Tank container

By forming a resin layer on the surface of the tank or using a diamond film mold necking tool with low dynamic friction coefficient for neck processing, the problem of bending and damage of the tank during processing is solved, and it is improved without adding a varnish layer. Durability and image quality of printed image layers.

CN118973731APending Publication Date: 2024-11-15TOYO SEIKAN KAISHA LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202380031859.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-07-01
Filing Date
2023-06-21
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The prior art tends to cause bending and damage during the neck processing of the tank body, and a varnish layer needs to be formed between the printing image layer and the tank body for protection, resulting in increased processes and increased costs.

Method used

Neck processing is performed by forming a resin layer on the surface of the tank or not using a varnish layer, but using a mold necking tool with a diamond film with a low dynamic friction coefficient, and forming a printed image layer on the resin layer, reducing the varnish layer's use.

Benefits of technology

The neck processing is achieved without damaging the can, reducing the manufacturing cost and process number, and improving the durability and image quality of the printed image layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118973731A_ABST
    Figure CN118973731A_ABST
Patent Text Reader

Abstract

In a first aspect of the present invention, there is provided a method for manufacturing a can container, the method including a step of forming a reduced diameter portion on one end of a can body, on the surface of which a varnish layer is not formed, by means of a die necking tool, the coefficient of dynamic friction between the die necking tool and the can body being 0.30 or less. Further, in a second aspect, a can container is provided, the can container comprising: a can body portion; a bottom part provided on one end side of the tank part; and a reduced-diameter part, the outer diameter of which is reduced on the other end side of the can body part, and at least the outer surface of which is not provided with a varnish layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to can containers. Background Art

[0002] In can containers such as beverage cans, it is known to prevent the can body from being damaged or metal powder from being attached to the can body by applying varnish to the surface of the can body.

[0003] Patent Document 1 describes that a varnish is applied to the neck of a can body after deep drawing to reduce the friction between the can body and the die necking tool, thereby suppressing buckling of the can body and damage to the die. Prior art literature Patent Literature

[0004] Patent Document 1: Japanese Patent Application Publication No. 2019-108138 Open to the public

[0005] A method for manufacturing a can container is disclosed. The method may include a step of forming a reduced diameter portion at one end of a can body having no varnish layer formed on the surface thereof by a die necking tool. The dynamic friction coefficient between the die necking tool and the can body may be 0.30 or less.

[0006] Any of the above-mentioned manufacturing methods may include, before the step of forming the reduced diameter portion, a step of forming a resin layer containing a thermoplastic resin on an outer surface of at least one end portion of the can body that forms the reduced diameter portion.

[0007] In any of the above production methods, the thermoplastic resin may be a polyester resin.

[0008] Any of the manufacturing methods may further include a step of heating the can body having the reduced diameter portion formed therein to soften the resin layer.

[0009] In any of the above manufacturing methods, a smooth diamond film may be formed on at least a portion of the portion of the die necking tool that contacts the can body.

[0010] Any of the above-mentioned mold necking tools may also include: a centering portion inserted into the interior of the can body; and an embedding portion that contacts the can body from the outside to mold the can body. In any of the above-mentioned mold necking tools, at least one of the embedding portion and the centering portion may also have the smooth diamond film on its surface that contacts the can body.

[0011] Any of the above-mentioned manufacturing methods may also include a stage of forming the bottom and the can body together by drawing a metal sheet.

[0012] Any of the above-mentioned manufacturing methods may include a step of printing an ink composition on the surface of the can body having the reduced diameter portion formed thereon to form a printed image layer.

[0013] A can container is provided. The can container may include: a can body; a bottom provided at one end of the can body; and a reduced diameter portion having an outer diameter reduced at the other end of the can body. In the can container, a varnish layer may not be formed at least on the outer surface of the reduced diameter portion.

[0014] In any of the above-mentioned can containers, a resin layer containing a thermoplastic resin may be formed on the metal layer on the outer surface of the reduced diameter portion.

[0015] In any of the above-mentioned can containers, the thermoplastic resin may be a polyester resin.

[0016] Any of the above-mentioned can containers may include a printed image layer formed on the resin layer.

[0017] Any of the above-mentioned can containers may also have a printed image layer formed directly on the metal layer.

[0018] It should be noted that the above invention content does not list all the necessary features of the present invention. In addition, sub-combinations of these feature groups can also become technical solutions. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 An example of a schematic diagram of a tank container before image printing according to the present embodiment is shown. Figure 2 An example of a schematic diagram showing a tank container after image printing according to the present embodiment. Figure 3 An example of the overall layer structure of the tank container according to the present embodiment is shown. Figure 4 An example of the overall layer structure of the tank container according to the present embodiment is shown. Figure 5 An example of the overall layer structure of the tank container according to the present embodiment is shown. Figure 6 An example of the overall layer structure of the tank container according to the present embodiment is shown. Figure 7 An example of the overall layer structure of the tank container according to the present embodiment is shown. Figure 8 An example of the overall layer structure of the tank container according to the present embodiment is shown. Fig. 9 An example of the flow of the manufacturing method of the can container by wet molding according to the present embodiment is shown. Fig.10An example of the wet molding flow of S10 in this embodiment is shown. Fig.11 An example of the component structure of the die necking tool used in this embodiment is shown. Fig.12 An example of the flow of the neck processing in S40 of the present embodiment is shown. Fig.13 An example of the flow of the manufacturing method of the can container by dry molding according to the present embodiment is shown. Fig.14 An example of the flow of dry molding in S110 of the present embodiment is shown. Fig.15 An example of a flow of forming the receiving layer according to the present embodiment is shown. Fig.16 An example of a flow of forming a base image layer according to the present embodiment is shown. DETAILED DESCRIPTION

[0020] Hereinafter, the present invention will be described by way of the embodiments of the invention, but the following embodiments are not limited to the technical solutions involved in the claims. In addition, not all combinations of features described in the embodiments are essential to the solution of the invention.

[0021] Figure 1 An example of a schematic diagram of a tank container 50 before image printing according to the present embodiment is shown. The tank container 50 of the present invention can be processed into a neck portion while protecting the surface of the tank container 50 even without applying varnish. The tank container 50 includes a reduced diameter portion 100 provided at one end, a tank body portion 200, and a bottom portion 250 provided at the other end.

[0022] The reduced diameter portion 100 is a portion where the outer diameter of one end of the can container 50 is reduced. The reduced diameter portion 100 may be provided at the opening of the can container 50. By providing the reduced diameter portion 100 at the can container 50, the amount of can lids to be mounted on the opening of the can container 50 can be reduced.

[0023] The reduced diameter portion 100 may be formed by performing neck processing on the tank container 50. The reduced diameter portion 100 may also be formed in a manner that the outer diameter gradually decreases as it approaches one end of the tank container 50. In addition, the reduced diameter portion 100 may have a flange 101 formed simultaneously during the neck processing. The formed flange 101 can be used to assemble the tank cover.

[0024] The can body 200 occupies most of the can container 50 except the reduced diameter portion 100. The outer diameter of the can body 200 can be substantially constant in the long axis direction of the can container 50. Compared with the reduced diameter portion 100, the outer peripheral surface of the can body 200 has a larger surface area and a substantially constant outer diameter, and is therefore suitable for printing on the surface of the can container 50.

[0025] The bottom 250 is a portion provided on the other end side of the tank container 50. The bottom 250 is a portion that is grounded when the tank container 50 is made self-standing. The outer diameter of the bottom 250 may be fixed or may be reduced. The shape of the bottom 250 is not particularly limited.

[0026] Figure 2 An example of a schematic diagram of a tank container 50 after image printing according to the present embodiment is shown. The tank container 50 may include a reduced diameter portion 100 provided at one end, a tank body portion 200, a bottom portion 250 provided at the other end, and a printing portion 300. The printing portion 300 is a region printed on at least a portion of the outer peripheral surface of the tank container 50 using an ink composition. The printing portion 300 may be provided at the tank body portion 200 of the tank container 50. The printing portion 300 may also be provided at the reduced diameter portion 100 (not shown) of the tank container 50. The printing portion 300 may also be provided at the bottom portion 250 (not shown) of the tank container 50.

[0027] Figure 3 An example of the overall layer structure of the can container 50 of the present embodiment is shown. The can container 50 may include the can body 1 and the printed image layer 3 as a layer structure in the overall reduced diameter portion 100, the can body portion 200, and the bottom portion 250.

[0028] The can body 1 is the main body of the can container 50 and contains most of the contents. The can body 1 is formed in a cylindrical shape and has an outer peripheral surface. The can body 1 can be either a seamless can or a welded can. The material of the can body 1 can be either an aluminum can or a steel can, but is not limited thereto.

[0029] The printed image layer 3 is a layer that expresses an image such as text or a pattern on the outer peripheral surface of the can container 50. The printed image layer 3 may be directly formed on the entire or at least a portion of the outer peripheral surface on the metal layer of the can body 1. The printed image layer 3 may constitute a printing unit 300 in the can container 50. The printed image layer 3 may be a layer formed by printing the entire or at least a portion of the can body 1 using an ink composition.

[0030] The printed image layer 3 may be a layer formed by printing the can container 50 using an ink composition. The ink composition may be an aqueous ink, a solvent ink, an ultraviolet curing ink, or an electron beam curing ink, but is not limited thereto. The image formed on the printed image layer 3 may be a color image using an ink composition of multiple colors. The image formed on the printed image layer 3 may also be a monochrome image using an ink composition of one color.

[0031] For example, the printed image layer 3 can be provided on the can body 1 by inkjet printing. As an example, the printed image layer 3 is provided on the can body 1 by direct inkjet printing. As an example, the printed image layer 3 is provided on the can body 1 by offset inkjet printing. Details of these inkjet printing methods will be described later.

[0032] Figure 3 The can container 50 of the embodiment shown has the minimum necessary structure including the can body 1 and the printed image layer 3. Generally, a varnish layer is formed between the can body 1 and the printed image layer 3 to prevent the can body 1 from buckling or being damaged during neck processing, but the can container 50 of the present embodiment does not have a varnish layer. Therefore, the can container 50 of the present embodiment can reduce the number of steps and costs for forming the varnish layer. In addition, the can container 50 of the present embodiment does not form a varnish layer between the can body 1 and the printed image layer 3, so even if the can body 1 is printed using an ink composition, the ink composition will not be repelled, and an image with excellent image quality can be obtained.

[0033] Figure 4 An example of the overall layer structure of the can container 50 of the present embodiment is shown. The can container 50 may include a can body 1, a printed image layer 3, and a varnish layer 2 as a layer structure. It should be noted that, unless otherwise specified, the description of each layer can be directly applied.

[0034] In this embodiment, the varnish layer 2 protects the printed image layer 3 from external impacts, etc. The varnish layer 2 may be provided on at least one of the tank body 200 and the bottom 250 of the tank container 50. The varnish layer 2 may also be provided on the entire or at least a portion of the printed image layer 3. The varnish layer 2 may also not be provided on at least the outer surface of the reduced diameter portion 100 of the tank container 50.

[0035] The thickness of the varnish layer 2 may be 0.5 μm or more and 15 μm or less. When the thickness of the varnish layer 2 is within the above range, the printed image layer 3 can be appropriately protected.

[0036] The varnish layer 2 may have a resin component. The varnish layer 2 may be formed by applying a solution obtained by dissolving the resin component in an organic solvent and sintering the solution. The solution obtained by dissolving the resin component in an organic solvent may be applied to the entire or at least a portion of the outer surface of the printed image layer 3. As the resin component of the varnish layer 2, a thermosetting acrylic resin, a thermosetting epoxy resin, or a thermosetting polyester resin may be contained. Sintering may be performed by heat, wind, ultraviolet irradiation, or electron beam irradiation.

[0037] By additionally providing the varnish layer 2 on the printed image layer 3, the varnish layer 2 protects the printed image of the printed image layer 3 from degradation caused by physical impact, oxygen, moisture, etc., and can improve durability. In addition, by providing the varnish layer 2, the color shift of the printed image of the printed image layer 3 can be prevented. In addition, by providing the varnish layer 2, the surface of the can container 50 can be made smooth. Moreover, the can container 50 of the present embodiment does not form a varnish layer between the can body 1 and the printed image layer 3, so even if the can body 1 is printed with an ink composition, the ink composition is not repelled, and an image with excellent image quality can be obtained.

[0038] By providing the varnish layer 2, Figure 4 The tank container 50 of the embodiment shown can properly protect the printed image of the printed image layer 3 and has improved durability. In addition, by properly protecting the printed image of the printed image layer 3, Figure 4 The can container 50 of the illustrated embodiment can have an image of the printing unit 300 with excellent image quality.

[0039] Figure 5 Another example of the overall layer structure of the can container 50 of the present embodiment is shown. The can container 50 may include a can body 1 , a resin layer 8 , and a printed image layer 3 .

[0040] The resin layer 8 has the function of improving the sliding property of the tank container 50 and preventing the surface damage during the processing of the tank container 50. The resin layer 8 can be provided on the whole or at least a part of the outer peripheral surface on the metal layer of the can body 1. The resin layer 8 can also be provided on at least the whole or a part of the outer surface of the reduced diameter portion 100 of the tank container 50. The printed image layer 3 can be provided on the whole or at least a part of the resin layer 8. The printed image layer 3 can be a layer formed by printing the whole or at least a part of the resin layer 8 using an ink composition.

[0041] The resin contained in the resin layer 8 may contain a thermoplastic resin. For example, the resin layer 8 may contain a structure composed of a polyester resin. For example, the resin layer 8 may also contain a structure derived from isophthalic acid. For example, the resin layer 8 may also contain a polyester resin containing a structure derived from isophthalic acid in a unit structure. In addition, the resin contained in the resin layer 8 may also contain a thermosetting acrylic resin, a thermosetting epoxy resin, a thermosetting polyurethane resin, or a thermosetting polyester resin instead of a thermoplastic resin. By including the above-mentioned structure, the resin layer 8 can have appropriate sliding properties, showing the characteristics of excellent strength of the resin layer 8 and excellent adhesion to the can body 1.

[0042] The thickness of the resin layer 8 can be not less than 0.5 μm and not more than 30 μm. When the thickness of the resin layer 8 is within the above range, the sliding property of the can container 50 can be improved, and printing with excellent image quality can be performed. When the thickness of the resin layer 8 is less than 0.5 μm, the surface of the resin layer 8 is difficult to slide, so when the reduced diameter portion 100 is formed in the can container 50, the can container 50 may be damaged, or metal powder may adhere to the mold used to form the reduced diameter portion 100 of the can container 50. When the thickness of the resin layer 8 exceeds 30 μm, the resin adhesion after the neck processing and the flange processing may deteriorate.

[0043] The coefficient of kinetic friction on the surface of the resin layer 8 may be 0.30 or less. The above-mentioned coefficient of kinetic friction can be achieved by the resin layer 8. In addition, the coefficient of kinetic friction on the surface of the resin layer 8 may be adjusted to 0.30 or less by subjecting the resin layer 8 to surface treatment such as atmospheric pressure plasma treatment or corona treatment as required. In the case where the coefficient of kinetic friction on the surface of the resin layer 8 exceeds 0.30, the sliding property with the mold necking tool deteriorates during neck processing, and the load during molding is unevenly applied to the processing portion, and the can body portion 200 may be buckled. In addition, in the case where the coefficient of kinetic friction on the surface of the resin layer 8 exceeds 0.30, the sliding property with the conveying guide and the adjacent tank container 50 deteriorates during the conveying of the tank container, and blockage and poor flow may occur in the manufacturing line of the tank container 50 and the subsequent filling line of the contents.

[0044] By providing the resin layer 8 on the can body 1, it is possible to prevent the can container 50 from being damaged when the reduced diameter portion 100 is formed on the can container 50, and prevent metal powder from adhering to the mold used to form the reduced diameter portion 100 of the can container 50. In addition, due to the softness and flexibility of the resin layer 8, it has an excellent effect of adhesion with the can body 1 and the printed image layer 3.

[0045] By providing the resin layer 8, Figure 5 The can container 50 of the embodiment shown can prevent the can container 50 from being damaged when the can container 50 is reduced in diameter, and metal powder can be prevented from being attached to the mold for forming the reduced diameter portion 100 of the can container 50. Generally, a varnish layer is formed on the can body 1 to prevent buckling and damage of the can body 1 during neck processing, so when the can body 1 is printed with an ink composition, the ink composition may be repelled. However, by providing the resin layer 8 instead of the varnish layer, Figure 5 The can container 50 of the illustrated embodiment can provide an image with excellent image quality without repelling the ink composition when printing is performed on the resin layer 8 using the ink composition.

[0046] Figure 6 Another example of the overall layer structure of the can container 50 of the present embodiment is shown. The can container 50 may include a can body 1 , a resin layer 8 , a printed image layer 3 , and a varnish layer 2 .

[0047] The resin layer 8 has the function of improving the sliding property of the tank container 50 and preventing the surface damage during the processing of the tank container 50. The resin layer 8 can be provided on the whole or at least a part of the outer peripheral surface on the metal layer of the can body 1. The resin layer 8 can also be provided on at least the whole or a part of the outer surface of the reduced diameter portion 100 of the tank container 50. The printed image layer 3 can be provided on the whole or at least a part of the resin layer 8.

[0048] The varnish layer 2 is a layer for protecting the printed image layer 3 from external impacts, etc. The varnish layer 2 may be provided on all or at least a part of the printed image layer 3. The varnish layer 2 may not be provided on at least the outer surface of the reduced diameter portion 100 of the can container 50.

[0049] By providing the resin layer 8, Figure 6 The can container 50 of the embodiment shown can prevent the can container 50 from being damaged when the can container 50 is reduced in diameter, and metal powder can be prevented from being attached to the mold for forming the reduced diameter portion 100 of the can container 50. In addition, by providing the varnish layer 2, Figure 6 The tank container 50 of the embodiment shown can appropriately protect the printed image of the printed image layer 3 and has improved durability. Figure 6 The can container 50 of the illustrated embodiment can provide an image with excellent image quality without repelling the ink composition when printing is performed on the resin layer 8 using the ink composition.

[0050] Figure 7 Another example of the overall layer structure of the can container 50 of the present embodiment is shown. The can container 50 may include a can body 1 , a resin layer 8 , a receiving layer 7 , and a printed image layer 3 .

[0051] The receiving layer 7 is a layer that receives the ink composition contained in the printed image layer 3. For example, the receiving layer 7 may be a porous layer. The resin layer 8, the receiving layer 7, and the printed image layer 3 may be provided on the entire or at least a portion of the outer peripheral surface of the can container 50. The printed image layer 3 may be provided on the entire or at least a portion of the receiving layer 7. The resin layer 8 may not be provided on the can container 50.

[0052] When the receiving layer 7 is a porous layer, when printing is performed using the ink composition, the ink composition can enter the receiving layer 7. Therefore, Figure 7 As shown, the printed image layer 3 does not necessarily have to be laminated on the receiving layer 7 in a layered manner.

[0053] The thickness of the receiving layer 7 may be 0.1 μm or more and 50 μm or less. When the thickness of the receiving layer 7 is within the above range, the ink composition contained in the printed image layer 3 can be appropriately received.

[0054] The receiving layer 7 can be formed by coating a solution formed by dissolving the resin component in an organic solvent and sintering. The solution formed by dissolving the resin component in an organic solvent can be applied to all or at least a part of the outer surface of the tank body 1 or the resin layer 8. As the resin component of the receiving layer 7, a thermosetting acrylic resin, a thermosetting epoxy resin, a thermosetting polyurethane resin or a thermosetting polyester resin can be contained. Sintering can be carried out by heat, wind, ultraviolet irradiation or electron beam irradiation.

[0055] By additionally providing the receiving layer 7 on the whole or at least a part of the can body 1 or the resin layer 8, the printed image layer 3 provided with the receiving layer 7 can be firmly held and fixed, thereby improving the adhesion between the can body 1 and the printed image layer 3 or between the resin layer 8 and the printed image layer 3. In addition, by providing the receiving layer 7, the can container 50 can have an image with better image quality.

[0056] By setting the receiving layer 7, Figure 7 The tank container 50 of the embodiment shown can have an image with better image quality. In addition, since the resin layer 8 has appropriate sliding properties, Figure 7 The can container 50 of the illustrated embodiment can prevent the can container 50 from being damaged when the can container 50 is reduced in diameter, and prevent metal powder from adhering to a mold used to form the reduced diameter portion 100 of the can container 50 .

[0057] Figure 8 Another example of the overall layer structure of the can container 50 of the present embodiment is shown. The can container 50 may include a can body 1 , a resin layer 8 , a base image layer 6 , and a printed image layer 3 .

[0058] The base image layer 6 has a function as a base for laminating the printed image layer 3. The base image layer 6 may be a layer formed by forming a base on the whole or at least a part of the can body 1 or the resin layer 8, and then printing on the base using an ink composition. The resin layer 8, the printed image layer 3, and the base image layer 6 may be provided on the whole or at least a part of the outer peripheral surface of the can container 50. The resin layer 8 may not be provided on the can container 50.

[0059] The substrate may contain acrylic resin, epoxy resin, polyurethane resin, rosin-modified phenolic resin, polyester resin, petroleum resin, ketone resin, rosin-modified maleic acid resin, amino resin or benzoguanamine resin. The printed image layer 3 may be provided on all or at least a portion of the substrate image layer 6.

[0060] The base of the base image layer 6 can be formed by applying a solution obtained by dissolving a resin component in an organic solvent and sintering the solution. The solution obtained by dissolving a resin component in an organic solvent can be applied to the entire surface of the can body 1 or the resin layer 8 or at least a part of the surface. The resin component of the base image layer 6 may contain a thermosetting acrylic resin, a thermosetting epoxy resin, or a thermosetting polyurethane resin. Sintering can be performed by heat, wind, ultraviolet irradiation, or electron beam irradiation.

[0061] The printing of the base image layer 6 can be set by performing solid printing. The base image layer 6 can be set by performing pattern printing. In the printing to form the base image layer 6, the ink composition can be used in a single color such as white or transparent. In the printing to form the base image layer 6, the ink composition can also be used in multiple colors.

[0062] The image of the printed image layer 3 becomes clearer by additionally providing the base image layer 6 on the can body 1 or the resin layer 8. In addition, by providing the base image layer 6, the decorativeness of the can container 50 and the degree of freedom of printing can be improved.

[0063] By setting the base image layer 6, Figure 8 The tank container 50 of the illustrated embodiment can have a clearer image of the printed image layer 3. In addition, Figure 8 The can container 50 of the embodiment shown can also make the image of the base image layer 6 overlap with the image of the printed image layer 3, and can have improved decorative properties. In addition, since the resin layer 8 has appropriate sliding properties, Figure 8 The can container 50 of the illustrated embodiment can prevent the can container 50 from being damaged when the can container 50 is reduced in diameter, and prevent metal powder from adhering to a mold used to form the reduced diameter portion 100 of the can container 50 .

[0064] Fig. 9 This is an example of a process for manufacturing the tank container 50 of this embodiment by wet molding. The tank container 50 of this embodiment can be manufactured by performing Fig. 9 It should be noted that, for the sake of convenience, the processes of S10 to S80 are described in sequence, but at least a part of these processes can be executed in parallel, or each step can be replaced within the scope of the present invention.

[0065] First, in S10, the metal sheet is wet-formed. In S10, the metal sheet is punched into a cup shape, and the side wall is stretched to form a can body and a bottom. In S10, Fig.10 As shown, the wet forming includes the steps of S11 to S16.

[0066] Fig.10 This is a diagram showing S10 in the flow.

[0067] First, in S11, a step of unwinding and unfolding a metal plate wound into a coil is performed. The metal may be aluminum or steel, but is not limited thereto.

[0068] Next, in S12, a lubricating step of applying a lubricant to the metal material is performed. The lubricant may be a lubricant. A known lubricant may be used as the lubricant.

[0069] Next, in S13, the metal material is punched into a cup shape, and a step of deep drawing and punching is performed to form the cup-shaped raw material.

[0070] Next, in S14, a main body manufacturing step is performed by drawing the cup-shaped raw material using a coolant to thin and stretch the can body and form the bottom. The coolant may be a lubricant. A known lubricant may be used as the lubricant.

[0071] Next, in S15, the cup-shaped raw material is subjected to a trimming step of removing unnecessary portions and making the height uniform.

[0072] Next, in S16, the cup-shaped raw material is cleaned and dried, and a cleaning step is performed to remove the applied coolant, etc. The cleaned and dried cup-shaped raw material is recorded as a can body. After S16, the process proceeds to step S40.

[0073] It should be noted that the inner circumference of the can body may be coated with paint and sintered before entering S40. By coating the inner circumference of the can body, it is not easy to cause damage to the inner circumference. The paint can use known paint. The coating of the paint can be carried out by spraying. Sintering can be carried out by known methods. For example, it can be carried out by hot air drying. The step of coating the inner circumference of the can body is not limited to being performed after the end of S16.

[0074] Next, in S40, neck processing is performed on at least one end of the can body to form a reduced diameter portion. The neck processing can be performed by a known method. For example, the neck processing can be performed by a method described in Japanese Patent Gazette No. 2748856 or Japanese Patent Gazette No. 2705571. The neck processing can be performed using a die necking tool. The die necking tool can be a tool described in Japanese Patent Gazette No. 2018-070181.

[0075] Fig.11 1 is a cross-sectional view showing an example of the component structure of a die necking tool 400 used in the neck processing of the present embodiment. The die necking tool 400 includes an inserting portion 410 , a positioning inserting portion 420 , a joining portion 430 , and a centering portion 440 .

[0076] The embedding portion 410 contacts the can body 1 from the outside of the can body 1 and serves as the main molding surface for molding the can body 1. The embedding portion 410 has a shape in which the width between the embedding portion 410 and the centering portion 440 gradually narrows as it approaches the joint portion 430 from the portion in contact with the positioning embedding portion 420. The embedding portion 410 has at least an open end 410a and a bent portion 410b on the surface. The open end 410a forms the open end of the can body 1. The bent portion 410b forms a portion in which the outer diameter of the can body 1 gradually decreases. During neck processing, the can body 1 contacts the open end 410a and the bent portion 410b of the embedding portion 410.

[0077] The positioning embedding portion 420 has the function of centering the can body 1. The joint portion 430 has the function of demolding the can body 1 that has been subjected to neck processing and formed with the reduced diameter portion 100. The centering portion 440 has the function of being a core inserted into the inside of the can body 1. The centering portion 440 has at least an open end 440a on the surface. The open end 440a forms the open end of the can body 1. During the neck processing, the can body 1 contacts the open end 440a of the centering portion 440.

[0078] The die necking tool 400 may form a smooth diamond film on the entire or at least a portion of the portion in contact with the can body 1. For example, a smooth diamond film may be formed on the surface in contact with the can body 1 of at least one of the embedding portion 410 and the centering portion 440. As an example, at least one of the opening end 410a of the embedding portion 410, the bending portion 410b, or the opening end 440a of the centering portion 440 is a surface formed with a smooth diamond. By forming a smooth diamond film on the portion in contact with the can body 1 of the die necking tool 400, the necking process can be performed without damaging the can body 1 even if varnish is not applied to the can body 1.

[0079] The diamond film can be formed on the substrate of the die necking tool by a plasma CVD method or the like. The surface of the diamond film can be polished mechanically or chemically to improve the smoothness. The surface can be polished so that the surface roughness Ry (JIS B-0601-1994) of the diamond film is less than 0.4 μm, preferably less than 0.2 μm.

[0080] In addition, the dynamic friction coefficient between the die necking tool 400 and the can body 1 may be 0.30 or less, preferably 0.15 or less. The above dynamic friction coefficient can be achieved by forming a smooth diamond film on all or at least a portion of the portion of the die necking tool 400 that contacts the can body 1. By setting the dynamic friction coefficient between the die necking tool 400 and the can body 1 to be 0.30 or less, even if the varnish layer 2 is not formed on the surface of the can body 1, good sliding properties between the die necking tool 400 and the can body 1 can be ensured without damaging the can body 1, and neck processing can be performed.

[0081] When the dynamic friction coefficient exceeds 0.30, the sliding property between the mold necking tool 400 and the can body 1 deteriorates during neck processing, and the load during molding is unevenly applied to the processing portion, which may cause the can body 200 to buckle. In addition, when the dynamic friction coefficient exceeds 0.30, when the can body 1 is conveyed, the sliding property between the conveying guide and the adjacent can body 1 deteriorates, and blockage and poor flow may occur in the manufacturing line of the can body 1 and the subsequent filling line of the content. It should be noted that, in addition to Fig.11 In addition to the die necking tool described in , a die necking tool having a smooth diamond film formed on the entire or at least a portion of the portion in contact with the can body 1 and satisfying the above-mentioned dynamic friction coefficient can also be used.

[0082] Fig.12 This is an example of a process for neck processing using a die necking tool 400. First, the open end of the can body is pressed between the embedding portion 410 and the centering portion 440 of the die necking tool ( Fig.12 The open end of the can body collides with the positioning embedding portion 420, and then collides with the embedding portion 410 to bend ( Fig.12 Then, the opening end of the can body collides with the centering portion 440 ( Fig.12 (C)) and bend back ( Fig.12 (D)), and finally a reduced diameter portion 100 ( Fig.12 (E)). The can body may also be flanged at the same time or after the neck processing to form a flange 101 ( Fig.12 (E)). The can body after the neck processing is completed is recorded as a can container.

[0083] Steps S10 to S40 can be performed in a canning factory. After S40, the process proceeds to step S50.

[0084] Next, in S50, the ink composition is printed on all or at least a portion of the surface of the tank container (e.g., the reduced diameter portion 100, the tank body portion 200, or the bottom portion 250). Printing can be performed on the metal layer of the tank body. Printing can be performed by inkjet printing. Printing can also be performed by offset printing. As an example, inkjet printing can be performed by the method described in Japanese Patent Gazette No. 6314468.

[0085] Inkjet printing may be inkjet printing in which an inkjet head provided in an inkjet printer directly ejects an ink composition onto a tank container. As an example, inkjet printing may be direct inkjet printing in which an inkjet head provided in an inkjet printer directly ejects an ink composition onto a tank container. As an example, inkjet printing may also be offset inkjet printing in which an inkjet head provided in an inkjet printer ejects an ink composition onto a blanket and transfers an inkjet image formed on the blanket onto the tank container.

[0086] The ink composition used for printing may be an aqueous ink, a solvent ink, an ultraviolet curing ink or an electron beam curing ink, but is not limited thereto. The image formed by printing may be a color image using an ink composition of multiple colors. The image formed by printing may also be a monochrome image using an ink composition of one color.

[0087] When the ink composition is printed on a can container, the ink composition can be printed by fixing the can container to a can container holding member. The can container holding member can use a known member such as a star wheel. For example, the can container can be fixed by the method described in Japanese Patent Gazette No. 6124024. For example, the can container can be fixed to the can container holding member by clamping the bottom of the can container. As an example, the can container can also be fixed by fixing the bottom of the can container to the can container holding member by vacuum suction.

[0088] In order to stably fix the tank container, a pressing component may be provided in addition to the tank container holding component. The tank container can be fixed more stably by providing the pressing component. In addition, the ink composition can be prevented from entering the interior of the tank container by providing the pressing component. The pressing component may be arranged at a position to press the reduced diameter portion or the opening portion of the tank container. The pressing component may cover the reduced diameter portion or may not cover the reduced diameter portion. In the case where the ink composition is highly irritating and allergenic to the skin, the ink composition can be prevented from being applied to the reduced diameter portion by arranging the pressing component in a manner that covers the reduced diameter portion, thereby reducing the irritation and allergenicity to the skin.

[0089] Next, in S60, the printed can container is sintered to form a printed image layer. The printed image is fixed to the can container by sintering. Sintering can be performed by hot air drying. Sintering can also be performed by ultraviolet irradiation. Sintering can also be performed by electron beam irradiation.

[0090] It should be noted that after forming the printed image layer, in order to protect the printed image layer, a varnish may be applied to the entire or at least a portion of the can container to form a varnish layer. The varnish layer may be formed by applying a solution obtained by dissolving a resin component in an organic solvent and sintering the solution. The resin component of the varnish layer may contain a thermosetting acrylic resin, a thermosetting epoxy resin, or a thermosetting polyester resin. Sintering may be performed by heat, wind, ultraviolet irradiation, or electron beam irradiation.

[0091] Next, in S70, the can container having the printed image layer formed thereon is inspected. For example, the inspection may include checking whether there are depressions, holes, etc. on the outer circumference or inner circumference of the can container. For example, the inspection may include checking whether the printed image of the printed image layer is clear. For example, the inspection may include checking whether there are dirt or flaws on the outer circumference of the can container.

[0092] Next, in S80, the inspected can container is filled with content. The can container filled with content is assembled with a can lid. The filling of content and the assembly of can lid can be performed by known methods. Fig. 9 The process to obtain Figure 3 or Figure 4 The tank container 50 is shown in the embodiment.

[0093] Steps S10 to S40 may be performed at a canning plant. Steps S50 to S80 may be performed at a bottling company. When the bottling company performs steps S50 and later, steps S10 to S40 are performed at the canning plant, and the can container without the printed image layer is stored.

[0094] In this case, even if the printed image of the printed image layer is changed, the changed image can be printed on the can container at the bottling company, so the can containers to be discarded can be reduced. In addition, the design of the printed image can be changed more flexibly and with a high degree of freedom. In addition, since it is not necessary to store a variety of printed cans in the canning factory, it is also excellent in storage costs, and it can meet the needs of multi-variety small batch production.

[0095] It should be noted that steps S10 to S70 may be performed at a canning factory, and step S80 may be performed at a bottling company. The sharing pattern of the steps between the canning factory and the bottling company is not limited to this.

[0096] Next, a modified example of the above-described embodiment will be described. A tank container may be manufactured by combining at least a part of the configurations of a plurality of the modified examples described below.

[0097] [First Modification] Fig.13 This is another example of a process for manufacturing the tank container 50 of this embodiment by dry molding rather than wet molding. Fig.13 It should be noted that, for the sake of convenience, the processes of S110 to S80 are described in sequence, but at least part of these processes can be executed in parallel, or each step can be replaced within the scope of the present invention.

[0098] First, in S110, the metal coil is dry-formed. In S110, the metal coil is covered with a resin film, punched into a cup shape, and the side wall is stretched to form a can body and a bottom. In S110, Fig.14 As shown, the dry forming includes the steps of S11 to S15.

[0099] Fig.14 This is a diagram showing S110 in the flow.

[0100] First, in S11, an uncoiler step is performed to uncoil and unfold the metal coiled material wound into a coil. The metal may be aluminum or steel, but is not limited thereto.

[0101] Next, in S120, a resin film is laminated on both surfaces or one surface of the metal to form a resin layer. For example, a laminator described in Japanese Patent Application Laid-Open No. 2004-25640 can be used for lamination of the resin film.

[0102] The resin contained in the resin film may be a resin containing a thermoplastic resin. For example, the resin film may contain a polyester resin. In addition, as the resin contained in the resin film, a thermosetting acrylic resin, a thermosetting epoxy resin, a thermosetting polyurethane resin or a thermosetting polyester resin may be contained instead of a thermoplastic resin. By covering the metal coil with a resin film, the metal coil has appropriate sliding properties, and even without applying varnish, the sliding properties of the can container can be improved during neck processing to prevent surface damage. In addition, since neck processing can be performed even without applying varnish, the cost and number of steps for manufacturing the can container can be reduced by not having varnish.

[0103] After the resin film is laminated to form the resin layer, the process may proceed to step S13. In addition, a lubricant may be applied to the outer surface as required before the process proceeds to step S13. Fig. 9 The can body after the dry molding is recorded as a can container.

[0104] S110 can be ended and the step S40 can be entered. In the step S40, at least the outer surface of the tank container formed with the resin layer can be necked to form a reduced diameter portion. At this time, the resin layer at least covers the reduced diameter portion to protect the tank container from the influence of the neck processing tool. The neck processing can be performed using a known mold necking tool. Since the tank container is provided with a resin layer, even if the neck processing is performed using a known mold necking tool, the dynamic friction coefficient between the mold necking tool and the resin layer can be set to less than 0.30.

[0105] The neck processing can be performed using the die necking tool on which the diamond film is formed. By using the die necking tool on which the diamond film is formed, the dynamic friction coefficient can be adjusted to a lower value.

[0106] The dynamic friction coefficient between the die necking tool and the resin layer may be 0.30 or less. When the dynamic friction coefficient between the die necking tool and the resin layer is 0.30 or less, the neck processing of the can container can be performed without damaging the can container even if a varnish layer is not formed on the surface of the resin layer. The can body may also be flanged at the same time or after the neck processing to form a flange for assembling the can lid.

[0107] In S40 , the neck of the tank container is processed, and after the reduced diameter portion is formed, the process can proceed to step S401 .

[0108] In S401, the tank container is heated to soften the resin layer. Even in the case where bumps, damage, etc. are formed on the resin layer due to neck processing, the bumps and damage generated on the surface of the tank container can be at least partially repaired or reduced by heating the tank container to soften the resin contained in the resin layer. The heating treatment is preferably based on the glass transition point (Tg) of the resin coating layer, and is generally carried out above Tg+50°C, especially in the temperature range of Tg+100°C to melting point (Tm)-5°C. The required heating treatment time is sufficient if it is short, and specifically, it is preferably carried out between 1 minute and 10 minutes. After heating, step S50 can be entered. It should be noted that step S401 can also be skipped, and after S40, step S50 is entered without heating the tank container.

[0109] By forming a resin layer on the metal layer of the metal coil, the sliding property of the can container can be improved even without applying varnish during neck processing, thereby preventing surface damage during neck processing of the can container. In addition, since neck processing can be performed even without applying varnish, the cost of manufacturing the can container can be reduced without varnish. Fig.13 The process to obtain Figure 5 The can container 50 shown in the embodiment. It should be noted that after the printed image layer is formed, in order to protect the printed image layer, a varnish may be applied to the entire or at least a portion of the can container to form a varnish layer. In this case, a Figure 6 The tank container 50 is shown in the embodiment.

[0110] [Second Modification] In this embodiment, the case where no receiving layer is formed is described, but Fig.15 This indicates a step of forming a receiving layer on the entire or at least a portion of the outer peripheral surface of the tank container before entering step S50 and after performing S40 or S401. The receiving layer may be formed on the entire or at least a portion of the tank container.

[0111] In S421 , a solution obtained by dissolving a resin component in an organic solvent is applied to the entire or at least a portion of the outer surface of the resin layer.

[0112] Next, in S422, the can container coated with the resin component can be subjected to hot air drying, ultraviolet irradiation, electron beam irradiation, etc. to form a receiving layer. The resin component of the receiving layer can contain a thermosetting acrylic resin, a thermosetting epoxy resin, a thermosetting polyurethane resin, or a thermosetting polyester resin. The thickness of the receiving layer can be greater than 0.1 μm and less than 50 μm. The receiving layer can be obtained by additionally performing the steps of S421 and S422. Figure 7 The tank container 50 shown in the embodiment. For the tank container formed with the receiving layer, the process proceeds to step S60.

[0113] By providing a receiving layer on the can container, an image with better quality can be obtained. By providing a receiving layer on the can container, the adhesion between the ink and the receiving layer can be improved, and an image of the printed image layer with better quality can be obtained.

[0114] [Third Modification] In this embodiment, the case where the base image layer is not formed is described. Fig.16 This indicates a step of forming a base image layer on the entire or at least a portion of the outer peripheral surface of the tank container after performing S40 or S401 before entering step S50.

[0115] In S411, a solution obtained by dissolving a resin component in an organic solvent may be applied to the entire or at least a portion of the outer peripheral surface of the tank container. The resin component of the base image layer may contain a thermosetting acrylic resin, a thermosetting epoxy resin, or a thermosetting polyurethane resin. The base image layer may be formed at least on the rear diameter reduction portion of the tank container. The applied resin component is sintered to form a base. The sintering may be performed by a known method.

[0116] Next, in S412, the ink composition is used to print on the substrate. The printing may be full-screen printing. The printing may also be pattern printing. The pattern may be a stripe pattern. The pattern may also be a gradient pattern. The printed color may be colorless and transparent. The printed color may also be white. The printed color may be a single color other than white, or may be multiple colors.

[0117] Next, in S413, the printed ink composition is sintered to form a base image layer. The sintering can be performed by a known method. Figure 8 The tank container 50 shown in the embodiment. After the base image layer is formed, the process proceeds to step S50.

[0118] By arranging the base image layer on the can container, the printed portion of the can container can have a clearer image. In addition, by arranging the base image layer on the can container, the image of the base image layer can be overlapped with the image of the printed image layer, so that the decorativeness can be improved. Example

[0119] The following specifically describes the experimental method and results of confirming the relationship between the dynamic friction coefficient between the can body or resin layer and the mold necking tool and the damage after the neck processing. It should be noted that the experimental method described below is an example and is not limited to the embodiments.

[0120] [Example 1] [Manufacturing of tank body] pass Fig.13 In the step S110 (S11 to S15), the aluminum coil (plate thickness 0.24 mm) is dry-formed to produce a can body. The can body is a seamless can. The height of the can body is 120 mm. No resin layer is formed. [Neck processing] The can body after dry forming was necked using a die necking tool. The die necking tool used a die necking tool with a smooth diamond film formed on the surface of both the embedding part and the centering part that contacted the can body. The diamond film was ground to a surface roughness Ry (JIS B-0601-1994) of 0.1 μm. The thickness of the diamond film was 12.5 μm. [Determination of dynamic friction coefficient] The dynamic friction coefficient between the can body and the die necking tool is difficult to measure directly using the can and the tool, so it was measured by a rotational friction test using a pin-on-disk instead. The pin used was a pin (diamond pin) with a diamond film formed on a superhard alloy pin as the raw material of the die necking tool. As the disk, aluminum (A3104) was used. <Sliding Characteristics> The pin-on-disk test was performed under the following conditions to determine the friction force. The friction coefficient (friction force / load) was calculated in the region where the friction force was stable. <Pin-on-disk test conditions> Pin material: Superhard alloy with diamond film formed on it. Pin Name: Diamond Pin. Pin surface roughness: Diamond pin Ry = 0.1 μm Disc material: Aluminum (A3104). Load: 59N (6kgf) Speed: 10rpm Feed speed: 20mm / min Sliding distance: 2m Test temperature: 30℃ Lubricant: None. [Formation of Printing Image Layer] The printed image layer was formed on the surface of the can body by inkjet printing. The inkjet printing was performed using a nozzle manufactured by Kyocera Corporation. The ink composition was performed using a solvent-based ink (manufactured by TOMATEC Corporation). The sintering of the ink composition printed by inkjet printing was performed by hot air drying. [Evaluation criteria for neck formability] The appearance of the can container was visually evaluated. The results are shown in Table 1. ○: No wrinkles, damage or buckling of the neck of the can container was found. ×: Any one or more of neck wrinkles, damage, and buckling were found in the can container. [Evaluation criteria for printed image quality] The quality of the printed image of the printed image layer was visually evaluated. ◎: The printed image is very clear including the outline. ○: The printed image is clear. ×: The printed image is not clear.

[0121] [Example 2] A can container was produced in the same manner as in Example 1 except that the surface was polished so that the surface roughness Ry of the diamond film was 0.2 μm.

[0122] [Example 3] A can container was produced in the same manner as in Example 1 except that the surface was polished so that the surface roughness Ry of the diamond film was 0.4 μm.

[0123] [Example 4] [Can body manufacturing and resin layer formation] Specifically, through Fig.14 The aluminum coil (plate thickness 0.24 mm) is dry-formed in steps S11 to S15 to produce a can body. The can body is a seamless can. The height of the can body is 120 mm. The rewound coil is covered with a resin film to form a resin layer. The resin film uses polyester resin (ester produced by Toyobo Co., Ltd.). The thickness of the resin layer is 10 μm. The dynamic friction coefficient between the resin layer and the mold necking tool is measured in the same manner as in Example 1, except that a superhard pin (pin material is superhard alloy, Ry=0.28 μm) without a diamond film is used instead of a diamond pin, and a resin-coated aluminum material is used as the disk material instead of aluminum. A resin layer is formed on the can body through the above process, but a can container is manufactured in the same manner as Example 1, except that a necking tool is used on which no diamond film is formed on the surfaces of the embedding part and the centering part in contact with the can body to perform neck processing, and a printed image layer is formed on the resin layer.

[0124] [Example 5] A can container was produced in the same manner as in Example 4 except that a step of heating the can at 200° C. for 2 minutes was additionally performed after the neck processing.

[0125] [Example 6] A resin layer was formed on the can body in the same process as in Example 4, and a printed image layer was formed on the resin layer. A can container was manufactured using a die necking tool having a smooth diamond film (surface roughness = 0.2 μm) formed on the surfaces of both the embedding portion and the centering portion that contact the can body. The dynamic friction coefficient between the resin layer and the die necking tool was measured in the same manner as in Example 2, except that a resin-coated aluminum material was used as the disc material instead of an aluminum material.

[0126] [Comparative Example 1] A can container was produced in the same manner as in Example 1 except that the surface was polished so that the surface roughness Ry of the diamond film was 0.6 μm.

[0127] [Comparative Example 2] A can container was produced in the same manner as in Example 1 except that the surface was polished so that the surface roughness Ry of the diamond film was 0.8 μm.

[0128] [Comparative Example 3] A can container is manufactured in the same manner as in Example 1, except that a die necking tool without a diamond film is used as the die necking tool, and a superhard pin without a diamond film is used instead of a diamond pin for the dynamic friction coefficient between the can body and the die necking tool (the pin is made of superhard alloy, Ry=0.28μm).

[0129] Table 1 shows the results of the experiment.

[0130] [Table 1]

[0131] As shown in the results of Table 1, by setting the dynamic friction coefficient between the can body or the resin layer and the die necking tool to 0.30 or less, a can container without damage or wrinkles in the reduced diameter portion can be provided even without applying varnish. In addition, by heating the can container after neck processing and performing neck processing using a die necking tool having a smooth diamond film formed on the can container formed with a resin layer, a can container with an image of better quality can be provided.

[0132] The present invention has been described above using the embodiments, but the technical scope of the present invention is not limited to the scope described in the above embodiments. It is obvious to those skilled in the art that various changes or improvements can be made to the above embodiments. According to the description of the claims, the method of making such changes or improvements can also be included in the technical scope of the present invention.

[0133] The order of execution of the actions, processes, steps, and stages of the tanks, tank containers, and methods shown in the claims, specifications, and drawings is not specifically indicated as "earlier," "before," etc. In addition, it should be noted that as long as the tank or tank container of the previous process is not used in the subsequent process, it can be implemented in any order. Even if the action flow in the claims, specifications, and drawings is described using "first," "next," etc. for convenience, it does not mean that it must be implemented in this order. Description of Reference Numerals

[0134] 1: Tank body; 2: varnish layer; 3: Printing image layer; 6: base image layer; 7: Receptive layer; 8: resin layer; 50: Tank container; 100: reduced diameter portion; 101: flange; 200: Tank body; 250: bottom; 300: Printing Department; 400: mold necking tool; 410: embedded part; 410a: open end; 410b: bending portion; 420: positioning embedded part; 430: Joint; 440: centering part; 440a: Open end.

Claims

1. A method for manufacturing a tank container, The process includes forming a reduced diameter portion at one end of the can body on which the varnish layer is not formed by a die necking tool, The dynamic friction coefficient between the mold necking tool and the can body is less than 0.

30.

2. The method for manufacturing a tank container according to claim 1, wherein: Before the stage of forming the reduced diameter portion, The method includes forming a resin layer containing a thermoplastic resin on an outer surface of at least one end portion of the can body that forms the reduced diameter portion.

3. The method for manufacturing a tank container according to claim 2, wherein: The thermoplastic resin is a polyester resin.

4. The method for manufacturing a tank container according to claim 3, The method further includes heating the can body having the reduced diameter portion to soften the resin layer.

5. The method for manufacturing a tank container according to claim 1, wherein: A smooth diamond film is formed on at least a portion of the portion of the die necking tool that contacts the can body.

6. The method for manufacturing a tank container according to claim 5, wherein: The die necking tool has: A centering portion inserted into the interior of the tank body; and The embedding portion is formed to contact the can body from the outside, A surface of at least one of the embedding portion and the centering portion that contacts the can body has the smooth diamond film.

7. The method for manufacturing a can container according to any one of claims 1 to 6, This involves forming the bottom and the body of the tank together by drawing the metal sheet.

8. The method for manufacturing a can container according to any one of claims 1 to 6, The method includes a step of printing an ink composition on the surface of the can body having the reduced diameter portion to form a printed image layer.

9. A tank container, comprising: Tank body; A bottom portion, disposed at one end side of the tank body; and The reduced diameter portion has an outer diameter reduced at the other end side of the tank body portion. No varnish layer is formed at least on the outer surface of the reduced diameter portion.

10. The tank container according to claim 9, wherein: A resin layer containing a thermoplastic resin is formed on the metal layer on the outer surface of the reduced diameter portion.

11. The tank container according to claim 10, wherein: The thermoplastic resin is a polyester resin.

12. The tank container according to claim 10 or 11, wherein: A printed image layer is formed on the resin layer.

13. The tank container according to claim 9, wherein: A printed image layer is formed directly on the metal layer.

Citation Information

Patent Citations

  • Production of light weight can drum body

    JP1995039971A

  • Opening curl section of metal can and manufacturing method for the same

    JP2004224417A

  • Manufacturing method of can body

    JP2019181549A

  • Can container

    JP2021178317A

  • Pressing die and press working method

    US20210394248A1