Separation of polymer blends comprising polyesters by solvent-based process
By using γ-valerol solvent to treat polymer blends at different temperatures, combined with physical separation and heating filtration techniques, polyester was successfully separated and recovered, solving the problem of difficult separation of polyester from other materials and achieving high recovery rate and preservation of material properties.
Patent Information
- Application Number
- CN202380031690.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-31
- Filing Date
- 2023-03-30
- Publication Date
- 2024-11-15
AI Technical Summary
Existing technologies struggle to effectively separate polyester from other materials in polymer blends, especially in the presence of other polymers, fillers, and colorants, resulting in low polyester recovery rates and compromised material properties.
Using γ-valerol as a solvent, the polyester is separated from other components by contacting it with polymer blends at different temperatures through a process of dissolution and precipitation. This is achieved by combining physical separation methods with heating and filtration technology.
The recovery rate of polyester was improved, the number-average molecular weight and intrinsic viscosity of polyester were maintained, fillers and colorants were effectively removed, and polyester with high purity and improved whiteness was obtained.
Smart Images

Figure BDA0005066299020000461 
Figure BDA0005066299020000471 
Figure BDA0005066299020000501
Abstract
Description
[0001] The present invention relates in a first aspect to a method for separating a polymer blend comprising (i) a polyester and (ii) one or more components selected from the group consisting of a second polymer, a third polymer and a filler, wherein the second polymer and the third polymer are different from each other and from the polyester of (i); the method comprising: in step (a), providing the polymer blend and providing a solvent comprising γ-valerolactone; in step (b), contacting the polymer blend with the solvent comprising γ-valerolactone at a temperature T1 of <170°C, thereby obtaining a solvent rich in dissolved second polymer; and / or in step (c), contacting the polymer blend provided in (a) or the residue of the polymer blend obtained in (b) with a solvent comprising γ-valerolactone at a temperature T2 of >170°C, thereby obtaining a solvent enriched in dissolved polyester and comprising optionally at least a portion of filler compared to the solvent provided in (a), and optionally a residue of the polymer blend depleted in polyester and comprising optionally a third polymer and optionally a filler or a portion of a filler.
[0002] In a second aspect, the invention relates to a polyester obtained or obtainable by the process according to the first aspect. A third aspect of the invention relates to the use of the precipitated polyester obtained or obtainable by the process according to the first aspect for textile applications, fiber applications, packaging applications, plastic applications, automotive applications, electronic applications. A fourth aspect relates to a method for preparing a textile and / or a method for preparing a cable or an automotive part based on a polyester obtained or obtainable by the process according to the first aspect.
[0003] In the past decades, the demand for polymeric materials has increased dramatically. However, poor biodegradability leads to a large amount of plastic waste, which is usually incinerated in Europe, thereby losing valuable materials and producing huge CO2 emissions. Worse is landfill due to poor biodegradability. Polymeric materials have been widely used in packaging fields, such as beverage packaging or food packaging. Today, most food and beverages are packaged in plastic bottles and containers made of polymeric materials such as polyethylene terephthalate (PET). PET is also the main component of current clothing. Since these materials typically have poor biodegradability and are still valuable products, it is expected that these plastics will be recovered and recycled. This also applies to polymer blends comprising, for example, polybutylene terephthalate (PBT), which are generally used in the electronics field, such as, as the insulating sheath in cable applications.
[0004] Although recycling processes have been adopted to convert these waste materials into new production materials, there are still many problems associated with the recycling and recovery of polymer materials. Due to mixtures with other polymers, cotton, colorants, etc., the recycling of polyesters, especially polyethylene terephthalate (PET) containing textiles is difficult. Therefore, a closed-loop mechanical recycling process is impossible without separation from other materials. In addition, for other PET scrap sources, pollutants and mixed polymer waste streams usually hinder mechanical recycling. Polymer blends have the same problems with other polyesters, especially polybutylene terephthalate (PBT).
[0005] Methods for recovering polymeric materials include dissolving the polymeric materials. WO 2016 / 12755A1 discloses extracting polyester from packaging, wherein a first solvent is used to remove a colorant and a second solvent is used to dissolve the polyester. Chen et al. (Wenjun Chen, Yuechao Yang, Xue Lan, Baolong Zhang, Xiaogang Zhang and Tiancheng Mu in Green Chem. [Green Chemistry Magazine], 2021, 23, 4065) describe methods for dissolving and accelerating alkaline hydrolysis of PET. However, these methods are limited in application, especially when they involve recovering polyester from a polymer blend containing a corresponding polyester as only one component of a plurality of other materials.
[0006] The underlying object of the present invention is therefore to provide an improved process which enables simple separation of polyester from other materials contained in a polymer blend, which also enables high recovery rates of polyester to be achieved without impairing the relevant properties of the polymer material, such as its number average molecular weight Mn, and which uses non-hazardous solvents.
[0007] Aspect 1 - Method - Method for separating polymer blends
[0008] In a first aspect, the present invention relates to a method for separating a polymer blend comprising
[0009] (i) polyester, and
[0010] (ii) one or more components selected from the group consisting of a second polymer, a third polymer, and a filler, wherein the second polymer and the third polymer are different from each other and from the polyester of (i);
[0011] The method includes:
[0012] (a) providing a polymer blend and providing a solvent comprising gamma-valerolactone;
[0013] (b) contacting the polymer blend with a solvent comprising gamma-valerolactone at a temperature T1 < 170°C, thereby obtaining a solvent rich in dissolved second polymer and a residue of the polymer blend depleted in said second polymer and comprising the polyester, optionally a third polymer and optionally a filler;
[0014] and / or
[0015] (c) contacting the polymer blend provided in (a) or the residue of the polymer blend obtained in (b) with a solvent comprising gamma-valerolactone at a temperature T2 of > 170°C, thereby obtaining a solvent enriched in dissolved polyester compared to the solvent provided in (a) and comprising optionally at least a portion of filler, and optionally a residue of the polymer blend depleted in polyester and comprising optionally a third polymer and optionally a filler or a portion of the filler.
[0016] γ-Valerolactone (C5H8O2; IUPAC: 5-methyloxolan-2-one, abbreviation: GVL) is obtainable from carbohydrate-based biomass, for example, it is easily obtainable from sugars and is therefore a "green" solvent. To date, it has only been described as being able to dissolve single polymer materials at best. It has now been surprisingly found that the use of a solvent comprising GVL in the above-mentioned process for separating a polymer blend comprising polyester leads to the recovery of the polyester in good yield and purity. In addition, not only a cessation of the decrease in the weight-average molecular weight Mw of the polyester recovered from the polymer blend can be achieved, but also an increase in the number-average molecular weight Mn. Fillers, if present, can be effectively removed and a decrease in the intrinsic viscosity can also be avoided.
[0017] "Polymer blend" means a combination of at least one polymer and at least one other component (which is another polymer or filler), which components are combined with each other in any suitable manner. For example, in the case of at least two polymers, the polymers are mixed, or one or more polymers are embedded in one or more other polymers, or the polymers are arranged in a separate layer, and mixed forms of these combinations. For example, a polymer blend is a textile, which comprises polyethylene terephthalate (PET) and spandex and / or polyamide (PA) and / or natural polymers such as cotton and / or polymers such as viscose. Another example of a polymer blend is a composite material, in which fillers such as glass fibers are embedded in polybutylene terephthalate (PBT). "Polymer" means natural and synthetic polymers, in which natural polymers are, for example, cotton, cellulose and lignin. Synthetic polymers are, for example, polyolefins such as polyethylene and polypropylene, polyester, polyurethane, polyamide, polyethylene glycol, polyethers such as polytetrahydrofuran and viscose. "Fillers" are, for example, glass fibers, coal fibers, carbon black, inorganic salts (e.g., talc, sodium carbonate), adhesives, thickeners, defoamers, finishing agents (e.g., water repellents / oil repellents / fouling repellents, flame retardants, anti-wrinkle agents, biocides), binders, surfactants (e.g., softeners, scouring agents, antistatic agents), desizing agents, bleaching agents, oxidants, UV filters, emulsifiers, fixatives, detergent dispersants, and conditioning agents. These components are known to the skilled person.
[0018] "Contacting" in step (b) preferably means that the polymer blend is at least partially immersed in the solvent. Preferably, the polymer blend is at least partially immersed in the solvent, based on the total surface of the polymer blend being 100%, at least 60%, more preferably at least 70%, more preferably at least 80%, more preferably at least 90%, more preferably at least 95%, more preferably at least 99% of the surface of the polymer blend is in contact with the solvent. The same applies to "contacting" in step (c), i.e. the polymer blend provided in (a) or the residue of the polymer blend obtained in (b) is at least partially immersed in the solvent. Preferably, the polymer blend provided in (a) or the residue of the polymer blend obtained in (b) is at least partially immersed in the solvent, based on the total surface of the respective polymer blend being 100%, at least 60%, more preferably at least 70%, more preferably at least 80%, more preferably at least 90%, more preferably at least 95%, more preferably at least 99% of the surface of the polymer blend provided in (a) or the surface of the residue of the polymer blend obtained in (b) is in contact with the solvent.
[0019] Generally, there are no specific restrictions as to the conditions under which the contacting in (b) and / or (c) occurs, provided that effective dissolution of the corresponding polymer occurs.
[0020] In step (b), the second polymer (which is preferably spandex) may not only dissolve, but also at least partially degrade - this is evident from, for example, differential scanning calorimetry (DSC) measurements. "Spandex" is preferably a copolymer of polyurethane and polyethylene glycol and / or polytetrahydrofuran, more preferably spandex is a copolymer of polyurethane and polyethylene glycol or a copolymer of polyurethane and polytetrahydrofuran.
[0021] Step (b) results not only in a second polymer-poor, but also in a residue of the polymer blend, which is poor in the second polymer and comprises polyester, optionally a third polymer and optionally a filler, and in the case of a colored polyester poor in colorant or part thereof. In addition, step (c), especially in combination with step (d) as described below, results in a polyester poor in colorant in the case of a colored polyester. "Poor in colorant" can be determined based on quantitative L*a*b* values, but in addition to optical brighteners, it can also be visually identified by the eye: the polymer blend provided in (a) has a color, wherein the residue of the polymer blend obtained in (b) and / or the polyester precipitated in (d) are brighter and whiter, respectively. "Color" comprises colored and non-colored (white, gray, black). This applies in particular to all non-optical brightener colorants. Poor colorant means, in particular for optical brighteners as colorant, that the intensity of the emitted fluorescent radiation (emission) (preferably in the range of 400 to 600 nm) is reduced for the residue of the polymer blend obtained in (b) and / or the precipitated polyester in (d) when irradiated with light having a wavelength in the range of 250 to 400 nm, compared to the intensity of the emitted fluorescent radiation (emission) (preferably in the range of 400-600 nm) of the polymer blend provided in (a). Methods for determining the intensity of the emitted fluorescent radiation are known to the skilled person and can be determined, for example, visually by using a UV lamp, by fluorescence determination or quantum yield determination.
[0022] With respect to L*a*b* values, "poor colorant", whether the colorant is visible to the human eye or an optical brightener, means
[0023] The absolute value of a* preferably changes by at least 0.2; and / or, preferably and,
[0024] The absolute value of b* preferably changes by at least 0.2; and / or, preferably and,
[0025] The L* value increase is preferably at least 4,
[0026] Each is compared to the L*a*b* values of the colored polymer blend provided in (a), wherein the L*a*b* values are determined according to DIN 5033 and DIN EN ISO 11664-1.6.
[0027] In some preferred embodiments, coloring agent is selected from the group consisting of dye and optical brightener and the mixture of dye and optical brightener." coloring agent " is the material causing the color impression of material to change. This includes dye and optical brightener absorbing visible light wavelength interval (400 to 780nm), which amplifies the light emission of material by UV light absorption and visible light emission (by fluorescence), i.e., optical brightener converts radiation invisible to human eyes (<400nm) into visible fluorescence radiation of blue-red spectral range (400 to 600nm). Coloring agent that can be used for or for changing the color impression of polymeric material is known to technicians. In the context of the present invention, term " dye " means any kind of dye such as dye, pigment, dispersion, wherein dye is one or more in the group consisting of for example selected from the following items: acid dye, basic dye, direct dye, disperse dye, azo dye, food dye, solvent dye, organic dye, inorganic dye, organic pigment, inorganic pigment, disperse ink, active ink, oxidation dye, active dye, sulfur dye, mordant dye and vat dye. The term "optical brightener" includes optical brighteners, fluorescent brighteners and fluorescent whitening agents.
[0028] An overview of colorants for polymer materials can be found, for example, in the following document: “Dyes and Pigments”. Kübra Günes, Ahmet Gürses Springer, 2016 (ISBN: 10: 3319338900); Industrial Organic Pigments - Klaus Hunger, Thomas Heber, Martin U. Schmidt, Friedrich Reisinger, Stefan Wanne Wiley-VCH, 4th edition, 2018 (ISBN: 978-3-527-32608-2); Chemistry and Technology of Natural and Synthetic Dyes and Pigments - Ashis Kumar Samanta, Nasser Awwad, IntechOpen, 2020 (ISBN: 9781789859980, 9781789859973, 9781839687587); Encyclopedia of Color, Dyes, Pigments, Volume 1, Gerhard Pfaff, de Gruyter, 2021 (ISBN: 311058588X); Heinrich Zollinger: Color Chemistry: Syntheses, Properties, and Applications of Organic Dyes and Pigments. 3rd ed. WILEY-VCH Verlag, Weinheim, 2003 (ISBN: 3-906390-23-3); Klaus Hunger (ed.): Industrial Dyes: Chemistry, Properties, Applications. WILEY-VCH Verlag, Weinheim, 2003 (ISBN: 3-662-01950-7); Hermann Rath: Lehrbuch der Textilchemie.einschl. der textilchemischen Technologie [Textile chemistry textbook: including textile chemical technology]. 2nd edition.Springer-Verlag, Berlin, Heidelberg, 1963 (ISBN: 978-3-662-00065-6); Wilfried Kratzert, Rasmus Peichert: Farbstoffe, Quelle & Meyer, Heidelberg, 1981 (ISBN: 3-494-01021-8); Ullmann's Encyclopedia of industrial chemistry, Wiley-VCH, 2000, sections "dyes and pigments" and "dyes, general survey" (ISBN: 9783527303854).
[0029] In some preferred embodiments of the method for separating a polymer blend, (b) comprises:
[0030] (b.1) contacting the polymer blend with a solvent comprising γ-valerolactone at a temperature T1 < 170°C, thereby obtaining a solvent rich in dissolved second polymer and a residue of the polymer blend depleted in said second polymer and comprising the polyester, optionally a third polymer and optionally a filler;
[0031] (b.2) The solvent rich in dissolved second polymer and the residue of the polymer blend obtained in (b.1) are preferably separated by a physical separation method, thereby obtaining a separated solvent rich in dissolved second polymer compared to the solvent provided in (a) and a residue of the polymer blend poor in said second polymer and containing polyester.
[0032] The separation in (b.2) is carried out by methods and means known to the skilled person, in particular solid-liquid separation methods such as filtration, for example, heated pressure filtration, sedimentation or centrifugation (see Handbuch der mechanischen Fest-Flüssig-Trennung Taschenbuch [Handbook of Mechanical Solid-Liquid Separation] - April 29, 2004 von Klaus Luckert (ed.)). The colorant, if present in the polymer blend, in particular in the polyester, remains at least partially in the separated solvent obtained in (b.2).
[0033] In some preferred embodiments of the method for separating a polymer blend, (c) comprises:
[0034] (c.1) contacting the polymer blend provided in (a) or the residue of the polymer blend obtained in (b) or (b.2) with a solvent comprising γ-valerolactone and having a temperature T1a ≤ T2 (T2 is a temperature > 170°C), thereby obtaining a mixture comprising the polymer blend and the solvent;
[0035] (c.2) heating the mixture obtained in (c.1) to a temperature T2> 170°C under continuous heating, wherein the heating from T1a to T2 is preferably carried out at a heating rate in the range of 20 K / h to 1000 K / h, 25 / K / h to 900 K / h, 30 k / h to 800 K / h, 40 k / h to 700 K / h, 60 k / h to 600 K / h, and preferably maintaining T2, thereby obtaining a solvent enriched in dissolved polyester compared to the solvent provided in (a) and optionally comprising at least a portion of the filler; and optionally a residue of the polymer blend, which is depleted in polyester and comprises a third polymer and optionally the filler or a portion of the filler;
[0036] (c.3) Optionally, the solvent rich in dissolved polyester obtained in (c.2) is separated from the residue of the polymer blend, wherein the separation is preferably carried out by heating filtration, more preferably by heating filtration at a temperature T3 in the range of T2 minus 20°C to T2 plus 20°C (T3 = T2 ± 20°C), more preferably at a temperature T3 in the range of T2 minus 10°C to T2 plus 10°C (T3 = T2 ± 10°C).
[0037] The expressions “(optionally) at least a part of the filler” and “(optionally) the filler or a part of the filler” in (c.2) mean that if there is a solvent in the polymer blend provided in (a) (which is soluble in a solvent containing γ-valerolactone at temperature T2), then the soluble filler is also dissolved in the solvent rich in the dissolved polyester obtained in (c.2). When there is not only a soluble filler in the polymer blend provided in (a), but also a filler that is insoluble in a solvent containing γ-valerolactone at temperature T2, the insoluble filler remains in the residue of the polymer blend that is poor in polyester and contains optionally a third polymer. When the polymer blend provided in (a) contains only a filler that is soluble in a solvent containing γ-valerolactone at temperature T2, no filler remains in the residue of the polymer blend. When the polymer blend provided in (a) contains only a filler that is insoluble in a solvent containing γ-valerolactone at temperature T2, all the filler remains in the residue of the polymer blend. When the polymer blend provided in (a) contains a filler that is insoluble in a solvent containing γ-valerolactone at temperature T2 and a filler that is soluble in a solvent containing γ-valerolactone at temperature T2, at least a part of the filler, i.e., the soluble filler, is contained in the solvent rich in the dissolved polyester obtained in (c.2), and the residue of the polymer blend that is poor in polyester and optionally contains a third polymer contains a part of the filler, i.e., the insoluble filler.
[0038] In hot filtration, the heating solution, filter, and funnel are heated, preferably heated so that each has temperature T3. Other means and methods for separation in (c.3) are known to those skilled in the art, such as non-heated filtration. In some embodiments, it is preferred that the hot filtration is carried out > at a pressure of 1 bar, more preferably in the range of 1 bar to 30 bar, preferably in the range of 1 to 10 bar, more preferably in the range of 1 to 6 bar (hot pressure filtration).
[0039] The temperature T1a indicated in (c.1) and (c.2) is the temperature of the solvent containing γ-valerolactone used in (c.1). T1a is the same temperature as T2, i.e., T1a > 170 °C, or T1a is a temperature < T2, for example, T1a is a temperature below 120 °C or T1a is a temperature in the range of 120 °C to < T2, preferably in the range of > 120 °C to < T2. If T1a is T2, heating in a continuously heated manner in step (c.2) means adjusting the heating to maintain T2, preferably adjusting the heating so that the temperature does not exceed T2 by more than 10 °C.
[0040] In some preferred embodiments, the residue of the polymer blend obtained in (c.3) still contains a residual amount of polyester. Therefore, it is preferred that in step (c.4), the residue of the polymer blend obtained in (c.3) containing a residual amount of polyester is contacted with a solvent containing γ-valerolactone, preferably at a temperature T3 as defined above, followed by filtration, preferably heated filtration at a temperature T3 as defined above, thereby obtaining a residue of the polymer blend further depleted in polyester and containing a third polymer and optionally a filler or a portion of the filler; and a solvent containing a residual amount of polyester. Preferably, the contact in (c.4) is carried out such that, in particular in the case of heated filtration used in (c.3), the residue of the polymer blend obtained in (c.3) remains on the filter and is contacted there with a solvent containing γ-valerolactone, wherein the solvent containing the residual amount of polyester obtained in (c.4) is separated due to the filtration. In some preferred embodiments, the solvent containing the residual amount of polyester obtained in (c.4) is combined with the solvent rich in dissolved polyester obtained in (c.3). In some preferred embodiments, the amounts of precipitated polyester finally obtained from the solvent containing the remaining amount of polyester obtained in (c.4) and the solvent enriched in dissolved polyester obtained in (c.3) are combined, before carrying out the further steps (d) and / or (e) and / or (f) and / or (g) as described in more detail below.
[0041] In some preferred embodiments of the method for separating a polymer blend, if T1a is below 120°C, heating is carried out as continuous heating, preferably at a heating rate in the range of 20 K / h to 1000 K / h, 25 / K / h to 900 K / h, 30 k / h to 800 K / h, 40 k / h to 700 K / h, 60 k / h to 600 K / h, preferably heating is carried out so that the mixture obtained in (c.1) is at a temperature range of 110°C-130°C for less than 60 minutes, preferably for less than 50 minutes, more preferably for less than 40 minutes, more preferably for less than 30 minutes, more preferably for less than 20 minutes, or if T1a is above 120°C, heating is carried out as continuous heating, preferably at a heating rate in the range of 0.1 to 1000 K / h, more preferably in the range of 5 to 500 K / h, more preferably in the range of 25 to 300 K / h.
[0042] In some preferred embodiments, the method for separating a polymer blend comprises:
[0043] (d) cooling the solvent obtained in (c) or (c.3) which is rich in dissolved polyester and optionally contains at least a portion of filler compared to the solvent provided in (a) to a temperature below 170°C, preferably below 150°C, more preferably below 140°C, more preferably below 100°C, thereby obtaining the precipitated polyester and the solvent which is poor in dissolved polyester and optionally contains at least a portion of filler.
[0044] The solvent obtained in (c) or (c.2) or (c.3) which is enriched in dissolved polyester compared to the solvent provided in (a) and optionally contains at least a portion of filler is preferably cooled in (d) without adding an antisolvent, i.e. the solvent obtained in (c) or (c.2) or (c.3) is cooled as it is obtained. The cooling is carried out by any suitable method, for example, by allowing the solvent obtained in (c) or (c.2) or (c.3) to stand under ambient conditions (1013 mbar and room temperature 20°C-25°C) or by applying cooling means such as slow cooling in a crystallizer, preferably with a cooling rate in the range of 3 to 25 K / h, in some preferred embodiments with a cooling rate in the range of 3 to 60 K / h, dripping into a GVL with a temperature below 30°C, rapid cooling, preferably with a cooling rate >100 K / h, etc. An "antisolvent" is a solvent having a solubility with respect to the polyester of <1 g / kg at a temperature in the range of 20°C to 25°C. In some alternative embodiments, the solvent obtained in (c) or (c.2) or (c.3) which is enriched in dissolved polyester compared to the solvent provided in (a) and optionally contains at least a portion of filler is preferably cooled in (d) with the addition of one or more antisolvents.
[0045] In some preferred embodiments, the method for separating a polymer blend comprises:
[0046] (e) separating the precipitated polyester obtained in (d) from the solvent lean in dissolved polyester, thereby obtaining the precipitated polyester and a solvent lean in dissolved polyester and optionally comprising at least a portion of the filler.
[0047] In some preferred embodiments, the method for separating a polymer blend comprises:
[0048] (f) optionally washing the precipitated polyester obtained in (e);
[0049] (g) drying the precipitated polyester obtained in (e) or the washed precipitated polyester obtained in (f).
[0050] The washing in the optional step (f) is preferably carried out with a solvent selected from the group consisting of: methanol, ethanol, propanol, isopropanol, acetonitrile, ethyl acetate, acetone, water, or a mixture of two or more of these solvents. In some embodiments, the washing in the optional step (f) is carried out with a solvent selected from the group consisting of: methanol, ethanol, propanol, isopropanol, acetonitrile, ethyl acetate, acetone, water, GVL, or a mixture of two or more of these solvents. The drying in step (g) is preferably carried out under one or more conditions selected from the group consisting of: a pressure in the range of 1 to 1013 mbar; a temperature in the range of 50°C to 210°C, preferably in the range of 60°C to 180°C, more preferably in the range of 80°C to 150°C; a drying time in the range of 30 minutes to 24 hours; in an atmosphere comprising nitrogen, preferably in an atmosphere having at least 90 volume-%, more preferably 95 volume-%, more preferably at least 98 volume-% nitrogen. Drying is carried out by one or more methods selected from the group consisting of contact drying, convection drying and radiation drying.
[0051] The precipitated polyester obtained in (d), (e), (f) and / or (g) is preferably less colored than the polymer blend provided in (a), more preferably the precipitated polyester is colorless. The precipitated polyester preferably has a higher number average molecular weight Mn than the polyester contained in the polymer blend and a mass weight average molecular weight Mw similar to the polyester contained in the polymer blend, i.e., based on the Mw of the polyester contained in the polymer blend being 100 weight-%, the mass weight average molecular weight Mw deviates from the Mw of the polyester contained in the polymer blend by a minimum of -5 weight-% and a maximum of +20 weight-%. The colorant, if present in the polymer blend, in particular in the polyester, is at least partially retained in the solvent of the poorly dissolved polyester obtained in (e).
[0052] In some preferred embodiments, the method for separating the polymer blend comprises recycling the separated solvent obtained in (b.2) and / or the separated solvent obtained in (e) at least partially to (b) and / or (c), optionally after one or more post-treatment steps. The one or more post-treatment steps are performed so as to achieve a suitable purity of the solvent for reuse. For example, the colorant and / or filler (if present) is preferably separated from the solvent by a physical separation method, more preferably by distillation.
[0053] In some preferred embodiments of the method for separating polymer blends, T1 is a temperature in the range of 110°C to <170°C, preferably a temperature in the range of 110°C to 165°C, more preferably a temperature in the range of 120°C to 150°C. In some preferred embodiments of the method for separating polymer blends, T2 is a temperature in the range of >170°C to 200°C, preferably a temperature in the range of 175°C to 190°C, more preferably a temperature in the range of 180°C to 190°C. In particular, T2 is a temperature in the corresponding range, i.e. in some embodiments, a constant temperature T2 is maintained, i.e. in these embodiments, "maintaining T2" also means maintaining about one temperature. In some embodiments, the temperature varies within the range of T2 during step (c) or during the maintenance of T2 in step (c.2), respectively.
[0054] In some preferred embodiments of the process for separating polymer blends, (a), (b), (c), and optionally (d) are performed at a pressure in the range of 800 to 200,000 hPa.
[0055] In some preferred embodiments of the method for separating polymer blends, the polyester according to (i) is based on at least one polyol and at least one organic dicarboxylic acid. The at least one polyol of the polyester of (i) is preferably at least one diol having 2 to 12 carbon atoms, more preferably 2 to 6 carbon atoms, more preferably the at least one polyol comprises at least 1,4-butanediol or 1,2-ethylene glycol. The at least one organic dicarboxylic acid of the polyester of (i) is preferably selected from the group consisting of terephthalic acid, adipic acid, 2,5-furandicarboxylic acid and a mixture of two or more of these dicarboxylic acids. In some preferred embodiments of the method for separating polymer blends, the polyester according to (i) is based on 1,4-butanediol or 1,2-ethylene glycol, more preferably the polyester according to (i) is selected from the group consisting of polymers based on 1,4-butanediol and terephthalic acid (polybutylene terephthalate, PBT), polymers based on 1,2-ethylene glycol and terephthalic acid (polyethylene terephthalate, PET), copolymers of 1,4-butanediol, adipic acid and terephthalic acid (polybutylene adipate terephthalate, PBAT), polymers of 1,2-ethylene glycol and 2,5-furandicarboxylic acid (polyethylene furandicarboxylate, PEF) and mixtures of two or more of these (co)polymers. In some preferred embodiments, the polyester comprises at least PET or PBT.
[0056] In some preferred embodiments of the method for separating polymer blends, the second polymer is preferably selected from the group consisting of polyurethane (PU), polyethylene glycol (PEG), polytetrahydrofuran (pTHF), mixtures of these polymers and copolymers of these polymers, wherein the second polymer is more preferably a copolymer of PU and PEG and / or pTHF, more preferably spandex (a copolymer of PU and PEG or PU and pTHF).
[0057] In some preferred embodiments of the method for separating a polymer blend, the third polymer is preferably selected from the group consisting of polyolefins, preferably polyethylene (PE) and polypropylene (PP), polyamide (PA) and viscose, natural polymers, preferably wool or cotton, mixtures of two or more of these polymers and copolymers of two or more of these polymers, wherein the third polymer is preferably selected from PA, wool, cotton, viscose and mixtures of two or more of these polymers. In some embodiments, there are one or more third polymers present in the polymer blend. Preferably, there are at least two third polymers selected from PA, wool, cotton, viscose, more preferably a mixture of PA with at least one of wool, cotton and viscose. More preferably, there are two third polymers, which are preferably PA and cotton or viscose.
[0058] In some preferred embodiments of the method for separating polymer blends, the filler is selected from the group consisting of: glass fiber, coal fiber, carbon black, inorganic salts (e.g., talc, sodium carbonate), adhesives, thickeners, defoamers, finishing agents (e.g., water repellents / oil repellents / fouling repellents, flame retardants, anti-wrinkle agents, biocides), binders, surfactants (e.g., softeners, scouring agents, antistatic agents), desizing agents, bleaching agents, oxidants, UV filters, emulsifiers, fixatives, detergent dispersants, and control agents. In the embodiment where the polyester is PBT, the filler is one or more selected from the group consisting of glass fiber, coal fiber, carbon black, inorganic salts (e.g., talc, sodium carbonate), adhesives, thickeners, defoamers, finishing agents (e.g., water repellents / oil repellents / fouling repellents, flame retardants, anti-wrinkle agents, biocides), binders, surfactants (e.g., softeners, scouring agents, antistatic agents), desizing agents, bleaching agents, oxidants, UV filters, emulsifiers, fixatives, detergent dispersants, and control agents. Preferably, the filler is one or more selected from the group consisting of glass fiber, coal fiber, carbon black, inorganic salts (e.g., talc, Na2CO3). In embodiments where the polyester is PET, the filler is one or more selected from the group consisting of glass fiber, coal fiber, carbon black, inorganic salts (e.g., talc, sodium carbonate), adhesives, thickeners, defoamers, finishing agents (e.g., water repellents / oil repellents / fouling agents, flame retardants, anti-wrinkle agents, biocides), binders, surfactants (e.g., softeners, scouring agents, antistatic agents), desizing agents, bleaching agents, oxidants, UV filters, emulsifiers, fixatives, detergents and dispersants, and conditioning agents. Preferably, the filler is one or more selected from the group consisting of adhesives, thickeners, defoamers, finishing agents (e.g., water repellents / oil repellents / fouling agents, flame retardants, anti-wrinkle agents, biocides), binders, surfactants (e.g., softeners, scouring agents, antistatic agents), desizing agents, bleaching agents, oxidants, UV filters, emulsifiers, fixatives, detergents and dispersants, and conditioning agents.
[0059] In some preferred embodiments of the method for separating polymer blends, the contacting in (b) or (b.1) is carried out for a period of at least 5 minutes, preferably in the range of 5 minutes to 10 hours, more preferably in the range of 5 minutes to 5 hours, and more preferably in the range of 5 minutes to 4 hours.
[0060] In some preferred embodiments of the method for separating polymer blends, the contacting in (c) or the maintaining T2 in (c.2) is carried out for a period of at least 0.1 hours, preferably in the range of 1 minute to 10 hours, more preferably in the range of 1 minute to 2 hours, more preferably in the range of 5 minutes to 1 hour, more preferably in the range of 5 to 30 minutes. As indicated above, T2 is a temperature in the corresponding range, i.e. in some embodiments, a constant temperature T2 is maintained, i.e. in these embodiments, "maintaining T2" also means maintaining about one temperature. In some embodiments, the temperature varies within the range of T2 during step (c) or during the maintenance of T2 in step (c.2), respectively.
[0061] Polyester+filling
[0062] In some preferred embodiments of the method for separating a polymer blend, wherein the polymer blend comprises, preferably consists of, a polyester and a filler, the method comprising:
[0063] (a) providing a polymer blend and providing a solvent comprising gamma-valerolactone;
[0064] (c) contacting the polymer blend provided in (a) with a solvent comprising γ-valerolactone at a temperature T2 of > 170°C, thereby obtaining a solvent enriched in dissolved polyester and optionally comprising at least a portion of filler compared to the solvent provided in (a) and a residue of the polymer blend depleted in polyester and comprising a portion of the filler.
[0065] In this context, a process comprising steps (a) and (c) or (c.1) to (c.3) means that there is no step (b) between (a) and (c). That is, (step) (c) follows immediately after step (a). Preferably, the process in this embodiment consists of steps (a) and (c), optionally wherein (c) is a combination of (c.1) and (c.2) and (c.3) as described above and also outlined in detail, and optionally with subsequent steps such as (d) and / or (e) and / or (f) and / or (g) and / or at least partly recycling the solvent to (c). In this embodiment, any heating from a temperature below T2 to T2 is carried out in a continuous manner, resulting in a linear increase in temperature for at least a portion of the heating time period, in particular at a heating rate in the range of 20K / h to 1000K / h, 25K / h to 900K / h, 30k / h to 800K / h, 40k / h to 700K / h, 60k / h to 600K / h.
[0066] In some preferred embodiments of the method for separating a polymer blend, wherein the polymer blend comprises, preferably consists of, a polyester and a filler, optionally with one or more colorants, the method comprises:
[0067] (a) providing a polymer blend and providing a solvent comprising gamma-valerolactone;
[0068] (c.1) contacting the polymer blend provided in (a) with a solvent comprising γ-valerolactone and having a temperature T1a ≤ T2 (T2 is a temperature > 170°C), thereby obtaining a mixture comprising the polymer blend and the solvent;
[0069] (c.2) heating the mixture obtained in (c.1) to a temperature T2> 170°C with continuous heating, wherein the heating from T1a to T2 is preferably carried out at a heating rate in the range of 20 K / h to 1000 K / h, 25 / K / h to 900 K / h, 30 k / h to 800 K / h, 40 k / h to 700 K / h, 60 k / h to 600 K / h, preferably maintaining T2, thereby obtaining a solvent enriched in dissolved polyester compared to the solvent provided in (a) and optionally comprising at least a portion of the filler; and optionally a residue of the polymer blend, which is depleted in polyester and comprises optionally the filler or a portion of the filler;
[0070] (c.3) optionally separating the solvent rich in dissolved polyester obtained in (c.2) from the residue of the polymer blend, wherein the separation is preferably carried out by heating filtration, more preferably by heating filtration at a temperature T3 in the range of T2 minus 20°C to T2 plus 20°C (T3=T2±20°C), more preferably at a temperature T3 in the range of T2 minus 10°C to T2 plus 10°C (T3=T2±10°C);
[0071] (d) optionally cooling the solvent obtained in (c.3) which is rich in dissolved polyester and optionally comprises at least a portion of filler compared to the solvent provided in (a) to a temperature below 170°C, preferably below 150°C, more preferably below 140°C, more preferably below 100°C, thereby obtaining precipitated polyester and a solvent which is poor in dissolved polyester and optionally comprises at least a portion of filler;
[0072] (e) optionally separating the precipitated polyester obtained in (d) from the solvent lean in dissolved polyester and optionally comprising at least a portion of the filler, thereby obtaining a precipitated polyester and a solvent lean in dissolved polyester and optionally comprising at least a portion of the filler.
[0073] As indicated above, step (c), especially in combination with step (d) as described above, leads to a polyester that is poor in colorant in the case of colored polyesters. The colorant may be found in the solvent rich in the dissolved polyester obtained in (c.2) and, after precipitation in (d), remains in the solvent poor in dissolved polyester and optionally containing at least a portion of the filler as obtained in (e). In some preferred embodiments, the residue of the polymer blend obtained in (c.3) still contains a residual amount of polyester. It is therefore preferred that in step (c.4), the residue of the polymer blend obtained in (c.3) containing a residual amount of polyester is contacted with a solvent containing γ-valerolactone, preferably at a temperature T3 as defined above, and subsequently filtered, preferably heated filtered at a temperature T3 as defined above, thereby obtaining a residue of a polymer blend that is further poor in polyester and contains a third polymer and optionally a filler or a portion of the filler; and a solvent containing a residual amount of polyester. Preferably, the contacting in (c.4) is carried out in such a way that, in particular in case heated filtration is used in (c.3), the residue of the polymer blend obtained in (c.3) remains on the filter and is contacted there with a solvent comprising γ-valerolactone, wherein the solvent containing the remaining amount of polyester obtained in (c.4) is separated due to the filtration. In some preferred embodiments, the solvent containing the remaining amount of polyester obtained in (c.4) is combined with the solvent enriched in dissolved polyester obtained in (c.3). In some preferred embodiments, the precipitated polyester amounts finally obtained from the solvent containing the remaining amount of polyester obtained in (c.4) and the solvent enriched in dissolved polyester obtained in (c.3) are combined, in case the further steps (d) and / or (e) and / or (f) and / or (g) as described above are carried out.
[0074] In some preferred embodiments, the method for separating a polymer blend comprises:
[0075] (f) optionally washing the precipitated polyester obtained in (e);
[0076] (g) drying the precipitated polyester obtained in (e) or the washed precipitated polyester obtained in (f).
[0077] The washing in optional step (f) is preferably carried out with a solvent selected from the group consisting of: methanol, ethanol, propanol, isopropanol, acetonitrile, ethyl acetate, acetone, water or a mixture of two or more of these solvents. In some embodiments, the washing in optional step (f) is preferably carried out with a solvent selected from the group consisting of: methanol, ethanol, propanol, isopropanol, acetonitrile, ethyl acetate, acetone, water, GVL or a mixture of two or more of these solvents. The drying in step (g) is preferably carried out under one or more conditions selected from the group consisting of: a pressure in the range of 1 to 1013 mbar; a temperature in the range of 50°C to 210°C, preferably in the range of 60°C to 180°C, more preferably in the range of 80°C to 150°C; a drying time in the range of 30 minutes to 24 hours; in an atmosphere comprising nitrogen, preferably in an atmosphere having at least 90 volume-%, more preferably 95 volume-%, more preferably at least 98 volume-% nitrogen. Drying is carried out by one or more methods selected from the group consisting of contact drying, convection drying and radiation drying.
[0078] Polyester + spandex + optional filling
[0079] In some preferred embodiments of the method for separating a polymer blend, wherein the polymer blend comprises, preferably consists of, a polyester, a second polymer, optionally a filler, and optionally one or more colorants, the method comprises:
[0080] (a) providing a polymer blend and providing a solvent comprising gamma-valerolactone;
[0081] (b) contacting the polymer blend with a solvent comprising gamma-valerolactone at a temperature T1 < 170°C, thereby obtaining a solvent rich in dissolved second polymer and a residue of the polymer blend depleted in said second polymer and comprising the polyester and optionally a filler.
[0082] In this context, a process comprising steps (a) and (b) means that there may be a step (c) after (b), which is used to separate the polyester from the filler if a filler is present in the polymer blend. Preferably, the process in this embodiment consists of steps (a) and (b), optionally wherein (b) is a combination of (b.1) and (b.2) as described above and optionally with a subsequent step, such as (c), more preferably (c.1), (c.2), (c.3), (d) and / or (e) and / or (f) and / or (g) and / or at least partly recycling the solvent to (b) and / or (c).
[0083] In some preferred embodiments of the method for separating a polymer blend, the polymer blend comprises, preferably consists of, a polyester, a second polymer, optionally a filler, and optionally one or more colorants, the method comprising:
[0084] (a) providing a polymer blend and providing a solvent comprising gamma-valerolactone;
[0085] (b) contacting the polymer blend with a solvent comprising γ-valerolactone at a temperature T1 < 170° C., thereby obtaining a solvent rich in dissolved second polymer and a residue of the polymer blend depleted in said second polymer and comprising the polyester and optionally a filler;
[0086] (c.1) contacting the residue of the polymer blend obtained in (b) with a solvent comprising γ-valerolactone and having a temperature T1a ≤ T2 (T2 being a temperature > 170°C), thereby obtaining a mixture comprising the polymer blend and the solvent;
[0087] (c.2) heating the mixture obtained in (c.1) to a temperature T2> 170°C with continuous heating, wherein the heating from T1a to T2 is preferably carried out at a heating rate in the range of 20 K / h to 1000 K / h, 25 / K / h to 900 K / h, 30 k / h to 800 K / h, 40 k / h to 700 K / h, 60 k / h to 600 K / h, preferably maintaining T2, thereby obtaining a solvent enriched in dissolved polyester compared to the solvent provided in (a) and optionally comprising at least a portion of the filler; and optionally a residue of the polymer blend, which is depleted in polyester and comprises a third polymer and optionally the filler or a portion of the filler;
[0088] (c.3) optionally separating the solvent rich in dissolved polyester obtained in (c.2) from the residue of the polymer blend, wherein the separation is preferably carried out by heating filtration, more preferably by heating filtration at a temperature T3 in the range of T2 minus 20°C to T2 plus 20°C (T3=T2±20°C), more preferably at a temperature T3 in the range of T2 minus 10°C to T2 plus 10°C (T3=T2±10°C);
[0089] (d) optionally cooling the solvent obtained in (c.3) which is rich in dissolved polyester and optionally comprises at least a portion of filler compared to the solvent provided in (a) to a temperature below 170°C, preferably below 150°C, more preferably below 140°C, more preferably below 100°C, thereby obtaining precipitated polyester and a solvent which is poor in dissolved polyester and optionally comprises at least a portion of filler;
[0090] (e) optionally separating the precipitated polyester obtained in (d) from the solvent lean in dissolved polyester and optionally comprising at least a portion of the filler, thereby obtaining a precipitated polyester and a solvent lean in dissolved polyester and optionally comprising at least a portion of the filler.
[0091] As indicated above, step (b) and also step (c), especially seen in combination with step (d) as described above, result in a polyester that is poor in colorant in the case of the use of a colored polyester. The colorant may be found in the solvent rich in the dissolved second polymer obtained in (b) and / or in the solvent rich in the dissolved polyester obtained in (c.2) and remains after precipitation in (d) in the solvent poor in dissolved polyester and optionally containing at least a portion of the filler as obtained in (e). In some preferred embodiments, the residue of the polymer blend obtained in (c.3) still contains a residual amount of polyester. It is therefore preferred that in step (c.4), the residue of the polymer blend obtained in (c.3) containing a residual amount of polyester is contacted with a solvent containing γ-valerolactone, preferably at a temperature T3 as defined above, followed by filtering, preferably heating filtering at a temperature T3 as defined above, thereby obtaining a residue of the polymer blend further poor in polyester and containing a third polymer and optionally a filler or a portion of the filler; and a solvent containing a residual amount of polyester. Preferably, the contacting in (c.4) is carried out in such a way that, in particular in case heated filtration is used in (c.3), the residue of the polymer blend obtained in (c.3) remains on the filter and is contacted there with a solvent comprising γ-valerolactone, wherein the solvent containing the remaining amount of polyester obtained in (c.4) is separated due to the filtration. In some preferred embodiments, the solvent containing the remaining amount of polyester obtained in (c.4) is combined with the solvent enriched in dissolved polyester obtained in (c.3). In some preferred embodiments, the precipitated polyester amounts finally obtained from the solvent containing the remaining amount of polyester obtained in (c.4) and the solvent enriched in dissolved polyester obtained in (c.3) are combined, in case the further steps (d) and / or (e) and / or (f) and / or (g) as described above are carried out.
[0092] In some preferred embodiments, the method for separating a polymer blend comprises:
[0093] (f) optionally washing the precipitated polyester obtained in (e);
[0094] (g) drying the precipitated polyester obtained in (e) or the washed precipitated polyester obtained in (f).
[0095] The washing in optional step (f) is preferably carried out with a solvent selected from the group consisting of: methanol, ethanol, propanol, isopropanol, acetonitrile, ethyl acetate, acetone, water or a mixture of two or more of these solvents. In some embodiments, the washing in optional step (f) is preferably carried out with a solvent selected from the group consisting of: methanol, ethanol, propanol, isopropanol, acetonitrile, ethyl acetate, acetone, water, GVL or a mixture of two or more of these solvents. The drying in step (g) is preferably carried out under one or more conditions selected from the group consisting of: a pressure in the range of 1 to 1013 mbar; a temperature in the range of 50°C to 210°C, preferably in the range of 60°C to 180°C, more preferably in the range of 80°C to 150°C; a drying time in the range of 30 minutes to 24 hours; in an atmosphere comprising nitrogen, preferably in an atmosphere having at least 90 volume-%, more preferably 95 volume-%, more preferably at least 98 volume-% nitrogen. Drying is carried out by one or more methods selected from the group consisting of contact drying, convection drying and radiation drying.
[0096] Polyester + PA and / or cotton + optional filling
[0097] In some preferred embodiments of the method for separating a polymer blend, wherein the polymer blend comprises, preferably consists of, a polyester, one or more third polymers and optionally a filler and optionally one or more colorants, the method comprises:
[0098] (a) providing a polymer blend and providing a solvent comprising gamma-valerolactone;
[0099] (c) contacting the polymer blend provided in (a) with a solvent comprising gamma-valerolactone at a temperature T2 of > 170°C, thereby obtaining a solvent enriched in dissolved polyester and optionally comprising at least a portion of filler compared to the solvent provided in (a) and a residue of the polymer blend depleted in polyester and comprising one or more third polymers and optionally filler or a portion of filler.
[0100] In some preferred embodiments of the method for separating a polymer blend, wherein the polymer blend comprises, preferably consists of, a polyester, one or more third polymers and optionally a filler and optionally one or more colorants, the method comprises:
[0101] (a) providing a polymer blend and providing a solvent comprising gamma-valerolactone;
[0102] (c.1) contacting the polymer blend provided in (a) with a solvent comprising γ-valerolactone and having a temperature T1a ≤ T2 (T2 is a temperature > 170°C), thereby obtaining a mixture comprising the polymer blend and the solvent;
[0103] (c.2) heating the mixture obtained in (c.1) to a temperature T2> 170°C with continuous heating, wherein the heating from T1a to T2 is preferably carried out at a heating rate in the range of 20 K / h to 1000 K / h, 25 / K / h to 900 K / h, 30 k / h to 800 K / h, 40 k / h to 700 K / h, 60 k / h to 600 K / h, preferably maintaining T2, thereby obtaining a solvent enriched in dissolved polyester compared to the solvent provided in (a) and optionally comprising at least a portion of filler; and optionally a residue of the polymer blend, which is depleted in polyester and comprises one or more third polymers and optionally filler or a portion of filler;
[0104] (c.3) optionally separating the solvent rich in dissolved polyester obtained in (c.2) from the residue of the polymer blend, wherein the separation is preferably carried out by heating filtration, more preferably by heating filtration at a temperature T3 in the range of T2 minus 20°C to T2 plus 20°C (T3=T2±20°C), more preferably at a temperature in the range of T2 minus 10°C to T2 plus 10°C (T3=T2±10°C);
[0105] (d) optionally cooling the solvent obtained in (c.3) which is enriched in dissolved polyester compared to the solvent provided in (a) to a temperature below 170°C, preferably below 150°C, more preferably below 140°C, more preferably below 100°C, thereby obtaining the precipitated polyester and a solvent which is depleted in dissolved polyester and optionally comprises the filler or a portion of the filler;
[0106] (e) optionally separating the precipitated polyester obtained in (d) from the solvent lean in dissolved polyester, thereby obtaining the precipitated polyester and the solvent lean in dissolved polyester and optionally comprising the filler or a portion of the filler.
[0107] In this context, a process comprising steps (a) and (c) or (c.1) to (c.3) means that there is no step (b) between (a) and (c). That is, (step) (c) follows immediately after step (a). Preferably, the process in this embodiment consists of steps (a) and (c), optionally wherein (c) is a combination of (c.1) and (c.2) and (c.3), and optionally with subsequent steps such as (d) and / or (e) and / or (f) and / or (g) and / or at least partially recycling the solvent to (c). In this embodiment, any heating from a temperature below T2 to T2 is performed in a continuous manner, resulting in a linear increase in temperature over the entire heating period, in particular at a heating rate in the range of 20 K / h to 1000 K / h, 25 / K / h to 900 K / h, 30 k / h to 800 K / h, 40 k / h to 700 K / h, 60 k / h to 600 K / h. In some preferred embodiments, the residue of the polymer blend obtained in (c.3) still contains a residual amount of polyester. Therefore, it is preferred that in step (c.4), the residue of the polymer blend obtained in (c.3) containing a residual amount of polyester is contacted with a solvent containing γ-valerolactone, preferably at a temperature T3 as defined above, and then filtered, preferably heated and filtered at a temperature T3 as defined above, thereby obtaining a residue of the polymer blend further depleted of polyester and containing a third polymer and optionally a filler or a portion of the filler; and a solvent containing a residual amount of polyester. Preferably, the contacting in (c.4) is carried out in such a way that, in particular in case heated filtration is used in (c.3), the residue of the polymer blend obtained in (c.3) remains on the filter and is contacted there with a solvent comprising γ-valerolactone, wherein the solvent containing the remaining amount of polyester obtained in (c.4) is separated due to the filtration. In some preferred embodiments, the solvent containing the remaining amount of polyester obtained in (c.4) is combined with the solvent enriched in dissolved polyester obtained in (c.3). In some preferred embodiments, the precipitated polyester amounts finally obtained from the solvent containing the remaining amount of polyester obtained in (c.4) and the solvent enriched in dissolved polyester obtained in (c.3) are combined, in case the further steps (d) and / or (e) and / or (f) and / or (g) as described above are carried out.
[0108] As indicated above, step (c), especially in combination with step (d) as described above, leads to a polyester poor in colorant in the case of a colored polyester. The colorant may be found in the solvent rich in the dissolved polyester obtained in (c.2) and, after precipitation in (d), remains in the solvent poor in dissolved polyester and optionally containing at least a portion of the filler as obtained in (e).
[0109] In some preferred embodiments, the method for separating a polymer blend comprises:
[0110] (f) optionally washing the precipitated polyester obtained in (e);
[0111] (g) drying the precipitated polyester obtained in (e) or the washed precipitated polyester obtained in (f).
[0112] The washing in optional step (f) is preferably carried out with a solvent selected from the group consisting of: methanol, ethanol, propanol, isopropanol, acetonitrile, ethyl acetate, acetone, water or a mixture of two or more of these solvents. In some embodiments, the washing in optional step (f) is preferably carried out with a solvent selected from the group consisting of: methanol, ethanol, propanol, isopropanol, acetonitrile, ethyl acetate, acetone, water, GVL or a mixture of two or more of these solvents. The drying in step (g) is preferably carried out under one or more conditions selected from the group consisting of: a pressure in the range of 1 to 1013 mbar; a temperature in the range of 50°C to 210°C, preferably in the range of 60°C to 180°C, more preferably in the range of 80°C to 150°C; a drying time in the range of 30 minutes to 24 hours; in an atmosphere comprising nitrogen, preferably in an atmosphere having at least 90 volume-%, more preferably 95 volume-%, more preferably at least 98 volume-% nitrogen. Drying is carried out by one or more methods selected from the group consisting of contact drying, convection drying and radiation drying.
[0113] Polyester + spandex + PA and / or cotton + optional filling
[0114] In some preferred embodiments of the method for separating a polymer blend, wherein the polymer blend comprises, preferably consists of, a polyester, a second polymer, one or more third polymers, and optionally a filler and optionally one or more colorants, the method comprises:
[0115] (a) providing a polymer blend and providing a solvent comprising gamma-valerolactone;
[0116] (b) contacting the polymer blend with a solvent comprising gamma-valerolactone at a temperature T1 < 170°C, thereby obtaining a solvent rich in dissolved second polymer and a residue of the polymer blend depleted in said second polymer and comprising the polyester, one or more third polymers and optionally a filler;
[0117] as well as
[0118] (c) contacting the residue of the polymer blend obtained in (b) with a solvent comprising gamma-valerolactone at a temperature T2> 170°C, thereby obtaining a solvent enriched in dissolved polyester and optionally comprising at least a portion of filler compared to the solvent provided in (a) and a residue of the polymer blend depleted in polyester and comprising one or more third polymers and optionally filler or a portion of filler.
[0119] In some preferred embodiments of the method for separating a polymer blend, wherein the polymer blend comprises, preferably consists of, a polyester, a second polymer, one or more third polymers, and optionally a filler and optionally one or more colorants, the method comprises:
[0120] (a) providing a polymer blend and providing a solvent comprising gamma-valerolactone;
[0121] (b) contacting the polymer blend with a solvent comprising gamma-valerolactone at a temperature T1 < 170°C, thereby obtaining a solvent rich in dissolved second polymer and a residue of the polymer blend depleted in said second polymer and comprising the polyester, one or more third polymers and optionally a filler;
[0122] (c.1) contacting the residue of the polymer blend obtained in (b) or (b.2) with a solvent comprising γ-valerolactone and having a temperature T1a ≤ T2 (T2 is a temperature > 170°C), thereby obtaining a mixture comprising the polymer blend and the solvent;
[0123] (c.2) heating the mixture obtained in (c.1) to a temperature T2> 170°C with continuous heating, wherein the heating from T1a to T2 is preferably carried out at a heating rate in the range of 20 K / h to 1000 K / h, 25 / K / h to 900 K / h, 30 k / h to 800 K / h, 40 k / h to 700 K / h, 60 k / h to 600 K / h, preferably maintaining T2, thereby obtaining a solvent enriched in dissolved polyester compared to the solvent provided in (a) and optionally comprising at least a portion of the filler; and optionally a residue of the polymer blend, which is depleted in polyester and comprises a third polymer and optionally the filler or a portion of the filler;
[0124] (c.3) optionally separating the solvent rich in the dissolved polyester obtained in (c.2) and optionally comprising at least a portion of the filler from the residue of the polymer blend, wherein the separation is preferably carried out by heating filtration, more preferably by heating filtration at a temperature T3 in the range of T2 minus 20°C to T2 plus 20°C (T3=T2±20°C), more preferably at a temperature in the range of T2 minus 10°C to T2 plus 10°C (T3=T2±10°C);
[0125] (d) optionally cooling the solvent obtained in (c.3) which is rich in dissolved polyester and optionally comprises at least a portion of filler compared to the solvent provided in (a) to a temperature below 170°C, preferably below 150°C, more preferably below 140°C, more preferably below 100°C, thereby obtaining precipitated polyester and a solvent which is poor in dissolved polyester and optionally comprises at least a portion of filler;
[0126] (e) optionally separating the precipitated polyester obtained in (d) from the solvent lean in dissolved polyester and optionally comprising at least a portion of the filler, thereby obtaining a precipitated polyester and a solvent lean in dissolved polyester and optionally comprising at least a portion of the filler.
[0127] As indicated above, step (b) and also step (c), especially seen in combination with step (d) as described above, result in a polyester that is poor in colorant in the case of the use of a colored polyester. The colorant may be found in the solvent rich in the dissolved second polymer obtained in (b) and / or in the solvent rich in the dissolved polyester obtained in (c.2) and remains after precipitation in (d) in the solvent poor in dissolved polyester and optionally containing at least a portion of the filler as obtained in (e). In some preferred embodiments, the residue of the polymer blend obtained in (c.3) still contains a residual amount of polyester. It is therefore preferred that in step (c.4), the residue of the polymer blend obtained in (c.3) containing a residual amount of polyester is contacted with a solvent containing γ-valerolactone, preferably at a temperature T3 as defined above, followed by filtering, preferably heating filtering at a temperature T3 as defined above, thereby obtaining a residue of the polymer blend further poor in polyester and containing a third polymer and optionally a filler or a portion of the filler; and a solvent containing a residual amount of polyester. Preferably, the contacting in (c.4) is carried out in such a way that, in particular in case heated filtration is used in (c.3), the residue of the polymer blend obtained in (c.3) remains on the filter and is contacted there with a solvent comprising γ-valerolactone, wherein the solvent containing the remaining amount of polyester obtained in (c.4) is separated due to the filtration. In some preferred embodiments, the solvent containing the remaining amount of polyester obtained in (c.4) is combined with the solvent enriched in dissolved polyester obtained in (c.3). In some preferred embodiments, the precipitated polyester amounts finally obtained from the solvent containing the remaining amount of polyester obtained in (c.4) and the solvent enriched in dissolved polyester obtained in (c.3) are combined, in case the further steps (d) and / or (e) and / or (f) and / or (g) as described above are carried out.
[0128] In some preferred embodiments of the method for separating polymer blends, at least one of (b) and (c), preferably both (b) and (c), is carried out in a continuous or discontinuous manner. According to this embodiment, step (b) and / or (c) is carried out under the flow of a solvent comprising γ-valerolactone (continuous mode) or in a stationary mode (discontinuous mode, batch mode). The contacting is carried out in one or more containers, for example, one or more containers are filled with a colored polymer blend material and a solvent comprising γ-valerolactone is guided through this container / these containers at a specific flow rate. A preferred example is a preferably stirred container cascade.
[0129] In some preferred embodiments of the method for separating the polymer blend, at least one of (b) and (c), preferably both (b) and (c) are in countercurrent mode. According to this embodiment, step (b) and / or (c) are performed in countercurrent mode. For example, if the contacting of step (b) is performed in a container, the solvent containing γ-valerolactone enters the container from one direction (side or top / bottom) and the colored polymer material enters the container from another, preferably opposite direction. In a preferred embodiment in which a vertically arranged container is used, the solvent containing γ-valerolactone enters the container from the bottom and the polymer material enters the container from the top.
[0130] Regardless of whether (b) and (c), preferably both (b) and (c) are carried out in a continuous manner or a discontinuous manner, and regardless of whether a co-current flow mode or a countercurrent flow mode is applied, it is preferred that the solvent is preheated to the corresponding temperature (T1, T1a, T2, T3) and then contacted with the polymer blend or the corresponding residue.
[0131] In some preferred embodiments of the method for separating polymer blends, at least one of (b) and (c), preferably both (b) and (c), is carried out under mechanical mixing, wherein the mechanical mixing preferably comprises one or more methods selected from stirring, blending and ultrasound.
[0132] In some preferred embodiments, the method for separating a polymer blend comprises:
[0133] (f) optionally washing the precipitated polyester obtained in (e);
[0134] (g) drying the precipitated polyester obtained in (e) or the washed precipitated polyester obtained in (f).
[0135] The washing in optional step (f) is preferably carried out with a solvent selected from the group consisting of: methanol, ethanol, propanol, isopropanol, acetonitrile, ethyl acetate, acetone, water or a mixture of two or more of these solvents. In some embodiments, the washing in optional step (f) is preferably carried out with a solvent selected from the group consisting of: methanol, ethanol, propanol, isopropanol, acetonitrile, ethyl acetate, acetone, water, GVL or a mixture of two or more of these solvents. The drying in step (g) is preferably carried out under one or more conditions selected from the group consisting of: a pressure in the range of 1 to 1013 mbar; a temperature in the range of 50°C to 210°C, preferably in the range of 60°C to 180°C, more preferably in the range of 80°C to 150°C; a drying time in the range of 30 minutes to 24 hours; in an atmosphere comprising nitrogen, preferably in an atmosphere having at least 90 volume-%, more preferably 95 volume-%, more preferably at least 98 volume-% nitrogen. Drying is carried out by one or more methods selected from the group consisting of contact drying, convection drying and radiation drying.
[0136] Solvent containing gamma-valerolactone
[0137] In some preferred embodiments of the method for separating a polymer blend, the solvent comprising γ-valerolactone comprises γ-valerolactone and optionally one or more solvents selected from the group consisting of water and a solvent having a log K in the range of -1.6 to +1.6. OW The organic solvent is preferably selected from the group consisting of water, C5 to C12 alkanes, aliphatic C1 to C10 alcohols, C3 to C10 ketones, C2 to C10 cyclic ketones, HO-[C1 to C10 alkyl-O-] n -H (wherein n is an integer in the range of 2 to 1000), C1 to C10 alkyl-O-C3 to C10 alkyl ether, C3 to C10 cyclic ether (optionally substituted with one or more C1 to C6 alkyl), C6 to C10 aromatic hydrocarbon (optionally substituted with one or more C1 to C6 alkyl), C2 to C10 aliphatic ester, C8 to C11 aromatic ester, C5 to C10 cyclic carboxylic acid ester (lactone), C3 to C12 amide, preferably R 1 R 2 NC(=O)-R 3 (where R 1 , R 2 are independently C1 to C4 alkyl and R 3Selected from the group consisting of C1 to C9 alkyl, C1 to C10 ester and C1 to C6 ether), C3 to C6 lactam (optionally substituted with one or more substituents selected from C1 to C6 alkyl, C1 to C6 ester and C1 to C6 ether) and C5 imidazolidine (optionally substituted with one or more C1 to C6 alkyl), C5 to C7 imidazolidinone (optionally substituted with one or more C1 to C6 alkyl).
[0138] Suitable solvents and the decimal logarithm of the octanol-water partition coefficient (log K OW ) is known to the skilled person. The octanol-water partition coefficient K of a given compound is OW Defined as the ratio of the chemical concentration of the compound in the octanol phase to the chemical concentration of the compound in the water phase in a two-phase system of 1-octanol and water at a temperature of 25°C (298K). Determine the octanol-water partition coefficient K for a given compound OW For example, the octanol-water partition coefficient K of a given compound is OW The shake flask method is used to determine the KOW values of various substances, which are known and easily found in, for example, the Dortmund database (DDB, see http: / / www.ddbst.com / ddb-search).
[0139] About suitable solvent, for example, aliphatic C1 to C10 alcohol is preferably C1 to C6 monohydric alcohol, more preferably one or more selected from the group consisting of methanol, ethanol and butanol. C3 to C10 ketone is preferably acetone or methyl ethyl ketone or a mixture of acetone and methyl ethyl ketone. C2 to C10 cyclic ketone is preferably cyclohexanone. C3 to C10 cyclic ethers optionally substituted by one or more C1 to C3 alkyls are preferably tetrahydrofuran or 2-methyltetrahydrofuran or a mixture of tetrahydrofuran and 2-methyltetrahydrofuran. C6 to C10 aromatic hydrocarbons optionally substituted by one or more C1 to C3 alkyls are preferably selected from the group consisting of benzene, toluene, ethylbenzene, xylene (ortho or para) and mesitylene. C1 to C10 esters are preferably selected from the group consisting of esters of C1 to C6 aliphatic monohydric alcohols and C2 to C5 aliphatic acids. C5 to C10 cyclic carboxylic acid esters (lactones) are preferably selected from one or more of the group consisting of δ-valerolactone, methylated γ-butyrolactone, ethylated γ-butyrolactone, propylated γ-butyrolactone and β-propiolactone. C3 to C6 lactams optionally substituted with one or more C1 to C3 alkyl groups are preferably selected from the group consisting of 2-pyrrolidone, 3-pyrrolidone, and a mixture of 2-pyrrolidone and 3-pyrrolidone, each optionally substituted with one or more C1 to C3 alkyl groups, preferably at the nitrogen atom, more preferably N-methyl-2-pyrrolidone. Imidazolidinone optionally substituted with one or more C1 to C3 alkyl groups is preferably 1,3-dimethyl-2-imidazolidinone.
[0140] In some preferred embodiments of the process for separating polymer blends, at least 1 wt-%, more preferably at least 5 wt-%, more preferably at least 10 wt-%, more preferably at least 20 wt-%, more preferably at least 30 wt-%, more preferably at least 40 wt-%, more preferably at least 50 wt-%, more preferably at least 80 wt-%, more preferably at least 90 wt-%, more preferably at least 95 wt-%, more preferably at least 99 wt-% of the solvent consists of γ-valerolactone.
[0141] In some preferred embodiments of the method for decolorization, the contacting in (b) and / or (c) is carried out with a mass-based ratio of solvent:polymer blend provided in (a) or the residue obtained in (b) in the range of 1:1 to 100:1, preferably in the range of 1:1 to 10:1.
[0142] In some preferred embodiments of the method for separating polymer blends, the same solvent containing γ-valerolactone is used in (b), (b.1), (b.2), (c), (c.1), (c.2), and (c.3).
[0143] Aspect 2 - Polyesters obtained or obtainable by the process
[0144] In a second aspect, the present invention relates to a polyester obtained or obtainable by the process according to the first aspect, preferably by (d) and / or (e) and / or (f) and / or (g) of the process according to the first aspect.
[0145] Aspect 3 - Purpose
[0146] In a third aspect, the present invention relates to the use of the precipitated polyester obtained or obtainable by (d) and / or (e) and / or (f) and / or (g) of the process according to the first aspect, or the polyester according to the second aspect for textile applications, fiber applications, packaging applications, plastic applications, automotive applications, electronic applications, preferably for the production of food packaging, beverage packaging, clothing, footwear, wires, cables, wherein preferably in the case where the polyester is selected from PBAT, PEF and PET, preferably PET, the precipitated polyester obtained or obtainable by (d) and / or (e) and / or (f) and / or (g) of the process according to the first aspect, or the polyester according to the second aspect, is used for textile applications, fiber applications, packaging applications, plastic applications, more preferably for the production of food packaging, beverage packaging, clothing and footwear; wherein in the case where the polyester is PBT, the precipitated polyester obtained or obtainable by (d) and / or (e) and / or (f) and / or (g) of the process according to the first aspect, or the polyester according to the second aspect, is used for textile applications, automotive applications, electronic applications, more preferably for the production of wires and / or cables.
[0147] Aspect 4 - Method for preparing a product
[0148] A fourth aspect of the present invention relates to a method for preparing a product, the method comprising
[0149] (I) providing the polyester of the second aspect;
[0150] (II) preparing textiles, fibers, packaging, plastics, automotive parts, electronic parts from the polyester provided in (I).
[0151] Preferably, especially if the polyester is selected from PBAT, PEF and PET, and more preferably PET, textiles, more preferably food packaging, beverage packaging, clothing and footwear are prepared in (II). Preferably, especially if the polyester is PBT, cables are prepared in (II).
[0152] The cable comprises polyester as described above and a conductor. A "conductor" is an electrical conductor or an optical waveguide. The electrical conductor is usually made of copper, and more rarely of aluminum or a suitable metal alloy. The optical waveguide comprises a quartz glass fiber.
[0153] The present invention is further illustrated by the following examples and combinations of the examples as indicated by the corresponding dependencies and back references. In particular, it should be noted that in each case where a series of embodiments is mentioned, for example in the context of a term such as "as any one of embodiments 1 to 4 ...", each embodiment in this series is intended to be disclosed explicitly to the skilled person, i.e. the wording of this term should be understood by the skilled person as being synonymous with "as any one of embodiments 1, 2, 3 and 4 ...".
[0154] 1. A method for separating a polymer blend, the polymer blend comprising
[0155] (i) polyester, and
[0156] (ii) one or more components selected from the group consisting of a second polymer, a third polymer, and a filler, wherein the second polymer and the third polymer are different from each other and from the polyester of (i);
[0157] The method includes:
[0158] (a) providing a polymer blend and providing a solvent comprising gamma-valerolactone;
[0159] (b) contacting the polymer blend with the solvent comprising γ-valerolactone at a temperature T1 of < 170° C., thereby obtaining a solvent rich in dissolved second polymer and a residue of the polymer blend depleted in said second polymer and comprising the polyester, optionally the third polymer and optionally the filler;
[0160] and / or
[0161] (c) contacting the polymer blend provided in (a) or the residue of the polymer blend obtained in (b) with a solvent comprising gamma-valerolactone at a temperature T2 of > 170°C, thereby obtaining a solvent enriched in dissolved polyester compared to the solvent provided in (a) and comprising optionally at least a portion of filler, and optionally a residue of the polymer blend depleted in polyester and comprising optionally a third polymer and optionally a filler or a portion of the filler.
[0162] 2. The method for separating a polymer blend as described in Example 1, wherein (b) comprises:
[0163] (b.1) contacting the polymer blend with the solvent comprising γ-valerolactone at a temperature T1 of < 170° C., thereby obtaining a solvent enriched in the dissolved second polymer and a residue of the polymer blend depleted in said second polymer and comprising the polyester, optionally the third polymer and optionally the filler;
[0164] (b.2) The solvent enriched in the dissolved second polymer and the residue of the polymer blend obtained in (b.1) are preferably separated by a physical separation method, thereby obtaining a separated solvent enriched in the dissolved second polymer compared to the solvent provided in (a) and a residue of the polymer blend depleted in the second polymer and containing the polyester.
[0165] 3. The method for separating a polymer blend as described in embodiment 1 or 2, wherein (c) comprises:
[0166] (c.1) contacting the polymer blend provided in (a) or the residue of the polymer blend obtained in (b) or (b.2) with a solvent comprising γ-valerolactone and having a temperature T1a ≤ T2 (T2 is a temperature > 170°C), thereby obtaining a mixture comprising the polymer blend and the solvent;
[0167] (c.2) heating the mixture obtained in (c.1) to a temperature T2> 170°C with continuous heating, wherein the heating from T1a to T2 is preferably carried out at a heating rate in the range of 20 K / h to 1000 K / h, 25 / K / h to 900 K / h, 30 K / h to 800 K / h, 40 K / h to 700 K / h, 60 K / h to 600 K / h, preferably maintaining T2, thereby obtaining a solvent enriched in dissolved polyester compared to the solvent provided in (a) and optionally comprising at least a portion of the filler; and optionally a residue of the polymer blend, which is depleted in polyester and comprises the third polymer and optionally the filler or a portion of the filler;
[0168] (c.3) optionally separating the solvent rich in dissolved polyester obtained in (c.2) from the residue of the polymer blend, wherein the separation is preferably carried out by heating filtration, more preferably by heating filtration at a temperature T3 in the range of T2 minus 20°C to T2 plus 20°C (T3=T2±20°C), more preferably at a temperature T3 in the range of T2 minus 10°C to T2 plus 10°C (T3=T2±10°C);
[0169] Wherein the method preferably further comprises:
[0170] (c.4) contacting the residue of the polymer blend obtained in (c.3) if it contains a remaining amount of the polyester with a solvent comprising γ-valerolactone, preferably at temperature T3 as defined above, and subsequently filtering, thereby obtaining a residue of the polymer blend further depleted in polyester and containing the third polymer and optionally the filler or a portion of the filler; and a solvent containing the remaining amount of the polyester.
[0171] 4. A method for separating a polymer blend as described in Example 3, wherein, if T1a is below 120°C, the heating is carried out as continuous heating, preferably at a heating rate in the range of 20 K / h to 1000 K / h, 25 / K / h to 900 K / h, 30k / h to 800 K / h, 40 K / h to 700 K / h, 60 K / h to 600 K / h, preferably the heating is carried out so that the mixture obtained in (c.1) is at a temperature range of 110°C-130°C for less than 60 minutes, preferably for less than 50 minutes, more preferably for less than 40 minutes, more preferably for less than 30 minutes, more preferably for less than 20 minutes, or if T1a is above 120°C, the heating is carried out as continuous heating, preferably at a heating rate in the range of 0.1 to 1000 K / h, more preferably in the range of 5 to 500 K / h, more preferably in the range of 25 to 300 K / h.
[0172] 5. A method for separating a polymer blend as described in any one of embodiments 1 to 4, comprising:
[0173] (d) cooling the solvent obtained in (c) or (c.3) which is enriched in dissolved polyester compared to the solvent provided in (a) and optionally comprises at least a portion of the filler to a temperature below 170°C, preferably below 150°C, more preferably below 140°C, more preferably below 100°C, thereby obtaining precipitated polyester and a solvent depleted in dissolved polyester and optionally comprising at least a portion of the filler.
[0174] 6. A method for separating a polymer blend as described in any one of embodiments 1 to 5, the method comprising
[0175] (e) separating the precipitated polyester obtained in (d) from the solvent lean in dissolved polyester, thereby obtaining precipitated polyester and the solvent lean in dissolved polyester and optionally comprising at least a portion of the filler;
[0176] Wherein preferably, the method for separating the polymer blend further comprises:
[0177] (f) optionally washing the precipitated polyester obtained in (e);
[0178] (g) drying the precipitated polyester obtained in (e) or the washed precipitated polyester obtained in (f).
[0179] 7. A method for separating a polymer blend as described in any one of Examples 1 to 5, which comprises, optionally after one or more post-treatment steps, at least partially recycling the separated solvent obtained in (b.2) and / or the separated solvent obtained in (e) to (b) and / or (c).
[0180] 8. A method for separating a polymer blend as described in any one of embodiments 1 to 7, wherein T1 is a temperature in the range of 110°C to <170°C, preferably a temperature in the range of 110°C to 165°C, more preferably a temperature in the range of 120°C to 150°C.
[0181] 9. A method for separating a polymer blend as described in any one of embodiments 1 to 8, wherein T2 is a temperature in the range of >170°C to 200°C, preferably a temperature in the range of 175°C to 190°C, more preferably a temperature in the range of 180°C to 190°C.
[0182] 10. The method for separating a polymer blend as described in any one of embodiments 1 to 9, wherein (a), (b), (c) and optionally (d) are carried out at a pressure in the range of 800 to 200,000 hPa.
[0183] 11. The method for separating polymer blends according to any one of embodiments 1 to 10, wherein the polyester according to (i) is based on at least one polyol and at least one organic dicarboxylic acid.
[0184] 12. A method for separating polymer blends as described in any one of Examples 1 to 11, wherein the at least one polyol of the polyester of (i) is at least one diol having 2 to 12 carbon atoms, preferably 2 to 6 carbon atoms, and more preferably, the at least one polyol contains at least 1,4-butanediol or 1,2-ethylene glycol.
[0185] 13. A method for separating polymer blends as described in any one of embodiments 1 to 12, wherein the at least one organic dicarboxylic acid of the polyester of (i) is selected from the group consisting of terephthalic acid, adipic acid, 2,5-furandicarboxylic acid and a mixture of two or more of these dicarboxylic acids, and is preferably at least terephthalic acid.
[0186] 14. A method for separating polymer blends as described in any one of embodiments 1 to 13, wherein the polyester according to (i) is selected from the group consisting of: polymers based on 1,4-butanediol and terephthalic acid (polybutylene terephthalate, PBT), polymers based on 1,2-ethylene glycol and terephthalic acid (polyethylene terephthalate, PET), copolymers of 1,4-butanediol, adipic acid and terephthalic acid (polybutylene adipate terephthalate, PBAT), polymers of 1,2-ethylene glycol and 2,5-furandicarboxylic acid (polyethylene furandicarboxylate, PEF) and mixtures of two or more of these (co)polymers, preferably the polyester according to (i) is a polymer based on 1,4-butanediol and terephthalic acid (PBT) or a polymer based on 1,2-ethylene glycol and terephthalic acid (PET).
[0187] 15. A method for separating a polymer blend as described in any one of Examples 1 to 14, wherein the second polymer is preferably selected from the group consisting of polyurethane (PU), polyethylene glycol (PEG), polytetrahydrofuran (pTHF), mixtures of these polymers and copolymers of these polymers, wherein the second polymer is more preferably a copolymer of PU and PEG and / or pTHF, more preferably spandex (a copolymer of PU and PEG or PU and pTHF).
[0188] 16. A method for separating polymer blends as described in any one of Examples 1 to 15, wherein the third polymer is preferably selected from the group consisting of polyolefins, preferably polyethylene (PE) and polypropylene (PP), polyamide (PA) and viscose fibers, natural polymers, preferably wool or cotton, mixtures of two or more of these polymers and copolymers of two or more of these polymers, wherein the third polymer is preferably selected from PA, wool, cotton, viscose fibers and mixtures of two or more of these polymers.
[0189] 17. A method for separating polymer blends as described in any one of Examples 1 to 16, wherein the filler is selected from the group consisting of: glass fiber, coal fiber, carbon black, inorganic salts (e.g., talc, sodium carbonate), adhesives, thickeners, defoamers, finishing agents (e.g., water repellents / oil repellents / fouling repellents, flame retardants, anti-wrinkle agents, biocides), binders, surfactants (e.g., softeners, scouring agents, antistatic agents), desizing agents, bleaching agents, oxidants, UV filters, emulsifiers, fixatives, detergent dispersants, and drive adjustment agents.
[0190] 18. A method for separating polymer blends as described in any of Examples 1 to 17, wherein the contacting in (b) or (b.1) is carried out for a period of at least 5 minutes, preferably in the range of 5 minutes to 10 hours, more preferably in the range of 5 minutes to 5 hours, more preferably in the range of 5 minutes to 4 hours.
[0191] 19. A method for separating polymer blends as described in any of Examples 1 to 18, wherein the contact in (c) or (c.1) is carried out for a period of at least 0.1 hour, preferably in the range of 1 minute to 10 hours, more preferably in the range of 1 minute to 2 hours, more preferably in the range of 5 minutes to 1 hour, and more preferably in the range of 5 to 30 minutes.
[0192] 20. The method for separating a polymer blend as described in any one of embodiments 1 to 19, wherein the polymer blend comprises, preferably consists of, a polyester and a filler, the method comprising:
[0193] (a) providing a polymer blend and providing a solvent comprising gamma-valerolactone;
[0194] (c) contacting the polymer blend provided in (a) with a solvent comprising γ-valerolactone at a temperature T2 of > 170°C, thereby obtaining a solvent enriched in the dissolved polyester and optionally comprising at least a portion of the filler compared to the solvent provided in (a) and a residue of the polymer blend depleted in the polyester and comprising the filler.
[0195] 21. A method for separating a polymer blend as described in any one of embodiment 20, wherein the polymer blend comprises polyester and filler, optionally with one or more colorants, preferably consisting thereof, the method comprising:
[0196] (a) providing a polymer blend and providing a solvent comprising gamma-valerolactone;
[0197] (c.1) contacting the polymer blend provided in (a) with a solvent comprising γ-valerolactone and having a temperature T1a ≤ T2 (T2 is a temperature > 170°C), thereby obtaining a mixture comprising the polymer blend and the solvent;
[0198] (c.2) heating the mixture obtained in (c.1) to a temperature T2> 170°C with continuous heating, wherein the heating from T1a to T2 is preferably carried out at a heating rate in the range of 20 K / h to 1000 K / h, 25 / K / h to 900 K / h, 30 k / h to 800 K / h, 40 k / h to 700 K / h, 60 k / h to 600 K / h, preferably maintaining T2, thereby obtaining a solvent enriched in dissolved polyester compared to the solvent provided in (a) and optionally comprising at least a portion of the filler; and optionally a residue of the polymer blend, which is depleted in polyester and comprises the third polymer and optionally the filler or a portion of the filler;
[0199] (c.3) optionally separating the solvent rich in dissolved polyester obtained in (c.2) from the residue of the polymer blend, wherein the separation is preferably carried out by heating filtration, more preferably by heating filtration at a temperature T3 in the range of T2 minus 20°C to T2 plus 20°C (T3=T2±20°C), more preferably at a temperature T3 in the range of T2 minus 10°C to T2 plus 10°C (T3=T2±10°C);
[0200] (d) optionally cooling the solvent obtained in (c.3) which is rich in dissolved polyester and optionally comprises at least a portion of filler compared to the solvent provided in (a) to a temperature below 170°C, preferably below 150°C, more preferably below 140°C, more preferably below 100°C, thereby obtaining precipitated polyester and a solvent which is poor in dissolved polyester and optionally comprises at least a portion of filler;
[0201] (e) optionally separating the precipitated polyester obtained in (d) from the solvent lean in dissolved polyester and optionally comprising at least a portion of the filler, thereby obtaining a precipitated polyester and the solvent lean in dissolved polyester and optionally comprising at least a portion of the filler;
[0202] Wherein preferably, the method for separating the polymer blend further comprises:
[0203] (f) optionally washing the precipitated polyester obtained in (e);
[0204] (g) drying the precipitated polyester obtained in (e) or the washed precipitated polyester obtained in (f); and / or
[0205] Wherein the method preferably further comprises:
[0206] (c.4) contacting the residue of the polymer blend obtained in (c.3) if it contains a remaining amount of the polyester with a solvent comprising γ-valerolactone, preferably at temperature T3 as defined above, and subsequently filtering, thereby obtaining a residue of the polymer blend further depleted in polyester and containing the third polymer and optionally the filler or a portion of the filler; and a solvent containing the remaining amount of the polyester.
[0207] 22. A method for separating a polymer blend as described in any one of embodiments 1 to 19, wherein the polymer blend comprises, preferably consists of, a polyester, a second polymer, optionally a filler, and optionally one or more colorants, the method comprising:
[0208] (a) providing a polymer blend and providing a solvent comprising gamma-valerolactone;
[0209] (b) contacting the polymer blend with the solvent comprising gamma-valerolactone at a temperature T1 < 170° C., thereby obtaining a solvent rich in dissolved second polymer and a residue of the polymer blend depleted in said second polymer and comprising the polyester and optionally the filler.
[0210] 23. The method for separating a polymer blend as described in embodiment 22, wherein the polymer blend comprises, preferably consists of, a polyester, a second polymer, optionally a filler, and optionally one or more colorants, the method comprising:
[0211] (a) providing a polymer blend and providing a solvent comprising gamma-valerolactone;
[0212] (b) contacting the polymer blend with the solvent comprising γ-valerolactone at a temperature T1 of < 170° C., thereby obtaining a solvent enriched in dissolved second polymer and a residue of the polymer blend depleted in said second polymer and comprising the polyester and optionally the filler;
[0213] (c.1) contacting the residue of the polymer blend obtained in (b) with a solvent comprising γ-valerolactone and having a temperature T1a ≤ T2 (T2 being a temperature > 170°C), thereby obtaining a mixture comprising the polymer blend and the solvent;
[0214] (c.2) heating the mixture obtained in (c.1) to a temperature T2> 170°C with continuous heating, wherein the heating from T1a to T2 is preferably carried out at a heating rate in the range of 20 K / h to 1000 K / h, 25 / K / h to 900 K / h, 30 k / h to 800 K / h, 40 k / h to 700 K / h, 60 k / h to 600 K / h, preferably maintaining T2, thereby obtaining a solvent enriched in dissolved polyester compared to the solvent provided in (a) and optionally comprising at least a portion of the filler; and optionally a residue of the polymer blend, which is depleted in polyester and comprises the third polymer and optionally the filler or a portion of the filler;
[0215] (c.3) optionally separating the solvent rich in dissolved polyester obtained in (c.2) from the residue of the polymer blend, wherein the separation is preferably carried out by heating filtration, more preferably by heating filtration at a temperature T3 in the range of T2 minus 20°C to T2 plus 20°C (T3=T2±20°C), more preferably at a temperature T3 in the range of T2 minus 10°C to T2 plus 10°C (T3=T2±10°C);
[0216] (d) optionally cooling the solvent obtained in (c.3) which is rich in dissolved polyester and optionally comprises at least a portion of filler compared to the solvent provided in (a) to a temperature below 170°C, preferably below 150°C, more preferably below 140°C, more preferably below 100°C, thereby obtaining precipitated polyester and a solvent which is poor in dissolved polyester and optionally comprises at least a portion of filler;
[0217] (e) optionally separating the precipitated polyester obtained in (d) from the solvent lean in dissolved polyester and optionally comprising at least a portion of the filler, thereby obtaining a precipitated polyester and the solvent lean in dissolved polyester and optionally comprising at least a portion of the filler;
[0218] Wherein preferably, the method for separating the polymer blend further comprises:
[0219] (f) optionally washing the precipitated polyester obtained in (e);
[0220] (g) drying the precipitated polyester obtained in (e) or the washed precipitated polyester obtained in (f); and / or
[0221] Wherein the method preferably further comprises:
[0222] (c.4) contacting the residue of the polymer blend obtained in (c.3) if it contains a remaining amount of the polyester with a solvent comprising γ-valerolactone, preferably at temperature T3 as defined above, and subsequently filtering, thereby obtaining a residue of the polymer blend further depleted in polyester and containing the third polymer and optionally the filler or a portion of the filler; and a solvent containing the remaining amount of the polyester.
[0223] 24. A method for separating a polymer blend as described in any one of embodiments 1 to 19, wherein the polymer blend comprises, preferably consists of, a polyester, one or more third polymers and optionally a filler and optionally one or more colorants, the method comprising:
[0224] (a) providing a polymer blend and providing a solvent comprising gamma-valerolactone;
[0225] (c) contacting the polymer blend provided in (a) with a solvent comprising gamma-valerolactone at a temperature T2 of > 170°C, thereby obtaining a solvent enriched in dissolved polyester and optionally comprising at least a portion of filler compared to the solvent provided in (a) and a residue of the polymer blend depleted in polyester and comprising one or more third polymers and optionally filler or a portion of filler.
[0226] 25. A method for separating a polymer blend as described in embodiment 24, wherein the polymer blend comprises, preferably consists of, a polyester, one or more third polymers and optionally a filler and optionally one or more colorants, the method comprising:
[0227] (a) providing a polymer blend and providing a solvent comprising gamma-valerolactone;
[0228] (c.1) contacting the polymer blend provided in (a) with a solvent comprising γ-valerolactone and having a temperature T1a ≤ T2 (T2 is a temperature > 170°C), thereby obtaining a mixture comprising the polymer blend and the solvent;
[0229] (c.2) heating the mixture obtained in (c.1) to a temperature T2> 170°C with continuous heating, wherein the heating from T1a to T2 is preferably carried out at a heating rate in the range of 20 K / h to 1000 K / h, 25 / K / h to 900 K / h, 30 k / h to 800 K / h, 40 k / h to 700 K / h, 60 k / h to 600 K / h, preferably maintaining T2, thereby obtaining a solvent enriched in dissolved polyester compared to the solvent provided in (a) and optionally comprising at least a portion of the filler; and optionally a residue of the polymer blend, which is depleted in polyester and comprises the one or more third polymers and optionally the filler or a portion of the filler;
[0230] (c.3) optionally separating the solvent rich in dissolved polyester obtained in (c.2) from the residue of the polymer blend, wherein the separation is preferably carried out by heating filtration, more preferably by heating filtration at a temperature T3 in the range of T2 minus 20°C to T2 plus 20°C (T3=T2±20°C), more preferably at a temperature in the range of T2 minus 10°C to T2 plus 10°C (T3=T2±10°C);
[0231] (d) optionally cooling the solvent obtained in (c.3) which is enriched in dissolved polyester compared to the solvent provided in (a) to a temperature below 170°C, preferably below 150°C, more preferably below 140°C, more preferably below 100°C, thereby obtaining the precipitated polyester and a solvent which is depleted in dissolved polyester and optionally comprises the filler or a portion of the filler;
[0232] (e) optionally separating the precipitated polyester obtained in (d) from the solvent depleted in dissolved polyester, thereby obtaining precipitated polyester and the solvent depleted in dissolved polyester and optionally comprising the filler or a portion of the filler;
[0233] Wherein preferably, the method for separating the polymer blend further comprises:
[0234] (f) optionally washing the precipitated polyester obtained in (e);
[0235] (g) drying the precipitated polyester obtained in (e) or the washed precipitated polyester obtained in (f); and / or
[0236] Wherein the method preferably further comprises:
[0237] (c.4) contacting the residue of the polymer blend obtained in (c.3) if it contains a remaining amount of the polyester with a solvent comprising γ-valerolactone, preferably at temperature T3 as defined above, and subsequently filtering, thereby obtaining a residue of the polymer blend further depleted in polyester and containing the third polymer and optionally the filler or a portion of the filler; and a solvent containing the remaining amount of the polyester.
[0238] 26. A method for separating a polymer blend as described in any one of embodiments 1 to 19, wherein the polymer blend comprises, preferably consists of, a polyester, a second polymer, one or more third polymers, and optionally a filler and optionally one or more colorants, the method comprising:
[0239] (a) providing a polymer blend and providing a solvent comprising gamma-valerolactone;
[0240] (b) contacting the polymer blend with the solvent comprising γ-valerolactone at a temperature T1 of < 170° C., thereby obtaining a solvent rich in dissolved second polymer and a residue of the polymer blend depleted in said second polymer and comprising the polyester, the one or more third polymers and optionally the filler;
[0241] as well as
[0242] (c) contacting the residue of the polymer blend obtained in (b) with a solvent comprising gamma-valerolactone at a temperature T2> 170°C, thereby obtaining a solvent enriched in dissolved polyester and optionally comprising at least a portion of filler compared to the solvent provided in (a) and a residue of the polymer blend depleted in polyester and comprising one or more third polymers and optionally filler or a portion of filler.
[0243] 27. A method for separating a polymer blend as described in embodiment 26, wherein the polymer blend comprises, preferably consists of, a polyester, a second polymer, one or more third polymers, and optionally a filler and optionally one or more colorants, the method comprising:
[0244] (a) providing a polymer blend and providing a solvent comprising gamma-valerolactone;
[0245] (b) contacting the polymer blend with the solvent comprising γ-valerolactone at a temperature T1 of < 170° C., thereby obtaining a solvent rich in dissolved second polymer and a residue of the polymer blend depleted in said second polymer and comprising the polyester, the one or more third polymers and optionally the filler;
[0246] (c.1) contacting the residue of the polymer blend obtained in (b) or (b.2) with a solvent comprising γ-valerolactone and having a temperature T1a ≤ T2 (T2 is a temperature > 170°C), thereby obtaining a mixture comprising the polymer blend and the solvent;
[0247] (c.2) heating the mixture obtained in (c.1) to a temperature T2> 170°C with continuous heating, wherein the heating from T1a to T2 is preferably carried out at a heating rate in the range of 20 K / h to 1000 K / h, 25 / K / h to 900 K / h, 30 k / h to 800 K / h, 40 k / h to 700 K / h, 60 k / h to 600 K / h, preferably maintaining T2, thereby obtaining a solvent enriched in dissolved polyester compared to the solvent provided in (a) and optionally comprising at least a portion of the filler; and optionally a residue of the polymer blend, which is depleted in polyester and comprises the third polymer and optionally the filler or a portion of the filler;
[0248] (c.3) optionally separating the solvent rich in the dissolved polyester obtained in (c.2) and optionally containing at least a portion of the filler from the residue of the polymer blend, wherein the separation is preferably carried out by heating filtration, more preferably by heating filtration at a temperature T3 in the range of T2 minus 20°C to T2 plus 20°C (T3 = T2 ± 20°C), more preferably in the range of T2 minus 10°C to T2 plus 10°C (T3 = T2 ± 10°C).
[0249] (d) optionally cooling the solvent obtained in (c.3) which is rich in dissolved polyester and optionally comprises at least a portion of filler compared to the solvent provided in (a) to a temperature below 170°C, preferably below 150°C, more preferably below 140°C, more preferably below 100°C, thereby obtaining precipitated polyester and a solvent which is poor in dissolved polyester and optionally comprises at least a portion of filler;
[0250] (e) optionally separating the precipitated polyester obtained in (d) from the solvent lean in dissolved polyester and optionally comprising at least a portion of the filler, thereby obtaining a precipitated polyester and the solvent lean in dissolved polyester and optionally comprising at least a portion of the filler;
[0251] Wherein preferably, the method for separating the polymer blend further comprises:
[0252] (f) optionally washing the precipitated polyester obtained in (e);
[0253] (g) drying the precipitated polyester obtained in (e) or the washed precipitated polyester obtained in (f); and / or
[0254] Wherein the method preferably further comprises:
[0255] (c.4) contacting the residue of the polymer blend obtained in (c.3) if it contains a remaining amount of the polyester with a solvent comprising γ-valerolactone, preferably at temperature T3 as defined above, and subsequently filtering, thereby obtaining a residue of the polymer blend further depleted in polyester and containing the third polymer and optionally the filler or a portion of the filler; and a solvent containing the remaining amount of the polyester.
[0256] 28. The method for separating a polymer blend as described in any one of embodiments 1 to 27, wherein the solvent comprising γ-valerolactone comprises γ-valerolactone and optionally one or more solvents selected from the group consisting of water and a solvent having a log K in the range of -1.6 to +1.6. OW The organic solvent is preferably selected from the group consisting of water, C5 to C12 alkanes, aliphatic C1 to C10 alcohols, C3 to C10 ketones, C2 to C10 cyclic ketones, HO-[C1 to C10 alkyl-O-] n -H (wherein n is an integer in the range of 2 to 1000), C1 to C10 alkyl-O-C3 to C10 alkyl ether, C3 to C10 cyclic ether (optionally substituted with one or more C1 to C6 alkyl), C6 to C10 aromatic hydrocarbon (optionally substituted with one or more C1 to C6 alkyl), C2 to C10 aliphatic ester, C8 to C11 aromatic ester, C5 to C10 cyclic carboxylic acid ester (lactone), C3 to C12 amide, preferably R 1 R 2 NC(=O)-R 3 (where R 1 , R 2 are independently C1 to C4 alkyl and R 3 Selected from the group consisting of C1 to C9 alkyl, C1 to C10 ester and C1 to C6 ether), C3 to C6 lactam (optionally substituted with one or more substituents selected from C1 to C6 alkyl, C1 to C6 ester and C1 to C6 ether) and C5 imidazolidine (optionally substituted with one or more C1 to C6 alkyl), C5 to C7 imidazolidinone (optionally substituted with one or more C1 to C6 alkyl).
[0257] 29. A method for separating polymer blends as described in any of Examples 1 to 28, wherein at least 1 wt-%, more preferably at least 5 wt-%, more preferably at least 10 wt-%, more preferably at least 20 wt-%, more preferably at least 30 wt-%, more preferably at least 40 wt-%, more preferably at least 50 wt-%, more preferably at least 80 wt-%, more preferably at least 90 wt-%, more preferably at least 95 wt-%, more preferably at least 99 wt-% of the solvent consists of γ-valerolactone.
[0258] 30. A method for separating polymer blends as described in any one of Examples 1 to 29, wherein the same solvent containing γ-valerolactone is used in (b), (b.1), (b.2), (c), (c.1), (c.2), and (c.3).
[0259] 31. A polyester obtained or obtainable by the process according to any one of embodiments 1 to 30, preferably by (d) and / or (e) and / or (f) and / or (g) according to any one of embodiments 5, 6, 21, 23, 25 and 27.
[0260] 32. Use of the polyester obtained or obtainable from (d) and / or (e) and / or (f) and / or (g) according to any one of embodiments 5, 6, 21, 23, 25 and 27 or the precipitated polyester according to embodiment 31 for textile applications, fiber applications, packaging applications, plastic applications, automotive applications, electronic applications, preferably for the production of food packaging, beverage packaging, clothing, footwear, wires, cables, wherein preferably in the case where the polyester is selected from PBAT, PEF and PET, preferably PET, the polyester obtained or obtainable from (d) and / or (e) and / or (f) and / or (g) according to any one of embodiments 5, 6, 21, 23, 25 and 27 or the precipitated polyester according to embodiment 31 is selected from the group consisting of PBAT, PEF and PET, preferably PET. ) and / or (f) and / or (g) obtained or obtainable precipitated polyester or the polyester according to embodiment 31 is used in textile applications, fiber applications, packaging applications, plastic applications, more preferably in the production of food packaging, beverage packaging, clothing and footwear; wherein when the polyester is PBT, the precipitated polyester obtained or obtainable by (d) and / or (e) and / or (f) and / or (g) according to any one of embodiments 5, 6, 21, 23, 25 and 27 or the polyester according to embodiment 31 is used in textile applications, automotive applications, electronic applications, more preferably in the production of wires and / or cables.
[0261] 33. A method for preparing a product, the method comprising
[0262] (I) providing a polyester as described in Example 31;
[0263] (II) preparing textiles, fibers, packaging, plastics, automotive parts, electronic parts from the polyester provided in (I).
[0264] The present invention is further illustrated by the following Reference Examples, Comparative Examples and Examples.
[0265] Examples
[0266] method
[0267] XRF screening analysis (before / after treatment)
[0268] XRF screening is performed directly on the sample material without preparation. The sample material is weighed into the measuring cuvette and the semi-quantitative program on the WD-XRF instrument is started after the cuvette is inserted. The screening method is used as a rough clustering method, assigning elements to concentration ranges.
[0269] Analysis of Ca, Fe, K, Sb and Ti (before treatment)
[0270] Samples were prepared using an automated acid digestion procedure using a mixture of different mineral acids. The analytes in the obtained solutions were determined by inductively coupled plasma-optical emission spectroscopy (ICP-OES). Sample preparation and analysis were performed in duplicate. The reported results are the average of two individual analytical results.
[0271] Analysis of Si (before treatment)
[0272] After incineration of the sample in a muffle furnace, the sample was prepared using the flux digestion method. The Si in the obtained solution was determined by inductively coupled plasma-optical emission spectroscopy (ICP-OES). Sample preparation and analysis were performed in duplicate. The reported results are the average of two individual analytical results.
[0273] Analysis of Cl and S (before treatment)
[0274] Chlorine (calculated from the sum of Cl, Br, I)
[0275] The sample is weighed into a quartz crucible and burned in oxygen with nitrogen as carrier gas. The combustion gases are scavenged from byproducts in concentrated sulfuric acid and then transferred to a coulometric cell. Detection is performed by coulometric method.
[0276] Analysis of Si (for PBT samples)
[0277] After incineration of the sample in a muffle furnace, the sample was prepared using an automated flux digestion procedure. The Si in the obtained solution was determined by inductively coupled plasma-optical emission spectroscopy (ICP-OES). Sample preparation and analysis were performed in duplicate. The reported results are the average of two individual analytical results.
[0278] Intrinsic viscosity:
[0279] General
[0280] To determine the intrinsic viscosity, a concentration series of the polymer in a specific solvent (here o-chlorophenol) is prepared. The concentration range of the polymer used for analyzing the intrinsic viscosity is determined by the relative viscosity and should be in the range between 1.2 and 2.5 [Kulicke 2003].
[0281] The value of intrinsic viscosity is the y-intercept of a plot of reduced viscosity as a function of concentration, obtained by extrapolating a linear fit to a concentration of zero.
[0282] Sample preparation and measurement
[0283] A concentration series is prepared which typically covers 3 to 7 different concentrations. The concentration range is determined by the range of relative viscosities (see above).
[0284] The polymers were dissolved in o-chlorophenol by stirring overnight.Before use, each polymer solution was filtered on a metal filter with a mesh size of 0,077 mm.
[0285] The measurements were carried out at 25° C. in a Lauda apparatus (Lauda Pro Line 24) using an effluent viscometer of the Ubbelohde capillary type (Micro-Ubbelohde II, k=0,10326, application number: 720-13-0573). The temperature was controlled by a thermostat, which kept the temperature constant within a range of + / - 0.01° C.
[0286] The viscosity of different polymer solutions is determined by measuring the time it takes for a sample to flow through a capillary of defined length and radius under the influence of gravity. To determine the relative viscosity, a reference liquid, here o-chlorophenol, is measured under the same conditions. The measured run time is calibrated according to Hagenbach (W.-M. Kulicke and C. Clasen, Viscosimetry of Polymers and Polyelectrolytes, Springer (2003)).
[0287] Hazen Color Index:
[0288] The Hazen color index (APHA color number) is determined according to DIN EN ISO 6271:2016-05 (Pt / Co, APHA, ASTM D1209, D5386).
[0289] CIE-LAB:
[0290] The determination of L*a*b* values is to measure the sample using an integrating sphere and obtain UV / VIS reflectance spectra (with a wavelength region of 400-700 nm). The data of these spectra are analyzed by the software OptLab-SPX using a 2° standard observer and standard light type C. The OptLab-SPX software calculates L*a*b* values based on DIN 5033 and DIN EN ISO 11664-1.6 from 2007-2014.
[0291] GC Area %:
[0292] The samples are analyzed by gas chromatography (GC), wherein the method detects the individual components based on their retention time in the sample. The concentration of the individual components in the sample is expressed as its percentage peak area as GC-area %.
[0293] GPC (Gel Permeation Chromatography):
[0294] Sample preparation:
[0295] 7.5 mg of sample were dissolved in 5 ml of eluent (HFIP + 0.05 wt-% potassium trifluoroacetate) overnight. All sample solutions were filtered through Millipore Millex FG (0.2 μm) before injection. The sealed sample vials were placed in the autosampler.
[0296] Experimental conditions:
[0297] Agilent 1100HPLC system was used, which consisted of an isocratic pump, a vacuum degasser, an autosampler and a column oven (40°C). In addition, an Agilent system, a differential refractive index (DRI) and a variable ultraviolet (UVW) detector were included as detectors. Data acquisition and data processing of conventional SEC data were performed by WinGPC Unichrom of PSS (Polymer Standard Service). A combination of Agilent's PL-HFIP guard column (7.5x 50mm) and 2 PL-HFIP gel columns (7.5x300mm, 9μ) were placed in series. As eluent, hexafluoroisopropanol+0.05 wt-% potassium trifluoroacetate was used at a flow rate of 1ml / min. 50μl of each sample solution was injected. Calibration was obtained by PMMA standards (Polymer Standard Service) with a narrow molar mass distribution in the molar mass range of M=800 to M=2.200.000g / mol. Molar masses outside this range were extrapolated.
[0298] Quantification 1 H NMR spectroscopy (q 1 H NMR):
[0299] By quantitative 1 The contents of polyethylene terephthalate (PET) and gamma-valerolactone (GVL) in the samples were determined by H-NMR spectroscopy. All NMR spectra were recorded at T = 298.2 K on a Bruker Avance III 400 spectrometer, which is suitable for 1 H was operated at 400.33 MHz. The spectrometer was equipped with a 5 mm z-gradient broadband observation smart probe. Chemical shifts were referenced to tetramethylsilane (TMS, δ(TMS)=0 ppm). 1H 1D spectra were recorded under quantitative conditions using the zg30 pulse program with 128k data point sampling, with the relaxation delay D1 selected as 40 seconds for the solvent chloroform-d1 (CDCl3) or 120 seconds for the solvent sulfuric acid-d2 (D2SO4). Eight transients were included for each spectrum. For processing in Bruker TopSpin 4.0.9 software, 64k data points were used, with an exponential window function with a line broadening of 0.3 Hz. An automatic baseline correction with a polynomial of 5 was performed, with phase correction and integration performed manually by the user.
[0300] For the determination of PET, samples were prepared by accurately weighing the internal standard 1,1,2,2-tetrachloroethane (TCE) and the analyte in appropriate vials (Mettler-Toledo XP205DR analytical balance) and subsequently dissolving in 2 mL of a 2:1 mixture of CDCl3 and trifluoroacetic acid (TFA) (with a trace amount of TMS as an internal reference).
[0301] For the determination of PET in cotton-containing textile samples, samples were prepared by accurately weighing the internal standard dimethylmalonic acid (DMMS) and the analyte in appropriate vials (Mettler Toledo XP205DR analytical balance) and subsequently dissolving in 2 ml D2SO4.
[0302] In all cases, samples were transferred to 5 mm NMR tubes for measurement. Deuterated solvents TFA and CDCl3 and TMS were purchased from Euriso-Top Ltd. D2SO4, TCE and DMMS (certified internal standard) were purchased from Sigma-Aldrich. All solvents and internal standards were used as received.
[0303] The content of the test item was calculated by using the following equation:
[0304]
[0305] In this equation: w = mass fraction of analyte in sample [g / 100g], I k = peak intensity of the analyte, I St = Peak intensity of the standard, E P = sample mass [g], E St = mass of standard sample [g], A K = proton / molecule of analyte, A St = proton / molecule of standard, M K = molecular weight of the analyte [g / mol], M St = molecular weight of the standard [g / mol], and R St =Purity of standard product [g / 100g].
[0306] For quantification, three determinations were performed.
[0307] The evaluation of PET in the pure PET sample was performed by using 2 protons / molecule of the internal standard TCE (at about 5.9 ppm) and 4 selected protons / molecule of the analyte PET (at about 8.1 ppm).
[0308] Evaluation of PET in cotton-containing textile samples was performed by using 6 protons per molecule of the internal standard DMMS (at approximately 1.80 ppm) and 4 protons per molecule of the analyte PET (at approximately 8.4 ppm).
[0309] Chemicals
[0310]
[0311] Reference Example 1a: PET Recycling with Gradual Heating (Comparative Procedure)
[0312] Colored polymer PET material (in any color) is cut / chopped into pieces and placed in a reaction vessel (e.g., flask, tube, reaction vessel). Degassed γ-valerolactone (GVL) (mass ratio of GVL: polymer material is 1:1 to 100:1, preferably 1:1-10:1) is added, and the mixture is first heated to 120°C for 5-60min at 1013 mbar, then heated to 170°C for 1-30min, then heated to 180°C for 1-30min and finally heated to 190°C for 1-30min, so that a solution is obtained, wherein PET is completely dissolved when visually inspected. Subsequently, the solution is filtered (e.g., heated pressure filtration). As the filtrate begins to cool, polyethylene terephthalate (PET) precipitates. The precipitate is filtered and washed with a small amount of GVL to obtain a color-poor PET powder. For easy removal of GVL and a faster drying process of the recovered color-poor PET powder, a small amount of acetone is optionally used in the second washing step. The solid thus obtained is dried (for example in a vacuum compartment dryer).
[0313] Reference Example 1b: PET Recycling with Continuous Heating
[0314] Colored polymer PET material (in any color) is cut / chopped into pieces and placed in a reaction vessel (e.g., flask, tube, reaction vessel). Degassed GVL (GVL: polymer material mass ratio is 1: 1 to 100: 1, preferably 1: 1-10: 1) is added, and the mixture is heated to 185 ° C at 1013 mbar by using a suitable heating system (e.g., oil bath, heating block, small factory container) so that a solution is obtained, wherein PET is completely dissolved during visual inspection. After 1-30 min, the mixture is filtered (e.g., heated pressure filtration), wherein the insoluble part of the filler (if present) that is insoluble in GVL is retained on the filter. As the filtrate begins to cool, PET precipitates. The precipitate is filtered, wherein the soluble part of the filler (if present) (soluble in GVL but not precipitated during cooling) is removed together with the filtrate. The precipitated PET is washed with a small amount of GVL. For easy removal of GVL and a faster drying process of the recovered color-poor PET powder, a small amount of acetone is optionally used in the second washing step. The solid thus obtained is dried (for example in a vacuum compartment dryer).
[0315] Reference Example 2: Separation of PET from cotton and / or PA
[0316] The colored polymer material (in any color) comprising PET and cotton and / or PA is cut / chopped into pieces and placed in a reaction vessel (e.g., flask, tube, reaction vessel). Degassed GVL (GVL: polymer material mass ratio is 1:1 to 100:1, preferably 1:1-10:1) is added, and the mixture is heated to 185°C at 1013 mbar by using a suitable heating system (e.g., oil bath, heating block, small factory container) so that a mixture is obtained in which PET is completely dissolved and the soluble part of the filler (if present) is dissolved, but the solid particles are retained in the mixture. After 5-30 min, the mixture is filtered (e.g., heated pressure filtration) to obtain a filter cake with undissolved polymer material (insoluble part of cotton and / or PA and filler (if present)) and a filtrate with PET. The filter cake is optionally further washed with a small amount of hot GVL. As the filtrate begins to cool, PET precipitates. The precipitate is filtered, wherein a portion of the filler (if present) (soluble in the GVL but not precipitated during the cooling process) is removed together with the filtrate. The precipitated PET is washed with a small amount of GVL. For an easier removal of the GVL and a faster drying process of the recovered color-poor PET powder, a small amount of acetone is optionally used in a second washing step. The filter cake is also washed with a small amount of GVL. For an easier removal of the GVL and a faster drying process of the cotton or PA flakes, a small amount of acetone is optionally used in a second washing step. The polymer material thus obtained (recovered PET and undissolved cotton or PA) is dried (for example in a vacuum compartment dryer).
[0317] Reference Example 3: Separation of spandex and PET
[0318] The colored polymer material (in any color) containing PET and spandex is cut / chopped into pieces and placed in a reaction vessel (e.g., flask, tube, reaction vessel). Degassed GVL (GVL: polymer material mass ratio is 1: 1 to 100: 1, preferably 1: 1-10: 1) is added, and the mixture is heated to 110 ° C-170 ° C at 1013 mbar by using a suitable heating system (e.g., oil bath, heating block, small factory container) so that a mixture is obtained, wherein the spandex is completely dissolved and the PET remains undissolved. A portion of the filler (if present) is also dissolved. After 0.1-4h, the mixture is filtered to obtain a GVL rich in spandex and colorant and a decolorized PET sheet, and the polymer material sheet is washed with a small amount of GVL. In order to easily remove the faster drying process of the decolorized PET sheet without GVL and spandex, a small amount of acetone is optionally used in the second washing step. The polymer material sheet thus obtained is dried (e.g., in a vacuum compartment dryer).
[0319] For reference example 1a and all reference examples 1b-4 the following applies:
[0320] To recycle the used solvent GVL, the filtrate is optionally distilled (50° C.-200° C., 2 hPa to ambient pressure, preferably 70° C.-110° C., 5-30 hPa) to obtain distilled GVL with a purity according to GC>99% area%. For the GLV, the Hazen color index is determined before treatment and after distillation. Distilled GVL as well as non-distilled GVL can be reused under the same conditions as fresh GVL.
[0321] Reference Example 4: PBT Recycling under Continuous Heating
[0322] Colored polymer PBT material (in any color) is cut / chopped into pieces and placed in a reaction vessel (e.g., flask, tube, reaction vessel). Degassed GVL (GVL: polymer material mass ratio is 1: 1 to 100: 1, preferably 1: 1-10: 1) is added, and the mixture is heated to 185 ° C at 1013 mbar by using a suitable heating system (e.g., oil bath, heating block, small factory container) so that a mixture is obtained in which the dissolved part of PBT and filler (if present) is completely dissolved, but solid particles are retained in the mixture. After 5-30min, the mixture is filtered (e.g., heated pressure filtration), thereby obtaining a filter cake with the remainder of an insoluble filler (e.g., glass fiber), and a filtrate with the dissolved part of PBT and filler (if present). The filter cake is optionally further washed with a small amount of hot GVL. As the filtrate begins to cool, PBT precipitates. The precipitate is filtered, wherein the dissolved portion of the filler (if present) (soluble in GVL but not precipitated during cooling) is removed together with the filtrate. The precipitated PBT is washed with a small amount of GVL. In order to easily remove the GVL and a faster drying process of the recovered color-poor PBT powder, a small amount of acetone is optionally used in the second washing step. The filter cake is also washed with a small amount of GVL. In order to easily remove the GVL and a faster drying process of the undissolved filler (e.g., glass fiber), a small amount of acetone is optionally used in the second washing step. The polymer material and filler (recovered PBT and undissolved glass fiber) thus obtained are dried (e.g., in a vacuum compartment dryer).
[0323] Examples 1 to 3 (E1-E3) and Comparative Examples 1 to 4 (C1-C4): PET Recycling
[0324] Colored polymer PET material was treated as described in Reference Example 1a or Reference Example 1b, wherein the type of polymer material and the experimental conditions and the results are indicated in Table 1. Samples were analyzed before treatment ((colored) polymer material, Table 1) and after the final drying step (recycled and recovered color-poor PET solid, Table 2) to determine the number average molecular weight Mn, weight average molecular weight Mw, dispersity Mw / Mn and quantitative 1H-NMR.
[0325] Table 1.
[0326] Analysis of starting PET material.
[0327]
[0328] Based on X-ray fluorescence analysis, the white textile has a titanium content of 0.1-1 wt-%, and contains <0.1 wt-% each of Si, S, Cl, K, Ca, Fe, Sb. The white textile has an intrinsic viscosity [η] of 0.501 in [100 ml / g].
[0329] Table 2. Experimental results of PET recycling.
[0330]
[0331]
[0332]
[0333] [a] Dry in a vacuum oven at 140°C instead of 80°C.
[0334] *CIE-LAB value: L*=82.4, a*=-0.8, b*=1.6
[0335] **CIE-LAB value: L*=84.4, a*=-0.8, b*=2.3
[0336] Obviously, the use of the continuous heating procedure according to Reference Example 1b leads not only to a cessation of the decrease in weight average molecular weight Mw, but also to an increase in number average molecular weight Mn.
[0337] The X-ray fluorescence results for the white textile in Example E1 showed that the amount of Si, Ti, Ni was significantly reduced (<0.1%), and the amount of other elements such as S, Cl, K, Ca, Fe, Sb was reduced to below the detection limit. This proves that the filler is removed by this method (compared to the starting material green textile). The intrinsic viscosity data obtained for Example E3 shows that the reduction of intrinsic viscosity (compared to the starting material white textile) can be avoided with this method.
[0338] Examples 4, 5 and 6 (E4, E5, E6): Separation of PET from cotton or PA
[0339] Colored polymeric materials (in any color) were processed as described in Reference Example 2, where the types of polymeric materials and experimental conditions and results are indicated in Tables 3 and 4.
[0340] The samples were analyzed before treatment ((colored) polymer material, Tables 3 and 4) and after the final drying step (recycled and recovered color-poor PET solids and undissolved polymer (cotton or PA), Tables 3 and 4), quantitative 1H-NMR was measured to determine the PET content in the case of cotton / PET separation and to determine the PA and PET contents in the case of PA / PET separation.
[0341] Table 3. Experimental results of PET / cotton separation.
[0342]
[0343] Table 4. Experimental results of PET / PA separation.
[0344]
[0345] The results show that the separation is carried out very efficiently (complete separation can be achieved), in particular the PET obtained has no residues of PA or cotton (E4, >98% PET) and almost all the PET contained in the starting material (at least 98%) can be recovered.
[0346] Example 7 (E7): Separation of spandex and PET
[0347] Colored polymeric materials (of any color) were processed as described in Reference Example 3, where the type of polymeric material and experimental conditions and results are indicated in Table 5. Samples were analyzed before processing ((colored) polymeric materials, Table 5) and after the final drying step (colorant and spandex-poor polymeric materials, Table 5), measuring quantitative 1H-NMR to determine the PET content.
[0348] Table 5. Experimental results of PET / Spandex separation.
[0349]
[0350] Obviously, the use of the procedure according to Reference Example 3 leads to almost complete recovery of the PET contained in the initial PET / spandex blend, and the obtained PET is completely free of spandex.
[0351] Example 8 (E8a, 8b): Separation of spandex, PET and viscose fibers
[0352] The polymer blend comprising spandex / PET / viscose fibers was subsequently treated according to the procedures of Reference Example 3 and Reference Example 2. The details and results are shown in Table 6.
[0353] Table 6. Experimental results of PET / viscose / spandex separation.
[0354]
[0355] Examples 8a and 8b illustrate a stepwise method for separating different polymers from each other. After the separation of spandex, the remaining material containing PET and viscose contains 67.3 g of PET. From this material, 12 g is treated according to Reference Example 2 and provides 8.0 PET with a purity of 99.3% (precisely 67.3% of 12 g). Thus, selective separation of PET and viscose can be achieved.
[0356] Example 9 (E9): PBT Recycling
[0357] The colored polymer PBT material was processed as described in Reference Example 4, where the type of polymer material and the experimental conditions and the results are indicated in Table 7. Samples were analyzed before processing ((colored) polymer material, Table 1) and after the final drying step (recycled and recovered color-poor PBT solids, Table 7) to determine the number average molecular weight Mn, weight average molecular weight Mw, dispersity Mw / Mn.
[0358] Table 7. Experimental results of PBT recycling and filler separation.
[0359]
[0360] It is clear that the use of the procedure for dissolving PBT according to Reference Example 4 leads at least to a very low stop-reduction ratio of less than 1% with respect to the weight average molecular weight Mw. The number average molecular weight Mn also increases. The PBT recovered is free of glass fibers and therefore complete separation can be achieved.
[0361] Comparative Examples 5 and 6 (C5, C6): Other Solvents
[0362] The colored polymeric material (in any color) was treated as described in reference example 1b, except that another solvent was used instead of GVL. The polymeric material was a white textile as described in Table 1. The experimental conditions and results are indicated in Table 8.
[0363] Table 8.
[0364] Comparative Example Using a Known PET Recycle Solvent.
[0365]
[0366] Obviously, under the same conditions as GVL, using DMI or ethyl benzoate as solvent, the quality of the recovered PET is lacking. By using DMI (C5), PET is not easily precipitated from the solvent and the recovered PET also has a lower yield. In addition, the reduction rate of PET is significantly increased compared to the use of GVL. In ethyl benzoate (C6), PET is not really dissolved (94% of the undissolved PET can be re-isolated as a filter cake after filtration), and only a very small amount of PET is separated during hot filtration and precipitation. The recovered PET has a poor quality.
[0367] Comparative Example 7 (C7): Reproduction of the Prior Art Procedure
[0368] Methods for dissolution / precipitation of PET are disclosed in Wenjun Chen et al. (Wenjun Chen et al.: "Biomass-derived [gamma]-valerolactone: efficient dissolution and accelerated alkaline hydrolysis of polyethylene terephthalate", Green Chemistry, Vol. 23, No. 11, June 9, 2021, pp. 4065-4073), see in particular the section "PET recycled by dissolution / precipitation method" on page 4071 and Table 2 on page 4068 and the right column on page 4067 for additional information on the time required for dissolution.
[0369] The samples of the white PET textile material used were preliminarily analyzed for number average molecular weight (Mn), weight average molecular weight (Mw), dispersity (Mw / Mn) and CIE-LAB characteristics thereof; the analysis results are indicated in Table 9 below.
[0370] For comparison purposes, an attempt was made to reproduce the experiment of Wenjun Chen et al., swelling at 120°C or within 1 hour and dissolving at 170°C within 2 minutes: 10 g of white PET textile flakes were placed in a reaction vessel. Side note: Wenjun Chen et al. performed their experiments with flakes from PET bottles, while here flakes from PET textiles were used. However, it is known that PET behaves the same regardless of the original form (bottle, textile). 200 g of degassed GVL (mass ratio of GVL:PET polymer material is 20:1) were added and the mixture was kept at 120°C (at 1013 mbar) for one hour. Afterwards, the temperature was raised to 170°C and kept at this temperature for 5 minutes - only partial dissolution was observed, i.e. solid material remained visible. Then, the mixture was filtered hot and water (antisolvent) was added to the liquid phase at 80°C and then filtered at a mass ratio of water:polymer material of 20:1. As a result of the filtration, most of 8.5 g of undissolved PET polymer material (85% of the initial PET textile flake) was recovered on the filter, and 1.3 g of PET (13% of the initial PET textile flake) was recovered as a precipitate from the liquid fraction after adding water. The precipitate obtained was analyzed and the results are indicated in Table 9 below.
[0371] For comparison, 10 g of the same white PET textile flakes were treated at 185° C. for 15 minutes according to Reference Example 1b, with a mass ratio of PET:GVL=1:10, wherein complete dissolution of the PET flakes was observed. After filtration, precipitation was achieved by cooling, i.e. without adding antisolvent. The precipitate obtained was analyzed and the results are indicated in Table 9 below.
[0372] Table 9
[0373] The analysis results of the precipitate obtained by the method of Wenjun Chen et al. were compared with those according to the method of Reference Example 1b.
[0374]
[0375] *"Dissolution" refers to the state achieved by treatment with GVL at the corresponding temperature and for the corresponding time, i.e. before filtration and precipitation.
[0376] Firstly, it must be noted that, contrary to what is described by Wenjun Chen et al., the PET textile flakes, even after so-called "swelling" at 120° C. for 1 hour, were largely not dissolved within 2 minutes - 85% of the PET textile flakes initially provided remained undissolved, despite the treatment step at 170° C. being extended to five minutes. On the other hand, the material was completely dissolved according to the procedure of Reference Example 1b and was completely recovered in the precipitate.
[0377] Secondly, the use of the procedure according to Reference Example 1b leads not only to a cessation of the decrease in weight average molecular weight Mw, but also to an increase in number average molecular weight Mn. In contrast, the procedure of Wenjun Chen et al. leads to a significant decrease in Mn and Mw.
[0378] Third, the CIE-LAB L*a*b* values show that the recycled PET obtained according to the procedure of Reference Example 1b is significantly whiter (higher L* value) than the material obtained using the method described by Wenjun Chen et al. - the recycled PET obtained according to the procedure of Reference Example 1b is as white as the original "white" PET material, while the recycled PET obtained according to the procedure of Wenjun Chen et al. shows a significant yellow coloration.
[0379] References
[0380] -WO 2016 / 12755A1
[0381] - Wenjun Chen, Yuechao Yang, Xue Lan, Baolong Zhang, Xiaogang Zhang and Tiancheng Mu, “Dyes and Pigments” in Green Chem., Vol. 23, No. 11, 9 June 2021, 23, pp. 4065-4073. Metin Acikyildiz, Kübra Günes, Ahmet Gürses Springer, 2016 (ISBN: 10: 3319338900)
[0382] -Industrial Organic Pigments - Klaus Hunger, Thomas Heber, Martin U.Schmidt, Friedrich Reisinger, Stefan Wanne Wiley-VCH, 4th edition, 2018 (ISBN: 978-3-527-32608-2)
[0383] -Chemistry and Technology of Natural and Synthetic Dyes and Pigments - Ashis Kumar Samanta, Nasser Awwad, IntechOpen Publishing, 2020 (ISBN: 9781789859980, 9781789859973, 9781839687587)
[0384] -Encyclopedia of Color, Dyes, Pigments - Volume 1, Gerhard Pfaff, de Gruyter, 2021 (ISBN: 311058588X)
[0385] -Heinrich Zollinger: Color Chemistry: Syntheses, Properties, and Applications of Organic Dyes and Pigments. 3rd edition. WILEY-VCH Verlag, Weinheim 2003 (ISBN: 3-906390-23-3)
[0386] -Klaus Hunger (editor): Industrial Dyes: Chemistry, Properties, Applications. WILEY-VCH Verlag, Weinheim 2003 (ISBN: 3-662-01950-7)
[0387] - Hermann Rath: Lehrbuch der Textilchemie.einschl.der textilchemischen Technologie [Textbook of Textile Chemistry: Including Textile Chemical Technology]. 2nd edition. Springer-Verlag, Berlin, Heidelberg, 1963 (ISBN: 978-3-662-00065-6)
[0388] -Wilfried Kratzert, Rasmus Peichert: Farbstoffe [Dyes]. Quelle & Meyer, Heidelberg 1981 (ISBN: 3-494-01021-8)
[0389] - Ullmann's Encyclopedia of industrial chemistry, Wiley-VCH, 2000, sections "dyes and pigments" and "dyes, general survey" (ISBN: 9783527303854).
[0390] -Handbook of mechanical solid-liquid separation [Handbook of mechanical solid-liquid separation] - April 29, 2004 von Klaus Luckert (editor)
[0391] - W.-M. Kulicke and C. Clasen, Viscosimetry of Polymers and Polyelectrolytes, Springer (2003).
Claims
1. A method for separating a polymer blend, the polymer blend comprising (i) polyester, and (ii) one or more components selected from the group consisting of a second polymer, a third polymer, and a filler, wherein the second polymer and the third polymer are different from each other and from the polyester of (i); The method includes: (a) providing the polymer blend and providing a solvent comprising gamma-valerolactone; (b) contacting the polymer blend with the solvent comprising γ-valerolactone at a temperature T1 of < 170° C., thereby obtaining a solvent rich in dissolved second polymer and a residue of the polymer blend depleted in said second polymer and comprising the polyester, optionally the third polymer and optionally the filler; and / or (c) contacting the polymer blend provided in (a) or the residue of the polymer blend obtained in (b) with a solvent comprising gamma-valerolactone at a temperature T2 of > 170°C, thereby obtaining a solvent enriched in dissolved polyester compared to the solvent provided in (a) and comprising optionally at least a portion of filler, and optionally a residue of the polymer blend depleted in polyester and comprising optionally a third polymer and optionally a filler or a portion of the filler.
2. The method for separating a polymer blend according to claim 1, wherein: (b) include: (b.1) contacting the polymer blend with the solvent comprising γ-valerolactone at a temperature T1 of < 170° C., thereby obtaining a solvent enriched in the dissolved second polymer and a residue of the polymer blend depleted in said second polymer and comprising the polyester, optionally the third polymer and optionally the filler; (b.2) The solvent enriched in the dissolved second polymer and the residue of the polymer blend obtained in (b.1) are preferably separated by a physical separation method, thereby obtaining a separated solvent enriched in the dissolved second polymer compared to the solvent provided in (a) and a residue of the polymer blend depleted in the second polymer and containing the polyester.
3. The method for separating a polymer blend according to claim 1 or 2, wherein: (c) include: (c.1) contacting the polymer blend provided in (a) or the residue of the polymer blend obtained in (b) or (b.2) with a solvent comprising γ-valerolactone and having a temperature T1a ≤ T2 (T2 is a temperature > 170°C), thereby obtaining a mixture comprising the polymer blend and the solvent; (c.2) heating the mixture obtained in (c.1) to a temperature T2> 170°C with continuous heating, wherein the heating from T1a to T2 is preferably carried out at a heating rate in the range of 20 K / h to 1000 K / h, 25 K / h to 900 K / h, 30 k / h to 800 K / h, 40 k / h to 700 K / h, 60 k / h to 600 K / h, preferably maintaining T2, thereby obtaining a solvent enriched in dissolved polyester compared to the solvent provided in (a) and optionally comprising at least a portion of the filler; and optionally a residue of the polymer blend, which is depleted in polyester and comprises the third polymer and optionally the filler or a portion of the filler; (c.3) optionally separating the solvent rich in dissolved polyester obtained in (c.2) from the residue of the polymer blend, wherein the separation is preferably carried out by heating filtration, more preferably by heating filtration at a temperature T3 in the range of T2 minus 20°C to T2 plus 20°C (T3=T2±20°C), more preferably at a temperature T3 in the range of T2 minus 10°C to T2 plus 10°C (T3=T2±10°C); Wherein the method preferably further comprises: (c.4) contacting the residue of the polymer blend obtained in (c.3) - if it contains a remaining amount of the polyester - with a solvent comprising γ-valerolactone, preferably at temperature T3 as defined above, and subsequently filtering, thereby obtaining a residue of the polymer blend further depleted in polyester and comprising the third polymer and optionally the filler or a portion of the filler; and a solvent containing the remaining amount of the polyester.
4. The method for separating a polymer blend according to claim 3, wherein: If T1a is below 120°C, the heating is carried out as continuous heating, preferably at a heating rate in the range of 20 K / h to 1000 K / h, 25 / K / h to 900 K / h, 30 K / h to 800 K / h, 40 K / h to 700 K / h, 60 K / h to 600 K / h, preferably the heating is carried out so that the mixture obtained in (c.1) is in the temperature range of 110°C-130°C for less than 60 minutes, preferably for less than 50 minutes, more preferably for less than 40 minutes, more preferably for less than 30 minutes, more preferably for less than 20 minutes, or if T1a is above 120°C, the heating is carried out as continuous heating, preferably at a heating rate in the range of 0.1 to 1000 K / h, more preferably in the range of 5 to 500 K / h, more preferably in the range of 25 to 300 K / h.
5. A method for separating a polymer blend as claimed in any one of claims 1 to 4, comprising: (d) cooling the solvent obtained in (c) or (c.3) which is enriched in dissolved polyester compared to the solvent provided in (a) and optionally comprises at least a portion of the filler to a temperature below 170° C., preferably below 150° C., more preferably below 140° C., more preferably below 100° C., thereby obtaining precipitated polyester and a solvent depleted in dissolved polyester and optionally comprising at least a portion of the filler; (e) optionally separating the precipitated polyester obtained in (d) from the solvent depleted in dissolved polyester, thereby obtaining precipitated polyester and the solvent depleted in dissolved polyester and optionally comprising at least a portion of the filler; Wherein preferably, the method for separating the polymer blend further comprises: (f) optionally washing the precipitated polyester obtained in (e); (g) optionally drying the precipitated polyester obtained in (e) or the washed precipitated polyester obtained in (f).
6. A method for separating a polymer blend as claimed in any one of claims 1 to 5, comprising at least partially recycling the separated solvent obtained in (b.2) and / or the separated solvent obtained in (e) to (b) and / or (c), optionally after one or more post-treatment steps.
7. The method for separating a polymer blend according to any one of claims 1 to 6, wherein: T1 is a temperature in the range of 110°C to <170°C, preferably in the range of 110°C to 165°C, more preferably in the range of 120°C to 150°C. and / or Therein, T2 is a temperature in the range of >170°C to 200°C, preferably in the range of 175°C to 190°C, more preferably in the range of 180°C to 190°C.
8. The method for separating a polymer blend according to any one of claims 1 to 7, wherein: The polyester according to (i) is selected from the group consisting of polymers based on 1,4-butanediol and terephthalic acid (polybutylene terephthalate, PBT), polymers based on 1,2-ethylene glycol and terephthalic acid (polyethylene terephthalate, PET), copolymers of 1,4-butanediol, adipic acid and terephthalic acid (polybutylene adipate terephthalate, PBAT), polymers of 1,2-ethylene glycol and 2,5-furandicarboxylic acid (polyethylene furandicarboxylate, PEF) and mixtures of two or more of these (co)polymers, preferably the polyester according to (i) is a polymer based on 1,4-butanediol and terephthalic acid (PBT) or a polymer based on 1,2-ethylene glycol and terephthalic acid (PET).
9. The method for separating a polymer blend according to any one of claims 1 to 8, wherein: The second polymer is preferably selected from the group consisting of polyurethane (PU), polyethylene glycol (PEG), polytetrahydrofuran (pTHF), mixtures of these polymers and copolymers of these polymers, wherein the second polymer is more preferably a copolymer of PU and PEG and / or pTHF, more preferably spandex (a copolymer of PU and PEG or PU and pTHF).
10. The method for separating a polymer blend according to any one of claims 1 to 9, wherein: The third polymer is preferably selected from the group consisting of polyolefins, preferably polyethylene (PE) and polypropylene (PP), polyamide (PA), natural polymers, preferably wool, cotton or viscose, mixtures of two or more of these polymers and copolymers of two or more of these polymers, wherein the third polymer is preferably selected from PA, wool, cotton, viscose and mixtures of two or more of these polymers.
11. The method for separating a polymer blend according to any one of claims 1 to 10, wherein: The γ-valerolactone-containing solvent comprises γ-valerolactone and one or more solvents selected from the group consisting of water and a solvent having a log K in the range of -1.6 to +1.
6. OW The organic solvent is preferably selected from the group consisting of water, C5 to C12 alkanes, aliphatic C1 to C10 alcohols, C3 to C10 ketones, C2 to C10 cyclic ketones, HO-[C1 to C10 alkyl-O-] n -H--wherein n is an integer in the range of 2 to 1000, C1 to C10 alkyl-O-C3 to C10 alkyl ether, C3 to C10 cyclic ether--optionally substituted with one or more C1 to C6 alkyl, C6 to C10 aromatic hydrocarbon--optionally substituted with one or more C1 to C6 alkyl, C2 to C10 aliphatic ester, C8 to C11 aromatic ester, C5 to C10 cyclic carboxylic acid ester (lactone), C3 to C12 amide, preferably R 1 R 2 NC(=O)-R 3 -- Among them R 1 , R 2 are independently C1 to C4 alkyl and R 3 Selected from the group consisting of C1 to C9 alkyl, C1 to C10 ester and C1 to C6 ether, C3 to C6 lactam--optionally substituted with one or more substituents selected from C1 to C6 alkyl, C1 to C6 ester and C1 to C6 ether, and C5 imidazolidine--optionally substituted with one or more C1 to C6 alkyl, C5 to C7 imidazolidinone--optionally substituted with one or more C1 to C6 alkyl.
12. A polyester obtained or obtainable by the process according to any one of claims 1 to 11, preferably by (d) and / or (e) and / or (f) and / or (g) according to claim 5.
13. Use of the precipitated polyester obtained or obtainable from (d) and / or (e) and / or (f) and / or (g) according to claim 5 or according to claim 12 for textile applications, fiber applications, packaging applications, plastic applications, automotive applications, electronic applications, preferably for the production of food packaging, beverage packaging, clothing, footwear, wires, cables, wherein Preferably, in the case where the polyester is selected from PBAT, PEF and PET, preferably PET, the precipitated polyester obtained or obtainable from (d) and / or (e) and / or (f) and / or (g) according to any one of claims 5 or the polyester according to claim 12 is used in textile applications, fiber applications, packaging applications, plastic applications, more preferably in the production of food packaging, beverage packaging, clothing and footwear; wherein in the case where the polyester is PBT, the precipitated polyester obtained or obtainable from (d) and / or (e) and / or (f) and / or (g) according to claim 5 or the polyester according to claim 12 is used in textile applications, automotive applications, or electronic applications, more preferably in the production of wires and / or cables.
14. A method for preparing a product, the method comprising (I) providing the polyester as claimed in claim 12; (II) preparing textiles, fibers, packaging, plastics, automotive parts, electronic parts from the polyester provided in (I).
Citation Information
Cited By
Method for recovering polyethylene in hybrid plastic and application thereof
CN121652459A
Method for recovering polyethylene in mixed plastics and applications thereof
CN121652459B