Aqueous process for preparing polyamic acids and polyamic acid related gel materials

Polyamic acid and polyimide gels are prepared by using water-soluble carbonate in water and reacting diamine and tetracarboxylic acid dianhydride, which solves the problem of using organic solvents in traditional methods, and achieves greening technology and high efficiency Prepared to obtain a robust and transparent gel material.

CN118973699APending Publication Date: 2024-11-15ASPEN AEROGELS INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380030429.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-06-15
Filing Date
2023-03-30
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The prior art When preparing polyamic acid and polyimide gel materials, it relies on organic solvents, which leads to environmental protection and safety problems. It is difficult to realize the greening process using harmful organic solvents and reagents.

Method used

Use water-soluble carbonate or bicarbonate in water to react with diamine and tetracarboxylic dianhydride to form an aqueous solution of polyamide salt and convert it into a polyimide gel through imidation, avoiding organic solvents and the use of reagents, supercritical drying and other methods are used to remove solvents to prepare aerogels.

Benefits of technology

The green preparation of polyamic acid and polyimide gels is achieved, reducing the cost of use and treatment of harmful substances, and obtaining a mechanically robust and optically transparent polyimide gel with similar physical properties to the traditional method.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005059772840000171
    Figure BDA0005059772840000171
  • Figure BDA0005059772840000181
    Figure BDA0005059772840000181
  • Figure BDA0005059772840000191
    Figure BDA0005059772840000191
Patent Text Reader

Abstract

The present disclosure relates to methods of forming polyamic acids, polyamic acid metal salts, and polyimide gels under aqueous conditions that utilize water-soluble carbonate or bicarbonate. These gels may be converted to aerogels or xerogels, which may further be converted to carbon aerogels or xerogels. Such carbon aerogels or xerogels have the same physical properties as carbon aerogels or xerogels prepared from polyimide aerogels obtained according to conventional methods, i.e., organic solvent-based methods.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to and the benefit of U.S. Provisional Patent Application No. 63 / 352,571, filed on June 15, 2022, entitled “Aqueous Process For Preparing Polyamic Acids and Polyamic Acid Related Gel Materials,” which is incorporated herein by reference in its entirety. Technical Field

[0003] The present disclosure generally relates to aqueous processes for preparing aqueous solutions of polyamic acid salts, and to methods for converting such materials into porous polyamic acids, polyimides, and corresponding porous carbon materials. Background Art

[0004] Aerogel is a solid material that includes a porous network structure of interconnected micropores, mesopores and macropores. Depending on the precursor material used and the processing experienced, the pores of the aerogel usually account for more than 90% of the volume. Aerogels are generally prepared by removing solvent from a wet gel (a solid network structure containing a solvent prepared by a sol-gel process) in a manner that causes the capillary force at its pore wall to cause minimal or no collapse to the wet gel. Solvent removal methods include, but are not limited to, supercritical drying (or drying with a supercritical fluid so that a low surface tension supercritical fluid replaces a high surface tension gelling solvent in the gel), exchanging a solvent with a supercritical fluid, exchanging a solvent with a fluid that is subsequently converted to a supercritical state, subcritical or near-critical drying, and sublimating a frozen solvent in a freeze-drying process. See, for example, PCT Patent Application No. WO2016127084A1. It should be noted that when dried under ambient conditions, gel collapse may occur as the solvent evaporates, and a xerogel may be formed. Thus, the preparation of aerogels by a sol-gel process (or optionally, a similar process) is typically carried out in a sequence of steps: dissolving a monomer or monomer mixture or gel precursor in a solvent, adding a catalyst or reagent that induces or promotes the reaction of the one or more monomers or gel precursors, forming a reaction mixture, forming a wet gel (which may include additional heating or cooling steps), and removing the solvent by supercritical drying techniques or any other method that removes the solvent from the gel without causing collapse or pore collapse.

[0005] Aerogels can be formed from inorganic materials, organic materials, or mixtures thereof. When an organic material is formed, the organic aerogel can be carbonizable (e.g., by pyrolysis at elevated temperatures in an inert atmosphere) to form a carbon aerogel, which can have properties that are different or overlapping with the corresponding organic material (e.g., pore volume, pore size distribution, morphology, etc.), depending on the precursor materials and methods used. Examples of carbonizable organic materials include, but are not limited to, phenolic polymers, including resorcinol-formaldehyde (RF) and phloroglucinol-furfural (PF); polyolefins, including polyacrylonitrile (PAN); selected polyimides (PI); polyurethanes (PU); polyureas (PUA); polyamides (PA); polydicyclopentadiene; precursors or polymeric derivatives thereof; and combinations thereof.

[0006] Recently, people have been committed to developing and characterizing carbon aerogels, xerogels and ambigels as electrode materials to improve their application performance in energy storage devices such as lithium ion batteries (LIBs). Therefore, there is a demand for corresponding organic aerogels. Such organic aerogels are generally prepared in organic solvents. For example, polyimide aerogels are generally prepared by reacting diamines with tetracarboxylic dianhydrides in organic solvents, and then dehydrating the resulting polymerizable primary reaction product polyamic acid to form a polyimide gel. For economic, safety and environmental reasons, it will be desirable to use a "green" chemical process (i.e., using a more environmentally friendly alternative to conventional organic solvents and / or organic reagents) to carry out the formation and gelation of such polyamic acid-based gel materials. Summary of the invention

[0007] The technology of the present invention generally relates to a method for forming polyamic acid and related gel materials (e.g., polyimide wet gel, aerogel, xerogel and bigel), while (a) minimizing or eliminating the use of harmful organic solvents and (b) minimizing the use of organic reagents. Specifically, the technology of the present invention relates to forming polyamic acid and polyimide in water, using water-soluble carbonate or bicarbonate to stabilize the polyamic acid. Optionally, the gel formed in this way can be subsequently converted into polyamic acid aerogel, polyimide gel and aerogel, and corresponding carbon aerogel, xerogel and / or other gel materials.

[0008] The disclosed method generally includes preparing an aqueous solution of polyamic acid salt from the reaction of water-soluble diamine and tetracarboxylic dianhydride in the presence of water-soluble carbonate or bicarbonate. Alternatively, an aqueous solution of polyamic acid salt can be prepared from a polyamic acid preformed by dissolving the acid in water in the presence of water-soluble carbonate or bicarbonate. Surprisingly, according to the present disclosure, it is found that such water-soluble carbonate or bicarbonate (including but not limited to carbonate and bicarbonate of certain alkali metals, ammonia and guanidine) leads to the formation of corresponding polyamic acid salt (also referred to as salt of polyamic acid, or simply referred to as polyamic acid salt), and further, after imidization, the resulting polyimide is mechanically robust and generally optically transparent. In particular, the resulting polyimide has substantially similar physical properties to those prepared by conventional (i.e., organic solvent-based) methods of polyimide. In contrast, using an amine base (e.g., triethylamine) with reduced nucleophilicity typically results in a generally translucent or opaque wet gel under the same conditions, and the wet gel is weaker in terms of its physical strength.

[0009] Accordingly, on the one hand, a method for preparing an aqueous solution of a polyamic acid salt is provided. In general non-limiting aspects, the method comprises: combining a water-soluble diamine, a water-soluble carbonate or bicarbonate, and a tetracarboxylic dianhydride in water; and reacting the components to provide a solution of the polyamic acid salt. The order of addition of the reaction components (i.e., a water-soluble diamine, a water-soluble carbonate or bicarbonate, and a tetracarboxylic dianhydride) can be changed.

[0010] In some aspects, the combining comprises: dissolving a water-soluble diamine in water to form an aqueous diamine solution; adding the water-soluble carbonate or bicarbonate to the aqueous diamine solution; adding tetracarboxylic dianhydride to the aqueous solution of the diamine and the water-soluble carbonate or bicarbonate to form a solution; and stirring the solution at a temperature in the range of about 4°C to about 60°C for a period of time of about 1 hour to about 4 days.

[0011] In some aspects, the water-soluble carbonate or bicarbonate salt comprises lithium, sodium, potassium, ammonium, alkylammonium, guanidine, or a combination thereof.

[0012] In some aspects, the water-soluble carbonate or bicarbonate is selected from the group consisting of lithium carbonate, lithium bicarbonate, sodium carbonate, sodium bicarbonate, potassium carbonate, potassium bicarbonate, and combinations thereof.

[0013] In some aspects, the water-soluble carbonate or bicarbonate is selected from the group consisting of guanidine carbonate, ammonium carbonate, and ammonium bicarbonate. In some aspects, the water-soluble carbonate or bicarbonate is guanidine carbonate.

[0014] In some aspects, the water soluble carbonate or bicarbonate is a carbonate salt, and the molar ratio of carbonate salt to diamine is from about 1 to about 1.4.

[0015] In some aspects, the water-soluble carbonate or bicarbonate is a bicarbonate salt, and the molar ratio of bicarbonate salt to diamine is from about 2 to about 2.8.

[0016] In some aspects, the molar ratio of tetracarboxylic dianhydride to diamine is from about 0.9 to about 1.1.

[0017] In some aspects, the tetracarboxylic dianhydride is selected from the group consisting of pyromellitic dianhydride (PMDA), diphthalic dianhydride (BPDA), oxydiphthalic dianhydride (ODPA), benzophenonetetracarboxylic dianhydride (BTDA), ethylenediaminetetraacetic dianhydride (EDDA), 1,4,5,8-naphthalenetetracarboxylic dianhydride, and combinations thereof. In some aspects, the tetracarboxylic dianhydride is pyromellitic dianhydride (PMDA). In some aspects, the tetracarboxylic dianhydride is benzophenonetetracarboxylic dianhydride (BTDA).

[0018] In some aspects, the water-soluble diamine is a C2-C6 alkylenediamine, wherein one or more of the carbon atoms of the C2-C6 alkylene are optionally substituted with one or more alkyl groups. In some aspects, the C2-C6 alkylenediamine is selected from the group consisting of 1,3-diaminopropane, 1,4-diaminobutane, 1,5-diaminopentane, 1,6-diaminohexane and ethylenediamine.

[0019] In some aspects, the water-soluble diamine is 1,3-phenylenediamine, 4,4'-methylenedianiline, or a combination thereof. In some aspects, the water-soluble diamine is selected from the group consisting of 1,4-phenylenediamine, 1,3-phenylenediamine, and a combination thereof. In some aspects, the water-soluble diamine is 1,4-phenylenediamine. In some aspects, the water-soluble diamine is 1,3-phenylenediamine.

[0020] In some aspects, the concentration of the polyamic acid salt in the aqueous solution ranges from about 0.01 to about 0.3 g / cm 3 .

[0021] In some aspects, the molar ratio of tetracarboxylic dianhydride to diamine is from about 0.9 to about 1.1.

[0022] In some aspects, the method further includes adding an electroactive substance to the aqueous solution of the polyamic acid salt. In some aspects, the electroactive material includes carbon, graphite, silicon, tin, sulfur, Prussian blue, lithium metal phosphate, lithium mixed metal phosphate or lithium metal fluorophosphate. In some aspects, the electroactive material includes one or more precursors of lithium iron phosphate, lithium magnesium phosphate, lithium vanadium phosphate, a combination thereof or any one thereof. In some aspects, the electroactive material is silicon. In some aspects, the electroactive material is lithium iron phosphate.

[0023] In some aspects, the method further includes forming a polyamic acid gel, wherein forming the polyamic acid gel includes: acidifying the polyamic acid salt solution to form a polyamic acid gel; and drying the polyamic acid gel to form a polyamic acid aerogel.

[0024] In some aspects, drying the polyamic acid gel comprises: optionally, washing the polyamic acid gel or subjecting it to solvent exchange; and subjecting the optionally washed or solvent-exchanged polyamic acid gel to elevated temperature conditions, freeze-drying the optionally washed or solvent-exchanged polyamic acid gel, or contacting the optionally washed or solvent-exchanged polyamic acid gel with supercritical fluid carbon dioxide.

[0025] In some aspects, the washing or solvent exchange is performed with water, a C1 to C4 alcohol, acetone, acetonitrile, ether, tetrahydrofuran, toluene, liquid carbon dioxide, or a combination thereof.

[0026] In yet another aspect, provided is a polyamic acid aerogel prepared by the method disclosed herein.

[0027] In some aspects, the polyamic acid aerogel includes residual amounts of water-soluble carbonates or bicarbonates.

[0028] In some aspects, the method further includes forming a polyimide aerogel, wherein forming the polyimide aerogel includes: imidizing a polyamic acid salt to form a polyimide gel; and drying the polyimide gel to form the polyimide aerogel.

[0029] In some aspects, imidizing the polyamic acid salt comprises adding a gelling initiator to an aqueous solution of the polyamic acid salt to form a gelling mixture and gelling the gelling mixture. In some aspects, the gelling initiator is a carboxylic acid anhydride. In some aspects, the gelling initiator is acetic anhydride.

[0030] In some aspects, drying the polyimide gel comprises: optionally, washing or solvent exchanging the polyimide gel; and subjecting the polyimide gel to elevated temperature conditions, freeze-drying the polyimide gel, or contacting the polyimide gel with supercritical fluid carbon dioxide.

[0031] In some aspects, the washing or solvent exchange is performed with water, a C1 to C4 alcohol, acetone, acetonitrile, ether, tetrahydrofuran, toluene, liquid carbon dioxide, or a combination thereof.

[0032] In another aspect, provided is a polyimide aerogel prepared by the method disclosed herein.

[0033] In some aspects, the polyimide aerogel includes residual amounts of water-soluble carbonates or bicarbonates.

[0034] In some aspects, the method further comprises converting the polyamic acid aerogel and / or polyimide aerogel as disclosed herein into an isostructural carbon aerogel, the conversion comprising pyrolyzing the aerogel at a temperature of at least about 500° C. under an inert atmosphere.

[0035] In another aspect, provided is a carbon aerogel prepared by the method disclosed herein.

[0036] In some aspects, the carbon aerogel includes an electroactive material.

[0037] In some aspects, the carbon aerogels have substantially similar properties to those carbon aerogels prepared by pyrolyzing corresponding polyimide aerogels that have been prepared by conventional non-aqueous methods.

[0038] On the other hand, a method for preparing an aqueous solution of a polyamic acid salt is provided, the method comprising providing a suspension of a preformed polyamic acid in water, and adding a water-soluble carbonate or bicarbonate to the suspension, wherein the water-soluble carbonate or bicarbonate is added in an amount sufficient to completely dissolve the polyamic acid to form an aqueous solution of the polyamic acid salt. Such an aqueous solution of a polyamic acid salt may be further processed according to any one of the above aspects.

[0039] The present disclosure includes but is not limited to the following aspects:

[0040] Aspect 1: A method for preparing an aqueous solution of a polyamic acid salt, the method comprising: providing a polyamic acid; and combining the polyamic acid and a water-soluble carbonate or bicarbonate in water to provide a solution of the polyamic acid salt.

[0041] Aspect 2: The method according to aspect 1, wherein the water-soluble carbonate or bicarbonate comprises lithium, sodium, potassium, ammonium or guanidinium cations.

[0042] Aspect 3: The method according to aspect 1 or 2, wherein the water-soluble carbonate or bicarbonate is selected from the group consisting of lithium carbonate, lithium bicarbonate, sodium carbonate, sodium bicarbonate, potassium carbonate, potassium bicarbonate, ammonium carbonate, ammonium bicarbonate, guanidine carbonate, and combinations thereof.

[0043] Aspect 4: A method for preparing an aqueous solution of a polyamic acid salt, the method comprising: combining a water-soluble diamine, a water-soluble carbonate or bicarbonate, and a tetracarboxylic dianhydride in water; and reacting the components to provide a solution of the polyamic acid salt.

[0044] Aspect 5: A method according to aspect 4, wherein the combining comprises: dissolving a water-soluble diamine in water to form an aqueous diamine solution; adding the water-soluble carbonate or bicarbonate to the aqueous diamine solution; adding tetracarboxylic dianhydride to the aqueous solution of the diamine and the water-soluble carbonate or bicarbonate to form a solution; and stirring the solution at a temperature in the range of about 4°C to about 60°C for a period of time in the range of about 1 hour to about 4 days.

[0045] Aspect 6: A method according to aspect 4, wherein the combining comprises: dissolving a water-soluble diamine in water to form an aqueous diamine solution; adding tetracarboxylic dianhydride to the aqueous diamine solution to form a suspension; stirring the suspension at a temperature in the range of about 4°C to about 60°C for a time period in the range of about 1 hour to about 4 days; adding the water-soluble carbonate or bicarbonate to the suspension; and stirring the suspension at a temperature in the range of about 4°C to about 60°C for a time period in the range of about 1 hour to about 4 days to provide an aqueous solution of the polyamic acid salt.

[0046] Aspect 7: A method according to aspect 4, wherein the combining comprises: adding a water-soluble diamine, a tetracarboxylic dianhydride and the water-soluble carbonate or bicarbonate to water simultaneously or in rapid succession; and stirring the resulting mixture at a temperature in the range of about 4°C to about 60°C for a period of time in the range of about 1 hour to about 4 days to provide an aqueous solution of the polyamic acid salt.

[0047] Aspect 8: The method according to any one of aspects 4 to 7, wherein the water-soluble carbonate or bicarbonate comprises lithium, sodium, potassium, ammonium or guanidinium cations.

[0048] Aspect 9: The method according to any one of aspects 4 to 8, wherein the water-soluble carbonate or bicarbonate is selected from the group consisting of lithium carbonate, lithium bicarbonate, sodium carbonate, sodium bicarbonate, potassium carbonate, potassium bicarbonate, ammonium carbonate, ammonium bicarbonate, guanidine carbonate, and combinations thereof.

[0049] Aspect 10: The method according to any one of Aspects 4 to 9, wherein the water-soluble carbonate or bicarbonate is a carbonate, and the molar ratio of the water-soluble carbonate to the diamine is about 1 to about 1.4, or the water-soluble carbonate or bicarbonate is a bicarbonate, and the molar ratio of the water-soluble bicarbonate to the diamine is 2 to about 2.8.

[0050] Aspect 11: The method according to any one of aspects 4 to 10, wherein the molar ratio of the tetracarboxylic dianhydride to the diamine is from about 0.9 to about 1.1.

[0051] Aspect 12: A method according to any one of Aspects 4 to 11, wherein the tetracarboxylic dianhydride is selected from the group consisting of: diphthalic dianhydride (BPDA), dibenzophenonetetracarboxylic dianhydride (BTDA), oxydiphthalic dianhydride (ODPA), naphthalenetetracarboxylic dianhydride, perylenetetracarboxylic dianhydride, and pyromellitic dianhydride (PMDA).

[0052] Aspect 13: The method according to any one of aspects 4 to 12, wherein the diamine is 1,3-phenylenediamine, 1,4-phenylenediamine, or a combination thereof.

[0053] Aspect 14: The method according to any one of aspects 4 to 13, wherein the diamine is 1,4-phenylenediamine.

[0054] Aspect 15: The method according to any one of aspects 4 to 14, wherein the concentration of the polyamic acid salt in the aqueous solution ranges from about 0.01 to about 0.3 g / cm based on the weight of the polyamic acid salt. 3 .

[0055] Aspect 16: The method according to any one of aspects 1 to 15, wherein the water-soluble carbonate or bicarbonate is guanidine carbonate, and wherein the solution of the polyamic acid salt exhibits thixotropic behavior.

[0056] Aspect 17: The method according to any one of aspects 1 to 16, further comprising adding an electroactive material to the aqueous solution of the polyamic acid salt.

[0057] Aspect 18: The method according to aspect 17, wherein the electroactive material comprises carbon, graphite, silicon, sulfur, Prussian blue, lithium iron phosphate, a combination thereof, or one or more precursors of any one thereof.

[0058] Aspect 19: The method according to any one of aspects 1 to 18, further comprising forming a polyamic acid gel, wherein forming the polyamic acid gel comprises: acidifying the polyamic acid salt solution to form a polyamic acid wet gel; and drying the polyamic acid wet gel to form a polyamic acid aerogel.

[0059] Aspect 20: The method according to Aspect 19, wherein drying the polyamic acid wet gel comprises: optionally, washing the polyamic acid wet gel or performing a solvent exchange thereon; and subjecting the polyamic acid wet gel to elevated temperature conditions, freeze-drying the polyamic acid wet gel, or contacting the polyamic acid wet gel with supercritical fluid carbon dioxide.

[0060] Aspect 21: The method according to aspect 19 or 20, further comprising converting the polyamic acid aerogel into an isostructural carbon aerogel, the conversion comprising pyrolyzing the polyamic acid aerogel material at a temperature of at least about 650°C under an inert atmosphere.

[0061] Aspect 22: The method according to any one of aspects 1 to 18, further comprising forming a polyimide gel, wherein forming the polyimide gel comprises: imidizing the polyamic acid salt to form a polyimide wet gel; and drying the polyimide wet gel to form a polyimide aerogel.

[0062] Aspect 23: The method according to aspect 22, wherein imidizing the polyamic acid salt comprises adding a gelation initiator to an aqueous solution of the polyamic acid salt to form a gelation mixture and gelling the gelation mixture.

[0063] Aspect 24: The method according to aspect 23, wherein the gelation initiator is acetic anhydride.

[0064] Aspect 25: The method according to any one of Aspects 22 to 24, wherein drying the polyimide wet gel comprises: optionally, washing the polyimide wet gel or subjecting it to solvent exchange; and subjecting the polyimide wet gel to elevated temperature conditions, freeze-drying the polyimide wet gel, or contacting the polyimide wet gel with supercritical fluid carbon dioxide.

[0065] Aspect 26: The method according to aspect 20 or 25, wherein the washing or solvent exchange is carried out with water, C1 to C4 alcohol, acetone, acetonitrile, ether, tetrahydrofuran, toluene, liquid carbon dioxide, or a combination thereof.

[0066] Aspect 27: The method according to any one of aspects 22 to 26, further comprising converting the polyimide aerogel to an isostructural carbon aerogel, the converting comprising pyrolyzing the polyimide aerogel at a temperature of at least about 650° C. under an inert atmosphere.

[0067] Aspect 28: A polyamic acid salt prepared by the method according to any one of aspects 1 to 18.

[0068] Aspect 29: A polyamic acid aerogel prepared by the method according to aspect 19 or 20.

[0069] Aspect 30: A polyimide aerogel prepared by the method according to any one of aspects 22 to 26.

[0070] Aspect 31: The polyamic acid aerogel according to aspect 29, comprising a residual amount of the water-soluble carbonate or bicarbonate.

[0071] Aspect 32: The polyimide aerogel according to aspect 30, comprising a residual amount of the water-soluble carbonate or bicarbonate.

[0072] Aspect 33: A carbon aerogel prepared by the method according to aspect 21 or 27. BRIEF DESCRIPTION OF THE DRAWINGS

[0073] In order to provide an understanding of the technical aspects, reference is made to the accompanying drawings, which are not necessarily drawn to scale. The accompanying drawings are merely illustrative and should not be construed as limiting the technology. The disclosure described herein is illustrative by way of example and not by way of limitation to the accompanying drawings.

[0074] Figure 1A is a solid-state nitrogen-15 nuclear magnetic resonance (NMR) spectrum of an organogel according to non-limiting aspects of the present disclosure.

[0075] Figure 1B is a solid-state nitrogen-15 NMR spectrum of an organogel according to non-limiting aspects of the present disclosure.

[0076] Figure 2 is a photograph of a thin film cast on an aluminum sheet according to non-limiting aspects of the present disclosure.

[0077] Figure 3 2 is a material characterization data sheet for aerogels according to non-limiting aspects of the present disclosure.

[0078] Figure 4 2 is a material characterization data sheet for aerogels according to non-limiting aspects of the present disclosure.

[0079] Figure 5A is a solid-state nitrogen-15 NMR spectrum of an organogel according to non-limiting aspects of the present disclosure.

[0080] Figure 5B is a solid-state nitrogen-15 NMR spectrum of an organogel according to non-limiting aspects of the present disclosure.

[0081] Figure 6 2 is a material characterization data sheet for aerogels according to non-limiting aspects of the present disclosure.

[0082] Figure 7 is a scanning electron microscope (SEM) micrograph of a carbonized sample of a polyimide according to non-limiting aspects of the present disclosure.

[0083] Figure 8 is a graphical depiction of oscillatory stress versus storage modulus (G') and loss modulus (G") for various polyamic acid guanidine aqueous solutions according to non-limiting aspects of the present disclosure.

[0084] Fig. 9 is a graphical depiction of temperature versus yield stress for polyamic acid guanidine solutions according to non-limiting aspects of the present disclosure.

[0085] Fig.10is a graphical depiction of the oscillatory viscoelastic response of an aqueous solution of polyamic acid guanidine versus time as measured by tan(d) according to non-limiting aspects of the present disclosure.

[0086] Fig.11 is a graphical depiction of shear rate versus viscosity for various aqueous solutions of polyamic acid salts according to non-limiting aspects of the present disclosure.

[0087] Fig.12 Detailed Description of the Invention Figures 2 and 3 are a series of gel permeation chromatograms (GPC) of various aqueous polyamic acid salt solutions according to non-limiting aspects of the present disclosure.

[0088] Fig.13 is a graphical depiction of the viscosity versus GPC molecular weight of various aqueous solutions of polyamic acid salts according to non-limiting aspects of the present disclosure. DETAILED DESCRIPTION

[0089] Before describing several exemplary aspects of the technology, it should be understood that the technology is not limited to the details of the construction or process described in detail in the following specific embodiments. The technology can be other aspects and can be practiced or implemented in a variety of ways. Generally, the technology of the present invention relates to a method for forming polyamic acid gel and polyimide gel without using harmful organic solvents.

[0090] On the one hand, the method generally includes: providing polyamic acid; and combining the polyamic acid and a water-soluble carbonate or bicarbonate in water to provide a solution of the polyamic acid salt. In other aspects, the method generally includes preparing polyamic acid salt in situ. In such aspects, the method generally includes: combining a water-soluble diamine, a water-soluble carbonate or bicarbonate, and a tetracarboxylic dianhydride in water; and reacting the components to provide a solution of a polyamic acid salt. In some aspects, the method further includes converting the polyamic acid salt into a polyamic acid wet gel or aerogel, a polyimide wet gel or aerogel, or a corresponding carbon aerogel.

[0091] The disclosed methods are economically advantageous over conventional methods for preparing polyimide and polyamic acid gel materials (e.g., expensive organic solvents are avoided and processing costs are minimized) and are "green" (i.e., beneficial from an environmental perspective because potentially toxic organic solvents and reagents are avoided or minimized and the production of toxic by-products is minimized or eliminated), and facilitate potentially reducing the total number of operations that must be performed to provide carbon gel materials.

[0092] The disclosed method generally relies on the use of water-soluble carbonates or bicarbonates (including but not limited to carbonates or bicarbonates of alkali metals, ammonium or guanidine) to neutralize the polyamic acid while forming it, and provide the charge-compensating cations of the resulting polyamic acid salt. Without being bound by theory, it is believed that carbonates and bicarbonates are particularly advantageous because their roles in neutralizing the substance and in providing cations are separate. Specifically, carbonates or bicarbonates react with the formed polyamic acid and are converted into CO2, which escapes from the reaction mixture in gaseous form, leaving a polyamic acid salt with cations (e.g., alkali metals, ammonium or guanidine cations) introduced using the carbonates or bicarbonates. Furthermore, such carbonates or bicarbonates have buffering activity, maintaining the pH of the solution within the desired range.

[0093] Surprisingly, according to the present disclosure, it has been found that polyamic acid salt solutions produced from the reaction of 1,4-phenylenediamine with pyromellitic dianhydride in water achieve high viscosities in carbonate solutions at lower target density (Td) values, in contrast to the viscosities achieved using triethylamine (abbreviated Et3N or TEA, which is generally considered a non-nucleophilic amine base) alone under similar conditions. Moreover, without wishing to be bound by any particular theory, it is believed that the nucleophilicity of some residual and non-negligible Et3N may be at least partially responsible for the lower viscosity obtained using it, perhaps by transferring some PMDA to side reactions, thereby limiting the length of the polyamic acid polymer. Another unbound theory is that the hydrolysis of Et3N produces a high concentration of hydroxide ions, while the buffering effect of the carbonate / bicarbonate / carbonic acid / CO2 system maintains a lower pH (lower hydroxide ion concentration) in comparison. Furthermore, as shown above, the protonation of bicarbonate and carbonate base produces H2CO3, which decomposes into CO2+H2O, which completely escapes from the reaction mixture in gaseous form, and leaves the cation of carbonate or bicarbonate as the charge-balancing cation of polyamic acid salt. Without being bound by any particular theory, it is believed that polymerization seems to proceed to relatively high molecular weight polymers in the absence of significant side reactions that interfere with polymer growth (such as those that may occur when using alkalis such as triethylamine). It is expected that lithium, sodium, potassium, ammonium and guanidine salts of polyamic acid (such as, for example, those produced from PDA and PMDA) are very soluble in water, and corresponding carbonates and bicarbonates are commercially easily available and cheap. More surprisingly, the polyimide gel prepared by chemical imidization under water-soluble conditions and by such polyamic acid is physically similar to the corresponding polyimide gel obtained from conventional organic solvent processes (for example, in organic solvents such as DMAC). Specifically, the gel is transparent, has a yellowish to amber color, and has a plastic feel.

[0094] More surprisingly, it has been found that, according to the present disclosure, some polyamic acid salt solutions produced from the reaction of polyamic acid and guanidine carbonate in water, or some polyamic acid salt solutions produced from the reaction of some diamines, tetracarboxylic dianhydride and guanidine carbonate in water, show thixotropic behavior. Thixotropy is a time-dependent shear-thinning property. Specifically, some gels or fluids that are viscous under static conditions become less viscous (e.g., flowing) when experiencing some stresses (e.g., when shaking, stirring or applying shear stress). Then, when stress is removed, they take a fixed time to recover to a more viscous state. Some thixotropic fluids are almost immediately restored to a gel state, while the rest take a long time to recover to a solid or nearly solid state. Thixotropic behavior is preferred for processing certain materials at high flow rates (i.e., shear rates). Such flow behavior is suitable for three-dimensional (3D) printing, in which a viscous solution will flow through an injection needle with less force, and it establishes a high shear situation in the needle, but then the solution will regain its high viscosity almost immediately after it leaves the needle to form a solid structure.

[0095] Accordingly, the present invention provides a method for preparing a polyamic acid salt solution, a polyamic acid gel and a polyimide gel under aqueous conditions. Further provided is a method for converting polyamic acid into polyimide under aqueous conditions, and a method for converting polyamic acid and polyimide gel materials into corresponding carbon gel materials. A variety of methods are each further described below.

[0096] definition

[0097] With respect to terms used in this disclosure, the following definitions are provided. This application will use the following terms as defined below, unless the textual context clearly requires a different meaning.

[0098] The words "a" and "an / kind" are used herein to refer to one / kind or more than one / kind (i.e., at least one / kind) of the grammatical object of the word. The term "about" used throughout this specification is used to describe and illustrate small fluctuations. For example, the term "about" can refer to less than or equal to ±10%, or less than or equal to ±5%, such as less than or equal to ±2%, less than or equal to ±1%, less than or equal to ±0.5%, less than or equal to ±0.2%, less than or equal to ±0.1%, or less than or equal to ±0.05%. All numerical values ​​herein are modified by the term "about", whether or not explicitly stated. The value modified by the term "about" certainly includes the specific value. For example, "about 5.0" must include 5.0.

[0099] In the context of the present disclosure, the term "framework" or "framework structure" refers to a network of interconnected oligomers, polymers or colloidal particles that form the solid structure of a gel or aerogel. The polymers or particles that make up the framework structure typically have a diameter of about 100 angstroms. However, the framework structure of the present disclosure may also include a network of interconnected oligomers, polymers or colloidal particles of all diameter sizes that form the solid structure within a gel or aerogel.

[0100] As used herein, the term "aerogel" refers to a solid object, regardless of shape or size, comprising a framework of interconnected solid structures, having a corresponding network of interconnected pores integrated within the framework, and containing a gas such as air as a dispersed interstitial medium. Therefore, and regardless of the drying method used, aerogels are open non-fluid colloid or polymer network structures that are expanded throughout their volume by a gas and formed by removing all swelling agents (e.g., solvents) from the corresponding wet gel without volume reduction or compaction. Unless otherwise specified, the expression "aerogel" herein includes any open porous material, which can be classified as aerogels, xerogels, cryogels, bigels, microporous materials, etc., regardless of the material (e.g., polyimide, polyamic acid, or carbon).

[0101] Typically, aerogels have one or more of the following physical and structural properties: (a) an average pore diameter in the range of about 2 nm to about 100 nm; (b) a porosity of about 60% or more; and (c) a specific surface area of ​​about 1, about 10, or about 20 to about 100 or about 1000 m 2 / g. Typically, such properties are measured using nitrogen absorption porosity testing and / or helium pycnometer determination. It should be understood that the addition of additives such as reinforcing materials or electrochemically active materials (e.g., silicon or lithium iron phosphate) may reduce the porosity and specific surface area of ​​the resulting aerogel composite. Densification may also reduce the porosity of the resulting aerogel composite.

[0102] In some aspects, the gel material may be specifically referred to as a xerogel. As used herein, the term "xerogel" refers to an aerogel comprising an open, non-fluid colloid or polymer network, which is formed by removing all swelling agents from a corresponding wet gel without taking any precautions to avoid substantial volume reduction or compaction. Xerogels typically include a compacted structure. Xerogels undergo substantial volume reduction during ambient pressure drying and generally have a porosity of about 40% or less.

[0103] As used herein, the term "gelation" or "gel transition" refers to the formation of a wet gel from a polymer system (e.g., a polyimide or polyamic acid as described herein). At a point during the reaction of gelation as described herein, defined as the "gel point," the sol loses fluidity. In the context of the present disclosure, gelation begins from an initial sol state (e.g., a solution of a polyamic acid salt), through a high viscosity dispersed state, until the dispersed state solidifies and the sol gels (gel point), thereby obtaining a wet gel (e.g., a polyimide or polyamic acid gel). Note that such definitions of gelation and gel point are simplified and do not take into account the potential for fluidity under stress, such as the thixotropic behavior of certain gels as described herein.

[0104] The time it takes for a polymer solution (e.g., an aqueous solution of a polyamic acid salt) to transform into a gel in a form that no longer flows is called the "phenomenal gelation time". Formally, the gelation time is measured using rheology. At the gel point, the elastic properties of the solid gel begin to dominate the viscous properties of the fluid sol. The formal gelation time is close to the time at which the real and imaginary parts of the complex modulus of the gelled sol intersect. A rheometer is used to monitor the changes in the two moduli over time. The time is counted from the moment the last component of the sol is added to the solution. See, for example, HH Winter “Can the Gel Point of a Cross-linking Polymer Be Detected by the G'-G' Crossover?” Polym. Eng. Sci., 1987, 27, 1698–1702; S.-Y. Kim, D.-G. Choi and S.-M. Yang “Rheological analysis of the gelation behavior of tetraethylorthosilane / vinyltriethoxysilane hybrid solutions” Korean J. Chem. Eng., 2002, 19, 190–196; and M. Muthukumar “Screening effect on viscoelasticity near the gel point” Macromolecules, 1989, 22, 4656–4658 for a discussion of gelation.

[0105] As used herein, the term "wet gel" refers to a gel in which the mobile interstitial phase within the interconnected pore network is primarily composed of a liquid phase such as a conventional solvent or water, a liquefied gas such as liquid carbon dioxide, or a combination thereof. Aerogels typically require initial production of a wet gel, followed by processing and extraction to replace the mobile interstitial liquid in the wet gel with air or another gas. Examples of wet gels include, but are not limited to, alcohol gels, hydrogels, ketone gels, carbonogels, and any other wet gels known to those skilled in the art.

[0106] As used herein, reference to a "conventional" or "organic solvent-based" process for forming a polyimide gel material refers to a process in which a polyamic acid solution is prepared from the condensation of a diamine with a tetracarboxylic dianhydride in an organic solvent, wherein the polyamic acid is subsequently dehydrated to form a polyimide gel. See, for example, U.S. Patent Nos. 7,071,287 and 7,074,880 issued to Rhine et al. and U.S. Patent Application Publication No. 2020 / 0269207 issued to Zafiropoulos et al.

[0107] As used herein, the term "alkyl" refers to a straight or branched chain saturated hydrocarbon group having 1 to 20 carbon atoms (i.e., C1 to 20). Representative alkyl groups include, but are not limited to, methyl, ethyl, n-propyl, n-butyl, n-pentyl, and n-hexyl; while branched alkyl groups include, but are not limited to, isopropyl, secondary butyl, isobutyl, tertiary butyl, isopentyl, and neopentyl. Alkyl groups may be unsubstituted or substituted.

[0108] As used herein, the term "alkenyl" refers to a hydrocarbon group generally having 1 to 20 carbon atoms (i.e., C1 to C20) and having at least one unsaturated site (i.e., a carbon-carbon double bond). Examples include, but are not limited to, ethylene or vinyl, allyl, 1-butenyl, 2-butenyl, isobutenyl, 1-pentenyl, 2-pentenyl, 3-methyl-1-butenyl, 2-methyl-2-butenyl, 2,3-dimethyl-2-butenyl, and the like. The alkenyl group may be unsubstituted or substituted.

[0109] As used herein, unless otherwise indicated, the term "substantially" means a large degree (e.g., greater than about 95%, greater than about 99%, greater than about 99.9%, greater than 99.99%, or even 100%) of a reference characteristic, quantity, etc. that is relevant to the particular context (e.g., substantially pure, substantially identical, etc.).

[0110] Methods for forming polyimide, polyamic acid, polyamic acid metal salt, and carbon aerogel

[0111] The method disclosed herein generally utilizes polyamic acid and polyimide wet gel, which can be prepared without using organic solvents and without using organic bases (e.g., amines). The preparation of polyamic acid and polyimide wet gels herein with respect to "without using organic bases" means that carbon-based alkaline materials such as amines are not utilized to dissolve preformed polyamic acid in water, nor are they used to dissolve polyamic acid in situ during formation (i.e., by reaction between diamines and tetracarboxylic dianhydride). For the avoidance of doubt, the representation of "organic bases" does not include carbonates and bicarbonates, and further does not include carbonates and bicarbonates with nitrogen-containing cationic substances (such as ammonium or guanidine).

[0112] The expression about aqueous solution herein means that the solution is substantially free of any organic solvent. As used herein, in the context of organic solvent, the term "substantially free" means that organic solvent is not intentionally added and there is no organic solvent exceeding trace amount. For example, in some aspects, the aqueous solution may be characterized by having less than 1% organic solvent by volume, or less than 0.1%, or less than 0.01%, or even 0% organic solvent by volume. These water-based methods are advantageous in reducing material and waste disposal costs and reducing potential safety and environmental hazards.

[0113] Preparation of polyamic acid and polyimide gel materials under aqueous conditions

[0114] Provided herein is a method for preparing polyamic acid and polyimide gel materials under aqueous conditions. The method generally includes preparing an aqueous solution of polyamic acid salt without using an organic base, and then converting the polyamic acid salt into a polyamic acid gel or aerogel material, a polyimide gel or aerogel material, or a corresponding carbon aerogel material. These materials and corresponding methods are each further described below.

[0115] Polyamic acid and polyamic acid salt

[0116] Provided herein is a method for preparing an aqueous solution of polyamic acid salt.Polyamic acid is a polymer amide with a repeating unit comprising a carboxylic acid group, a carboxamide group and an aromatic or aliphatic part, and the aromatic or aliphatic part includes the diamine and tetracarboxylic acid derived from the polyamic acid.As defined herein, "repeat unit" is a part of polyamic acid (or corresponding polyimide), and its repetition will produce a complete polymer chain (except the terminal amino group or the unreacted anhydride end) by continuously connecting the repeating unit along the polymer chain.Those skilled in the art will recognize that the polyamic acid repeating unit is formed by the partial condensation of the amino group of the tetracarboxylic dianhydride carboxyl group and the diamine.

[0117] On the one hand, the method includes: providing polyamic acid; and merging the polyamic acid and water-soluble carbonate or bicarbonate in water to provide a solution of the polyamic acid salt. In such aspects, the polyamic acid is a preformed polyamic acid, or a commercially available material purchased or a material prepared by suitable diamines and tetracarboxylic dianhydride according to conventional known techniques (such as prepared in an organic solvent solution). Suitable preformed polyamic acid is as described below for polyamic acid synthesized in situ. Suitable water-soluble carbonate or bicarbonate is further described below.

[0118] Alternatively, polyamic acid can be prepared in situ. Accordingly, on the other hand, an aqueous solution of polyamic acid salt is prepared by the reaction of water-soluble diamines and tetracarboxylic dianhydride in the presence of water-soluble carbonates or bicarbonates. Generally speaking, diamines and tetracarboxylic dianhydride are reacted in the presence of the carbonate or bicarbonate to form polyamic acid salt. Accordingly, the method includes: merging water-soluble diamines, water-soluble carbonates or bicarbonates, and tetracarboxylic dianhydride in water; and reacting the components to provide a solution of the polyamic acid salt. Polyamic acid salts include anionic carboxylate groups, which are compensated by cationic charges from carbonates or bicarbonates, and the polyamic acid salts are soluble in water. The components used in the method (e.g., water-soluble diamines, tetracarboxylic dianhydride, water-soluble carbonates or bicarbonates, etc.) are each further described below.

[0119] The order of addition of the various components can vary. For example, in some aspects, the combining includes: dissolving a water-soluble diamine in water to form an aqueous diamine solution; adding the water-soluble carbonate or bicarbonate to the aqueous diamine solution; adding tetracarboxylic dianhydride to the aqueous diamine and water-soluble carbonate or bicarbonate solution to form a solution; and stirring the solution at a temperature in the range of about 15° C. to about 60° C. for a period of time in the range of about 1 hour to about 4 days.

[0120] In some aspects, the combining includes: dissolving a water-soluble diamine in water to form an aqueous diamine solution; adding a tetracarboxylic dianhydride to the aqueous diamine solution to form a suspension; stirring the suspension at a temperature in the range of about 15°C to about 60°C for a time period in the range of about 1 minute to about 24 hours; adding the water-soluble carbonate or bicarbonate to the suspension; and stirring the suspension at a temperature in the range of about 15°C to about 60°C for a time period in the range of about 1 hour to about 4 days to provide an aqueous solution of the polyamic acid salt.

[0121] In some aspects, combining comprises: adding a water-soluble diamine, a tetracarboxylic dianhydride, and the water-soluble carbonate or bicarbonate to water simultaneously or in rapid succession; and stirring the resulting mixture at a temperature in the range of about 15° C. to about 60° C. for a period of time in the range of about 1 hour to about 4 days to provide an aqueous solution of the polyamic acid salt.

[0122] A non-limiting general reaction sequence is provided in Scheme 1. In some cases, the reaction occurs generally according to Scheme 1, and the reagents and products have structures according to the formula of Scheme 1.

[0123] Scheme 1. Formation of polyamic acid salts via reaction of monomers in the presence of water-soluble carbonates or bicarbonates Aqueous solution

[0124]

[0125] The diamines disclosed herein are generally described as "water-soluble diamines". As used herein, the term "water-soluble diamine" means that the diamine has an appropriate solubility in water such that a synthetically useful concentration of the diamine can be obtained under the utilization conditions disclosed herein. For example, a diamine suitable for use in the disclosed method can have a solubility in water at 20°C of at least about 0.01 g per 100 mL, at least about 0.1 g per 100 mL, at least about 1 g per 100 mL, or at least about 10 g per 100 mL.

[0126] In some aspects, a combination of more than one diamine can be used. A combination of diamines can be used in order to optimize the properties of the gel material. In some aspects, a single diamine is used.

[0127] With reference to Scheme I, the structure of the diamine is variable. In some aspects, the diamine has a structure according to Formula I, wherein Z is aliphatic (i.e., alkylene, alkenylene, alkynylene or cycloalkylene) or aryl, each as described above. In some aspects, Z is an alkylene, such as C2 to C12 alkylene or C2 to C6 alkylene. In some aspects, the diamine is C2 to C6 alkane diamine, such as but not limited to 1,3-diaminopropane, 1,4-diaminobutane, 1,5-diaminopentane, 1,6-diaminohexane and ethylenediamine. In some aspects, the C2 to C6 alkylene of alkane diamine is substituted with one or more alkyl groups such as methyl.

[0128] In some aspects, Z is an aryl group. In some aspects, the aryl diamine is 1,3-phenylenediamine, methylenedianiline, 1,4-phenylenediamine (PDA), or a combination thereof. In some aspects, the diamine is 1,3-phenylenediamine. In some aspects, the diamine is 1,4-phenylenediamine (PDA).

[0129] Continuing with reference to Scheme 1, tetracarboxylic dianhydride is added. In some aspects, more than one tetracarboxylic dianhydride is added. A combination of tetracarboxylic dianhydrides can be used to optimize the properties of the gel material. In some aspects, a single tetracarboxylic dianhydride is added. The structure of the tetracarboxylic dianhydride is variable. In some aspects, the tetracarboxylic dianhydride has a structure according to Formula II, wherein L comprises an alkylene, a cycloalkylene, an arylene or a combination thereof, each as described above. In some aspects, L comprises an arylene. In some aspects, L comprises a phenyl, a biphenyl or a diphenyl ether group. In some aspects, the tetracarboxylic dianhydride of Formula II has one or more structures selected from as provided in Table 1.

[0130] Table 1. Non-limiting list of potential tetracarboxylic dianhydrides

[0131]

[0132]

[0133] In some aspects, the tetracarboxylic dianhydride is selected from the group consisting of pyromellitic dianhydride (PMDA), diphthalic dianhydride (BPDA), oxydiphthalic dianhydride (ODPA), benzophenonetetracarboxylic dianhydride (BTDA), ethylenediaminetetraacetic dianhydride (EDDA), 1,4,5,8-naphthalenetetracarboxylic dianhydride, and combinations thereof. In some aspects, the tetracarboxylic dianhydride is PMDA.

[0134] The method as disclosed herein utilizes water-soluble carbonate or bicarbonate. The water-soluble carbonate or bicarbonate can be variable. As used herein, "water-soluble" with respect to the salt means that the carbonate or bicarbonate has a considerable solubility in water, so that the synthetic usable concentration of the carbonate or bicarbonate can be obtained under the disclosed utilization conditions. For example, the solubility of a water-soluble carbonate or bicarbonate suitable for the disclosed method in water at 20°C can be at least about 0.1 g per 100 mL, at least about 1 g per 100 mL, or at least about 10 g per 100 mL.

[0135] As used herein, the term "carbonate or bicarbonate" refers to a basic material containing a carbonate or bicarbonate anion, and specifically excludes basic materials containing a carbon-hydrogen covalent bond (i.e., organic bases, including, but not limited to, alkylamines, arylamines, and heteroaromatic amines). Water-soluble carbonates or bicarbonates suitable for use in the disclosed methods can be further described as non-nucleophilic, meaning that the carbonate or bicarbonate will not participate in chemical reactions by donating an electron pair other than as a proton acceptor.

[0136] In certain aspects, the water-soluble carbonate or bicarbonate is a carbonate. In other certain aspects, the water-soluble carbonate or bicarbonate is a bicarbonate. Continuing with reference to Scheme 1, the water-soluble carbonate or bicarbonate has the general formula M2CO3 or MHCO3, wherein M is a cationic species having a +1 valence state.

[0137] In some aspects, the cationic species M comprises or is an ammonium ion, a guanidine ion, or an alkali metal ion. In some aspects, the cationic species M comprises lithium, sodium, potassium, ammonium, guanidine, or a combination thereof. In some aspects, the cationic species M is lithium. In some aspects, the cationic species M is sodium. In some aspects, the cationic species M is potassium. In some aspects, the cationic species M is ammonium (NH4 + In some aspects, the cationic species M is guanidine (NH2-C(=NH2 + )-NH2).

[0138] Particularly suitable water-soluble carbonates and bicarbonates include those of alkali metals. In some aspects, the water-soluble carbonate or bicarbonate is selected from the group consisting of lithium carbonate, lithium bicarbonate, sodium carbonate, sodium bicarbonate, potassium carbonate, potassium bicarbonate, and combinations thereof. In some aspects, the water-soluble carbonate or bicarbonate is selected from the group consisting of lithium carbonate, lithium bicarbonate, sodium carbonate, sodium bicarbonate, potassium carbonate, and potassium bicarbonate.

[0139] In some aspects, the water-soluble carbonate or bicarbonate is selected from the group consisting of ammonium carbonate, ammonium bicarbonate, guanidine carbonate, and combinations thereof.

[0140] In some aspects, the water-soluble carbonate or bicarbonate is guanidine carbonate. As described above and hereinafter described in relation to the embodiments, some polyamic acid salt solutions prepared using guanidine carbonate are thixotropic. This thixotropy may be desirable in, for example, 3D printing applications. For example, a 3D printed structure prepared by needle deposition (moving the needle in a predetermined manner to form a desired pattern as the polymer solution leaves the needle) of a thixotropic solution (for example, polyamic acid guanidine aqueous solution) as used herein. The resulting structure can be processed as previously described in the literature to form a polymer or aerogel retaining the applied structure.

[0141] The amount of water-soluble carbonate or bicarbonate added can vary and can depend, for example, on the stoichiometry of the particular salt utilized. For example, one skilled in the art will recognize that depending on the charge associated with the particular anionic species (carbonate or bicarbonate) present in the salt. For example, sodium bicarbonate (NaHCO3) will supply one equivalent of base (bicarbonate ion, HCO3 -), each capable of reacting with one proton, and each molar equivalent of sodium bicarbonate will further provide one equivalent of sodium ions. In contrast, sodium carbonate (Na2CO3) will provide two equivalents of base (carbonate ions, CO3) that can react with two equivalents of protons from each repeating unit of polyamic acid. 2- ), and each molar equivalent of sodium carbonate provides two equivalents of sodium ions.

[0142] The amount of water-soluble carbonate or bicarbonate can be expressed as a mol ratio with another reaction component (for example, diamine). The mol ratio of water-soluble carbonate or bicarbonate to diamine may need to be optimized for each group of reactants and conditions. In some aspects, the mol ratio is selected to maintain the solubility of polyamic acid. In some aspects, the mol ratio is selected to avoid any precipitation of polyamic acid. In some aspects, the mol ratio of water-soluble carbonate or bicarbonate to diamine is in the range of about 1 to about 4 or about 2 to about 3. In some aspects, the mol ratio is from about 1.0, about 1.1, about 1.2, about 1.3, about 1.4 or about 1.5 to about 1.6, about 1.7, about 1.8, about 1.9 or about 2.0. In some aspects, the molar ratio of the water-soluble carbonate or bicarbonate to the diamine is from about 2.0 to about 2.6, such as about 2.0, about 2.1, about 2.2, about 2.3, about 2.4, about 2.5, or about 2.6. Without being bound by any particular theory, it is believed that in some exemplary aspects, at least enough base is needed to neutralize (i.e., form a salt with) substantially all of the free carboxylic acid groups of the polyamic acid. In some aspects, the amount of water-soluble carbonate or bicarbonate used is an amount to neutralize substantially all of the carboxylic acid groups present in the polyamic acid formed during the reaction.

[0143] In some aspects, the water-soluble salt is a carbonate salt, such as lithium carbonate, sodium carbonate, potassium carbonate, ammonium carbonate, or guanidine carbonate, and the molar ratio of carbonate ion to diamine is from about 1.0 to about 1.3.

[0144] In some aspects, the water-soluble carbonate or bicarbonate is a bicarbonate salt, such as lithium bicarbonate, sodium bicarbonate, potassium bicarbonate, or ammonium bicarbonate, and the molar ratio of bicarbonate ion to diamine is from about 2.0 to about 2.6.

[0145] In some respects, the amount of the water-soluble carbonate or bicarbonate present can be expressed relative to the carboxylic acid group of the polyamic acid formed during the reaction or otherwise present in the reaction mixture. In some respects, the water-soluble carbonate or bicarbonate is a bicarbonate, such as lithium bicarbonate, sodium bicarbonate, potassium bicarbonate or ammonium bicarbonate, and the mol ratio of bicarbonate ion to the carboxylic acid group of polyamic acid is about 2.0. In some respects, the water-soluble carbonate or bicarbonate is a carbonate, such as lithium carbonate, sodium carbonate, potassium carbonate or ammonium carbonate, and the mol ratio of carbonate ion to the carboxylic acid group of polyamic acid is about 1.0.

[0146] The relative quantity of the diamines and dianhydrides present can be expressed by mol ratio. The mol ratio of diamines and dianhydrides can be changed according to the desired reaction time, reagent structure and desired material properties. In some aspects, the mol ratio is about 0.1 to about 10, such as from about 0.1, about 0.5 or about 1 to about 2, about 3, about 5 or about 10. In some aspects, the ratio is about 0.5 to about 2. In some aspects, the ratio is about 1 (that is, stoichiometric), such as about 0.9 to about 1.1. In specific aspects, the ratio is about 0.99 to about 1.01.

[0147] The molecular weight of polyamic acid can be changed based on reaction conditions (e.g., concentration, temperature, reaction duration, properties of diamines and dianhydrides, etc.). The molecular weight is based on the number of polyamic acid repeating units, as represented by the value of the integer "n" of the structure of formula III in scheme 1. The specific molecular weight range of the polymer material produced by the disclosed method is variable. In general, the reaction conditions of interest can be changed to provide a gel with a desired physical property without specifically considering the molecular weight. In some aspects, an alternative index of molecular weight is provided with the viscosity of a polyamic acid salt solution, which is determined by variables such as temperature, concentration, the molar ratio of reactants, reaction time, etc.

[0148] The temperature for carrying out the reaction can be variable. Suitable ranges are generally between about 4 ° C and about 100 ° C. In some aspects, the reaction temperature is about 15 ° C to about 60 ° C, such as about 20 ° C, about 25 ° C, about 30 ° C, about 35 ° C, about 40 ° C, about 45 ° C, about 50 ° C, about 55 ° C or about 60 ° C. In some aspects, the temperature is about 15 ° C to about 25 ° C. In some aspects, the temperature is about 50 ° C to about 60 ° C.

[0149] The reaction is carried out for a period of time, and generally it is carried out until all available reactants (for example, diamines and dianhydrides) have reacted with each other. The time required for complete reaction can be changed based on reagent structure, concentration, temperature. In some aspects, the reaction time is about 1 minute to about 1 week, for example, about 15 minutes to about 5 days, about 30 minutes to about 3 days or about 1 hour to about 1 day. In some aspects, the reaction time is about 1 hour to about 12 hours.

[0150] The concentration of the polyamic acid salt in the aqueous solution can vary. For example, in some aspects, the concentration of the polyamic acid salt in the aqueous solution ranges from about 0.01 to about 0.3 g / cm based on the weight of the polyamic acid salt. 3 .

[0151] In some aspects, polyamic acid, polyimide or carbon gel and aerogel materials as disclosed herein may be doped with one or more additional materials, such as electroactive materials, conventional polymer fillers, carbon materials, etc. Such dopants or their precursors may be introduced at various stages and in various ways. In some aspects, the dopant is introduced during the formation of the polyamic acid salt solution or introduced immediately after formation. Accordingly, in some aspects, the method further includes adding the dopant to the aqueous solution of the polyamic acid salt or the solution of the water-soluble diamine.

[0152] In some aspects, the dopant is an electroactive material or a precursor thereof. Suitable electroactive materials include, but are not limited to, graphite, silicon such as silicon particles, tin, or substances such as Prussian blue, lithium iron phosphate, lithium iron manganese phosphate, combinations thereof, other anode and / or cathode active materials, or one or more precursors thereof. In some aspects, the electroactive material or its precursor is in particle form. In some aspects, the dopant is a particle material in the nanometer or micrometer range (i.e., having two or three dimensions of 1 nm to about 10 micrometers or larger).

[0153] In some aspects, the dopant in the form of particles includes silicon, such as silicon, silicon wire, crystalline silicon, amorphous silicon, silicon alloys, silicon oxide (SiOx), silicon carbide, silicon nitride, coated silicon (e.g., carbon-coated silicon), and any combination of the silicon particle materials disclosed herein.

[0154] In some aspects, the dopant in particulate form includes carbon, graphite, tin, sulfur, nickel, manganese, cobalt, iron, vanadium, manganese, or a combination thereof. For example, in some aspects, the dopant in particulate form is lithium iron phosphate or a manganese or vanadium variant thereof.

[0155] Dopant particles (e.g., lithium iron phosphate) can be incorporated into polyamic acid, polyimide or carbon gel as disclosed herein in many ways. In general, electrically active dopant particles (e.g., lithium iron phosphate) are incorporated during the sol-gel process. In a non-limiting aspect, electrically active dopant particles (e.g., lithium iron phosphate) are dispersed in polyamic acid gel before imidization. In some aspects, electrically active dopant particles (e.g., lithium iron phosphate) are dispersed in a solvent (e.g., water or a polar aprotic solvent) and then merged with a polyimide precursor. In some aspects, electrically active dopant particles (e.g., lithium iron phosphate) are dispersed in polyamic acid sol during the imidization process. In some aspects, electrically active dopant particles (e.g., lithium iron phosphate) are added to an aqueous solution of polyamic acid salt. In other aspects, precursors to electroactive materials (e.g., sulfur or sulfur itself, or materials including nickel, manganese, cobalt, iron, vanadium, manganese, phosphates, Prussian blue, etc.) can be introduced at various stages, including but not limited to, during the preparation of the polyamic acid salt.

[0156] In some aspects, residual lithium, sodium, potassium, ammonium or guanidinium ions from, for example, water-soluble carbonate or bicarbonate salts remain in the polyamic acid, polyimide or carbon gel material.

[0157] Polyamic acid and polyimide gel

[0158] In some aspects, the method further includes converting the aqueous solution of polyamic acid salt into the corresponding polyamic acid gel. Generally speaking, the method for converting the polyamic acid salt solution into the corresponding polyamic acid gel includes acidifying the polyamic acid salt solution to convert the polyamic acid salt into polyamic acid, causing the polyamic acid to separate into a gel. The acid may also be referred to as a gelling initiator. Acidification to form polyamic acid generally follows Scheme 2.

[0159] The method of acidification can be varied. For example, in some aspects, a polyamic acid salt solution is added to an acid solution, wherein the acidification of the polyamic acid salt solution is rapid. Alternatively, the polyamic acid salt solution can be acidified by adding an acid to the polyamic acid salt solution. In some aspects, conditions or techniques known to those skilled in the art can be used to gradually or slowly acidify the polyamic acid salt solution. For example, in a non-limiting aspect, an acid precursor is utilized. An acid precursor is a material that can be gradually converted into an acid, such as by hydrolysis. A suitable acid precursor of this type is acetic anhydride, which generates acetic acid in the presence of water.

[0160] Scheme 2. Reaction of polyamic acid salt with acid to form polyamic acid gel

[0161]

[0162] In some aspects, the polyamic acid wet gel prepared as disclosed herein or the corresponding aerogel as described below includes residual carbonate or bicarbonate. Generally speaking, the residual amount is a trace amount, but carbonate or bicarbonate, and / or associated counter cations (e.g., alkali metal ions, guanidine ions, etc.) can be detected by analytical methods known to those skilled in the art.

[0163] The resulting polyamic acid gel material can then be dried to form a polyamic acid aerogel. The acidification and formation methods of polyamic acid gel materials are described in, for example, International Patent Application Publication No. WO2022125835, which is incorporated herein in its entirety. The method of drying to form the corresponding aerogel is further described below.

[0164] In some aspects, the method further includes forming a polyimide aerogel from an aqueous solution of a polyamic acid salt. In general, the method includes imidizing a polyamic acid salt to form a polyimide gel; and drying the polyimide gel to form a polyimide aerogel. The method of imidizing an aqueous solution of a polyamic acid salt is described in, for example, International Patent Application PCT / US2021 / 062706, which is incorporated herein in its entirety, and suitable methods are also further described below. The method of drying to form a corresponding polyimide aerogel is further described below.

[0165] In some aspects, the imidization of polyamic acid salt includes the thermal imidization of the corresponding polyamic acid. It is a particularly suitable thermal treatment to irradiate the wet gel polyamic acid material with microwave frequency energy. Compared with the conventional heating that relies on slow heat conduction, microwave heating allows fast and effective energy transfer. Accordingly, microwave heating is particularly suitable for performing current imidization reactions. Generally speaking, microwave frequency radiation is carried out at a certain power for a certain length of time, and this power and time are enough to convert most of the amide and carboxyl groups of polyamic acid into imide groups. As used herein, in the context of converting amide and carboxyl groups into imide groups, "most of" means greater than 80%, such as 85%, 90%, 95%, 99%, or 99.9%, or 99.99%, or even 100% of the amide and carboxyl groups are converted into imide groups.

[0166] In other aspects, the polyamic acid salt imidization includes chemical imidization, wherein the chemical imidization includes adding a gelling initiator to an aqueous solution of a polyamic acid salt to form a gelling mixture ("sol"), and gelling the gelling mixture (e.g., in a mold, or cast on a sheet, or in other various forms such as beads). In such aspects, a gelling initiator is added to initiate and drive imidization, thereby forming a polyimide wet gel from the polyamic acid salt. A non-limiting general reaction sequence is provided in Scheme 3. In some aspects, the polyimide has a structure according to Formula V as shown in Scheme 3, wherein L, Z, and n are each as described above for forming a polyamic acid salt of Formula III.

[0167] Scheme 3. Conversion of polyamic acid salt to polyimide

[0168]

[0169] The structure of the gelling initiator can vary but is generally a reagent that is at least partially soluble in the reaction solution, reacts with the carboxylate groups of the polyamic acid salt and is effective in driving the imidization of the polyamic acid carboxyl and amide groups while having minimal reactivity with aqueous solutions. An example of a class of suitable gelling initiators is a carboxylic acid anhydride, such as acetic anhydride, propionic anhydride, and the like. In some aspects, the gelling initiator is acetic anhydride.

[0170] In some aspects, the amount of gelling initiator can be based on the amount of tetracarboxylic dianhydride or polyamic acid. For example, in some aspects, gelling initiator exists in various molar ratios with tetracarboxylic dianhydride. In some aspects, gelling initiator exists in various molar ratios with polyamic acid. The molar ratio of gelling initiator to tetracarboxylic dianhydride or polyamic acid can be changed according to the desired reaction time, reagent structure and desired material properties. In some aspects, the molar ratio is from about 2 to about 10, such as from about 2, about 3, about 4 or about 5 to about 6, about 7, about 8, about 9 or about 10. In some aspects, the ratio is from about 2 to about 5.

[0171] The temperature at which the gelling reaction is allowed to proceed can vary, but is typically below about 50°C, such as about 10°C to about 50°C, or about 15°C to about 25°C.

[0172] Regarding the mode of implementing gelation, the above-mentioned gelation conditions (both acidification and imidization) are general and are intended to be non-limiting. For example, those skilled in the art will recognize various arrangements for preparing monolithic materials or beads (including microbeads). For example, it is contemplated herein that a method of forming a monolithic material by casting a gel mixture in a mold, a method of forming beads of various sizes by dripping or spraying a polyamic acid solution into an acidic receiving solution, or a method of forming micron-sized beads of polyamic acid or polyimide gel in an emulsion. It is further contemplated herein that a method of forming a polyamic acid metal salt gel by contacting a polyamic acid salt solution with certain metal ions in a solution (see, for example, Scheme 4). With reference to Scheme 4, certain metal salts (e.g., alkaline earth metal salts, d-block element salts, p-block element salts, lanthanide metal salts, actinide metal salts) form metal polyamic acid salt gels with desired properties. These additional gelation methods (i.e., metal polyamic acid salts, beads, monolithic materials) are described, for example, in International Patent Application Publication No. WO2022 / 125835 to Leventis et al., which is incorporated herein by reference for disclosures regarding the formation of polyamic acid, polyimide, and metal polyamic acid salt gels from aqueous solutions.

[0173] Scheme 4. Formation of Metal Polyamic Acid Gel

[0174]

[0175] Those skilled in the art will recognize that the polyimide wet gel prepared according to the methods described herein will have unreacted terminal amino groups at one or both ends of a single polymer chain. The percentage concentration of such amino groups in the polyimide wet gel will be inversely proportional to the average number of repeating units (i.e., molecular weight) present in the polyimide wet gel. In some aspects, the terminal amino group can undergo a reaction with a gelling initiator (e.g., acetic anhydride) to form, for example, terminal amides such as acetamide. The relative concentration of such terminal amines or amides can be measured according to methods known in the art, including but not limited to, nuclear magnetic resonance spectroscopy, such as solid-state 15N-NMR.

[0176] In some aspects, the water content of a polyimide wet gel prepared as disclosed herein, prior to any solvent exchange or drying, is substantially all of the water initially used as the reaction solvent, not accounting for any water that evaporates, or is created or destroyed in the various reactions that occur during the polyimide synthesis as described above.

[0177] In some aspects, the polyimide wet gel prepared as disclosed herein or the corresponding aerogel as described below includes residual carbonate or bicarbonate. Generally speaking, the residual amount is a trace amount, but carbonate or bicarbonate, and / or associated counter cations (e.g., alkali metal ions, guanidine ions, etc.) can be detected by analytical methods known to those skilled in the art.

[0178] Polyamic acid, polyimide and metal polyamic acid salt aerogel

[0179] As shown above, in some aspects, the method further includes converting polyamic acid salt into aerogel material via corresponding polyamic acid, polyimide or metal polyamic acid salt wet gel. Generally speaking, the formation of aerogel includes drying the wet gel in one or more stages. In some aspects, the wet gel (polyamic acid, polyimide or metal polyamic acid salt) is aged. After any aging, (for example, demoulding) obtained wet gel material can be collected, and first washed with water or solvent exchange is performed to remove any unreacted organic salt or acid, then washed in a suitable second solvent or solvent exchange is performed to replace the main reaction solvent (that is, water) present in the wet gel. Such second solvent should be intermixed with supercritical fluid carbon dioxide (CO2), and include linear alcohols with 1 or more aliphatic carbon atoms, glycols with 2 or more carbon atoms or branched alcohols, cyclic alcohols, alicyclic alcohols, aromatic alcohols, polyols, ethers, ketones, cyclic ethers or their derivatives. In some aspects, the second solvent is water, C1 to C4 alcohol (e.g., methanol, ethanol, propanol, isopropanol, n-butanol, isobutanol or sec-butanol), acetone, tetrahydrofuran, ethyl acetate, acetonitrile, supercritical fluid carbon dioxide (CO2), or a combination thereof. In some aspects, the second solvent is ethanol.

[0180] Once the wet gel has been formed and processed, the liquid phase of the wet gel is then extracted at least partially from the wet gel material using an extraction method (including processing and extraction techniques) to form an aerogel material (i.e., "drying"). Liquid phase extraction plays an important role in engineering the characteristics of aerogels such as porosity and density and related properties such as thermal conductivity, among other factors. Typically, an aerogel is obtained when the liquid phase is extracted from the wet gel in a manner that causes low shrinkage to the porous network structure and solid framework of the wet gel. The wet gel can be dried using a variety of techniques to provide an aerogel or a xerogel. In exemplary aspects, the wet gel material can be dried at normal pressure, under vacuum (e.g., by freeze drying), under subcritical conditions, or under supercritical conditions to form a corresponding dried gel (e.g., an aerogel, such as a xerogel).

[0181] In some aspects, it may be desirable to reduce the surface area of ​​the dried gel. If it is desirable to reduce the surface area, the aerogel may be fully or partially converted into a xerogel with various porosities. The high surface area of ​​the aerogel may be reduced by forcing some of the pores to collapse. This may be accomplished by soaking the aerogel in a solvent such as ethanol or acetone for a period of time or by exposing them to solvent vapors. The solvent is subsequently removed by drying at normal pressure.

[0182] Aerogels are generally formed by removing a liquid mobile phase from a wet gel material at a temperature and pressure close to or above the critical point of the liquid mobile phase. Once the critical point is reached (near critical) or exceeded (supercritical; that is, the pressure and temperature of the system are at or above the critical pressure and critical temperature, respectively), a new supercritical phase, different from the liquid or vapor phase, appears in the fluid. The solvent can then be removed without introducing a liquid-vapor interface, capillary forces, or any related mass transfer limitations typically associated with a receding liquid-vapor boundary. In addition, the supercritical phase is generally more miscible with organic solvents, thereby enabling better extraction. Co-solvents and solvent exchange are also commonly used to optimize supercritical fluid drying processes.

[0183] If evaporation or extraction occurs below the critical point, the capillary forces generated by the evaporation of the liquid may cause shrinkage and pore collapse within the gel material. Maintaining the mobile phase at near or above the critical pressure during the solvent extraction process reduces the negative effects of such capillary forces. In certain aspects of the present disclosure, the use of near-critical conditions just below the critical point of the solvent system can allow the production of aerogels or compositions with sufficiently low shrinkage, thereby producing a commercially viable end product.

[0184] The wet gel can be dried using a variety of techniques to provide an aerogel. In exemplary aspects, the wet gel material can be dried at atmospheric pressure, under subcritical conditions, or under supercritical conditions.

[0185] Both room temperature and high temperature processes can be used to dry the gel material at atmospheric pressure. In some aspects, a slow atmospheric drying process can be used, wherein the wet gel is exposed to air in an open container for a period of time sufficient to remove the solvent, e.g., a period of time ranging from hours to weeks, depending on the solvent, the amount of wet gel, the exposed surface area, the size of the wet gel, etc.

[0186] In another aspect, the wet gel material is dried by heating. For example, the wet gel material can be heated in a convection oven for a period of time to evaporate most of the solvent (e.g., ethanol). After partial drying, the gel can be placed at room temperature to completely dry for a period of time, for example, several hours to several days. This drying method produces a xerogel. Note that according to the present disclosure, it was found that drying a wet gel in the form of a monolithic material resulted in cracking, but a wet gel in the form of beads maintained its spherical shape, even from a lower target density Td (e.g., Td = 0.05 g cm 3 ) solution.

[0187] In some aspects, the wet gel material is dried by freeze drying. "Freeze drying" or "lyophilization" means a low temperature process for removing solvents, which involves freezing a material (e.g., a wet gel material), reducing the pressure, and then removing the frozen solvent by sublimation. Since water is an ideal solvent to be removed by freeze drying, and water is a solvent in the methods disclosed herein, freeze drying is particularly suitable for forming aerogels from the disclosed polyimide wet gel materials. This drying method produces crystal gels, which may be very similar to aerogels.

[0188] Both supercritical and subcritical drying can be used to dry the wet gel material. In some aspects, the wet gel material is dried under subcritical or supercritical conditions. In exemplary aspects of supercritical drying, the gel material can be placed in a high pressure container to perform solvent extraction with supercritical CO2. After removing the solvent, such as ethanol, the container can be kept above the critical point of CO2 for a period of time, for example, about 30 minutes. After supercritical drying, the container is depressurized to atmospheric pressure. In general, aerogels are obtained by this process.

[0189] In an exemplary aspect of subcritical drying, liquid CO2 is used to dry the gel material at room temperature at a pressure in the range of about 800 psi to about 1200 psi. This operation is faster than supercritical drying; for example, the solvent (e.g., ethanol) can be extracted in about 15 minutes. In general, aerogels are obtained by this process.

[0190] Several additional aerogel extraction techniques are known in the art, including a range of different methods for drying aerogels using supercritical fluids and ambient drying techniques. For example, U.S. Pat. No. 6,670,402 teaches the extraction of a liquid phase from a gel by rapid solvent exchange by injecting supercritical (rather than liquid) carbon dioxide into an extractor that has been preheated and pre-pressurized to substantially critical conditions or above.

[0191] In some aspects, extraction of the liquid phase from the wet gel uses supercritical CO2.

[0192] Formation of carbon aerogel from polyamic acid or polyimide aerogel

[0193] In some aspects, the method further includes converting polyamic acid or polyimide aerogel into isostructural carbon aerogel, and the conversion includes pyrolyzing corresponding aerogel under suitable conditions. Accordingly, in some aspects, the method further includes pyrolyzing (for example, carbonizing) polyamic acid or polyimide aerogel as disclosed herein, meaning that aerogel is heated at a certain temperature for a certain time, and the temperature and time are enough to convert substantially all organic materials into carbon. As used in the context of pyrolysis, "substantially all" means that more than 80% of organic materials are converted into carbon by weight, such as 80%, 85%, 90% or more by weight, such as up to 99%, 99.9%, 99.99% or even 100% of organic materials are converted into carbon. Pyrolysis aerogel converts the aerogel into isostructural carbon aerogel, meaning that physical properties (for example, porosity, surface area, pore size, diameter, etc.) are substantially maintained in corresponding carbon aerogel. The time and temperature required for pyrolysis are variable. In some aspects, the polyimide aerogel is subjected to a treatment temperature of about 650°C or more, 800°C or more, 1000°C or more, 1200°C or more, 1400°C or more, 1600°C or more, 1800°C or more, 2000°C or more, 2200°C or more, 2400°C or more, 2600°C or more, 2800°C or more, or in a range between any two of these values, to carbonize the aerogel. Typically, pyrolysis is performed under an inert atmosphere to prevent combustion of organic or carbon materials. Suitable atmospheres include, but are not limited to, nitrogen, argon, or a combination thereof. In some aspects, pyrolysis is performed under nitrogen.

[0194] In some aspects, the aerogel is a metal polyamic acid salt aerogel as described above. After pyrolysis of such metal polyamic acid salt aerogel, the resulting carbon aerogel may contain (i.e., be doped with) the corresponding metal, metal oxide, metal carbide, or a combination thereof. The substances present depend on the pyrolysis conditions, such as temperature and reducing atmosphere, and the specific metal ions.

[0195] Aerogel properties

[0196] Aerogels as disclosed herein have a density. As used herein, the term "density" refers to a measurement of the mass of an aerogel material or composition per unit volume. The term "density" generally refers to the true or skeletal density of an aerogel material, as well as the bulk density of an aerogel article. Density is typically reported as kg / m 3 or g / cm 3 . The skeleton density of the aerogel (polyamic acid, polyimide, polyamic acid metal salt or carbon) can be determined by methods known in the art, including but not limited to helium pycnometer determination. The bulk density of the aerogel (polyamic acid, polyimide or carbon) can be determined by methods known in the art, including but not limited to: Standard Test Method for Size and Density of Prefabricated Block and Board Insulation Materials (ASTM C303, ASTM International, West Conshohocken, Pa.); Standard Test Method for Thickness and Density of Felt or Cotton Wool Insulation Materials (ASTM C167, ASTM International, West Conshohocken, Pa.); or Determination of Apparent Density of Preformed Tube Insulation Materials (ISO 18098, International Organization for Standardization, Switzerland). In the context of the present disclosure, unless otherwise specified, density measurements are obtained according to the ASTM C167 standard. In some aspects, the aerogels (polyamic acid, polyimide, polyamic acid metal salt, or carbon) disclosed herein have a carbon content of about 0.01 to about 1, such as about 0.1 to about 0.3 g / cm 3 The bulk density.

[0197] Aerogels as disclosed herein have a pore size distribution. As used herein, the term "pore size distribution" refers to the statistical distribution or relative amount of each pore size within the sample volume of a porous material. A narrower pore size distribution refers to a relatively large portion of pores within a narrow pore size range. In some aspects, for example, a narrow pore size distribution may be desirable in terms of optimizing the amount of pores that may surround the electrochemically active material and maximizing the available pore volume. In contrast, a wider pore size distribution refers to a relatively small portion of pores within a narrow pore size range. Therefore, the pore size distribution is typically measured as a function of pore volume and is recorded in a pore size distribution diagram as a unit size of the full width at the half maximum of the main peak. The pore size of the porous material can be measured by methods known in the art. Suitable methods for determining pore size distribution include, but are not limited to, measurements of gas adsorption / desorption (e.g., nitrogen), mercury porosimeter, etc. Unless otherwise specified, the pore size distribution measurements recorded herein are obtained by nitrogen adsorption analysis. In certain aspects, the aerogels of the present disclosure (eg, polyamic acid, polyimide, polyamic acid metal salt, or carbon) have a relatively narrow pore size distribution.

[0198] The aerogel materials disclosed herein have a pore volume. As used herein, the term "pore volume" refers to the total volume of pores within a porous material sample. Pore volume is specifically measured as the volume of void space within a porous material and is typically reported as cubic centimeters per gram (cm 3 / g or cc / g). The pore volume of the porous material can be determined by methods known in the art, such as, but not limited to, nitrogen porosimetry, mercury porosimetry, or a combination of helium pycnometer determination and bulk density determination. In certain aspects, the aerogel (polyamic acid, polyimide or carbon) of the present disclosure has a pore volume of about 1 cc / g or more, 1.5 cc / g or more, 2 cc / g or more, 2.5 cc / g or more, 3 cc / g or more, 3.5 cc / g or more, 4 cc / g or more, or in a range between any two of these values. In other aspects, the aerogels and xerogels (polyamic acid, polyimide, or carbon) of the present disclosure have a pore volume of about 0.03 cc / g or more, 0.1 cc / g or more, 0.3 cc / g or more, 0.6 cc / g or more, 0.9 cc / g or more, 1.2 cc / g or more, 1.5 cc / g or more, 1.8 cc / g or more, 2.1 cc / g or more, 2.4 cc / g or more, 2.7 cc / g or more, 3.0 cc / g or more, 3.3 cc / g or more, 3.6 cc / g or more, or in a range between any two of these values.

[0199] In some aspects of the present disclosure, the aerogel material (polyamic acid, polyimide, or carbon, aerogel or xerogel) may include a fibrous morphology. In the context of the present disclosure, the term "fibrous morphology" refers to the structural morphology of a nanoporous material (e.g., carbon aerogel), including pillars, rods, fibers or filaments.

[0200] In some aspects, the carbon aerogels produced by any of the disclosed methods have substantially similar properties to those prepared by pyrolyzing corresponding polyimide aerogels that have been prepared by conventional non-aqueous methods. See, e.g., U.S. Patent Nos. 7,071,287 and 7,074,880 issued to Rhine et al.

[0201] In some aspects, the carbon aerogel materials of the present disclosure (e.g., polyamic acid derived, polyamic acid metal salt derived, or polyimide derived carbon aerogels) can have a residual "heteroatom" (i.e., non-carbon atom) nitrogen content of at least about 1 wt%. For example, the carbon aerogel material can have a residual nitrogen content of at least about 1 wt% and up to about 10 wt%. In some aspects, the residual nitrogen content is about 1, about 2, about 3, about 4, about 5, about 6, about 7, about 8, about 9, or about 10 wt%.

[0202] Unless otherwise indicated herein or clearly conflicting with the context, all methods described herein can be performed in any suitable order. Unless otherwise claimed, the use of any or all embodiments or exemplary language (e.g., "such as") provided herein is intended only to better illustrate the materials and methods without attempting to limit the scope. Any text in the specification should not be interpreted as indicating any unclaimed element as an element necessary for practicing the disclosed materials and methods.

[0203] It will be apparent to those of ordinary skill in the relevant art that suitable modifications and adaptations may be made to the compositions, methods, and applications described herein without departing from the scope of any aspect thereof. The compositions and methods provided are exemplary and are not intended to limit the scope of the claimed aspects. All of the various aspects and options disclosed herein may be combined in all variations. The scope of the compositions, formulations, methods, and processes described herein includes all actual and possible combinations of the aspects, options, examples, and preferences herein.

[0204] Although the technology herein has been described with reference to specific aspects, it should be understood that these aspects are merely illustrative of the principles and applications of the technology disclosed herein. It will be apparent to those skilled in the art that various modifications and changes may be made to the methods and apparatus of the technology disclosed herein without departing from the spirit and scope of the technology. Therefore, it is intended that the technology disclosed herein include modifications and changes within the scope of the appended claims and their equivalents.

[0205] Throughout this specification, reference to "an aspect," "certain aspects," "one or more aspects," or "aspects" means that a particular feature, structure, material, or characteristic described in connection with that aspect is included in at least one aspect of the technology. Thus, phrases such as "in one or more aspects," "in certain aspects," "in an aspect," or "in an aspect" appearing in various places throughout this specification do not necessarily refer to the same aspect of the technology. Furthermore, particular features, structures, materials, or characteristics may be combined in any suitable manner in one or more aspects. Any ranges cited herein are inclusive.

[0206] Aspects of the technology disclosed herein are more fully illustrated with reference to the following examples. Before describing several exemplary aspects of the technology, it should be understood that the technology is not limited to the details of the construction or process steps described in detail in the following specific embodiments. The technology can be used in other aspects and can be practiced or implemented in a variety of ways. The following examples are described in detail to illustrate certain aspects of the disclosed technology, but are not to be considered as limiting it.

[0207] Example

[0208] The invention is further illustrated by the following non-limiting examples which describe the methods.

[0209] Example 1. Preparation of polyimide aerogel in water using Li2CO3 as base (target density 0.05 g / cc) And pyrolyzed into the corresponding carbon aerogel

[0210] Paraphenylenediamine (3.315 g, 0.03065 mol) was dissolved in 200 mL of deionized water. Lithium carbonate (2.718 g, 1.2 mol excess) was added and dissolved in the same aqueous solution. Pyromellitic dianhydride (6.685 g) was suspended in the same solution. After a few minutes, no solids remained in the suspension. Gas evolution (CO2) was observed in the initial stages of the reaction. The viscous yellow solution was stirred for up to 4 days. Small aliquots were taken every 24 hours and the viscosity was measured using a rheometer. The values ​​were: Day 1, 76.6 cP; Day 2, 74.2 cP; Day 3, 71.0 cP; and Day 4, 70.8 cP.

[0211] On the second day, a 50 g aliquot of the viscous solution was taken out and acetic anhydride (1.471 g, 2.0 molar excess relative to the monomer repeating units contained in the aliquot) was added. The resulting solution after the addition of acetic anhydride was stirred for about 30 seconds and then divided into multiple cylindrical molds. The solution gelled in less than 5 minutes. The resulting gel was transparent, light brown, rubbery, and was very similar to the gel obtained by conventional means (i.e., prepared in an organic solvent). The gel was aged in its mold at room temperature for 24 hours, then washed with ethanol (4 times) and dried with supercritical fluid CO2 to provide the corresponding monolithic polyimide aerogel. These aerogels are called Td005-Li2-d2-AA2. The monolithic material was pyrolyzed at 1050°C under flowing nitrogen to the corresponding carbon aerogel, designated as C-Td005-Li2-d2-AA2. The material characterization data for both Td005-Li2-d2-AA2 and C-Td005-Li2-d2-AA2 are provided in Tables 2 and 3.

[0212] Still on the second day, another 50 g aliquot of the viscous solution was taken out and acetic anhydride (1.471 g, 2.0 molar excess relative to the monomer repeating units contained in the aliquot) was added. The resulting solution after the addition of acetic anhydride was stirred for about 30 seconds and then divided into multiple cylindrical molds. The solution gelled in less than 5 minutes. The resulting gel was a transparent light brown rubbery state, very similar to the gel obtained by conventional means (i.e., prepared in an organic solvent). The gel was aged at 68° C. in its mold for 24 hours, then cooled to room temperature, removed from the mold, washed with ethanol (4 times) and dried with supercritical fluid CO2 to provide the corresponding monolithic polyimide aerogels. These aerogels are called Td005-Li2-d2-AA2-68. Figure 1A Provided are solid-state polyimide aerogels obtained by aging wet gels at 68°C 15 N NMR spectrum, and Figure 1B Provided are solid-state polyimide aerogels obtained by aging wet gels at 25°C. 15 N NMR spectrum. Figure 1A and Figure 1B Together, the overlapping spectra indicate that imidization is more complete when aging is carried out at elevated temperatures.

[0213] Selected monolithic materials were pyrolyzed at 1050°C under flowing nitrogen to the corresponding carbon aerogels, designated as C-Td005-Li2-d2-AA2-68. Material characterization data for both Td005-Li2-d2-AA2-68 and C-Td005-Li2-d2-AA2-68 are provided in Tables 2 and 3.

[0214] On the fourth day, a 50 g aliquot of the viscous solution was taken out and acetic anhydride (3.163 g, 4.3 molar excess relative to the monomer repeating units contained in the aliquot) was added. The resulting solution after the addition of acetic anhydride was stirred for about 30 seconds and then divided into multiple molds. The solution gelled in about 1 minute. The resulting gel was transparent, light brown, rubbery, and was very similar to the gel obtained by conventional means (i.e., prepared in an organic solvent). The gel sample was aged in its mold for 24 hours, then washed with ethanol (4 times) and dried with supercritical fluid CO2 to provide the corresponding polyimide aerogel. These aerogel monoliths were called Td005-Li2-d4. The selected monoliths were pyrolyzed at 1050°C under flowing nitrogen to the corresponding carbon aerogels, designated as C-Td005-Li2-d4. The material characterization data for both Td005-Li2-d4 and C-Td005-Li2-d4 are provided in Tables 2 and 3.

[0215] A portion of the remaining viscous yellow solution of the 4th day was dropped into an aqueous hydrochloric acid solution (30% concentrated HCl in deionized water). Polyamic acid beads were formed immediately. The beads were aged for 24 hours in a receiving HCl solution, then washed with water (4 times, 12 hours each time, 1L of water was used each time), then washed with ethanol similarly, and dried with supercritical fluid CO2 to provide corresponding polyamic acid aerogel beads. These aerogel beads are called PAA-beads-Td005-Li2-d4. A portion of those beads were pyrolyzed at 1050°C under flowing nitrogen to corresponding carbon aerogel beads, designated as C-PAA-beads-Td005-Li2-d4. Material characterization data for both PAA-beads-Td005-Li2-d4 and C-PAA-beads-Td005-Li2-d4 are provided in Tables 2 and 3. It is noteworthy that the residual amount of lithium in both PAA-beads-Td005-Li2-d4 and C-PAA-beads-Td005-Li2-d4 measured by elemental analysis (0.02% and 0.05% w / w, respectively) is much smaller than the remaining lithium in Td005-Li2-d4 and C-Td005-Li2-d4 (1.45% and 1.52% w / w, respectively). The reduced amount of lithium in the aerogel beads is attributed to the water washing of the wet gel beads.

[0216] A portion of the viscous yellow solution on day 4 was treated with acetic anhydride as described above, and the gelled material was cast on an aluminum sheet to form a thin film. The film was tough and flexible. A photographic image of the film is provided as Figure 2 . refer to Figure 2 , one end of the membrane was 50 microns thick and the other end was 120 microns thick.

[0217] Example 2. Preparation of polyimide aerogel in water using Li2CO3 as base (target density 0.1 g / cc) And pyrolyzed into the corresponding carbon aerogel

[0218] Polyimide at twice the target density was prepared as described in Example 1, and p-phenylenediamine (6.63 g, 0.06131 mol) was dissolved in 200 mL of deionized water. Lithium carbonate (5.435 g, 1.2 mol excess) was added and dissolved in the same aqueous solution. Pyromellitic anhydride (13.37 g, 0.06130 mol) was suspended in the solution. After a few minutes, no solids remained in the suspension. A large amount of gas evolution (CO2) was observed in the initial stage of the reaction. The viscous yellow solution was stirred for 2 days. Aliquots were taken every 24 hours, and the viscosity of the aliquots was measured using a rheometer. The values ​​were: 422 cP on the first day; and 348 cP on the second day. On the second day, acetic anhydride was added to a very viscous solution in an excess of 3.43 mol relative to the monomer repeat unit (amount of acetic anhydride: 21.512 g). The resulting solution was stirred for about 30 seconds and then divided into multiple molds. The solution gelled in less than 1 minute. The gel was very dark but still transparent rubbery, comparable to gels obtained by classical routes in organic solvents. The gel was aged in its mold for 24 hours, then washed with ethanol (4 times) and dried with supercritical fluid CO2. These aerogel monoliths are called Td01-Li2-d2-AA3.43. The selected monoliths were pyrolyzed at 1050°C under flowing nitrogen to the corresponding carbon aerogels, designated as C-Td01-Li2-d2-AA3.43. The material characterization data for both Td01-Li2-d2-AA3.43 and C-Td01-Li2-d2-AA3.43 are provided in Tables 2 and 3.

[0219] Example 3. Preparation of polyimide aerogels in water with other target densities using Li2CO3 as a base and thermal Solved to the corresponding carbon aerogel

[0220] Polyimide gels, aerogels, and carbon aerogels with target densities (Td) of 0.02 and 0.085 were prepared as described in Example 2 by adjusting the monomer concentration in the reaction mixture accordingly.

[0221] For Td = 0.085, p-phenylenediamine (5.64 g, 0.0521 mol) was dissolved in 200 mL of deionized water. Lithium carbonate (4.620 g, 1.2 mol excess) was added and dissolved in the same aqueous solution. Pyromellitic dianhydride (11.36 g, 0.0521 mol) was suspended in the same solution. After a few minutes, no solid remained in the suspension. A large amount of gas evolution (CO2) was observed in the initial stage of the reaction. The viscous yellow solution was stirred for 2 days. The viscosity was measured using a rheometer on the second day: 126.7 cP. On the second day, acetic anhydride was added to the very viscous solution in an excess of 4.3 mol relative to the monomer repeating unit (amount of acetic anhydride: 22.87 g). The new solution after the addition of acetic anhydride was stirred for about 30 seconds and then divided into multiple molds. The solution gelled in less than 1 minute. The gel was dark but still transparent rubbery, similar to the gel obtained in organic solvents by the classical route. The gels were aged in their molds at room temperature for 24 hours. Then, they were washed with ethanol (4 times) and dried with supercritical fluid CO2 to obtain the corresponding monolithic polyimide aerogels. These aerogel monolithic materials are called Td0085- L Selected monolithic materials were pyrolyzed at 1050°C under flowing nitrogen to the corresponding carbon aerogels, designated as C-Td0085-Li2-d2. Material characterization data for both Td0085-Li2-d2 and C-Td0085-Li2-d2 are provided in Tables 2 and 3.

[0222] For Td = 0.02, p-phenylenediamine (1.33 g, 0.0123 mol) was dissolved in 200 mL of deionized water. Lithium carbonate (1.087 g, 1.2 mol excess) was added and dissolved in the same aqueous solution. Pyromellitic anhydride (2.674 g, 0.0123 mol) was suspended in the same solution. After a few minutes, no solid remained in the suspension. The gas (CO2) escape was almost unnoticeable. The pale yellow solution was stirred for 2 days. The viscosity was measured using a rheometer on the second day: 2.7 cP. On the second day, acetic anhydride was added to the solution in an excess of 4.3 mol relative to the monomer repeating unit (amount of acetic anhydride: 5.399 g). The new solution after the addition of acetic anhydride was stirred for about 30 seconds and then divided into multiple molds. Gelation occurred in more than one hour. The gel was light yellow transparent jelly. The gel was aged in its mold at room temperature for 7 days. During this period, a very small amount of syneresis occurred, allowing the gel to be removed from the mold. They were then washed with ethanol (4 times) and dried with supercritical fluid CO2 to obtain the corresponding monolithic polyimide aerogels. These aerogel monoliths are called Td002-Li2-d2-age7. The selected monoliths were pyrolyzed at 1050°C under flowing nitrogen to the corresponding carbon aerogels, designated as C-Td002-Li2-d2-age7. The material characterization data for both Td002-Li2-d2-age7 and C-Td002-Li2-d2-age7 are provided in Tables 2 and 3.

[0223] Table 2. Material characterization data of the aerogels of Examples 1 to 3.

[0224]

[0225]

[0226] Table 3. Elemental analysis data of aerogels of Examples 1 to 3.

[0227] sample C(%,w / w) H(%,w / w) N(%,w / w) O(%,w / w) Li(%,w / w) Whole piece of material Td005-Li2-d4 52.67 4.10 7.40 32.52 1.52 C-Td005-Li2-d4 77.81 1.19 3.54 11.72 1.45 Td01-Li2-d2-AA3.43 53.33 3.89 7.75 29.94 1.48 C-Td01-Li2-d2-AA3.43 76.2 1.18 5.07 11.36 1.81 Beads PAA-beads-Td005-Li2-d4 54.19 3.87 8.10 29.58 0.02 C-PAA-beads-Td005-Li2-d4 83.31 0.98 7.34 4.63 0.05

[0228] Example 4. Polyimide aerogel with Td of 0.05 g / cc in water using NaHCO3 as base and heat Solve for the corresponding carbon aerogel.

[0229] Paraphenylenediamine (3.315 g, 0.03065 mol) was dissolved in 200 mL of deionized water. Sodium bicarbonate (5.666 g, 2.2 mol in excess) was added and dissolved in the same aqueous solution. Pyromellitic anhydride (6.685 g, 0.03065 mol) was suspended in the same solution. After a few minutes, no solid remained in the suspension. Gas evolution (CO2) was observed in the initial stage of the reaction. The viscous yellow solution was stirred for 3 days. Small aliquots were taken every 24 hours, and the viscosity of the aliquots was measured using a rheometer. The values ​​were: 43.2 cP on the first day; 44.7 cP on the second day; and 44.8 cP on the third day. On the fourth day, 50 g of the viscous solution was separated and 4.3 mol of acetic anhydride (amount of acetic anhydride: 3.120 g) was added to this portion relative to the monomer repeating units contained in this amount. The resulting solution was stirred for about 30 seconds and then divided into multiple molds. The solution gelled in about 1 minute. The gel was a transparent light brown rubbery substance comparable to the gel obtained in organic solvents by the classical route. The gel was aged in its mold for 24 hours and then washed with ethanol (4 times) and dried with supercritical fluid CO2.

[0230] The remaining viscous yellow solution from day 3 was dropped into aqueous hydrochloric acid (30% concentrated HCl in deionized water). Beads formed immediately. The beads were aged in the receiving HCl solution for 24 hours and then washed with water (4 times, 12 hours each, using 1 L of water each time). The beads were then washed similarly with ethanol and then dried with supercritical fluid CO2. Material characterization data for both Td005-NaH-d3 and C-Td005-NaH-d3, monolithic material and beads are provided in Figure 3 (Table 4).

[0231] Example 5. Polyimide aerogel with Td of 0.05 g / cc in water using ammonium carbonate as base and heat Solve for the corresponding carbon aerogel.

[0232] Paraphenylenediamine (3.315 g, 0.03065 mol) was dissolved in 200 mL of deionized water. Ammonium carbonate (3.535 g, 1.2 mol in excess) was added and dissolved in the same aqueous solution. Pyromellitic anhydride (6.685 g, 0.03065 mol) was suspended in the same solution. After a few minutes, no solid remained in the suspension. Gas evolution (CO2) was observed in the initial stage of the reaction. The viscous light yellow solution was stirred for 1 day. The viscosity was measured using a rheometer. The value was: 205 cP. Then, acetic anhydride in excess of 4.3 mol relative to the monomer repeating unit was added to the solution (amount of acetic anhydride: 13.563 g). The new solution after adding acetic anhydride was stirred for about 30 seconds and then divided into multiple molds. The solution gelled in about 1 minute. The gel was transparent, light brown, rubbery, similar to the gel obtained in an organic solvent by the classical route. The gel was aged in its mold at room temperature for 24 hours. Then, they were washed with ethanol (4 times) and dried with supercritical fluid CO2 to obtain the corresponding monolithic polyimide aerogels. These aerogel monolithic materials are called Td005-Am2-d1. The selected monolithic materials were pyrolyzed at 1050°C under flowing nitrogen to the corresponding carbon aerogels, designated as C-Td005-Am2-d1. The material characterization data of both Td005-Am2-d1 and C-Td005-Am2-d1 are provided in Figure 4 (Table 5).

[0233] Example 6. Polyimide aerogel with a target density of 0.05 g / cc in water using guanidine carbonate as the base. And pyrolyzed into the corresponding carbon aerogel.

[0234] Paraphenylenediamine (PDA; 3.32 g, 0.0307 mol) was dissolved in 200 mL of deionized water. Guanidine carbonate (6.63 g, 1.2 mol in excess) was added and dissolved in the PDA aqueous solution. Pyromellitic dianhydride (PMDA; 6.69 g, 0.0307 mol) was suspended in the solution. Gas evolution (CO2) was observed in the initial stages of the reaction. Within a few minutes after the addition, no solid PMDA remained in the suspension. The solution quickly became viscous (within a few minutes). The viscous solution was divided into two parts and processed into a gel 2 or 3 hours after the reaction was started by acetic anhydride (13.48 g, 4.3 mol in excess relative to the monomer repeat unit). After the addition of acetic anhydride, the solution was briefly stirred and gelation was observed within a few seconds. The resulting monolithic gel was yellow and opaque. The monolith was aged at room temperature (25°C) or 68°C for 24 hours, divided into smaller pieces, washed 4 times with ethanol, and dried with supercritical fluid CO2 to obtain the corresponding monolith aerogels with foam appearance. These aerogel monoliths were named Td005-G2-1.2-2_ hours and Td005-G2-1.2-3_ hours, depending on whether the gelation with acetic anhydride was initiated 2 hours or 3 hours after the start of the reaction, respectively.

[0235] Another set of aerogel monoliths, designated Td005-G2-1.0-2_h and Td005-G2-1.0-3_h, were prepared in the same manner, but using only 1 equivalent of guanidine carbonate to the monomer. Samples of aerogel monoliths prepared using one equivalent of guanidine carbonate and aged at room temperature (25°C) or at 68°C were solid-state 15 N NMR analysis. Figure 5A and Figure 5B The overlapping solid-state structures of the aerogels obtained by aging at elevated temperature and room temperature, respectively. 15 N NMR spectrum. Figure 5A , aging at 68°C promotes imidization (the larger peak is at 177 ppm), while Figure 5B The spectrum of indicates that aging at room temperature results in more amide (132 ppm) groups than imide groups. Again, continue to refer to Figure 5B , in the case of room temperature aging, the sample contained residual polyamic acid guanidine salt as indicated by the guanidine cation resonance at 74 ppm.

[0236] Selected monolithic materials were pyrolyzed at 1050 °C under flowing nitrogen to the corresponding carbon aerogels, designated with the prefix C. Material characterization data are provided in Figure 6 (Table 6), and Figure 7 This is a SEM micrograph of a carbonized sample. Figure 7 , under high magnification (50,000x), the walls of the larger pores that provide the foam-like appearance are composed of tangled nanofibers.

[0237] A similar solution of PDA+PMDA polyamic acid guanidine salt (Td=0.05) was reacted for 24 hours. At this point, the solution (called Td005-G2-1.0-24_ hours) became so viscous that it stopped flowing. However, it flows when agitated (stirred). In order to further study this phenomenon, solutions of PDA+PMDA polyamic acid guanidine salts with different amounts of guanidine carbonate and at different target densities were similarly prepared. The linear viscoelastic response of the polyamic acid salt solution was measured on a temperature-controlled Peltier plate using a rheometer with a cone (60 mm diameter 2 ° tilt) and plate geometry ( Figure 8 ). Specifically, Figure 8 The target concentrations (Td, where Td refers to the total solid (PDA+PMDA) concentration in the sol (g / cm)) of the prepared sols from guanidine carbonate at various carbonate to PDA (monomer) ratios were calculated. 3 )) is a graphical depiction of the oscillatory stress versus storage modulus and loss modulus for an oscillatory amplitude sweep of a polyamic acid guanidine solution under ). Figure 8 In oscillatory mode and at low shear stress, some polyamic acid guanidine solutions exhibit solid-like behavior (G'>G"), including a storage modulus (G') that is independent of the oscillation stress, and a loss modulus (G"). However, above a critical stress (referred to as the yield stress), the storage modulus G' drops sharply and the system flows. Reducing the polyamic acid guanidine concentration results in a lower plateau modulus and a lower yield stress because the polymer network structure becomes more dispersed. Continue to refer to Figure 8 At sufficiently low polymer concentrations where the solution has a 2% solids content (Td = 0.02), the polymer no longer forms an osmotic gel and flows at all observed stresses. In addition, it has been observed that some solutions with polyamic acid guanidine concentrations slightly above the critical gel concentration do not gel when the polymer is restricted to a lower molecular weight. In addition to polyamic acid guanidine concentration, the yield stress is also sensitive to temperature, with lower temperatures requiring higher critical stresses to initiate flow, such as Fig. 9 as shown in .

[0238] At the termination of the experiment, the solution quickly reverted to solid behavior. Cyclic shear amplitude values ​​below and then above the yield stress exhibited a rapid and reproducible switch from a solid-like (tan(δ) < 1) to a liquid-like (tan(δ) > 1) viscoelastic response, as shown in Figure 2. Fig.10 where tan(δ) is the ratio G" / G'. Fig.10 , for polyamic acid guanidine solution (Td = 0.05; ratio of monomer to guanidine carbonate is 1:2), the material undergoes shear thinning (thixotropy) with increasing shear rate.

[0239] Fig.11Graphical depiction of shear rate versus viscosity for steady-state rotational scans of aqueous solutions of various polyamide salts. Fig.11 For aqueous solutions of polyamic acid salts based on guanidine carbonate, a viscosity (thixotropy) that decreases (shear thinning) with increasing shear rate is observed. Fig.11 , for monovalent metal cations Na + No thixotropic behavior was observed for aqueous polyamic acid solutions formed by (Na2CO3 at Td = 0.05). Other monovalent metal cations such as Li + , K + The presence of ammonium and thixotropic agents also did not result in thixotropic behavior of the corresponding polyamic acid salt solutions (not shown). Gels formed by exposing polyamic acid salt solutions to solutions containing multivalent cations also did not exhibit a thixotropic viscoelastic response; data for the gels they formed were not shown. In this regard, without wishing to be bound by theory, it is believed that thixotropic behavior requires cations (e.g., guanidine cations) that are able to dynamically interact (e.g., via hydrogen bonding) with multiple polymer chains.

[0240] Example 7. Polyimide aerogels using other water-soluble carbonates as bases in water

[0241] Other commonly used water-soluble carbonates not included in the above specific embodiments include lithium bicarbonate (LiHCO3), sodium carbonate (Na2CO3), potassium carbonate (K2CO3), potassium bicarbonate (KHCO3) and ammonium bicarbonate (NH4HCO3). According to the process of the above embodiments, each of these forms an aqueous solution of polyamic acid salt.

[0242] Example 8. Molecular Weight Determination of Polyamic Acid Salts Produced Using Sodium Carbonate as Base

[0243] According to the aforementioned embodiment, sodium carbonate was used as a base (i.e., PDA-PMDA from aqueous solution) to prepare a polyamic acid sodium salt solution. A reference polyamic acid salt was prepared using a conventional process (dimethylformamide as a solvent, triethylamine as a base, and washed with acetone before precipitation) and the aforementioned aqueous process (water as a solvent, triethylamine as a base). The precipitated polymer was dissolved in water and a Na2CO3 solution (5% solid PAA, containing 1.2 mol equivalent Na2CO3:monomer). The reference and inventive polyamic acid salt solutions were analyzed by gel permeation chromatography (GPC) for the molecular weight of the polyamic acid polymer using a previous polyamic acid salt with a known molecular weight as a molecular weight standard ( Fig.12 ). The polyamic acid was eluted in water with 0.2 M Na2SO4, and the molecular weight was calculated from the peak elution time using the polyamic acid polymer with the previously measured molecular weight. Fig.12, the product of the disclosed carbonate / water process (solid black line) shows an earlier elution time (higher molecular weight) relative to the reference TEA water process (solid gray line) and a molecular weight peak distribution that overlaps with a higher MW sample (dashed black line) prepared in DMF according to the conventional method. In general, the GPC results show that the molecular weight peaks and distributions are comparable for the products of the solvent-based conventional method and the disclosed carbonate-based inventive method, with the molecular weight peaks from both methods being around 20,000 to 30,000 g / mol. In contrast, the GPC results for the products of the previous aqueous process (water as solvent, triethylamine as base) indicate much lower product molecular weights (2,000-8,000 g / mol).

[0244] Rheological analysis of the solutions (viscosity determination; measured at 1 rad / s with continuous flow) was performed. Specifically, the viscosities of the three polyamic acid sodium salt solutions described above (conventional DMF method, reconstitution; previous water-TEA method; and the disclosed water-carbonate method) were determined and plotted against the respective molecular weights as determined by GPC ( Fig.13 ). refer to Fig.13 , the viscosities of equivalent solutions (same polymer concentration and same Na2CO3 concentration) showed a power law relationship and confirmed the GPC analysis results.

Claims

1. A method for preparing an aqueous solution of a polyamic acid salt, the method comprising: Providing polyamic acid; as well as The polyamic acid and a water-soluble carbonate or bicarbonate are combined in water to provide a solution of the polyamic acid salt.

2. The method of claim 1, wherein the water-soluble carbonate or bicarbonate comprises lithium, sodium, potassium, ammonium or guanidinium cations.

3. The method of claim 1 or 2, wherein the water-soluble carbonate or bicarbonate is selected from the group consisting of lithium carbonate, lithium bicarbonate, sodium carbonate, sodium bicarbonate, potassium carbonate, potassium bicarbonate, ammonium carbonate, ammonium bicarbonate, guanidine carbonate, and combinations thereof.

4. A method for preparing an aqueous solution of a polyamic acid salt, the method comprising: combining a water-soluble diamine, a water-soluble carbonate or bicarbonate, and a tetracarboxylic dianhydride in water; as well as The components are reacted to provide a solution of the polyamic acid salt.

5. The method of claim 4, wherein the merging comprises: dissolving a water-soluble diamine in water to form a diamine aqueous solution; adding the water-soluble carbonate or bicarbonate to the aqueous diamine solution; adding tetracarboxylic dianhydride to the aqueous solution of the diamine and the water-soluble carbonate or bicarbonate to form a solution; and The solution is stirred at a temperature in the range of about 4°C to about 60°C for a period of time in the range of about 1 hour to about 4 days.

6. The method of claim 4, wherein the merging comprises: dissolving a water-soluble diamine in water to form a diamine aqueous solution; adding tetracarboxylic dianhydride to the aqueous diamine solution to form a suspension; stirring the suspension at a temperature in the range of about 4° C. to about 60° C. for a period in the range of about 1 hour to about 4 days; adding the water-soluble carbonate or bicarbonate to the suspension; The suspension is stirred at a temperature in a range of about 4° C. to about 60° C. for a period in a range of about 1 hour to about 4 days to provide an aqueous solution of the polyamic acid salt.

7. The method of claim 4, wherein the merging comprises: adding a water-soluble diamine, a tetracarboxylic dianhydride and the water-soluble carbonate or bicarbonate to water simultaneously or in rapid succession; as well as The resulting mixture is stirred at a temperature in a range of about 4° C. to about 60° C. for a period of time in a range of about 1 hour to about 4 days to provide an aqueous solution of the polyamic acid salt.

8. The method of any one of claims 4 to 7, wherein the water-soluble carbonate or bicarbonate comprises lithium, sodium, potassium, ammonium or guanidinium cations.

9. The method of any one of claims 4 to 8, wherein the water-soluble carbonate or bicarbonate is selected from the group consisting of lithium carbonate, lithium bicarbonate, sodium carbonate, sodium bicarbonate, potassium carbonate, potassium bicarbonate, ammonium carbonate, ammonium bicarbonate, guanidine carbonate, and combinations thereof.

10. The method according to any one of claims 4 to 9, wherein: The water-soluble carbonate or bicarbonate is a carbonate, and the molar ratio of the water-soluble carbonate to the diamine is from about 1 to about 1.4; or The water-soluble carbonate or bicarbonate is a bicarbonate, and the molar ratio of the water-soluble bicarbonate to the diamine is from about 2 to about 2.

8.

11. The method of any one of claims 4 to 10, wherein the molar ratio of the tetracarboxylic dianhydride to the diamine is from about 0.9 to about 1.

1.

12. The method according to any one of claims 4 to 11, wherein the tetracarboxylic dianhydride is selected from the group consisting of diphthalic dianhydride (BPDA), benzophenonetetracarboxylic dianhydride (BTDA), oxydiphthalic dianhydride (ODPA), naphthalenetetracarboxylic dianhydride, perylenetetracarboxylic dianhydride, and pyromellitic dianhydride (PMDA).

13. The method of any one of claims 4 to 12, wherein the diamine is 1,3-phenylenediamine, 1,4-phenylenediamine, or a combination thereof.

14. The method according to any one of claims 4 to 13, wherein the diamine is 1,4-phenylenediamine.

15. The method according to any one of claims 4 to 14, wherein the concentration of the polyamic acid salt in the aqueous solution ranges from about 0.01 to about 0.3 g / cm based on the weight of the polyamic acid salt. 3 .

16. The method of any one of claims 1 to 15, wherein the water-soluble carbonate or bicarbonate is guanidine carbonate, and wherein the solution of the polyamic acid salt exhibits thixotropic behavior.

17. The method according to any one of claims 1 to 16, further comprising adding an electroactive material to the aqueous solution of the polyamic acid salt.

18. The method of claim 17, wherein the electroactive material comprises one or more precursors of carbon, graphite, silicon, sulfur, Prussian blue, lithium iron phosphate, combinations thereof, or any thereof.

19. The method according to any one of claims 1 to 18, further comprising forming a polyamic acid aerogel, wherein forming the polyamic acid aerogel comprises: acidifying the polyamic acid salt solution to form a polyamic acid wet gel; as well as The polyamic acid wet gel is dried to form the polyamic acid aerogel.

20. The method of claim 19, wherein drying the polyamic acid wet gel comprises: Optionally, washing the polyamic acid wet gel or subjecting it to solvent exchange; as well as The polyamic acid wet gel is subjected to elevated temperature conditions, the polyamic acid wet gel is freeze-dried, or the polyamic acid wet gel is contacted with supercritical fluid carbon dioxide.

21. The method of claim 19 or 20, further comprising converting the polyamic acid aerogel to an isostructural carbon aerogel, the converting comprising pyrolyzing the polyamic acid aerogel material at a temperature of at least about 650°C under an inert atmosphere.

22. The method of any one of claims 1 to 18, further comprising forming a polyimide aerogel, wherein forming the polyimide aerogel comprises: imidizing the polyamic acid salt to form a polyimide wet gel; as well as The polyimide wet gel is dried to form the polyimide aerogel.

23. The method of claim 22, wherein imidizing the polyamic acid salt comprises adding a gelation initiator to an aqueous solution of the polyamic acid salt to form a gelation mixture and gelling the gelation mixture.

24. The method of claim 23, wherein the gelation initiator is acetic anhydride.

25. The method of any one of claims 22 to 24, wherein drying the polyimide wet gel comprises: Optionally, washing the polyimide wet gel or subjecting it to solvent exchange; as well as The polyimide wet gel is subjected to elevated temperature conditions, the polyimide wet gel is freeze-dried, or the polyimide wet gel is contacted with supercritical fluid carbon dioxide.

26. The method of claim 20 or 25, wherein the washing or solvent exchange is performed with water, a C1 to C4 alcohol, acetone, acetonitrile, ether, tetrahydrofuran, toluene, liquid carbon dioxide, or a combination thereof.

27. The method of any one of claims 22 to 26, further comprising converting the polyimide aerogel to an isostructural carbon aerogel, the converting comprising pyrolyzing the polyimide aerogel at a temperature of at least about 650°C under an inert atmosphere.

28. A polyamic acid salt prepared by the method according to any one of claims 1 to 18.

29. A polyamic acid aerogel prepared by the method according to claim 19 or 20.

30. A polyimide aerogel prepared by the method according to any one of claims 22 to 26.

31. The polyamic acid aerogel according to claim 29, comprising a residual amount of the water-soluble carbonate or bicarbonate.

32. The polyamic acid aerogel according to claim 30, comprising a residual amount of the water-soluble carbonate or bicarbonate.

33. A carbon aerogel prepared by the method according to claim 21 or 27.