60 to 180 seconds.

[0077] In combination with the first aspect, in some embodiments provided in the present application, the tempering treatment further includes shot peening treatment, wherein the shot peening treatment includes a first shot peening treatment and a second shot peening treatment, and the diameter of the steel shot in the second shot peening treatment is 0.3 to 0.8 mm.

[0078] In combination with the first aspect, in some embodiments provided in the present application, the tempering treatment further includes shot peening treatment, wherein the shot peening treatment includes a first shot peening treatment and a second shot peening treatment, and the time of the first shot peening treatment is 60 to 180 seconds.

[0079] First, coarser steel shot (diameter 1.0 ~ 1.4mm) is used for shot peening to form a higher residual compressive stress (≥500Mpa) on the material surface; then finer steel shot (diameter 0.3`0.8mm) is used for shot peening to improve the surface quality of the material and reduce the surface roughness of the reed.

[0080] In a second aspect, the present application provides a leaf spring, comprising the spring steel prepared in the first aspect. The leaf spring has all the beneficial effects of the processing method of the spring steel, which will not be described in detail in this application.

[0081] In a third aspect, the present application provides a car, comprising the leaf spring of the second aspect. The car has all the beneficial effects of the processing method of the spring steel, which will not be described in detail in this application.

[0082] The technical solution provided in this application is described in detail below in conjunction with embodiments.

[0083] Example 1

[0084] Embodiment 1 of the present application provides a method for processing spring steel, which processes a single leaf spring. The material specifications of the part are: width 90 mm×thickness 50 mm.

[0085] The raw material composition includes, by mass fraction, C: 0.61%, Si: 1.37%, Mn: 1.06%, Cr: 1.18%, Mo: 0.082%, V: 0.23%, Nb: 0.038%, Ni: 1.13%, Ti: 0.017%, Al: 0.027%, N: 0.0043%, and the remainder is Fe and unavoidable impurity elements.

[0086] The raw materials of spring steel are cut, drilled, rolled, quenched and tempered to obtain spring steel;

[0087] Among them, the center positioning hole is a blind hole, and the depth of the blind hole is about 1 / 2.8 of the thickness of the leaf spring, which is 18mm;

[0088] After rolling heating, high-pressure water is used to remove phosphorus, and then rolling is carried out. The water pressure is 15MPa. After rolling, it is slowly cooled in the heat preservation cover, and the temperature out of the cover is 180℃.

[0089] Before quenching and heating, the leaf spring is coated with anti-decarburization paint. The quenching and heating temperature of the leaf spring is 900℃, and the holding time is 30min. The oil temperature during oil quenching is 780℃. To ensure the cooling rate of the spring is 2℃ / s, the leaf spring is swung with the quenching fixture for 100 seconds, and the swung frequency is 25 times / min.

[0090] Tempering temperature is 400℃, holding time is 300min, and water cooling is performed after tempering;

[0091] The steel shot with a diameter of 1.0 mm was used for shot peening for 60 seconds, and then the steel shot with a diameter of 0.3 mm was used for shot peening for 60 seconds.

[0092] Example 2

[0093] Embodiment 2 of the present application provides a method for processing spring steel, which processes a single front leaf spring. The material specifications of the part are: width 90 mm×thickness 40 mm.

[0094] The raw material composition includes, by mass fraction, C: 0.61%, Si: 1.28%, Mn: 0.98%, Cr: 1.06%, Mo: 0.078%, V: 0.22%, Nb: 0.027%, Ni: 0.92%, Ti: 0.015%, Al: 0.024%, N: 0.0052%, and the remainder is Fe and unavoidable impurity elements.

[0095] The raw materials of spring steel are cut, drilled, rolled, quenched and tempered to obtain spring steel;

[0096] Among them, the center positioning hole is a blind hole, and the depth of the blind hole is about 1 / 2.7 of the thickness of the leaf spring, which is 15mm;

[0097] After rolling and heating, high-pressure water is used to remove phosphorus, and then rolling is carried out. The water pressure is 25MPa. After rolling, it is slowly cooled in the heat preservation cover, and the temperature out of the cover is 190℃.

[0098] Before quenching and heating, the leaf spring is coated with anti-decarburization paint. The quenching and heating temperature of the leaf spring is 930℃, and the holding time is 30min. The oil temperature during oil quenching is 850℃. To ensure the cooling rate of the spring is 1.5℃ / s, the leaf spring is swung with the quenching fixture for 200 seconds, and the swung frequency is 20 times / min.

[0099] Tempering temperature is 450℃, holding time is 30min, and water cooling is performed after tempering;

[0100] The steel shot with a diameter of 1.4 mm was used for shot peening for 180 s. Then the steel shot with a diameter of 0.8 mm was used for shot peening for 180 s.

[0101] Example 3

[0102] Embodiment 3 of the present application provides a method for processing spring steel, which processes two rear leaf springs. The material specifications of the part are: width 90 mm×thickness 33 mm.

[0103] The raw material composition includes, by mass fraction, C: 0.60%, Si: 1.31%, Mn: 0.82%, Cr: 0.97%, Mo: 0.076%, V: 0.21%, Nb: 0.025%, Ni: 0.84%, Ti: 0.014%, Al: 0.031%, N: 0.0051%, and the remainder is Fe and unavoidable impurity elements.

[0104] The raw materials of spring steel are cut, drilled, rolled, quenched and tempered to obtain spring steel;

[0105] Among them, the center positioning hole is a blind hole, and the depth of the blind hole is about 1 / 2.2 of the thickness of the leaf spring, which is 15mm;

[0106] After rolling and heating, high-pressure water is used to remove phosphorus, and then rolling is carried out. The water pressure is 20MPa. After rolling, it is slowly cooled in the heat preservation cover, and the temperature out of the cover is 150℃.

[0107] Before quenching and heating, the leaf spring is coated with anti-decarburization paint. The quenching and heating temperature of the leaf spring is 850℃, and the holding time is 120min. The oil temperature during oil quenching is 800℃. To ensure the cooling rate of the spring is 3℃ / s, the leaf spring is swung with the quenching fixture for 150 seconds, and the swung frequency is 23 times / min.

[0108] Tempering temperature is 380℃, holding time is 180min, and water cooling is performed after tempering;

[0109] The steel shot with a diameter of 1.2 mm was used for shot peening for 120 s. Then the steel shot with a diameter of 0.5 mm was used for shot peening for 120 s.

[0110] Examples 4 to 15 and Comparative Examples 1 to 6 are similar to Example 1, and the raw material compositions are expressed in mass fraction (%). The differences are shown in Table 1.

[0111] Table 1 Parameters of the processing method of spring steel of Examples 4 to 15 and Comparative Examples 1 to 6

[0112]

[0113] The leaf springs obtained by the processing methods of the spring steels of Examples 1 to 15 and Comparative Examples 1 to 6 were subjected to performance tests, and their tensile strength Rm, yield strength Rp0.2, elongation after fracture A, cross-sectional shrinkage Z, hardness HRC at J40, metallographic structure and grain size were tested, wherein the tensile strength Rm, yield strength Rp0.2, elongation after fracture A, and cross-sectional shrinkage Z were measured using GB / T 228 "Method for tensile test of metallic materials at room temperature". The end quenching test was used to measure the hardness at J40 using GB / T 225 "End quenching test method for hardenability of steel (Jominy test)". The metallographic structure was measured using GB / T 13299 "Method for testing the microstructure of steel". The grain size was measured using GB / T 6394 "Method for determining the average grain size of metals". The test results are shown in Table 2.

[0114] Table 2 Performance of Examples 1 to 15 and Comparative Examples 1 to 6

[0115]

[0116]

[0117] The leaf springs obtained by the processing methods of the spring steels of Examples 1 to 3 were prepared into leaf spring assemblies and then subjected to fatigue life tests. The specific test method is: GB / T19844 "Leaf Spring", test stress 850±550MPa. The test results are shown in Table 3:

[0118] Table 3 Fatigue life of leaf springs obtained by the processing methods of spring steels in Examples 1 to 3

[0119]

[0120] It can be seen from Tables 2 and 3 that in Examples 1 to 15, V, Nb, Mo, Ti, Ni, Als, and N composite microalloying is used to improve the toughness of the material, and C, Si, Mn, Cr, and Mo are adjusted to improve the tempering stability and hardenability of the spring steel material, thereby ensuring the comprehensive mechanical properties, tensile strength of 1950-2100 MPa, yield strength of 1700-1850 MPa; elongation after fracture ≥9%, cross-sectional reduction rate ≥30%, and fatigue life of high stress leaf spring (test stress 850±550 MPa) ≥200,000 times.

[0121] Figure 1 is the hardenability curve of the leaf spring in the spring steel processing method of Example 1, Figure 1 It can be seen that the material of Example 1 has good hardenability, J50>59HRC, which can ensure that the 50mm thick leaf spring can be fully hardened.

[0122] Figure 2is the grain growth curve of the leaf spring in the spring steel processing method of Example 1, Figure 2 It can be seen that the grains of the material of Example 1 grow as the heating temperature increases. When the heating temperature exceeds 930°C, the grains grow significantly and can no longer meet the requirement of grain size level 10.

[0123] Figure 3 is the tempering stability curve of the leaf spring in the spring steel processing method of Example 1, Figure 3 It can be seen that as the tempering temperature of the material in Example 1 increases, the hardness of the material decreases accordingly.

[0124] Figure 4 is the metallographic structure diagram of the leaf spring in the spring steel processing method of Example 1, Figure 4 It can be seen that after the heat treatment, the metallographic structure of the material of Example 1 is fine troostite (grade 1), which can ensure that the material of Example 1 has high comprehensive mechanical properties.

[0125] Figure 5 is a grain size diagram of a leaf spring in the spring steel processing method of Example 1, Figure 5 It can be seen that after the heat treatment, the grain size of the material in Example 1 is 10, and the grains are fine, which can ensure that the material in Example 1 has high comprehensive mechanical properties.

[0126] Comparative Example 1 has the same composition as Example 14, and Comparative Example 2 has the same composition as Example 15. When the quenching heating temperature is high (950°C), the grains grow significantly, and the grain size is level 9. Although the strength does not decrease, the elongation after fracture decreases, resulting in a decrease in toughness, and the performance of the leaf spring does not meet the standard.

[0127] Comparative Example 3 does not contain Nb, and the V content of Comparative Example 4 is too low. After heat treatment, the grains are relatively coarse, and the grain size is level 9 and level 9.5. Although the strength does not decrease, the elongation after fracture decreases, resulting in a decrease in toughness, and the performance of the leaf spring does not meet the standard.

[0128] In Comparative Examples 5 and 6, when the Mn and Cr contents are too low, the hardenability of the material decreases, and the values ​​at J40 are 56.8HRC and 57.4HRC, respectively, which cannot guarantee that the 50mm thick spring leaf can be fully hardened.

[0129] In summary, high-stress leaf springs are used under high stress conditions, and their sensitivity to defects is enhanced, which requires the material to have high tensile strength and yield strength as well as high toughness. Grain refinement is an effective way to improve the strength and toughness of materials. Through composite microalloying of elements such as V, Nb, Ti, Als and N, the material has fine grains with a grain size of ≥10. The comprehensive mechanical properties of the material are improved. The material with a thickness of less than 50mm can be fully hardened, ensuring the heat treatment quality of high-stress leaf springs. The material strength and toughness are improved, with a tensile strength of 1950-2100MPa and a yield strength of 1700-1850MPa; the elongation after fracture is ≥9%, and the cross-sectional shrinkage is ≥30%. The fatigue performance of high-stress leaf spring products is improved, and the fatigue life of leaf springs (test stress 850±550MPa) is ≥200,000 times, which improves product quality and load-bearing capacity.

[0130] In the description of this specification, the description with reference to the terms "one embodiment / method", "some embodiments / methods", "example", "specific example" or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment / method or example are included in at least one embodiment / method or example of the present application. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment / method or example. Moreover, the specific features, structures, materials or characteristics described may be combined in a suitable manner in any one or more embodiments / methods or examples. In addition, those skilled in the art may combine and combine the different embodiments / methods or examples described in this specification and the features of the different embodiments / methods or examples, unless they are contradictory.

[0131] It should be noted that, in the present application, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that the process, method, article or equipment including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or equipment. In the absence of more restrictions, the elements defined by the sentence "comprise one..." do not exclude the existence of other identical elements in the process, method, article or equipment including the elements. In the present application, the meaning of "multiple" is at least two, such as two, three, etc., unless otherwise clearly and specifically stipulated.

[0132] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.

Claims

1. A method for processing spring steel, characterized in that: The raw materials include, by mass fraction, C: 0.57%-0.62%; Si: 1.22%-1.38%; Mn: 0.70%-1.10%; Cr: 0.90%-1.20%; Ni: 0.20-2.00%; Mo: 0.08%-0.10%; V: 0.15%-0.25%; Nb: 0.02%-0.04%|; Ti: 0.010%-0.018%; Al: 0.010%-0.040%; N: 0.0040%-0.0080%; P: ≤0.020%; S: ≤0.020%, and the remainder is Fe and unavoidable impurity elements; The processing method of the spring steel comprises the following steps: The raw materials of spring steel are cut, drilled, rolled, quenched and tempered to obtain spring steel; Among them: the quenching temperature is 850~930℃.

2. The method for processing spring steel according to claim 1, characterized in that: The central positioning hole of the drilled hole is a blind hole, wherein: the depth of the central positioning hole is h, and the thickness of the spring steel is d: 1 / 3≤h / d≤1 / 2.

3. The method for processing spring steel according to claim 1, characterized in that: After the drilling and before the rolling, a dephosphorization treatment is also included, wherein: The water pressure for dephosphorization treatment is 15-25 MPa.

4. The method for processing spring steel according to claim 1, characterized in that: After the rolling and before the quenching, a heat preservation and cooling treatment is also included, and the termination temperature of the heat preservation and cooling is less than or equal to 200°C.

5. The method for processing spring steel according to claim 1, characterized in that: The quenching time is 30 to 200 minutes; and / or, The initial temperature of the parts during quenching is 780-850°C.

6. The method for processing spring steel according to claim 1, characterized in that: A cooling process is also included after the quenching and before the tempering, wherein: The cooling rate of the cooling process is greater than or equal to 1°C / s.

7. The method for processing spring steel according to claim 1, characterized in that: The tempering temperature is 380-450°C; and / or, The tempering time is 30 to 300 minutes.

8. The method for processing spring steel according to claim 1, characterized in that: The tempering treatment further includes shot peening treatment, wherein the shot peening treatment includes a first shot peening treatment and a second shot peening treatment: The diameter of the steel shot in the first shot peening treatment is 1.0 to 1.4 mm; and / or, The first shot peening treatment lasts for 60 to 180 seconds; and / or, The diameter of the steel shot in the second shot peening treatment is 0.3 to 0.8 mm; and / or, The first shot peening treatment takes 60 to 180 seconds.

9. A leaf spring, characterized in that: A spring steel obtained by the spring steel processing method as described in any one of claims 1 to 8.

10. An automobile, characterized in that: Comprising the leaf spring as claimed in claim 9.