Secondary battery and electronic device

By using an insulating layer containing inorganic additives and a specific electrolyte combination in the secondary battery, the performance problems in cycling performance and low temperature environments under high voltage are solved, and the lithium ion receptivity and output characteristics are significantly improved, and the low temperature of the battery is improved. Performance and security.

CN118970230AActive Publication Date: 2024-11-15NINGDE AMPEREX TECHNOLOGY LTD

Patent Information

Application Number
CN202411068158.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-27
Publication Date
2024-11-15
Estimated Expiration
2044-05-27

AI Technical Summary

Technical Problem

The cycling performance of existing secondary batteries becomes worse at high voltages, and the lithium ion acceptability and output characteristics are poor in low temperature environments. Especially after the high voltage positive electrode film forming additive improves the circulation characteristics, the low temperature characteristics are affected.

Method used

In the secondary battery, a positive electrode includes an insulating layer disposed on the current collector and a positive electrode active material layer. The insulating layer contains inorganic additives. Fluorine-free chain carboxylic acid ester, vinyl sulfate and lithium difluorophosphate are added to the electrolyte solution. , adjust its mass content to improve low temperature performance.

Benefits of technology

It significantly suppresses the increase in interface resistance at low temperatures, improves lithium ion acceptability and output characteristics, and improves the low-temperature and safety performance of secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004979965630000121
    Figure BDA0004979965630000121
  • Figure BDA0004979965630000131
    Figure BDA0004979965630000131
  • Figure FDA0004979965570000011
    Figure FDA0004979965570000011
Patent Text Reader

Abstract

The invention relates to a secondary battery and an electronic device. Specifically, the secondary battery comprises a positive electrode, a negative electrode and an electrolyte, the positive electrode comprises an insulating layer and a positive electrode active material layer which are arranged on a current collector, the insulating layer comprises an inorganic additive, and the electrolyte does not contain fluorine chain carboxylic ester, ethylene sulfate and lithium difluorophosphate. The lithium ion acceptability at low temperature can be improved, the increase of low-temperature DC resistance can be suppressed, and the low-temperature output characteristics can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application with application number 202410658437.8, application date May 27, 2024, and invention name “Secondary battery and electronic device”. Technical Field

[0002] The present application relates to the field of energy storage, and in particular to a secondary battery and an electronic device. Background Art

[0003] With the rapid development of electronic products such as smart phones, tablet computers and smart wearables, higher requirements are placed on the service life and safety performance of secondary batteries, taking into account the different usage time and working environment temperature of electronic digital products. With the increase of charging cut-off voltage, the energy density of the battery has been significantly improved. However, in the prior art, as the voltage of the secondary battery increases, the cycle performance of the high-voltage secondary battery deteriorates. After using high-voltage positive electrode film-forming additives to improve the cycle characteristics, the low-temperature characteristics are greatly affected. Summary of the invention

[0004] The embodiments of the present application solve the problems existing in the prior art to some extent by adjusting the composition of the positive electrode used in the secondary battery and the components in the electrolyte.

[0005] The inventors of the present application discovered that the positive electrode includes an insulating layer and a positive electrode active material layer arranged on a current collector, the insulating layer includes an inorganic additive, and the electrolyte chain carboxylate, vinyl sulfate and lithium difluorophosphate can not only improve the lithium ion acceptance at low temperatures, but also inhibit the increase of low-temperature DC resistance and improve low-temperature output characteristics, thereby completing the present application.

[0006] On the one hand, the present application provides a secondary battery, comprising: a positive electrode, a negative electrode and an electrolyte; the positive electrode comprises: an insulating layer and a positive electrode active material layer arranged on a current collector; the insulating layer comprises: an inorganic additive; the inorganic additive comprises: a metal element; the metal element in the inorganic additive comprises: at least one of aluminum, magnesium, titanium, zirconium, niobium, indium, tungsten, tin, zinc or antimony; the electrolyte contains fluorine-free chain carboxylic acid ester, vinyl sulfate and lithium difluorophosphate, wherein, based on the mass of the electrolyte, the total mass content of vinyl sulfate and lithium difluorophosphate is greater than 0.02wt% and less than 3.26wt%, and the mass content of the fluorine-free chain carboxylic acid ester is greater than 8.6wt% and less than 65wt%. Based on the mass of the electrolyte, the total mass content of (II) and (III) is greater than 0.02wt% and less than 3.26wt%; the mass content of (I) is greater than 8.6wt% and less than 65wt%. This is important for the stability of the positive electrode structure and is very critical to significantly suppress the increase in interface resistance at low temperatures. This design can not only improve the lithium ion acceptance at low temperatures, but also suppress the increase in low-temperature DC resistance and improve low-temperature output characteristics.

[0007] In some embodiments, based on the mass of the electrolyte, the total mass content of vinyl sulfate and lithium difluorophosphate is greater than 0.05 wt % and less than 1.98 wt %, which helps to further improve the low temperature performance.

[0008] In some embodiments, the mass content of the fluorine-free chain carboxylic acid ester is 17.3 wt % or more and 52.6 wt % or less based on the mass of the electrolyte, thereby improving low temperature performance.

[0009] In some embodiments, the inorganic additive is selected from at least one of aluminum oxide, aluminum hydroxide, boehmite, magnesium oxide, magnesium hydroxide, titanium dioxide, zirconium dioxide, niobium monoxide, niobium dioxide, niobium trioxide, niobium pentoxide, indium trioxide, tungsten trioxide, tin dioxide, zinc oxide or antimony trioxide to improve low temperature performance.

[0010] In some embodiments, the fluorine-free linear carboxylic acid ester is selected from at least one of methyl acetate, ethyl acetate, n-propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl isobutyrate, ethyl isobutyrate, n-propyl isobutyrate, methyl pivalate, ethyl pivalate, n-propyl pivalate, methyl acrylate, ethyl acrylate, n-propyl acrylate, methyl methacrylate, ethyl methacrylate or n-propyl methacrylate.

[0011] In some embodiments, based on the mass of the electrolyte, the mass content of vinyl sulfate is greater than 0.01wt% and less than 1.67wt%; or, based on the mass of the electrolyte, the mass content of lithium difluorophosphate is greater than 0.01wt% and less than 1.95wt%, thereby improving lithium ion acceptance.

[0012] In some embodiments, the electrolyte further includes: other additives; the other additives include: at least one of 1,2-bis(difluorophosphine)ethane, a compound of formula 1, a compound of formula 2, vinylene carbonate, lithium fluorosulfonate, succinonitrile, adiponitrile, 1,3,6-hexatriconitrile, 1,2,3-tris(2-cyanoethoxy)propane, fluorobenzene, cyclohexylbenzene, biphenyl, tris(trimethylsilyl)phosphate or tris(trimethylsilyl)borate;

[0013] Compounds, compound; based on the mass of the electrolyte, the mass content of other additives is greater than 0.5wt% and less than 7wt%, which can improve the stability of the aforementioned coating at low temperatures and increase the ion conduction rate of lithium ions, thereby further improving the low temperature performance.

[0014] In some embodiments, a pole ear is provided on one side of the current collector, and an insulating layer is provided on the edge surface of the current collector having the pole ear. The insulating layer is used to improve the insulation of the positive electrode edge and the negative electrode edge, thereby improving the safety performance of the secondary battery, especially the insulation under high voltage.

[0015] In some embodiments, the secondary battery has a wound structure, and the insulating layer is disposed on the surface of the tail section in the length direction of the current collector, thereby improving the safety of the tail section.

[0016] In another aspect of the present application, the present application provides an electronic device, which includes the secondary battery described in the present application.

[0017] The present application uses a specific positive electrode composition and electrolyte combination, which is designed to not only improve lithium ion acceptance at low temperatures, but also suppress the increase in low-temperature DC resistance and improve low-temperature output characteristics.

[0018] Additional aspects and advantages of the embodiments of the present application will be described, shown, or explained in part in the subsequent description through implementation of the embodiments of the present application. DETAILED DESCRIPTION

[0019] The embodiments of the present application will be described in detail below. The embodiments of the present application should not be interpreted as limiting the present application.

[0020] The present application uses a specific positive electrode composition and electrolyte combination, which is designed to not only improve lithium ion acceptance at low temperatures, but also suppress the increase in low-temperature DC resistance and improve low-temperature output characteristics.

[0021] In one embodiment, the present application provides a secondary battery, which includes a positive electrode, a negative electrode, and an electrolyte as described below.

[0022] I. Electrolyte

[0023] The electrolyte in the secondary battery of the present application includes an electrolyte and a solvent for dissolving the electrolyte.

[0024] In some embodiments, the electrolyte of the present application includes (I) a fluorine-free chain carboxylic acid ester, (II) vinyl sulfate, and (III) lithium difluorophosphate.

[0025] When an insulating layer is set on the lug side or the tail section of a secondary battery to improve the safety performance of the battery, but in the presence of inorganic additives in the insulating layer, it is easy to catalyze the fluorine-free chain carboxylic acid ester to form a film on the surface of the positive electrode active material, causing the film impedance to increase and affecting the low-temperature characteristics of the secondary battery. The inventors found that when the electrolyte also contains vinyl sulfate and lithium difluorophosphate, the increase in the impedance of the film can be significantly suppressed, thereby not only improving the lithium ion acceptance at low temperatures, but also suppressing the increase in low-temperature DC resistance and improving low-temperature output characteristics.

[0026] Examples of the fluorine-free chain carboxylic acid esters include saturated chain carboxylic acid esters such as methyl acetate, ethyl acetate, n-propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl isobutyrate, ethyl isobutyrate, n-propyl isobutyrate, methyl pivalate, ethyl pivalate, n-propyl pivalate, and the like; and unsaturated chain carboxylic acid esters such as methyl acrylate, ethyl acrylate, n-propyl acrylate, methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, and the like.

[0027] Among these, methyl acetate, ethyl acetate, n-propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl pivalate, ethyl pivalate, and n-propyl pivalate are preferred from the perspective of less side reactions occurring at the positive electrode; methyl acetate, ethyl acetate, n-propyl acetate, methyl propionate, ethyl propionate, and propyl propionate are more preferred from the perspective of improving ion conductivity by reducing the viscosity of the electrolyte; methyl acetate, ethyl acetate, n-propyl acetate, methyl propionate, ethyl propionate, and propyl propionate are further preferred; and methyl acetate, ethyl propionate, and propyl propionate are particularly preferred.

[0028] The fluorine-free carboxylic acid ester may be used alone or in combination of two or more in any combination and ratio.

[0029] Specifically, from the viewpoint of improving low-temperature resistance, based on the mass of the electrolyte, the mass content of the fluorine-free carboxylic acid ester (the total amount in the case of more than two types) can be 8.6wt% or more, preferably 10.3wt% or more, more preferably 13.7wt% or more, further preferably 21.9wt% or more, and particularly preferably 23.4wt% or more. In addition, it can be 65wt% or less, preferably 52.6wt% or less, and more preferably 47.3wt% or less.

[0030] Specifically, from the viewpoint of improving lithium ion acceptance, based on the mass of the electrolyte, the mass content of vinyl sulfate is 0.01wt% or more, preferably 0.02wt% or more, preferably 0.04wt% or more, and more preferably 0.08wt% or more. In addition, as the upper limit of the mass content of vinyl sulfate, from the viewpoint of improving low-temperature DC resistance, the mass content of vinyl sulfate is 1.67wt% or less, preferably 1.59wt% or less, more preferably 1.45wt% or less, further preferably 1.23wt% or less, and particularly preferably 0.88wt% or less. When within the above range, it helps to further improve the increase in low-temperature DC resistance.

[0031] Specifically, from the viewpoint of improving lithium ion acceptance, based on the mass of the electrolyte, the mass content of lithium difluorophosphate is 0.01wt% or more, preferably 0.05wt% or more, preferably 0.07wt% or more, and more preferably 0.11wt% or more. In addition, as the upper limit of the mass content of lithium difluorophosphate, from the viewpoint of improving low-temperature output, the mass content of lithium difluorophosphate is 1.95wt% or less, preferably 1.87wt% or less, more preferably 1.59wt% or less, further preferably 1.22wt% or less, and particularly preferably 0.93wt% or less. When within the above range, it helps to further improve low-temperature output.

[0032] Furthermore, from the viewpoint of improving lithium ion acceptance, based on the mass of the electrolyte, the total mass content of (II) and (III) is 0.02wt% or more, preferably 0.05wt% or more. In addition, as the upper limit of the total mass content of (II) and (III), from the viewpoint of improving electrochemical characteristics under low temperature environment, the total mass content of (II) and (III) is 3.26wt% or less, preferably 2.81wt% or less.

[0033] In some embodiments, the total mass content of (II) and (III) is a wt%, and a is 0.02, 0.05, 0.09, 0.13, 0.19, 0.29, 0.46, 0.68, 1.17, 1.57, 1.98, 2.38, 2.81, 3.26, or within a range consisting of any two of the above values. When within the above range, it helps to further improve the low temperature DC resistance increase.

[0034] In addition, the electrolyte may further include other additives, such as at least one of 1,2-bis(difluorophosphine)ethane, a compound of formula 1, a compound of formula 2, vinylene carbonate, lithium fluorosulfonate, succinonitrile, adiponitrile, 1,3,6-hexatriconitrile, 1,2,3-tris(2-cyanoethoxy)propane, fluorobenzene, cyclohexylbenzene, biphenyl, tris(trimethylsilyl)phosphate, and tris(trimethylsilyl)borate;

[0035] Compounds, Compound.

[0036] The inventors also unexpectedly discovered that other additives can improve the stability of the aforementioned film at low temperatures and increase the ion conductivity of lithium ions, thereby further improving the low-temperature resistance increase characteristics. The aforementioned other additives can be only one or more.

[0037] Specifically, from the viewpoint of improving the conduction of lithium ions in the aforementioned coating, based on the mass of the electrolyte, the mass content of other additives is 0.01wt% or more, preferably the mass content of other additives is 0.1wt% or more, preferably 0.3wt% or more, and more preferably 0.5wt% or more. In addition, as the upper limit of the mass content of other additives, from the viewpoint of improving the increase in low-temperature DC resistance, the mass content of other additives is 10wt% or less, preferably 9wt% or less, more preferably 8wt% or less, further preferably 7wt% or less, and particularly preferably 5wt% or less. When within the above range, it helps to further improve the low-temperature DC resistance increase characteristics.

[0038] In some embodiments, the electrolyte in the electrode solution is not particularly limited, and any substance known as an electrolyte can be used arbitrarily. The quality of the electrolyte is not particularly limited, as long as it does not damage the effect of the present application. For example, the lithium salt used in the electrolyte of the present application includes lithium hexafluorophosphate, and the mass content of lithium hexafluorophosphate is 9% to 15wt% based on the mass of the electrolyte, preferably 9% to 13wt%, and more preferably 9% to 12wt%. By setting the above content range, the increase in low-temperature DC resistance can be improved.

[0039] In some embodiments, the electrolyte further comprises any non-aqueous solvent known in the prior art that can be used as a solvent for the electrolyte. In some embodiments, the non-aqueous solvent includes, but is not limited to, one or more of the following: cyclic carbonates, linear carbonates, cyclic carboxylates, cyclic ethers, linear ethers, phosphorus-containing organic solvents, and sulfur-containing organic solvents.

[0040] II. Positive electrode

[0041] The positive electrode includes a positive electrode current collector and a positive electrode mixture layer provided on the positive electrode current collector. The positive electrode mixture layer contains positive electrode active materials, and the positive electrode mixture layer may be one layer or multiple layers. The positive electrode mixture layer includes a positive electrode active material layer and an insulating layer. The insulating layer may be provided on the edge surface of the current collector on the side with the tab, that is, the insulating layer is located on the tab side. Or the insulating layer is provided on the surface of the winding type secondary battery current collector at the end section in the length direction, that is, the insulating layer is located at the end section. The insulating layer is used to improve the insulation between the positive electrode edge and the negative electrode edge, thereby improving the safety performance of the secondary battery, especially the insulation at high voltages. The positive electrode active material is any material that can reversibly intercalate and deintercalate lithium ions.

[0042] For example, as the positive electrode active material for a secondary battery, a composite metal oxide containing one or more selected from the group consisting of cobalt, manganese, and nickel and lithium, or a lithium-containing olivine-type phosphate containing one or more selected from iron, cobalt, nickel, and manganese is used. These positive electrode active materials can be used alone or in combination of two or more.

[0043] As such a lithium composite metal oxide, for example, those selected from LiCoO2, LiMn2O4, LiNiO2, LiCo 1-x Ni x O2(0.01 < x < 1), LiNi x Mn y Co z O2(x + y + z = 1), a solid solution of Li2MnO3 and LiMO2 (M is a transition metal such as Co, Ni, Mn, Fe, etc.), LiNi 1 / 2 Mn 3 / 2 O4, LiFePO4, LiMnPO4, and LiMn 1-x FexPO4(0.01 < x < 1) are preferably one or more, more preferably two or more. A part of these composite metal oxides with lithium or lithium-containing olivine-type phosphates can be replaced with other elements, or a part of cobalt, nickel, manganese, and iron can be replaced with one or more elements selected from Co, Mn, Ni, Mg, Al, B, Ti, V, Nb, Cu, Zn, Mo, Ca, Sr, W, and Zr, or coated with a compound or carbon material containing these other elements.

[0044] Regarding the voltage during charging, from the perspective of high voltage, the positive electrode potential is preferably 4.4 V (vs. Li / Li+) or more, more preferably 4.5 V (vs. Li / Li+) or more, and particularly preferably 4.6 V (vs. Li / Li+) or more.

[0045] The conductive agent of the positive electrode is not particularly limited as long as it is an electronic conductive material that does not cause chemical changes. Examples thereof include graphites such as natural graphite (flaky graphite, etc.), artificial graphite, acetylene black, Ketjen black, channel black, furnace black, lamp black, or carbon black such as thermal black. In addition, graphite and carbon black can also be appropriately mixed for use. The amount of the conductive agent added to the positive electrode mixture is preferably 1 to 10% by weight, and particularly preferably 1.5 to 5% by weight.

[0046] The binder of the positive electrode includes at least one of polyvinylidene fluoride, polyacrylonitrile and polyacrylic acid. Polyacrylonitrile is preferred from the viewpoint of improving lithium ion acceptance and increasing low-temperature DC resistance of the secondary battery.

[0047] From the viewpoint of improving the increase of low-temperature DC resistance, the insulating layer contains an inorganic additive. The metal element in the inorganic additive includes at least one of aluminum, magnesium, titanium, zirconium, niobium, indium, tungsten, tin, zinc, and antimony.

[0048] Specifically, the inorganic additive may be at least one of an inorganic metal oxide and an inorganic metal hydroxide, such as aluminum oxide, aluminum hydroxide, boehmite, magnesium oxide, magnesium hydroxide, titanium dioxide, zirconium dioxide, niobium monoxide, niobium dioxide, niobium trioxide, niobium pentoxide, indium trioxide, tungsten trioxide, tin dioxide, zinc oxide, and antimony trioxide.

[0049] The positive electrode is made as follows:

[0050] The inorganic additives, conductive agents such as acetylene black and carbon black, and binders such as polyvinylidene fluoride or polyacrylonitrile are mixed, and deionized water is added thereto and mixed evenly to prepare slurry 1.

[0051] The above-mentioned positive electrode active material is mixed with a conductive agent such as acetylene black or carbon black, and a binder such as polyvinylidene fluoride or polyacrylonitrile, and a high boiling point solvent such as 1-methyl-2-pyrrolidone is added thereto and kneaded to prepare a slurry 2 .

[0052] Slurry 1 and slurry 2 were applied in parallel on the aluminum foil of the current collector, and then dried and pressed to form a positive electrode.

[0053] The density of the positive electrode active material layer is usually 3.5 g / cm 3 In order to further increase the capacity of the battery, it is preferably 3.8 g / cm 3 More preferably 4 g / cm 3 More preferably, 4.1 g / cm 3 In addition, the upper limit is preferably 4.6 g / cm 3 the following.

[0054] There is no particular limitation on the type of positive electrode current collector, which can be any material known to be suitable for use as a positive electrode current collector. Examples of positive electrode current collectors may include, but are not limited to, metal materials such as aluminum, stainless steel, nickel plating, titanium, and tantalum; and carbon materials such as carbon cloth and carbon paper. In some embodiments, the positive electrode current collector is a metal material. In some embodiments, the positive electrode current collector is aluminum foil.

[0055] III. Negative electrode

[0056] The negative electrode includes a negative electrode current collector and a negative electrode mixture layer disposed on the surface of the negative electrode current collector, wherein the negative electrode mixture layer contains a negative electrode active material. In some embodiments, the chargeable capacity of the negative electrode active material is greater than the discharge capacity of the positive electrode active material to prevent lithium metal from being accidentally precipitated on the negative electrode during charging.

[0057] The negative electrode active material is not particularly limited, and examples thereof include carbon-based negative electrode active materials, metal-based negative electrode active materials, and negative electrode active materials obtained by combining these.

[0058] Carbon-based negative electrode active material

[0059] Here, the carbon-based negative electrode active material refers to an active material having a carbon-based skeleton into which lithium can be inserted, and examples of the carbon-based negative electrode active material include carbonaceous materials and graphite materials.

[0060] As carbonaceous materials, for example, graphitizable carbon, non-graphitizable carbon with amorphous structure represented by glassy carbon, etc. can be cited. Here, as graphitizable carbon, for example, carbon materials obtained from petroleum or coal using tar pitch as raw material can be cited. When giving specific examples, coke, mesocarbon microbeads (MCMB), mesophase pitch-based carbon fibers, and pyrolysis vapor-grown carbon fibers can be cited. In addition, as non-graphitizable carbon, for example, phenolic resin sintered bodies, polyacrylonitrile-based carbon fibers, quasi-isotropic carbon, furfuryl alcohol resin sintered bodies (PFA), hard carbon, etc. can be cited.

[0061] Furthermore, as graphite materials, for example, natural graphite, artificial graphite, etc. can be cited. Among them, as artificial graphite, for example: artificial graphite obtained by heat-treating carbon containing graphitized carbon mainly at 2800°C or above, graphite MCMB obtained by heat-treating MCMB at 2000°C or above, graphite mesophase pitch-based carbon fiber obtained by heat-treating mesophase pitch-based carbon fiber at 2000°C or above, etc. can be cited. In addition, in the present application, as a carbon-based negative electrode active material, natural graphite (amorphous coated natural graphite) in which at least a portion of its surface is coated with amorphous carbon can be used.

[0062] In addition, the metal-based negative electrode active material is an active material containing a metal, generally referring to an active material having an element capable of inserting lithium or alloying with lithium in the structure, and an active material having a theoretical current capacity of 500 mAh / g or more per unit mass when inserting lithium or alloying with lithium. As a metal-based negative electrode active material, for example, lithium metal, a single metal that can form a lithium alloy (such as Ag, Al, Ba, Bi, Cu, Ga, Ge, In, Ni, P, Pb, Sb, Si, Sn, Sr, Zn, Ti, etc.) and its alloy, and their oxides, sulfides, nitrides, silicides, carbides, phosphides, etc. can be used. Among them, as a metal-based negative electrode active material, an active material containing silicon (silicon-based negative electrode active material) is preferably used. This is because the use of a silicon-based negative electrode active material can increase the capacity of the secondary battery.

[0063] Examples of the silicon-based negative electrode active material include silicon (Si), alloys containing silicon, silicon oxides, and composites of a silicon-containing material and conductive carbon in which a silicon-containing material is coated with conductive carbon or composited with conductive carbon.

[0064] From the viewpoint of improving battery capacity, a silicon-carbon material, for example, a porous carbon-supported silicon composite material is preferred.

[0065] The negative electrode active material may be used alone or in combination of two or more at any ratio.

[0066] The negative electrode mixture layer may further include a negative electrode binder. The negative electrode binder can improve the bonding between the negative electrode active material particles and the bonding between the negative electrode active material and the current collector. The type of negative electrode binder is not particularly limited, as long as it is a material that is stable to the solvent used in the electrolyte or electrode manufacturing. In some embodiments, the negative electrode binder includes a resin binder. Examples of resin binders include, but are not limited to, fluororesins, polyacrylonitrile (PAN), polyimide resins, acrylic resins, polyolefin resins, and the like. When an aqueous solvent is used to prepare the negative electrode mixture slurry, the negative electrode binder includes, but is not limited to, carboxymethyl cellulose (CMC) or its salt, styrene-butadiene rubber (SBR), polyacrylic acid (PAA) or its salt, polyvinyl alcohol, and the like.

[0067] As a current collector for holding the negative electrode active material, any known current collector can be used. Examples of negative electrode current collectors include, but are not limited to, metal materials such as copper, nickel, stainless steel, and nickel-plated steel. In some embodiments, the negative electrode current collector is copper foil.

[0068] The negative electrode can be prepared by applying a negative electrode mixture slurry containing a negative electrode active material, a resin binder, etc. on a negative electrode current collector, drying it, and then rolling it to form a negative electrode mixture layer on both sides of the negative electrode current collector, thereby obtaining a negative electrode.

[0069] IV. Isolation membrane

[0070] In order to prevent short circuit, a separator is usually provided between the positive electrode and the negative electrode. In this case, the electrolyte of the present application is usually used by infiltrating the separator.

[0071] There is no particular restriction on the material and shape of the isolation membrane, as long as the effect of the present application is not significantly impaired. The isolation membrane may be a resin, glass fiber, inorganic substance, etc. formed of a material that is stable to the electrolyte of the present application. In some embodiments, the isolation membrane includes a porous sheet or a non-woven fabric-like material with excellent liquid retention. Examples of materials for resin or glass fiber isolation membranes may include, but are not limited to, polyolefins, aromatic polyamides, polytetrafluoroethylene, polyether sulfone, etc. In some embodiments, the polyolefin is polyethylene or polypropylene. In some embodiments, the polyolefin is polypropylene. The materials of the above isolation membranes may be used alone or in any combination.

[0072] The isolation film may also be a material formed by laminating the above materials, and examples thereof include, but are not limited to, a three-layer isolation film formed by laminating polypropylene, polyethylene, and polypropylene in this order.

[0073] Examples of inorganic materials may include, but are not limited to, oxides such as aluminum oxide and silicon dioxide, nitrides such as aluminum nitride and silicon nitride, and sulfates (e.g., barium sulfate, calcium sulfate, etc.) The form of the inorganic material may include, but is not limited to, granular or fibrous.

[0074] The separator may be in the form of a thin film, examples of which include, but are not limited to, nonwoven fabrics, woven fabrics, microporous films, etc. In the thin film form, the separator has a pore size of 0.01 μm to 1 μm and a thickness of 5 μm to 50 μm. In addition to the above-mentioned independent thin film separators, the following separators may also be used: a separator formed by forming a composite porous layer containing the above-mentioned inorganic particles on the surface of the positive electrode and / or the negative electrode using a resin-based adhesive, for example, a separator formed by using a fluororesin as an adhesive to form a porous layer on both sides of the positive electrode with aluminum oxide particles having a particle size of 90% less than 1 μm.

[0075] The thickness of the isolation film is arbitrary. In some embodiments, the thickness of the isolation film is greater than 1 μm, greater than 5 μm, or greater than 8 μm. In some embodiments, the thickness of the isolation film is less than 50 μm, less than 40 μm, or less than 30 μm. When the thickness of the isolation film is within the above range, insulation and mechanical strength can be ensured, and the DC resistance increase characteristics and energy density of the secondary battery can be ensured.

[0076] The present application further provides an electronic device, which includes the secondary battery described in the present application.

[0077] The use of the secondary battery of the present application is not particularly limited, and it can be used for any electronic device known in the prior art. In some embodiments, the secondary battery of the present application can be used for, but not limited to, laptop computers, pen-input computers, mobile computers, e-book players, portable phones, portable fax machines, portable copiers, portable printers, head-mounted stereo headphones, video recorders, LCD TVs, portable cleaners, portable CD players, mini-discs, transceivers, electronic notepads, calculators, memory cards, portable recorders, radios, backup power supplies, motors, cars, motorcycles, power-assisted bicycles, bicycles, lighting fixtures, toys, game consoles, clocks, power tools, flashlights, cameras, large household batteries and lithium-ion capacitors, etc.

[0078] The preparation of the secondary battery is described below in conjunction with specific embodiments. Those skilled in the art will understand that the preparation method described in this application is only an example, and any other suitable preparation method is within the scope of this application.

[0079] Example

[0080] Examples of the nonaqueous electrolyte solution of the present application are shown below, but the present application is not limited to these examples.

[0081] Secondary battery manufacturing

[0082] Production of positive electrode:

[0083] 65 wt % of the inorganic additive in Table 1, 15 wt % of acetylene black, and 20 wt % of the binder polyvinylidene fluoride were mixed, and deionized water was added thereto and mixed evenly to prepare a positive electrode slurry 1.

[0084] The positive electrode active material of lithium cobalt oxide: 97wt%, acetylene black: 1.5wt%, and the binder polyacrylonitrile 1.5wt% are dissolved in 1-methyl-2-pyrrolidone to obtain a solution and mixed to prepare positive electrode slurry 2. Among them, slurry 1 can be applied on the ear side or the end section, and slurry 1 and slurry 2 are applied on aluminum foil in parallel. The coated aluminum foil is dried, pressurized, and then cut into a specified size to make a positive electrode.

[0085] Negative electrode production:

[0086] The negative electrode active material artificial graphite and silicon carbon (mass ratio 90:10): 96wt%, styrene butadiene rubber: 2wt% are mixed, added to a solution obtained by dissolving carboxymethyl cellulose lithium: 2wt% in deionized water in advance and mixed to prepare a negative electrode slurry. The negative electrode slurry is coated on one side of a copper foil, dried, pressurized, and then cut into a specified size to make a negative electrode.

[0087] Battery production:

[0088] The positive electrode and negative electrode prepared as above are each connected to a wire. They are stacked via a polypropylene porous membrane having a thickness of 10 μm. In addition, LiPF6 as an electrolyte is dissolved in a solution comprising (I) non-fluorinated carboxylic acid ester, (II) vinyl sulfate and (III) lithium difluorophosphate as well as ethylene carbonate and propylene carbonate (mass ratio 1: 1.2). Based on 100 parts by mass of the total mass of the non-aqueous electrolyte, the contents and components of (I) to (III) and other additives are shown in Table 2, and the mass content of LiPF6 is 13wt%.

[0089] Then, the laminate and 3.2 g of electrolyte were placed in an aluminum plastic film. The opening of the shell was heat-sealed and the secondary battery was made through steps such as formation and capacity. The secondary battery was in the shape of a bag with a width of 35 mm, a height of 48 mm and a thickness of 5 mm.

[0090] Table 1 Positive electrode insulation layer settings

[0091] Insulation layer position Inorganic additives Positive electrode 1 Ear side Alumina Positive 2 Ear side Boehmite Positive electrode 3 Ear side Magnesium hydroxide Positive electrode 4 Ear side Titanium Dioxide Positive electrode 5 Ear side Zirconium Dioxide Positive electrode 6 Ear side Niobium trioxide Positive electrode 7 Ear side Indium trioxide Positive electrode 8 Ear side Tungsten Trioxide Positive electrode 9 Ear side Tin dioxide Positive electrode 10 Ear side Antimony trioxide Positive electrode 11 Ending Alumina Positive electrode 12 Ending Boehmite Positive electrode 13 Ending Magnesium hydroxide Positive electrode 14 Ending Titanium Dioxide Positive electrode 15 Ending Zirconium Dioxide Positive electrode 16 Ending Niobium trioxide Positive electrode 17 Ending Indium trioxide Positive electrode 18 Ending Tungsten Trioxide Positive electrode 19 Ending Tin dioxide Positive electrode 20 Ending Antimony trioxide Positive electrode 21 No insulation

[0092] Table 2 Electrolyte

[0093]

[0094]

[0095] The values ​​in () in the above table are all wt%, and a is the total mass content of (II) and (III).

[0096] The abbreviations in the above table represent the following substances:

[0097] abbreviation Substance name abbreviation Substance name PP Propyl Propionate EP Ethyl propionate DTD Vinyl Sulfate <![CDATA[LiPO2F2]]> Lithium difluorophosphate C1 Succinonitrile C2 Adiponitrile C3 1,3,6-hexanetricarbonitrile C4 1,2,3-Tris(2-cyanoethoxy)propane C5 Vinyl Sulfate C6 Compound of formula 1 C7 Compound of formula 2

[0098] Test Method

[0099] Lithium ion acceptance at low temperatures

[0100] After the secondary battery is allowed to stand for 24 hours at 25°C, it is charged at a constant current of 1.0C for 1 hour at 25°C to measure the normal temperature charge capacity (C0). Then, at 25°C, the discharge is stopped at a constant current of 0.1C until it reaches 3V. Next, at -20°C, the charge is performed at a constant current of 1.0C for 1 hour to measure the low temperature charge capacity (C1). Then, the ratio of C1 to C0 (C1 / C0) is calculated and evaluated according to the following criteria. The larger the value of C1 / C0, the better the lithium ion acceptance of the secondary battery at low temperatures.

[0101] A: C1 / C0 is greater than or equal to 0.65 and less than or equal to 1;

[0102] B: C1 / C0 is greater than 0.5 and less than 0.65;

[0103] C: C1 / C0 is less than 0.5.

[0104] Low temperature DC resistance (-20℃)

[0105] The secondary battery was charged at 140 mA at 25°C to a 50% state of charge (SOC). Thereafter, it was discharged at 140 mA for 20 seconds and charged at 140 mA for 20 seconds at -20°C, and the voltage change during discharge was recorded as ΔV0.2. Next, the 140 mA in the above steps was replaced with 350 mA, 700 mA, and 1050 mA, respectively, and the voltage changes were calculated and recorded as ΔV0.5, ΔV1.0, and ΔV1.5, respectively.

[0106] Next, a graph was drawn with the discharge current value as the X-axis and ΔV as the Y-axis to find an approximate straight line passing through the intercept zero point. The slope of the approximate straight line was taken as the direct current resistance (DCR), and the evaluation was performed according to the following criteria.

[0107] A: DCR is less than 0.7Ω;

[0108] B: DCR is greater than 0.7Ω and less than 1Ω;

[0109] C: DCR is greater than 1Ω and less than 1.2Ω;

[0110] D: DCR is 1.2Ω or more.

[0111] Low temperature output characteristics

[0112] The secondary battery was left at rest for 24 hours at 25°C. Then, the battery was charged at a charging rate of 0.1C for 5 hours at 25°C, and the voltage V0 at that time was measured. Then, the battery was discharged at a discharge rate of 1C at -10°C, and the voltage V1 was measured 15 seconds after the discharge started. The voltage change ΔV was calculated according to ΔV=V0-V1. The smaller the value of the voltage change ΔV, the better the low-temperature output characteristics were, and the evaluation was performed according to the following criteria.

[0113] A: Voltage change ΔV is less than 350mV;

[0114] B: The voltage change ΔV is greater than 350mV and less than 500mV;

[0115] C: The voltage change ΔV is 500 mV or more.

[0116] Test Results

[0117] Table 3-1

[0118] positive electrode Electrolyte Lithium ion acceptance DC resistance Low temperature output Example 1-1 Positive electrode 1 Electrolyte 1 B B B Example 1-2 Positive electrode 2 Electrolyte 2 A B B Examples 1-3 Positive electrode 3 Electrolyte 3 A B B Examples 1-4 Positive electrode 4 Electrolyte 4 A B B Examples 1-5 Positive electrode 5 Electrolyte 5 A B B Examples 1-6 Positive electrode 6 Electrolyte 6 A B B Examples 1-7 Positive electrode 7 Electrolyte 7 A B B Examples 1-8 Positive electrode 8 Electrolyte 8 A B B Examples 1-9 Positive electrode 9 Electrolyte 9 A B B Examples 1-10 Positive electrode 10 Electrolyte 10 A B B Examples 1-11 Positive electrode 1 Electrolyte 11 A B B Examples 1-12 Positive 2 Electrolyte 12 A B B Examples 1-13 Positive electrode 3 Electrolyte 13 A B B Examples 1-14 Positive electrode 4 Electrolyte 14 B B B Examples 1-15 Positive electrode 5 Electrolyte 15 B B B Examples 1-16 Positive electrode 6 Electrolyte 16 B B B Examples 1-17 Positive electrode 7 Electrolyte 17 A A A Examples 1-18 Positive electrode 8 Electrolyte 18 A A A Examples 1-19 Positive electrode 9 Electrolyte 19 A A A Examples 1-20 Positive electrode 10 Electrolyte 20 A A A Embodiment 1-21 Positive electrode 1 Electrolyte 21 A A A Examples 1-22 Positive 2 Electrolyte 22 A A A Examples 1-23 Positive electrode 3 Electrolyte 23 A A A Examples 1-24 Positive electrode 4 Electrolyte 24 A A A Examples 1-25 Positive electrode 5 Electrolyte 25 A A A Examples 1-26 Positive electrode 6 Electrolyte 26 A A A Examples 1-27 Positive electrode 7 Electrolyte 27 A A A Examples 1-28 Positive electrode 8 Electrolyte 28 A A A Comparative Example 1-1 Positive electrode 21 Electrolyte 1 C C C Comparative Example 1-2 Positive electrode 1 Electrolyte 29 C C C Comparative Examples 1-3 Positive 2 Electrolyte 30 C C C Comparative Examples 1-4 Positive electrode 3 Electrolyte 31 C C C Comparative Examples 1-5 Positive electrode 4 Electrolyte 32 C C C Comparative Examples 1-6 Positive electrode 5 Electrolyte 33 C C C Comparative Examples 1-7 Positive electrode 6 Electrolyte 34 C C C Comparative Examples 1-8 Positive electrode 21 Electrolyte 29 C D C

[0119] Table 3-2

[0120] positive electrode Electrolyte Lithium ion acceptance DC resistance Low temperature output Example 2-1 Positive electrode 11 Electrolyte 1 B A B Example 2-2 Positive electrode 12 Electrolyte 2 A A B Example 2-3 Positive electrode 13 Electrolyte 3 A A B Embodiment 2-4 Positive electrode 14 Electrolyte 4 A A B Embodiment 2-5 Positive electrode 15 Electrolyte 5 A A B Embodiment 2-6 Positive electrode 16 Electrolyte 6 A A B Embodiment 2-7 Positive electrode 17 Electrolyte 7 A A B Embodiment 2-8 Positive electrode 18 Electrolyte 8 A A B Embodiment 2-9 Positive electrode 19 Electrolyte 9 A A B Embodiment 2-10 Positive electrode 20 Electrolyte 10 A A B Example 2-11 Positive electrode 11 Electrolyte 11 A A B Example 2-12 Positive electrode 12 Electrolyte 12 A A B Example 2-13 Positive electrode 13 Electrolyte 13 A A B Embodiment 2-14 Positive electrode 14 Electrolyte 14 B A B Example 2-15 Positive electrode 15 Electrolyte 15 B A B Example 2-16 Positive electrode 16 Electrolyte 16 B A B Example 2-17 Positive electrode 17 Electrolyte 17 A A A Example 2-18 Positive electrode 18 Electrolyte 18 A A A Example 2-19 Positive electrode 19 Electrolyte 19 A A A Embodiment 2-20 Positive electrode 20 Electrolyte 20 A A A Example 2-21 Positive electrode 11 Electrolyte 21 A A A Example 2-22 Positive electrode 12 Electrolyte 22 A A A Example 2-23 Positive electrode 13 Electrolyte 23 A A A Example 2-24 Positive electrode 14 Electrolyte 24 A A A Example 2-25 Positive electrode 15 Electrolyte 25 A A A Example 2-26 Positive electrode 16 Electrolyte 26 A A A Example 2-27 Positive electrode 17 Electrolyte 27 A A A Example 2-28 Positive electrode 18 Electrolyte 28 A A A Comparative Example 2-1 Positive electrode 21 Electrolyte 1 C C C Comparative Example 2-2 Positive electrode 11 Electrolyte 29 C C C Comparative Examples 2-3 Positive electrode 11 Electrolyte 30 C C C Comparative Examples 2-4 Positive electrode 11 Electrolyte 31 C C C Comparative Examples 2-5 Positive electrode 11 Electrolyte 32 C C C Comparative Examples 2-6 Positive electrode 11 Electrolyte 33 C C C Comparative Examples 2-7 Positive electrode 11 Electrolyte 34 C C C Comparative Examples 2-8 Positive electrode 21 Electrolyte 29 C D C

[0121] In a secondary battery in which the positive electrode includes an insulating layer and a positive electrode active material layer arranged on a current collector, and the insulating layer includes an inorganic additive, the electrolyte contains (I) a fluorine-free chain carboxylic acid ester, (II) vinyl sulfate and (III) lithium difluorophosphate, wherein based on the mass of the electrolyte, the total content of (II) and (III) is greater than 0.02wt% and less than 3.26wt%; the content of (I) is greater than 8.6wt% and less than 65wt%, which is important and is very critical to the stability of the positive electrode structure, and significantly suppresses the increase of interface resistance at low temperatures. This design can not only improve the lithium ion acceptance of the secondary battery at low temperatures, but also suppress the increase of low-temperature DC resistance and improve low-temperature output characteristics.

[0122] When the insulating layer is located at the lug side or the tail section, excellent secondary battery characteristics are obtained. Especially when the insulating layer is located at the tail section, it has a further effect on improving the low-temperature characteristics.

[0123] When the electrolyte also contains other additives such as 1,2-bis(difluorophosphine)ethane, a compound of formula 1, a compound of formula 2, vinylene carbonate, lithium fluorosulfonate, succinonitrile, adiponitrile, 1,3,6-hexanetricarbonitrile, 1,2,3-tris(2-cyanoethoxy)propane, vinyl sulfate, fluorobenzene, cyclohexylbenzene, biphenyl, tris(trimethylsilyl)phosphate, and tris(trimethylsilyl)borate, the increase in low-temperature DC resistance is further suppressed and the low-temperature output characteristics are improved.

[0124] References to "embodiments", "partial embodiments", "one embodiment", "another example", "example", "specific example" or "partial example" throughout the specification mean that at least one embodiment or example in the present application includes the specific features, structures, materials or characteristics described in the embodiment or example. Therefore, descriptions appearing in various places throughout the specification, such as: "in some embodiments", "in an embodiment", "in one embodiment", "in another example", "in an example", "in a specific example" or "example", do not necessarily refer to the same embodiment or example in the present application. In addition, the specific features, structures, materials or characteristics in the present application may be combined in one or more embodiments or examples in any suitable manner.

[0125] Although illustrative embodiments have been demonstrated and described, those skilled in the art should understand that the above embodiments should not be construed as limitations on the present application, and that changes, substitutions and modifications may be made to the embodiments without departing from the spirit, principles and scope of the present application.

Claims

1. A secondary battery, characterized in that: include: Positive electrode, negative electrode and electrolyte; The positive electrode comprises: an insulating layer and a positive electrode active material layer disposed on a current collector; the insulating layer comprises: an inorganic additive; the inorganic additive comprises: a metal element; the metal element in the inorganic additive comprises: at least one of aluminum, magnesium, titanium, zirconium, niobium, indium, tungsten, tin, zinc or antimony; The electrolyte contains a fluorine-free chain carboxylate, vinyl sulfate and lithium difluorophosphate, wherein the total mass content of the vinyl sulfate and the lithium difluorophosphate is greater than 0.02wt% and less than 3.26wt% based on the mass of the electrolyte, and the mass content of the fluorine-free chain carboxylate is greater than 8.6wt% and less than 65wt%; The electrolyte further comprises: other additives; the other additives comprise: at least one of 1,2-bis(difluorophosphine)ethane, a compound of formula 1, a compound of formula 2, vinylene carbonate, lithium fluorosulfonate, succinonitrile, adiponitrile, 1,3,6-hexatriconitrile, 1,2,3-tris(2-cyanoethoxy)propane, fluorobenzene, cyclohexylbenzene, biphenyl, tris(trimethylsilyl)phosphate or tris(trimethylsilyl)borate; 2. The secondary battery according to claim 1, characterized in that: The total mass content of the vinyl sulfate and the lithium difluorophosphate is greater than or equal to 0.05 wt % and less than or equal to 1.98 wt % based on the mass of the electrolyte.

3. The secondary battery according to claim 1, characterized in that: The mass content of the fluorine-free chain carboxylic acid ester is 17.3 wt % or more and 52.6 wt % or less based on the mass of the electrolyte.

4. The secondary battery according to claim 1, characterized in that: The inorganic additive is selected from at least one of aluminum oxide, aluminum hydroxide, boehmite, magnesium oxide, magnesium hydroxide, titanium dioxide, zirconium dioxide, niobium monoxide, niobium dioxide, niobium trioxide, niobium pentoxide, indium trioxide, tungsten trioxide, tin dioxide, zinc oxide or antimony trioxide.

5. The secondary battery according to any one of claims 1 to 4, characterized in that: The fluorine-free chain carboxylic acid ester is selected from at least one of methyl acetate, ethyl acetate, n-propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl isobutyrate, ethyl isobutyrate, n-propyl isobutyrate, methyl pivalate, ethyl pivalate, n-propyl pivalate, methyl acrylate, ethyl acrylate, n-propyl acrylate, methyl methacrylate, ethyl methacrylate or n-propyl methacrylate.

6. The secondary battery according to any one of claims 1 to 4, characterized in that: Based on the mass of the electrolyte, the mass content of the vinyl sulfate is greater than 0.01wt% and less than 1.67wt%; Alternatively, based on the mass of the electrolyte, the mass content of the lithium difluorophosphate is greater than or equal to 0.01 wt % and less than or equal to 1.95 wt %.

7. The secondary battery according to any one of claims 1 to 4, characterized in that: The mass content of the other additives is greater than or equal to 0.5 wt % and less than or equal to 7 wt % based on the mass of the electrolyte.

8. The secondary battery according to any one of claims 1 to 4, characterized in that: A pole lug is arranged on one side of the current collector, and the insulating layer is arranged on an edge surface of the current collector on the side with the pole lug.

9. The secondary battery according to any one of claims 1 to 4, characterized in that: The secondary battery has a winding structure, and the insulating layer is arranged on the surface of the end section of the current collector in the length direction.

10. An electronic device, characterized in that: include: The secondary battery according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Lithium secondary battery electrolyte and lithium secondary battery

    CN107369849A

  • High-voltage rate electrolyte with high-and-low temperature performance and lithium ion battery using electrolyte

    CN107706455A

  • Electrolyte, and electrochemical device and electronic device comprising same

    CN113767500A

  • Electrolyte and battery comprising same

    CN116093429A

  • Antibacterial biogradable film composition comprising propyl gallate and the manufacturing method thereof

    KR1020250082979A

Cited By

  • Secondary battery and electronic device

    WO2025246523A1