Nickel foil-based nonmetal two-phase doped alkaline complete water splitting difunctional heterojunction electrocatalyst and preparation method and application thereof

By forming a heterostructure electrocatalyst of transition metal-based sulfide and sulfur-hydroxide on nickel foil, the problems of insufficient catalyst activity and electrolyte corrosion during electrocatalytic hydrogen production are solved, and high efficiency and stable alkalinity are achieved The dual-function catalytic performance of electrolytic water is suitable for integration with solar cells.

CN118957651AActive Publication Date: 2024-11-15NANKAI UNIV

Patent Information

Application Number
CN202410927353.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-15
Estimated Expiration
2044-07-11

AI Technical Summary

Technical Problem

During the electrocatalytic hydrogen production process, the single reaction catalyst is insufficient in activity and the electrocatalyst is prone to corrosion when integrated with the solar cell, resulting in damage to the solar cell by the electrolyte.

Method used

Using a heterostructure electrocatalyst composed of transition metal-based sulfide and sulfur-hydroxide based on nickel foil, a three-dimensional porous nanosphere branch structure is formed by co-doping of non-metallic two phases, and using in-situ electrochemical deposition and electrochemical activation Prepare the method to achieve the efficiency and stability of the dual-function catalyst.

Benefits of technology

In an alkaline environment, efficient oxygen evolution and hydrogen evolution reactions are achieved, the overpotential range is optimized, the current density reaches 10mA/cm2, and the stable operation time exceeds 50 hours, reducing system complexity and cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957651A_ABST
    Figure CN118957651A_ABST
Patent Text Reader

Abstract

The invention discloses a nickel foil-based nonmetal two-phase doped alkaline complete water splitting difunctional heterojunction electrocatalyst and a preparation method and application thereof, and belongs to the field of new energy technologies and application of electrocatalytic materials, the electrocatalyst is a three-dimensional porous nanosphere branch knot, the chemical formula of the electrocatalyst is NiS < x > / S-NiFeOOH, the preparation method comprises the following steps: dissolving transition-state metal nitrate corresponding to Ni and Fe in deionized water, mixing with an aqueous solution in which sodium sulfide is dissolved to obtain an electrolyte, carrying out electro-deposition by taking a nickel foil treated in advance as an anode, and carrying out electro-deposition in a solution containing a sulfur source and a nickel precursor by taking the nickel foil as the anode. According to the invention, the problem of competitive adsorption of two-pole reaction at active sites in the water electrolysis process is solved, and the catalytic efficiency is greatly improved. And meanwhile, the material has the advantage of low cost and excellent alkaline oxygen evolution / hydrogen evolution electrocatalytic activity, is expected to be applied to industrial large-scale water electrolysis hydrogen production, and has certain practical significance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention discloses a novel electrocatalyst material and a preparation method thereof, which belongs to the field of new energy technology and electrocatalytic material application, and relates to a low-cost electrocatalyst material for alkaline complete water splitting reaction with a heterostructure composed of two non-metallic phases co-doped and a preparation method thereof, and particularly relates to a low-cost electrocatalyst material for alkaline complete water splitting reaction with a heterostructure composed of two non-metallic phases co-doped and a preparation method thereof. Background Art

[0002] Electrocatalytic hydrogen production is a green and sustainable method of hydrogen production, which uses catalysts to promote the splitting of water through electrochemical reactions. Compared with traditional fossil fuel hydrogen production methods, such as coal gasification or steam reforming, electrocatalytic hydrogen production has lower carbon emissions and is environmentally friendly. In addition, electrocatalytic hydrogen production can utilize renewable energy sources, such as wind power and solar energy, to achieve sustainable production of hydrogen, and is expected to become an important part of the future clean energy system.

[0003] In the process of electrocatalytic hydrogen production, the catalyst should have high activity and stability to promote the reaction rate and increase the yield of hydrogen. The electrocatalytic water decomposition reaction mainly includes two reactions: cathode hydrogen evolution and anode oxygen evolution. For the hydrogen evolution reaction, the precipitation of hydrogen ions needs to overcome the limitations of the polarity and redox potential of water molecules, and high-energy active sites are required to catalyze the precipitation of hydrogen. The oxygen evolution reaction has slow kinetics due to its four-electron transfer process, which limits its reaction rate. Therefore, it is necessary to design catalysts that can overcome the reaction energy barrier. In recent years, many studies have been devoted to the development of efficient electrocatalysts involving a variety of materials, including precious metals, transition metals, carbon materials, etc. By regulating the structure, composition and surface properties of the catalyst, precise control and optimization of the electrocatalytic hydrogen production process can be achieved.

[0004] In the traditional water electrolysis process, the oxygen evolution reaction and the hydrogen evolution reaction compete for the same catalytic site, resulting in limited catalyst activity. The design of the bifunctional catalyst can solve the competitive adsorption problem in the water electrolysis process and has active centers that promote both oxygen and hydrogen evolution reactions. This integrated design simplifies the structure of the electrolysis device, reduces the complexity and cost of the system, and also helps to improve energy conversion efficiency.

[0005] In metal-based electrocatalytic reactions, the general active sites are usually atoms or lattice defects on the metal surface. These sites have specific surface properties and activities, can adsorb reactants and promote the reaction. The formation and properties of catalytic active sites can be effectively regulated by adjusting the structure and composition of the metal surface. The doping of non-metallic elements can introduce additional active sites in metal catalysts to promote the reaction. This doping usually changes the electronic structure, surface chemical properties and crystal structure of the catalyst, thereby affecting the interaction and reaction path between the catalyst and the reactants. In addition, it may also change the adsorption capacity, surface active site density and charge transfer characteristics of the catalyst surface, thereby affecting the interaction strength and reaction rate between the catalyst and the reactants. Therefore, by rationally designing and regulating the doping method of non-metallic elements, the performance and efficiency of the catalyst can be effectively improved. In addition, the electrocatalyst with low-cost nickel foil as the substrate can be directly used in combination with photovoltaic cells, which can achieve efficient conversion and utilization of energy, and has long-term significance for the practical application of low-cost alkaline water electrolysis catalysts in the field of large-scale water splitting to promote the development of clean energy. Summary of the invention

[0006] The purpose of the present invention is to solve the activity defects of single reaction catalysts in full hydrolysis and the corrosion problem of electrolyte on solar cells in the hydrogen production system integrated with electrocatalysts and solar cells, and propose a low-cost alkaline full water splitting bifunctional electrocatalyst based on nickel foil, which is a heterogeneous structure material composed of transition metal-based sulfide and sulfur-hydroxide; the present invention also provides a preparation method of the transition metal-based sulfur-hydroxide.

[0007] The technical solution of the present invention:

[0008] The first aspect of the present invention is to provide a non-metallic two-phase doped alkaline water splitting bifunctional heterojunction electrocatalyst based on nickel foil, wherein the electrocatalyst is a heterostructure NiS composed of a transition metal-based sulfide and a sulfur-hydroxide. x / S-NiFeOOH is a three-dimensional porous nanosphere branch structure; the non-metallic two-phase doped transition metal-based heterostructure catalyst is grown on nickel foil by in-situ electrochemical deposition during the preparation process, wherein the content ratio of Ni to Fe elements is 1.25:1.

[0009] The electrocatalytic performance of the non-metallic two-phase doped transition metal-based heterostructure material based on nickel foil in an alkaline medium with a pH of 13.8 is 10 mA / cm 2 The overpotential range required for catalytic current density is 180-230 mV; its hydrogen evolution activity is 10 mA / cm 2 The overpotential required under current density conditions is in the range of 70 to 120 mV; the total water splitting activity is 10 mA / cm 2The voltage range required for the catalytic current density is 1.50-1.57 V, and the stable operation time exceeds 50 hours.

[0010] The second aspect of the present invention is to provide a method for preparing the above-mentioned non-metallic two-phase doped alkaline water splitting bifunctional heterojunction electrocatalyst based on nickel foil, the steps are as follows:

[0011] 1) Dissolve the corresponding nitrates of Ni and Fe in deionized water at a molar ratio of 1.25:1 and a total molar amount of 0.05M or 0.1M, then add the prepared sulfur source to the above solution, mix, and perform ultrasonic treatment;

[0012] 2) After the solution is fully mixed, a precursor solution is obtained as an electrolyte, 0.05 nm, 0.15 nm, and 0.25 nm nickel foils treated in advance are used as working electrodes, platinum sheets are used as counter electrodes, and saturated Ag / AgCl is used as reference electrodes. The electrochemical deposition reaction is carried out at 40° C. and 50° C. using a three-electrode system for 180 s, 300 s, and 600 s, and the obtained product is washed with deionized water and anhydrous ethanol, and then dried to obtain S-NiFe(oxy)hydroxide / Ni foil electrodes;

[0013] 3) dissolving Ni-based nitrate and sulfur source in deionized water, using the nickel foil electrode obtained in 1) as the working electrode, the platinum sheet as the counter electrode, and the saturated Ag / AgCl as the reference electrode, using a three-electrode system to perform an electrochemical deposition reaction for 5 to 60 minutes, washing the obtained product with deionized water and anhydrous ethanol, and then vacuum drying to obtain an electrode loaded with the precursor on the nickel foil substrate;

[0014] 4) The nickel foil electrode loaded with the precursor is fixed with a platinum sheet electrode clamp, and electrochemically activated using a three-electrode system with an electrolyte of 1 M KOH to obtain the final three-dimensional nanosphere branched electrocatalyst.

[0015] The nitrates corresponding to Ni and Fe are nickel nitrate hexahydrate and iron nitrate nonahydrate respectively; the sulfur source is sodium sulfide and thiourea;

[0016] The size of the nickel foil is 2cm*1cm;

[0017] The nickel foil pretreatment method is: immersing the nickel foil in hydrochloric acid, anhydrous ethanol, and water in sequence and ultrasonicating for 10 minutes respectively;

[0018] The three-electrode system electrochemical activation method is as follows: a nickel foam electrode loaded with a precursor catalyst is used as a working electrode, Ag / AgCl is used as a reference electrode, and a platinum sheet is used as a working electrode. The voltage is set to -0.3-0.8V, and CV activation is performed at a scan rate of 50mV / s. The number of turns is set to 50 turns.

[0019] In one embodiment, the total molar amount in step 1) is 0.05M; the thickness of the nickel foil in step 2) is 0.25nm, the deposition temperature and setting time are 40°C and 300s respectively; the electrochemical reaction deposition time in step 3) is set to 5min, 10min, 20min, 30min, and 60min respectively, among which 30min is the optimal setting temperature.

[0020] The electrochemical activation and electrochemical performance testing steps of the non-metallic two-phase doped alkaline water splitting bifunctional heterojunction electrocatalyst based on nickel foil provided by the present invention are as follows:

[0021] 1) Electrochemical measurements were evaluated in a three-electrode setup with an Ag / AgCl electrode as the reference electrode and a platinum sheet electrode as the counter electrode, and a catalyst-loaded nickel foil electrode as the working electrode;

[0022] 3) Potential reference reversible hydrogen electrode (RHE): E RHE =E Ag / AgCl + 0.098 + 0.059 × pH (1 M KOH solution). The overpotential (η) was calculated according to the following equation: η = E RHE -1.23 V. Cyclic voltammetry (CV) was performed in a saturated 1 M KOH solution at a scan rate of 50 mV / s to obtain the target catalyst after electrochemical activation. Linear sweep voltammetry (LSV) was recorded in a saturated 1 M KOH solution at a scan rate of 5 mV / s to obtain polarization curves. All electrode potential data were compensated for 85% voltage drop.

[0023] The advantages and effects of the present invention are as follows:

[0024] The nickel foil-based non-metallic two-phase doped alkaline water-splitting bifunctional heterojunction electrocatalyst is a low-cost composite material. It uses transition metal-based compounds with abundant raw material reserves, low price and easy purchase as the source of catalytic active centers. The bifunctional water-splitting electrocatalyst with multiple active sites and high stability is synthesized by electrochemical deposition and electrochemical in-situ activation. The operation process of the electrocatalyst material is simple and suitable for large-scale production and preparation.

[0025] The electrocatalyst is applied to oxygen evolution reaction in alkaline environment, and only 181 mV overpotential is required to obtain a 10 mA cm -2 The current density of the hydrogen evolution reaction is -10mA cm -2 The overpotential at a current density of only 75 mV indicates that the non-precious metal electrocatalyst exhibits excellent oxygen and hydrogen evolution kinetics in an alkaline environment. At the same time, the prepared electrocatalyst has excellent stability in alkaline electrolytes at 20 mA cm -2The current density is stable for more than 50 hours.

[0026] The high performance is attributed to the interface effect of the non-metal-doped two-phase composite structure and the non-metal bonding interaction, which optimizes the overall structural performance. The surface reconstruction also forms more sulfur vacancies and active high-valent metal compounds, which improves the oxygen and hydrogen evolution performance of the catalyst. This new material solves the competitive adsorption problem of the bipolar reaction at the active site during the electrolysis of water, greatly improving the catalytic efficiency. At the same time, the material designed based on nickel foil will promote the development of coupling integration with solar cells, provide strategic guidance for the design of the overall structure and catalyst, and has important practical significance for the research and application of low-cost materials in the production of hydrogen by full water splitting. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 Example 1 (NiS x / S-NiFeOOH), Comparative Example 1 (NiFeOOH), Comparative Example 2 (S-NiFeOOH) and Comparative Example 3 (NiS x The prepared electrocatalyst was subjected to linear sweep voltammetry (LSV) in 1 M KOH solution at a scan rate of 1 mV / s to obtain the anodic reaction polarization curve;

[0028] Figure 2 Example 1 (NiS x / S-NiFeOOH), Comparative Example 1 (NiFeOOH), Comparative Example 2 (S-NiFeOOH) and Comparative Example 3 (NiS x ) The prepared electrocatalyst was subjected to linear sweep voltammetry (LSV) in 1 M KOH solution at a scan rate of 1 mV / s to obtain the cathode reaction polarization curve;

[0029] Figure 3 Example 1 (NiS x / S-NiFeOOH), Comparative Example 1 (NiFeOOH), Comparative Example 2 (S-NiFeOOH) and Comparative Example 3 (NiS x ) OER AC impedance spectrum of the prepared electrocatalyst obtained in 1M KOH solution;

[0030] Figure 4 Example 1 (NiS x / S-NiFeOOH), Comparative Example 1 (NiFeOOH), Comparative Example 2 (S-NiFeOOH) and Comparative Example 3 (NiS x ) Tafel slope (Tafel) plot of the prepared electrocatalyst in 1 M KOH solution;

[0031] Figure 5 Example 1 (NiSx The electrocatalyst prepared by using S-NiFeOOH) was tested in 1M KOH solution by two electrodes and the linear sweep voltammetry (LSV) was recorded to obtain the polarization curve of complete water splitting.

[0032] Figure 6 Example 1 (NiS x / S-NiFeOOH) electrocatalyst under 20 mA cm -2 The stability test curve is maintained at a constant current density for 50 hours, in which all electrode potential data are compensated for 85% iR;

[0033] Figure 7 Example 1 (NiS x In the two-electrode test of the S-NiFeOOH (NiFeOOH) electrocatalyst, linear sweep voltammetry (LSV) was recorded before and after the stability test to obtain the polarization curves for complete water splitting.

[0034] Figure 8 The comparative examples 1 (NiFeOOH), 2 (S-NiFeOOH), and 3 (NiS x ) and Example 1 (NiS x / S-NiFeOOH) prepared electrocatalyst SEM morphology test results;

[0035] Fig. 9 Example 1 (NiS x / S-NiFeOOH) prepared electrocatalyst SEM morphology test results;

[0036] Fig.10 The comparative examples 2 (S-NiFeOOH) and 3 (NiS x ) and Example 1 (NiS x / S-NiFeOOH) corresponding to the XRD spectrum of the electrocatalyst prepared. DETAILED DESCRIPTION

[0037] The technical solution of the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments.

[0038] Embodiment 1:

[0039] The nickel foil was soaked in hydrochloric acid, anhydrous ethanol and deionized water for 10 minutes in sequence, and the prefabricated 2cm*1cm nickel foil with a thickness of 0.25nm was used as the working electrode, the platinum sheet was used as the counter electrode, and the saturated Ag / AgCl was used as the reference electrode to form a three-electrode system for electrodeposition. The electrolyte was composed of 0.03M nickel nitrate hexahydrate, 0.02M iron nitrate nonahydrate, 0.05g sodium sulfide ultrasonically dissolved in 30 ml deionized water, and then 200μl of hydrogen peroxide solution was added. Electrodeposition was performed at a constant voltage of -1.1V vs. Ag / AgCl at 40℃, and the time was set to 300s. After deposition, it was rinsed with deionized water and anhydrous ethanol in sequence, and dried in an oven at 60℃ for 12 hours to obtain the target precursor. Then, the precursor supported by nickel foil is used as the working electrode, the platinum sheet is used as the counter electrode, and the three-electrode system formed by saturated Ag / AgCl is used as the reference electrode for electrodeposition, and 0.05M nickel nitrate hexahydrate, 0.05M sodium citrate, and 0.75M thiourea are used as electrolytes. The electrodeposition is performed under the condition of a constant voltage of -1.0V vs.Ag / AgCl, and the time is set to 30min. After the deposition is completed, it is rinsed with deionized water and anhydrous ethanol in turn, and then freeze-dried for 12 hours to obtain the electrocatalyst of the present invention.

[0040] Embodiment 2:

[0041] The nickel foil was soaked in hydrochloric acid, anhydrous ethanol and deionized water for 10 minutes in sequence, and the prefabricated 2cm*1cm nickel foil with a thickness of 0.25nm was used as the working electrode, the platinum sheet was used as the counter electrode, and the saturated Ag / AgCl was used as the reference electrode to form a three-electrode system for electrodeposition. The electrolyte was composed of 0.06M nickel nitrate hexahydrate, 0.04M iron nitrate nonahydrate, 0.05g sodium sulfide ultrasonically dissolved in 30 ml deionized water, and then 200μl of hydrogen peroxide solution was added. Electrodeposition was performed at 40℃ with a constant voltage of -1.1V vs.Ag / AgCl, and the time was set to 300s. After deposition, it was rinsed with deionized water and anhydrous ethanol in sequence, and dried in an oven at 60℃ for 12 hours to obtain the target precursor. Then, the precursor loaded on nickel foil was used as the working electrode, the platinum sheet was used as the counter electrode, and the saturated Ag / AgCl was used as the reference electrode to form a three-electrode system for electrodeposition. 0.05M nickel nitrate hexahydrate, 0.05M sodium citrate, and 0.75M thiourea were used as electrolytes. Electrodeposition was performed at a constant voltage of -1.0V vs.Ag / AgCl, and the time was set to 30min. After deposition, it was rinsed with deionized water and anhydrous ethanol in turn, and then freeze-dried for 12 hours to obtain the target electrocatalyst.

[0042] Embodiment 3:

[0043] The nickel foil was soaked in hydrochloric acid, anhydrous ethanol and deionized water for 10 minutes in sequence, and the prefabricated 2cm*1cm nickel foil with a thickness of 0.05nm was used as the working electrode, the platinum sheet was used as the counter electrode, and the saturated Ag / AgCl was used as the reference electrode to form a three-electrode system for electrodeposition. The electrolyte was composed of 0.03M nickel nitrate hexahydrate, 0.02M iron nitrate nonahydrate, 0.05g sodium sulfide ultrasonically dissolved in 30 ml of deionized water, and then 200μl of hydrogen peroxide solution was added. Electrodeposition was performed at a constant voltage of -1.1V vs. Ag / AgCl at 40℃, and the time was set to 300s. After deposition, it was rinsed with deionized water and anhydrous ethanol in sequence, and dried in an oven at 60℃ for 12 hours to obtain the target precursor. Then, the precursor loaded on nickel foil was used as the working electrode, the platinum sheet was used as the counter electrode, and the saturated Ag / AgCl was used as the reference electrode to form a three-electrode system for electrodeposition. 0.05M nickel nitrate hexahydrate, 0.05M sodium citrate, and 0.75M thiourea were used as electrolytes. Electrodeposition was performed at a constant voltage of -1.0V vs.Ag / AgCl, and the time was set to 30min. After deposition, it was rinsed with deionized water and anhydrous ethanol in turn, and then freeze-dried for 12 hours to obtain the target electrocatalyst.

[0044] Embodiment 4:

[0045] The nickel foil was soaked in hydrochloric acid, anhydrous ethanol and deionized water for 10 minutes in sequence, and the prefabricated 2cm*1cm nickel foil with a thickness of 0.15nm was used as the working electrode, the platinum sheet was used as the counter electrode, and the saturated Ag / AgCl was used as the reference electrode to form a three-electrode system for electrodeposition. The electrolyte was composed of 0.03M nickel nitrate hexahydrate, 0.02M iron nitrate nonahydrate, 0.05g sodium sulfide ultrasonically dissolved in 30 ml deionized water, and then 200μl of hydrogen peroxide solution was added. Electrodeposition was performed at 40℃ with a constant voltage of -1.1V vs.Ag / AgCl, and the time was set to 300s. After deposition, it was rinsed with deionized water and anhydrous ethanol in sequence, and dried in an oven at 60℃ for 12 hours to obtain the target precursor. Then, the precursor loaded on nickel foil was used as the working electrode, the platinum sheet was used as the counter electrode, and the saturated Ag / AgCl was used as the reference electrode to form a three-electrode system for electrodeposition. 0.05M nickel nitrate hexahydrate, 0.05M sodium citrate, and 0.75M thiourea were used as electrolytes. Electrodeposition was performed at a constant voltage of -1.0V vs.Ag / AgCl, and the time was set to 30min. After deposition, it was rinsed with deionized water and anhydrous ethanol in turn, and then freeze-dried for 12 hours to obtain the target electrocatalyst.

[0046] Embodiment 5:

[0047] The nickel foil was soaked in hydrochloric acid, anhydrous ethanol and deionized water for 10 minutes in sequence, and the prefabricated 2cm*1cm nickel foil with a thickness of 0.25nm was used as the working electrode, the platinum sheet was used as the counter electrode, and the saturated Ag / AgCl was used as the reference electrode to form a three-electrode system for electrodeposition. The electrolyte was composed of 0.03M nickel nitrate hexahydrate, 0.02M iron nitrate nonahydrate, 0.05g sodium sulfide ultrasonically dissolved in 30 ml deionized water, and then 200μl of hydrogen peroxide solution was added. Electrodeposition was performed at a constant voltage of -1.1V vs. Ag / AgCl at 50℃, and the time was set to 300s. After deposition, it was rinsed with deionized water and anhydrous ethanol in sequence, and dried in an oven at 60℃ for 12 hours to obtain the target precursor. Then, the precursor supported by nickel foil is used as the working electrode, the platinum sheet is used as the counter electrode, and the three-electrode system formed by saturated Ag / AgCl is used as the reference electrode for electrodeposition, and 0.05M nickel nitrate hexahydrate, 0.05M sodium citrate, and 0.75M thiourea are used as electrolytes. The electrodeposition is performed under the condition of a constant voltage of -1.0V vs.Ag / AgCl, and the time is set to 30min. After the deposition is completed, it is rinsed with deionized water and anhydrous ethanol in turn, and then freeze-dried for 12 hours to obtain the electrocatalyst of the present invention.

[0048] Embodiment 6:

[0049] The nickel foil was soaked in hydrochloric acid, anhydrous ethanol and deionized water for 10 minutes in sequence, and the prefabricated 2cm*1cm nickel foil with a thickness of 0.25nm was used as the working electrode, the platinum sheet was used as the counter electrode, and the saturated Ag / AgCl was used as the reference electrode to form a three-electrode system for electrodeposition. The electrolyte was composed of 0.03M nickel nitrate hexahydrate, 0.02M iron nitrate nonahydrate, 0.05g sodium sulfide ultrasonically dissolved in 30 ml of deionized water, and then 200μl of hydrogen peroxide solution was added. Electrodeposition was performed at a constant voltage of -1.1V vs. Ag / AgCl at 40℃, and the time was set to 180s. After deposition, it was rinsed with deionized water and anhydrous ethanol in sequence, and dried in an oven at 60℃ for 12 hours to obtain the target precursor. Then, the precursor supported by nickel foil is used as the working electrode, the platinum sheet is used as the counter electrode, and the three-electrode system formed by saturated Ag / AgCl is used as the reference electrode for electrodeposition, and 0.05M nickel nitrate hexahydrate, 0.05M sodium citrate, and 0.75M thiourea are used as electrolytes. The electrodeposition is performed under the condition of a constant voltage of -1.0V vs.Ag / AgCl, and the time is set to 30min. After the deposition is completed, it is rinsed with deionized water and anhydrous ethanol in turn, and then freeze-dried for 12 hours to obtain the electrocatalyst of the present invention.

[0050] Embodiment 7:

[0051] The nickel foil was soaked in hydrochloric acid, anhydrous ethanol and deionized water for 10 minutes in sequence, and the prefabricated 2cm*1cm nickel foil with a thickness of 0.25nm was used as the working electrode, the platinum sheet was used as the counter electrode, and the saturated Ag / AgCl was used as the reference electrode to form a three-electrode system for electrodeposition. The electrolyte was composed of 0.03M nickel nitrate hexahydrate, 0.02M iron nitrate nonahydrate, 0.05g sodium sulfide ultrasonically dissolved in 30 ml deionized water, and then 200μl of hydrogen peroxide solution was added. Electrodeposition was performed at a constant voltage of -1.1V vs. Ag / AgCl at 40℃, and the time was set to 600s. After deposition, it was rinsed with deionized water and anhydrous ethanol in sequence, and dried in an oven at 60℃ for 12 hours to obtain the target precursor. Then, the precursor supported by nickel foil is used as the working electrode, the platinum sheet is used as the counter electrode, and the three-electrode system formed by saturated Ag / AgCl is used as the reference electrode for electrodeposition, and 0.05M nickel nitrate hexahydrate, 0.05M sodium citrate, and 0.75M thiourea are used as electrolytes. The electrodeposition is performed under the condition of a constant voltage of -1.0V vs.Ag / AgCl, and the time is set to 30min. After the deposition is completed, it is rinsed with deionized water and anhydrous ethanol in turn, and then freeze-dried for 12 hours to obtain the electrocatalyst of the present invention.

[0052] Embodiment 8:

[0053] The nickel foil was soaked in hydrochloric acid, anhydrous ethanol and deionized water for 10 minutes in sequence, and the prefabricated 2cm*1cm nickel foil with a thickness of 0.25nm was used as the working electrode, the platinum sheet was used as the counter electrode, and the saturated Ag / AgCl was used as the reference electrode to form a three-electrode system for electrodeposition. The electrolyte was composed of 0.03M nickel nitrate hexahydrate, 0.02M iron nitrate nonahydrate, 0.05g sodium sulfide ultrasonically dissolved in 30 ml deionized water, and then 200μl of hydrogen peroxide solution was added. Electrodeposition was performed at a constant voltage of -1.1V vs. Ag / AgCl at 40℃, and the time was set to 300s. After deposition, it was rinsed with deionized water and anhydrous ethanol in sequence, and dried in an oven at 60℃ for 12 hours to obtain the target precursor. Then, the precursor supported by nickel foil is used as the working electrode, the platinum sheet is used as the counter electrode, and the three-electrode system formed by saturated Ag / AgCl is used as the reference electrode for electrodeposition, and 0.05M nickel nitrate hexahydrate, 0.05M sodium citrate, and 0.75M thiourea are used as electrolytes. The electrodeposition is performed under the condition of a constant voltage of -1.0V vs.Ag / AgCl, and the time is set to 5min. After the deposition is completed, it is rinsed with deionized water and anhydrous ethanol in turn, and then freeze-dried for 12 hours to obtain the electrocatalyst of the present invention.

[0054] Embodiment 9:

[0055] The nickel foil was soaked in hydrochloric acid, anhydrous ethanol and deionized water for 10 minutes in sequence, and the prefabricated 2cm*1cm nickel foil with a thickness of 0.25nm was used as the working electrode, the platinum sheet was used as the counter electrode, and the saturated Ag / AgCl was used as the reference electrode to form a three-electrode system for electrodeposition. The electrolyte was composed of 0.03M nickel nitrate hexahydrate, 0.02M iron nitrate nonahydrate, 0.05g sodium sulfide ultrasonically dissolved in 30 ml deionized water, and then 200μl of hydrogen peroxide solution was added. Electrodeposition was performed at a constant voltage of -1.1V vs. Ag / AgCl at 40℃, and the time was set to 300s. After deposition, it was rinsed with deionized water and anhydrous ethanol in sequence, and dried in an oven at 60℃ for 12 hours to obtain the target precursor. Then, the precursor supported by nickel foil is used as the working electrode, the platinum sheet is used as the counter electrode, and the three-electrode system formed by saturated Ag / AgCl is used as the reference electrode for electrodeposition, and 0.05M nickel nitrate hexahydrate, 0.05M sodium citrate, and 0.75M thiourea are used as electrolytes. The electrodeposition is performed under the condition of a constant voltage of -1.0V vs.Ag / AgCl, and the time is set to 10min. After the deposition is completed, it is rinsed with deionized water and anhydrous ethanol in turn, and then freeze-dried for 12 hours to obtain the electrocatalyst of the present invention.

[0056] Embodiment 10:

[0057] The nickel foil was soaked in hydrochloric acid, anhydrous ethanol and deionized water for 10 minutes in sequence, and the prefabricated 2cm*1cm nickel foil with a thickness of 0.25nm was used as the working electrode, the platinum sheet was used as the counter electrode, and the saturated Ag / AgCl was used as the reference electrode to form a three-electrode system for electrodeposition. The electrolyte was composed of 0.03M nickel nitrate hexahydrate, 0.02M iron nitrate nonahydrate, 0.05g sodium sulfide ultrasonically dissolved in 30 ml deionized water, and then 200μl of hydrogen peroxide solution was added. Electrodeposition was performed at a constant voltage of -1.1V vs. Ag / AgCl at 40℃, and the time was set to 300s. After deposition, it was rinsed with deionized water and anhydrous ethanol in sequence, and dried in an oven at 60℃ for 12 hours to obtain the target precursor. Then, the precursor supported by nickel foil is used as the working electrode, the platinum sheet is used as the counter electrode, and the three-electrode system formed by saturated Ag / AgCl is used as the reference electrode for electrodeposition, and 0.05M nickel nitrate hexahydrate, 0.05M sodium citrate, and 0.75M thiourea are used as electrolytes. The electrodeposition is performed under the condition of a constant voltage of -1.0V vs.Ag / AgCl, and the time is set to 20min. After the deposition is completed, it is rinsed with deionized water and anhydrous ethanol in turn, and then freeze-dried for 12 hours to obtain the electrocatalyst of the present invention.

[0058] Embodiment 11:

[0059] The nickel foil was soaked in hydrochloric acid, anhydrous ethanol and deionized water for 10 minutes in sequence, and the prefabricated 2cm*1cm nickel foil with a thickness of 0.25nm was used as the working electrode, the platinum sheet was used as the counter electrode, and the saturated Ag / AgCl was used as the reference electrode to form a three-electrode system for electrodeposition. The electrolyte was composed of 0.03M nickel nitrate hexahydrate, 0.02M iron nitrate nonahydrate, 0.05g sodium sulfide ultrasonically dissolved in 30 ml deionized water, and then 200μl of hydrogen peroxide solution was added. Electrodeposition was performed at a constant voltage of -1.1V vs. Ag / AgCl at 40℃, and the time was set to 300s. After deposition, it was rinsed with deionized water and anhydrous ethanol in sequence, and dried in an oven at 60℃ for 12 hours to obtain the target precursor. Then, the precursor supported by nickel foil is used as the working electrode, the platinum sheet is used as the counter electrode, and the three-electrode system formed by saturated Ag / AgCl is used as the reference electrode for electrodeposition, and 0.05M nickel nitrate hexahydrate, 0.05M sodium citrate, and 0.75M thiourea are used as electrolytes. The electrodeposition is performed under the condition of a constant voltage of -1.0V vs.Ag / AgCl, and the time is set to 60min. After the deposition is completed, it is rinsed with deionized water and anhydrous ethanol in turn, and then freeze-dried for 12 hours to obtain the electrocatalyst of the present invention.

[0060] Embodiment 12:

[0061] Electrochemical Activation and Electrochemical Performance Test of Electrocatalysts Prepared in Examples 1 to 11

[0062] (1) Electrochemical activation and evaluation of electrochemical measurements were performed in a three-electrode setup with an Ag / AgCl electrode as the reference electrode and a platinum electrode as the counter electrode; the potential was referenced to the reversible hydrogen electrode (RHE): E RHE =E Ag / AgCl + 0.098 + 0.059 × pH (1 M KOH solution). The overpotential (η) was calculated according to the following equation: η = E RHE -1.23V. The three-dimensional porous nanosphere branch electrocatalyst obtained in Example 1 after electrochemical activation is the electrocatalyst of the present invention, and its chemical formula is NiS x / S-NiFeOOH. Linear sweep voltammetry (LSV) was recorded in saturated 1 M KOH solution at a scan rate of 1 mV / s to obtain polarization curves, see Figure 1 . AC impedance test at constant voltage to obtain electronic transport properties, see Figure 2 Stability test: Maintain the stability test curve for 50 hours at a constant current density of 20. Figure 3 , and the LSV polarization curve after long-term testing is basically the same as before the test. All electrode potential data of the three-electrode test were compensated for 85% of the voltage drop.

[0063] (2) The catalyst loaded on nickel foil prepared after electrochemical activation in Example 1 was tested by SEM. It has a porous mesh spherical structure. Fig. 9 .

[0064] (3) The XRD spectrum of the catalyst loaded on nickel foil prepared after electrochemical activation in Example 1 was tested. Only the peak of the base nickel showed its amorphous structure. Fig.10 .

[0065] Comparative Example 1:

[0066] (1) Preparation of NiFeOOH: Soak nickel foil in hydrochloric acid, anhydrous ethanol and deionized water for 10 minutes in sequence, and then perform ultrasonic treatment. Electrodeposition is performed in a three-electrode system formed by using a prefabricated nickel foil of 2cm*1cm size and thickness of 0.25nm as the working electrode, a platinum sheet as the counter electrode, and saturated Ag / AgCl as the reference electrode. The electrolyte consists of 0.03M nickel nitrate hexahydrate and 0.02M iron nitrate nonahydrate. Electrodeposition is performed at a constant voltage of -1.1V vs. Ag / AgCl at 40°C for 300s. After deposition, rinse with deionized water and anhydrous ethanol in sequence, and dry in an oven at 60°C for 12 hours to obtain the target precursor. Cyclic voltammetry is performed in a 1M KOH solution to obtain the electrochemically activated catalyst.

[0067] (2) Electrochemical activation and evaluation of electrochemical measurements in a three-electrode setup with an Ag / AgCl electrode as the reference electrode and a platinum electrode as the counter electrode; the potential is referenced to the reversible hydrogen electrode (RHE): E RHE =E Ag / AgCl + 0.098 + 0.059 × pH (1 M KOH solution). The overpotential (η) was calculated according to the following equation: η = E RHE -1.23 V. Linear sweep voltammetry (LSV) was recorded in saturated 1 M KOH solution at a scan rate of 1 mV / s to obtain anodic / cathodic polarization curves, see Figure 1 / Figure 2 . AC impedance test at constant voltage to obtain electronic transport properties, see Figure 3 Tafel slope test to obtain reaction kinetics, see Figure 4 All electrode potential data were compensated for 85% voltage drop.

[0068] Comparative Example 2:

[0069] (1) Preparation of S-NiFeOOH: Soak nickel foil in hydrochloric acid, anhydrous ethanol and deionized water for 10 minutes in sequence, and use the prefabricated 2cm*1cm nickel foil with a thickness of 0.25nm as the working electrode, platinum sheet as the counter electrode, and saturated Ag / AgCl as the reference electrode to form a three-electrode system for electroplating. The electrolyte is composed of 0.03M nickel nitrate hexahydrate, 0.02M iron nitrate nonahydrate, 0.05g sodium sulfide ultrasonically dissolved in 30ml deionized water, and then 200μl of hydrogen peroxide solution is added. Electroplating is carried out at 40℃ with a constant voltage of -1.1V vs.Ag / AgCl, and the time is set to 300s. After deposition, rinse with deionized water and anhydrous ethanol in sequence, dry in an oven at 60℃ for 12 hours to obtain the target precursor, and cyclic voltammetry is performed in 1M KOH solution to obtain the electrochemically activated catalyst.

[0070] (2) Electrochemical activation and evaluation of electrochemical measurements in a three-electrode setup with an Ag / AgCl electrode as the reference electrode and a platinum electrode as the counter electrode; the potential is referenced to the reversible hydrogen electrode (RHE): E RHE =E Ag / AgCl + 0.098 + 0.059 × pH (1 M KOH solution). The overpotential (η) was calculated according to the following equation: η = E RHE -1.23 V. Linear sweep voltammetry (LSV) was recorded in saturated 1 M KOH solution at a scan rate of 1 mV / s to obtain anodic / cathodic polarization curves, see Figure 1 / Figure 2 . AC impedance test at constant voltage to obtain electronic transport properties, see Figure 3 Tafel slope test to obtain reaction kinetics, see Figure 4 All electrode potential data were compensated for 85% voltage drop.

[0071] Comparative Example 3:

[0072] (1)NiS x Preparation: Soak nickel foil in hydrochloric acid, anhydrous ethanol and deionized water for 10 minutes in sequence, and use the prefabricated 2cm*1cm nickel foil with a thickness of 0.25nm as the working electrode, the platinum sheet as the counter electrode, and the saturated Ag / AgCl as the reference electrode to form a three-electrode system for electrodeposition. 0.05M nickel nitrate hexahydrate, 0.05M sodium citrate, and 0.75M thiourea are used as electrolytes. Electrodeposition is performed under a constant voltage of -1.0V vs.Ag / AgCl, and the time is set to 20min. After deposition, rinse with deionized water and anhydrous ethanol in sequence, and then freeze-dry for 12 hours to obtain the product as the electrocatalyst.

[0073] (2) Electrochemical activation and evaluation of electrochemical measurements in a three-electrode setup with an Ag / AgCl electrode as the reference electrode and a platinum electrode as the counter electrode; the potential is referenced to the reversible hydrogen electrode (RHE): E RHE =E Ag / AgCl + 0.098 + 0.059 × pH (1 M KOH solution). The overpotential (η) was calculated according to the following equation: η = E RHE -1.23 V. Linear sweep voltammetry (LSV) was recorded in saturated 1 M KOH solution at a scan rate of 1 mV / s to obtain anodic / cathodic polarization curves, see Figure 1 / Figure 2 . AC impedance test at constant voltage to obtain electronic transport properties, see Figure 3 Tafel slope test to obtain reaction kinetics, see Figure 4 All electrode potential data were compensated for 85% voltage drop.

[0074] Figure 1 In 1M KOH, the NiS obtained in Example 1 x / S-NiFeOOH, NiFeOOH obtained in Comparative Example 1, S-NiFeOOH obtained in Comparative Example 2, and NiS obtained in Comparative Example 3 x OER linear sweep voltammetry curve. As can be seen from the figure, the current density reaches 10mA / cm 2 When NiS x / S-NiFeOOH catalyst has the lowest overpotential, indicating that NiS x The synergistic effect of NiFeOOH and S-NiFeOOH promoted the oxygen evolution catalytic performance.

[0075] Figure 2 In 1M KOH, the NiS obtained in Example 1 x / S-NiFeOOH, NiFeOOH obtained in Comparative Example 1, S-NiFeOOH obtained in Comparative Example 2, and NiS obtained in Comparative Example 3 x HER linear sweep voltammetry curve. As can be seen from the figure, the current density reaches 10mA / cm 2 When NiS x / S-NiFeOOH catalyst has the lowest overpotential, indicating that NiS x The synergistic effect of NiFeOOH and S-NiFeOOH promoted the hydrogen evolution catalytic performance.

[0076] Figure 3 In 1M KOH, the NiS obtained in Example 1 x / S-NiFeOOH, NiFeOOH obtained in Comparative Example 1, S-NiFeOOH obtained in Comparative Example 2, and NiS obtained in Comparative Example 3 xElectrochemical impedance spectroscopy of NiS x / S-NiFeOOH catalyst has the smallest interfacial resistance, indicating that NiS x The synergistic effect of S-NiFeOOH promotes the catalytic kinetic characteristics of the electrochemical reaction.

[0077] Figure 4 In 1M KOH, the NiS obtained in Example 1 x / S-NiFeOOH, NiFeOOH obtained in Comparative Example 1, S-NiFeOOH obtained in Comparative Example 2, and NiS obtained in Comparative Example 3 x Tafel slope plot of . It can be seen from the figure that NiS x The / S-NiFeOOH catalyst has the smallest Tafel slope, indicating that NiS x The synergistic effect of S-NiFeOOH promotes electron transfer at the heterogeneous interface and improves the electronic properties of the catalyst surface.

[0078] Figure 5 In 1M KOH, the NiS obtained in Example 1 x Two-electrode linear sweep voltammetry curves with / S-NiFeOOH as cathode / anode respectively.

[0079] Figure 6 In 1M KOH, the NiS obtained in Example 1 x The stability test of the two electrodes with / S-NiFeOOH as cathode / anode respectively was carried out under constant voltage conditions for 50 hours.

[0080] Figure 7 The stability test before and after the comparison of NiS obtained in Example 1 is shown in 1M KOH. x The LSV curves of the two-electrode linear sweep voltammetry curves of / S-NiFeOOH as cathode / anode respectively are almost overlapped, indicating that the performance of the catalyst has not been significantly attenuated before and after the stability test and has excellent long-term stability.

[0081] Figure 8 They are NiFeOOH obtained in Comparative Example 1, S-NiFeOOH obtained in Comparative Example 2, and NiS obtained in Comparative Example 3. x and NiS obtained in Example 1 x Scanning electron microscope images (AD) of / S-NiFeOOH. Image D has the common structural morphology of B and C, and the surface shows porous mesh-like nanosphere branches.

[0082] Fig. 9 NiS obtained in Example 1 x The high-magnification scanning electron microscope image of / S-NiFeOOH shows an obvious surface porous state.

[0083] Fig.10 NiS obtained in Example 1 x / S-NiFeOOH, NiFeOOH obtained in Comparative Example 1, S-NiFeOOH obtained in Comparative Example 2, and NiS obtained in Comparative Example 3 x XRD diagram. However, only the (111), (200) and (220) planes corresponding to the strong diffraction peaks of Ni are shown, indicating that the catalyst is mainly in an amorphous structure. In addition, the exposed active surface in the heterojunction mainly turns to the (220) plane with lower surface energy, which is easier to adsorb species and catalytic reactions.

[0084] In summary, a new type of non-metallic two-phase doped alkaline water electrolysis bifunctional low-cost electrocatalyst based on nickel foil and its preparation method optimizes the overall microstructure performance of the material through the interface effect of the two-phase composite structure and the non-metallic bonding during the in-situ electrochemical activation process, forming a new material structure and being applicable to both oxygen evolution and hydrogen evolution reactions of complete water splitting under alkaline conditions. The activity of the target catalyst material has been significantly improved compared to non-doped and single-phase catalysts, and the catalyst stability has also been well maintained.

[0085] The above is only a preferred specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A non-metallic two-phase doped alkaline water splitting bifunctional heterojunction electrocatalyst based on nickel foil, characterized in that: The electrocatalyst is a heterogeneous structure composed of transition metal-based sulfide and sulfur-hydroxide, and the catalyst exhibits a three-dimensional porous nanosphere branch structure. The catalyst is described as NiS x / S-NiFeOOH, the ratio of Ni to Fe is 1.25:

1.

2. The non-metallic two-phase doped alkaline water splitting bifunctional heterojunction electrocatalyst based on nickel foil according to claim 1, characterized in that: The oxygen evolution activity of the catalyst reaches 10 mA / cm in an alkaline medium at pH = 13.

8. 2 The overpotential range required for the catalytic current density is 180-230 mV; the voltage range required for the catalytic current density is 1.50-1.57 V.

3. The non-metallic two-phase doped alkaline water splitting bifunctional heterojunction electrocatalyst based on nickel foil according to claim 1, characterized in that: The hydrogen evolution activity of the catalyst under the same conditions reaches -10mA / cm 2 The overpotential required for catalytic current density is in the range of 70 to 120 mV.

4. The non-metallic two-phase doped alkaline water splitting bifunctional heterojunction electrocatalyst based on nickel foil according to claim 1, characterized in that: The catalyst was tested in a two-electrode system at 20 mA / cm 2 The stable operation time under current density conditions exceeds 50 hours.

5. The method for preparing the non-metallic two-phase doped alkaline water splitting bifunctional heterojunction electrocatalyst based on nickel foil according to any one of claims 1 to 4, comprising the following steps: 1) Dissolve the corresponding nitrates of Ni and Fe in deionized water at a molar ratio of 1.25:1 and a total molar amount of 0.05M or 0.1M, then add the prepared sulfur source to the above solution, mix, and perform ultrasonic treatment; 2) After the solution is fully mixed, a precursor solution is obtained as an electrolyte, 0.05 nm, 0.15 nm, and 0.25 nm nickel foils processed in advance are used as working electrodes, platinum sheets are used as counter electrodes, and saturated Ag / AgCl is used as reference electrodes. The electrochemical deposition reaction is carried out at 25° C. to 50° C. using a three-electrode system for 180 to 600 s. The obtained product is washed with deionized water and anhydrous ethanol, and then dried to obtain a S-NiFe(oxy)hydroxide / Ni foil electrode; 3) dissolving Ni-based nitrate and sulfur source in deionized water, using the nickel foil electrode obtained in 1) as the working electrode, the platinum sheet as the counter electrode, and the saturated Ag / AgCl as the reference electrode, using a three-electrode system to perform an electrochemical deposition reaction for 5 to 60 minutes, washing the obtained product with deionized water and anhydrous ethanol, and then vacuum drying to obtain an electrode loaded with the precursor on the nickel foil substrate; 4) The nickel foil electrode loaded with the precursor is fixed with a platinum electrode clamp and electrochemically activated using a three-electrode system with an electrolyte of 1 M KOH to obtain the final three-dimensional nanosphere branched electrocatalyst.

6. The method for preparing the non-metallic two-phase doped alkaline water splitting bifunctional heterojunction electrocatalyst based on nickel foil according to claim 5, characterized in that: The nitrates corresponding to Ni and Fe are nickel nitrate hexahydrate and iron nitrate nonahydrate respectively; the sulfur source is sodium sulfide or thiourea.

7. The method for preparing the non-metallic two-phase doped alkaline water splitting bifunctional heterojunction electrocatalyst based on nickel foil according to claim 5, characterized in that: The nickel foil pretreatment method comprises: soaking the nickel foil in hydrochloric acid, anhydrous ethanol and deionized water in sequence and ultrasonicating them for 10 minutes respectively.

8. The method for preparing the non-metallic two-phase doped alkaline water splitting bifunctional heterojunction electrocatalyst based on nickel foil according to claim 5, characterized in that: The three-electrode system electrochemical activation method is as follows: a nickel foil electrode loaded with a precursor is used as a working electrode, Ag / AgCl is used as a reference electrode, and a platinum sheet is used as a working electrode; the voltage is set to -0.3-0.8V, CV activation is performed, the scan rate is 50mV / s; and the number of turns is set to 50 turns.

9. The method for preparing the non-metallic two-phase doped alkaline water splitting bifunctional heterojunction electrocatalyst based on nickel foil according to claim 5, characterized in that: In step 3), the electrochemical reaction deposition time is set to 5 min, 10 min, 20 min, 30 min and 60 min respectively.

10. Use of the non-metallic two-phase doped alkaline overall water splitting bifunctional heterojunction electrocatalyst based on nickel foil as described in any one of claims 1 to 4 in oxygen evolution reaction under alkaline environment.

Citation Information

Patent Citations

  • Foamed nickel loaded bimetallic phosphide / sulfide heterostructure hydrogen evolution catalyst and preparation method thereof

    CN115572998A

Cited By

  • Ferro-nickel / sulfide composite photo-anode using sacrificial nickel to trigger reconstruction activation and preparation method and application of ferro-nickel / sulfide composite photo-anode

    CN121951606A