Recycled carbon black obtained by solvolysis of tyres

By thermally chemically converting waste tires with aromatic hydrocarbon fractions as solvents under low temperature and low pressure conditions, the problem of carbon-based sediment formation on carbon black is solved, the redispersion performance and yield of carbon black is improved, and the Gas formation achieves efficient carbon black recovery.

CN118974179APending Publication Date: 2024-11-15IFP ENERGIES NOUVELLES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380031484.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-30
Filing Date
2023-03-14
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The prior art is difficult to effectively limit the formation of carbon-based deposits on carbon black when thermally chemically converting waste tires, resulting in differences in carbon black redispersion performance and yield. In addition, conventional methods produce a large amount of non-condensable gas, affecting liquid products. Recyclable.

Method used

At a temperature below 400°C and a pressure below 1.5 MPa, the waste tire raw material is contacted with the hydrocarbon fraction of high-content aromatic compounds as solvents, and the presence of carbon-based residues is restricted through the thermal decomposition and washing process, and Recycled carbon black with low carbon-based residue content was obtained by multi-stage fractionation and drying.

Benefits of technology

The carbon-based residue content in carbon black is achieved, the redispersion performance and yield of carbon black is improved, the gas formation is reduced, and the recovery of liquid products is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005064672800000181
    Figure BDA0005064672800000181
  • Figure BDA0005064672800000191
    Figure BDA0005064672800000191
  • Figure BDA0005064672800000192
    Figure BDA0005064672800000192
Patent Text Reader

Abstract

Recycled carbon black (rCB) comprises carbon black, inorganic ash and a carbon-based residue resulting from the decomposition of pneumatic rubber and / or elastomer residues, characterized in that the content of said carbon-based residue, determined by X-ray photoelectron spectroscopy for the percentage of C1 peak area, is less than or equal to 1% of said C1 peak area, the percentage of C1 peak area is calculated with respect to the total area of C0 to C5 peaks.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of carbon-based materials of the carbon black type, and in particular to "recycled" carbon black (or rCB) obtained by thermochemical conversion of scrap tires. The invention also relates to a process for preparing these rCBs by a process of solvolysis of scrap tires with recycling of a hydrocarbon fraction containing aromatic compounds. Background Art

[0002] Tires are mainly made of rubber and textile and metal fibers, because of their elastic properties (a mixture of elastomers of the cross-linked synthetic and natural rubber type, with the addition of additives of the silica, resins, sulphur, zinc oxide, carbon black, etc. type) and their reinforcing properties. Carbon black (or CB) is used in particular in rubber formulations to increase the durability of the rubber (in terms of firmness and service life), to limit deformations of the tire in use and to facilitate heat transfer between the tire and the ground during driving. Carbon black is usually obtained by incomplete combustion of vegetable oils or hydrocarbons, exists in more than 35 grades, sold and used as fillers (mainly in the formulation of pneumatic tires). Their quality varies due to their intrinsic properties.

[0003] Most carbon blacks are characterized by a high elemental carbon content (>90% by weight, relative to the total weight of the carbon black) and may contain other chemical elements, such as hydrogen, oxygen, nitrogen and sulfur, chemically bonded to the carbon. They are usually supplied in the form of black powders consisting of elementary graphite particles (more or less highly crystalline) which are almost spherical (10 to 500 nm) forming aggregates (100 to 1000 nm) which themselves may be aggregated together in the form of agglomerates (1 to 100 μm), the whole of which may then be further converted into granules (0.1 to 1 mm). The size of the elementary particles and the structure of the bodies (morphology, size, density / permeability of the aggregates / agglomerates) will greatly influence the ability of the carbon black to be dispersed in the elastomer matrix and thus ultimately the reinforcing properties of these carbon blacks in the tire. The "specific surface area" (or S) determined by the physical adsorption of nitrogen is the surface area of ​​the carbon black. BET ) parameter is characteristic of the elementary particle size and provides information about the possible interaction of the carbon black surface with the elastomer matrix. The structural characteristic of carbon black is that, for its part, it has the ability to form pores that can be filled with liquid paraffin and thus ultimately with the elastomer matrix. The structural index (equivalent to the oil adsorption value) is then determined, and the relevant analytical method is the OAN (Oil Adsorption Number) method. Then, an abbreviation of the type NXYZ is associated with each carbon black, where X is the S of the carbon black. BET The characteristic numbers of S, Y, and Z are arbitrarily assigned numbers based on the observed structures. BETThere is a relationship between the carbon black grade and the OAN structure index, which makes it possible to classify different carbon blacks according to their grade and their reinforcing or non-reinforcing properties. For example, carbon blacks N110, N120 and N234 are very good reinforcing agents, characterized by high specific surface area and high structure index. According to the intrinsic properties of carbon black, it will be used to formulate different rubbers, which themselves are used in various components of tires.

[0004] In the tire recycling process, the tires are usually first ground to obtain ground tire materials (usually fragments of 1 to 10 cm) that still contain some textile fibers and metal fibers or particles (usually less than 6 mm in size) without any fibers. They can then be converted into gaseous fractions, liquid fractions or solid fractions by a thermal decomposition conversion process. The solid fraction obtained mainly consists of a mixture of carbon blacks of various grades, plus inorganic ash (mainly silica and zinc-based compound types). In addition, the thermal decomposition of the "elastomer" fraction produces carbon-based compounds of various natures (various optionally recondensed decomposition products) that can be deposited on the surface of the carbon black. Similarly, depending on the operating conditions of the process, polymer chains of undecomposed elastomers can be adsorbed on the surface. For a given conversion process applied to a specific "waste tire" raw material, rCB then represents all solid fractions consisting of the initial carbon black as a mixture and modified on the surface by various carbon-based deposits (decomposition products and / or elastomer residues) and inorganic ash. Therefore, the intrinsic properties of rCB are a function of the elements that constitute it. In particular, the chemical composition of the rCB, the degree of agglomeration of the aggregates and their structure, and the resulting redispersion properties of the rCB in the elastomeric matrix, relative to those of the starting carbon black, vary greatly depending on the composition of the scrap tires processed (choice of feedstock) and the recycling process envisaged.

[0005] Among the thermal decomposition conversion processes that can be used to treat scrap tires, the pyrolysis process is very common (J. Yu et al., Frontiers of Environmental Science & Engineering, 2020, 14, 2, 7982; SQLi et al., Ind. Eng. Chem. Res., 2004, 43, 5133; EP 2 661 475). The pyrolysis process generally involves exposing the tire to a temperature of 350° C. to 800° C. under anaerobic conditions or in the presence of a very small amount of oxygen or air intended to provide the energy required for the pyrolysis process by very incomplete combustion. The pyrolysis process is operated at the atmospheric pressure of the gas under consideration or sometimes under vacuum to minimize the post-degradation side reactions of the pneumatic tire, which often lead to the formation of residual carbon-based deposits on the surface of the final rCB as mentioned above. A variety of techniques are used, such as the use of fixed beds, moving beds or rotary kiln reactors. The yields of these rCB processes vary widely (approximately 25% to 60%), as do the intrinsic characteristics of the rCB (e.g., the content of residual inorganic ash can vary from 8% to 41% by weight). On the other hand, the rCB obtained after pyrolysis (often also referred to as "pCB") has in common the presence of a non-negligible carbon-based deposit on the surface of the starting carbon black. The carbon-based deposit is characterized in particular by means of the surface analysis technique of X-ray photoelectron spectroscopy (XPS), also known as ESCA (Electron Spectroscopy for Chemical Analysis). Firstly, this surface analysis allows the determination of the basic chemical composition of the material and thus of the amounts of C, O, N, S, Si, Al, Zn, etc. present. Subsequently, precise analysis of the energy spectrum associated with elemental carbon (C1s spectrum) provides information about the chemical environment of the constituent carbon atoms of rCB (paper Ludovic Moulin: Valorisation du noir de carbone récupéré, relation procédé-produit [Upgrading of Recovered Carbon Black, Process-Product Relationship]. Process engineering. Ecole des Mines d'Albi-Carmaux, 2018). In particular, it can separate the carbon associated with the starting carbon black (C 0 peaks, corresponding to binding energies of about 284.2 / 284.8 eV, which are characteristic of the CC / CH bonds of graphite structures) and carbon associated with carbon-based compounds (C 1The peaks correspond to the binding energies of about 284.8 / 285.6 eV, which are characteristic of the CC / CH bonds of aliphatic structures or small aromatic molecules and in this case are associated with the carbon-based deposits formed during pyrolysis. Therefore, the carbon-based deposit content exhibited by pCB is 5% to 40% (based on the above C 0 and C 1 The peaks are attributed to CO, C=O and COOH bonds and π-π* transitions. 2 , C 3 , C 4 and C 5 The total area of ​​the peaks is calculated). These carbon-based deposits are largely responsible for the agglomeration phenomenon that binds together the various structures of the rCB at different scales; the solids discharged from the reactor are usually in the form of lumps of a few mm / cm, which then need to be finely ground for reuse (especially as additives for new rubber formulations), which requires a lot of energy consumption. It should be noted that these carbon-based deposits seem to be firmly bound to the surface of the starting carbon black, since even post-thermal treatment at higher temperatures than the pyrolysis process itself is not sufficient to remove them (in the case of a post-pyrolysis heat treatment at 600 °C, C 1 The peak area changes from 40% to 20%: H. Darmstadt et al., Carbon, 1995, 33, 10, 1449).

[0006] In order to limit the formation of carbon-based deposits on rCB, the partial pressure of hydrocarbons can be reduced by injecting steam during the cracking reaction (steam pyrolysis process). Unfortunately, the high temperature conditions commonly applied (often above 500 °C) still lead to the formation of carbon-based deposits, albeit in limited proportions (5% to 6% of C 1 Peak area). In addition, these gas-solid processes also have other disadvantages. This is because they usually produce a large amount of non-condensable gases (under atmospheric conditions), usually 10% to 25% by weight relative to the waste tire raw material entering the reactor, which will damage the amount of liquid products that are potentially recyclable and easy to upgrade. This is because these liquid fractions can be used to produce new hydrocarbon fractions (naphtha, gasoline, kerosene, gas oil, vacuum distillate, residual oil), which are used in refineries to produce fuels or in petrochemicals to produce bases for subsequent use in the preparation of plastics.

[0007] Another alternative approach favourable to limiting the presence of these carbon-based deposits on the rCB consists in bringing the tyre raw material into contact with a liquid under appropriate operating conditions (in particular temperature) and dissolving and converting the tyre in a homogeneous liquid phase in which it will be stirred and gradually disappear. Patents US 3 978 199 and US 3 704 108 disclose processes for converting waste tyres, comprising a phase of dissolving a solid raw material based on waste tyres in the presence of a solvent corresponding to the recycling of a heavy liquid fraction of the filtrate obtained after distillation, comprising compounds rich in aromatics, preferably monoaromatics. Unfortunately, the conditions for carrying out such processes, and more particularly the choice of a heavy liquid fraction as solvent, are not favourable for not forming carbon-based deposits in the final rCB.

[0008] The Applicant Company has developed a new process for the conversion of waste tires, which allows obtaining "recycled" carbon black (rCB) containing a very low content of carbon-based residues (decomposition products of pneumatic rubber and / or elastomer residues), which also limits the agglomeration phenomena of rCB of various structures usually encountered during the process adopted in the literature. The process consists in recycling the waste tire raw material by an operation of contacting the raw material with a solvent composed of at least a hydrocarbon fraction, containing a high content of aromatic compounds, a low content of C40+ compounds (vacuum residue) and a medium content of C5-C10 hydrocarbon compounds (gasoline), at a temperature lower than or equal to 400° C. and a pressure lower than 1.5 MPa, the solvent can be generated (recycled) by the process itself. The process is also characterized by a weight ratio of liquid solvent to specific raw material, i.e. a weight ratio greater than 3 weight / weight. The defined operating conditions, the composition of the hydrocarbon fraction and the weight ratio of solvent / solid raw material make it possible to maximize the rCB yield by better dissolving / decomposing the solid raw material, while limiting the presence of carbon-based residues in the final rCB. Furthermore, this method limits the formation of gases to a content of 1 to 7% by weight of the raw material to be treated. Summary of the invention

[0009] The present invention relates to a recycled carbon black (rCB) comprising carbon black, inorganic ash and carbon-based residues resulting from the decomposition of aerated rubber and / or elastomer residues, characterized in that the carbon black content of the rCB is 0.0447 W / m, as measured by X-ray photoelectron spectroscopy. 1 The content of the carbon-based residue determined by the percentage of the peak area is less than or equal to 1% of the C 1 Peak area, the C 1 The percentage of peak area relative to C 0 To C 5 The total area of ​​the peaks was calculated.

[0010] According to one or more embodiments, the recycled carbon black comprises 50 wt% to 98 wt% of elemental carbon, relative to the total weight of the recycled carbon black.

[0011] According to one or more embodiments, the recycled carbon black comprises 0.5 wt % to 4 wt % of elemental oxygen, relative to the total weight of the recycled carbon black.

[0012] According to one or more embodiments, the recycled carbon black comprises 0.2 wt% to 3 wt% elemental hydrogen, relative to the total weight of the recycled carbon black.

[0013] According to one or more embodiments, the recycled carbon black comprises 0.05 wt % to 1 wt % of elemental nitrogen, relative to the total weight of the recycled carbon black.

[0014] According to one or more embodiments, the recycled carbon black comprises 0.5 wt % to 6 wt % of elemental sulfur, relative to the total weight of the recycled carbon black.

[0015] According to one or more embodiments, the recycled carbon black comprises an extracted volatile organic compound content of 0.2 wt. % to 20 wt. %, relative to the total weight of the recycled carbon black.

[0016] According to one or more embodiments, the recycled carbon black comprises an inorganic ash content of 4 wt % to 50 wt % relative to the total weight of the recycled carbon black.

[0017] According to one or more embodiments, the recycled carbon black has a carbon content of 30 to 150 m 2 / g specific surface area.

[0018] According to one or more embodiments, the recycled carbon black has a -5 m 3 / kg to 110×10 -5 m 3 / kg structure index, the structure index is determined by the OAN analysis method according to standard ASTM D2414.

[0019] According to one or more embodiments, the C 1 The content of the carbon-based residue calculated as the percentage of the peak area (%) is 0.001% to 0.05% of C 1 Peak area, the C 1 The percentage of peak area relative to C 0 To C 5 The total area of ​​the peaks was calculated.

[0020] Another subject matter relates to a method for converting waste tires to obtain recovered carbon black (rCB) according to the invention, said method comprising at least the following stages:

[0021] a) feeding a waste tire-based solid feedstock into a reaction zone in the presence of a liquid solvent comprising an aromatic compound to at least partially dissolve the solid feedstock, and thermally decomposing the at least partially dissolved solid feedstock at a temperature below 400° C. and a pressure below 1.5 MPa to obtain a gaseous effluent and a first liquid effluent comprising carbon black, wherein a weight ratio of the liquid solvent to the solid feedstock is greater than 3 weight / weight;

[0022] b) sending the first liquid effluent obtained in stage a) to a filtering and washing zone in the presence of a washing solvent to obtain a filtered and washed carbon black filter cake and a second liquid effluent, said stage b) being carried out at a temperature of 55° C. to 95° C.;

[0023] c) sending at least part of said gaseous effluent obtained at the end of stage a) to a fractionation zone and sending at least part of the second liquid effluent obtained at the end of stage b) to a fractionation zone to obtain at least a hydrocarbon fraction comprising an aromatics content greater than 30% by weight relative to the total weight of said hydrocarbon fraction and also comprising:

[0024] - a content of C5-C10 hydrocarbon compounds of less than 20% by weight relative to the total weight of said hydrocarbon fraction; and

[0025] - a content of C40+ hydrocarbon compounds of less than 5% by weight relative to the total weight of said hydrocarbon fraction;

[0026] d) passing at least part of the hydrocarbon fraction obtained at the end of stage c) to the reaction zone as liquid solvent for stage a);

[0027] e) drying the filtered and washed carbon black cake obtained at the end of stage b) at a temperature ranging from 50° C. to 200° C. to recover the carbon black.

[0028] According to one or more embodiments, phase a) comprises the following sub-phases:

[0029] a1) feeding the solid raw material and the liquid solvent into a first stirred reactor to at least partially dissolve the solid raw material;

[0030] a2) feeding the at least partially dissolved solid feedstock obtained at the end of stage a1) into a second stirred reactor for thermal decomposition of the solid feedstock at a temperature less than or equal to 400° C. to obtain a liquid effluent containing suspended carbon black particles.

[0031] According to one or more embodiments, the content of aromatic compounds in the hydrocarbon fraction is greater than 40% by weight relative to the total weight of said fraction.

[0032] According to one or more embodiments, the content of C40+ hydrocarbon compounds in the hydrocarbon fraction is less than 3 wt.-%, relative to the total weight of said fraction.

[0033] Another subject matter according to the invention relates to recovered carbon black (rCB) obtained by a waste tire conversion process comprising at least the following stages:

[0034] a) feeding a waste tire based solid feedstock into a reaction zone in the presence of a liquid solvent comprising an aromatic compound to at least partially dissolve the solid feedstock, and thermally decomposing the at least partially dissolved solid feedstock at a temperature below 400° C. and a pressure below 1.5 MPa to obtain a gaseous effluent and a first liquid effluent comprising carbon black, wherein the weight ratio of the liquid solvent to the solid feedstock is greater than 3 weight / weight;

[0035] b) sending the first liquid effluent obtained in stage a) to a filtering and washing zone in the presence of a washing solvent to obtain a filtered and washed carbon black filter cake and a second liquid effluent, said stage b) being carried out at a temperature of 55° C. to 95° C.;

[0036] c) sending at least part of said gaseous effluent obtained at the end of stage a) to a fractionation zone, and sending at least part of the second liquid effluent obtained at the end of stage b) to a fractionation zone, so as to obtain at least a hydrocarbon fraction comprising an aromatics content greater than 30% by weight relative to the total weight of said hydrocarbon fraction, and also comprising:

[0037] - a content of C5-C10 hydrocarbon compounds of less than 20% by weight relative to the total weight of said hydrocarbon fraction; and

[0038] - a content of C40+ hydrocarbon compounds of less than 5% by weight relative to the total weight of said hydrocarbon fraction;

[0039] d) passing at least part of the hydrocarbon fraction obtained at the end of stage c) to the reaction zone as liquid solvent for stage a);

[0040] e) drying the filtered and washed carbon black cake obtained at the end of stage b) at a temperature ranging from 50° C. to 200° C. to recover the carbon black. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 is a schematic diagram of an embodiment of obtaining carbon black according to the present invention.

[0042] Figure 2 yes Figure 1 A schematic diagram of the process is shown with the reaction zone as well as the filtration and wash zones of the process shown in more detail. DETAILED DESCRIPTION

[0043] 1. Definition

[0044] A Cn hydrocarbon fraction is understood to mean a fraction which comprises hydrocarbons having n carbon atoms.

[0045] A Cn+ fraction is understood to mean a fraction which comprises hydrocarbons having at least n carbon atoms.

[0046] The BET specific surface area is measured by nitrogen physical adsorption. The BET specific surface area is measured by nitrogen physical adsorption according to standard ASTM D3663-03 as described in Rouquerol F., Rouquerol J. and Singh K., "Adsorption by Powders & Porous Solids: Principles, Methodology and Applications", Academic Press, 1999.

[0047] The CHNS-O elemental analysis carried out according to standard ASTM D5291 is a method well known to those skilled in the art and allows the rapid determination of the carbon (C), hydrogen (H), oxygen (O), nitrogen (N) and sulfur (S) contents of organic substances and other types of materials, based on the complete combustion of the analysis sample taken out in oxygen at 1000°C.

[0048] The content of carbon-based residues was evaluated by X-ray photoelectron spectroscopy (XPS) surface analysis technique well known to those skilled in the art, in particular, by accurate analysis of the energy spectrum associated with elemental carbon (C1s spectrum), which provides information on the chemical environment of the constituent C atoms of rCB. Specifically, the content of carbon-based residues is determined by the C1s corresponding to the binding energy of about 284.8 / 285.6 eV. 1 The peak area percentage (%) is determined, which is characteristic of the CC / CH bonds of aliphatic structures or small aromatic compounds associated with the residue, relative to the C 0 To C 5 The total area of ​​the peak was calculated (C 0 is the peak associated with the CC / CH bond of graphite structure, C 2 , C 3 , C 4 and C 5The method for measuring the carbon-based residue content is described in detail in Darmstadt H., Roy C. and Kaliaguine S. in their paper “Characterization of pyrolytic carbon blacks from commercial tire pyrolysis plants”, Carbon, Volume 33, No. 10 (1995), pp. 1449-1455, and also in Bendida Sahouli, Silvia Blacher, Brouers, Hans Darmstadt, Christian Roy and Serge Kaliaguine published a paper: "Surface morphology and chemistry of commercial carbon black and carbon black from vacuum pyrolysis of used tyres", Fuel, Vol. 75, No. 10 (1996), pp. 1244–1250, or is also described in the paper by Ludovic Moulin: Valorisation du noirde carbone récupéré, relation procédé-produit [Upgrading of Recovered Carbon Black, Process-Product Relationship]. Process engineering. Ecole des Mines d'Albi-Carmaux, 2018.

[0049] Thermogravimetric analysis is a widely used and well-known technique for those skilled in the art, and is also applicable to measuring the moisture content, volatile content and ash content of rCB. The scheme used is derived from standard ISO 9924-2, which is mainly used for vulcanized rubber (vulcanisates) and non-vulcanized mixtures. In nitrogen, the temperature is first increased from 25°C to 600°C, and the water content (weight loss from 25°C to 150°C, in %) and the content of volatiles and / or pyrolyzable phases (weight loss from 150°C to 600°C) can be measured. After this first stage, the sample is subsequently cooled to 400°C in nitrogen. In air, the temperature is increased to 400°C to 950°C for the second time, and the combustion of carbon can be carried out and the amount of carbon (rCB and possible carbon-based residues) can be measured. The final weight measured at the end of the scheme can determine the content of inorganic matter. The analysis method is described in detail in the paper published by Norris, C., Hale, Mike and Bennett, M., "Pyrolytic carbon: Factors controlling in-rubber performance", Plastics, Rubber and Composites, Vol. 43 (2014), pp. 245–256.

[0050] 2. Recycled Carbon Black (rCB)

[0051] The recycled carbon black (rCB) according to the present invention comprises carbon black (CB), inorganic ash and carbon-based residues resulting from the decomposition of pneumatic rubber and / or elastomeric residues associated with the pneumatic rubber, preferably consisting of carbon black (CB), inorganic ash and the carbon-based residues, characterized in that the carbon content of the carbon-based residues measured by X-ray photoelectron spectroscopy is 1 The carbon-based residue content determined by the percentage of the peak area is less than or equal to 1% of the C 1 peak area, preferably 0.001% to 0.08% by area, more preferably 0.001% to 0.07% by area and still more preferably 0.001% to 0.05% by area, the C 1 The percentage of peak area relative to C 0 To C 5 The total area of ​​the peaks was calculated.

[0052] More specifically, the rCB comprises 50 to 98 wt.-%, preferably 60 to 90 wt.-%, still more preferably 65 to 85 wt.-% of elemental carbon relative to the total weight of said rCB.The carbon content is evaluated by CHNS-O elemental analysis.

[0053] More specifically, the rCB comprises from 0.2% to 4% by weight, preferably from 0.4% to 3% by weight, still more preferably from 0.8% to 2.7% by weight of elemental oxygen relative to the total weight of the rCB.

[0054] More specifically, the rCB comprises from 0.2% to 3% by weight, preferably from 0.4% to 2.5% by weight, still more preferably from 0.5% to 1.5% by weight of elemental hydrogen relative to the total weight of the rCB.

[0055] More specifically, the rCB comprises from 0.05% to 1% by weight, preferably from 0.1% to 0.7% by weight, still more preferably from 0.15% to 0.4% by weight of elemental nitrogen relative to the total weight of the rCB.

[0056] More specifically, the rCB comprises from 0.5 to 6 wt.-%, preferably from 1.5 to 5 wt.-%, still more preferably from 2 to 3.5 wt.-% of elemental sulfur relative to the total weight of the rCB.

[0057] The carbon (C), hydrogen (H), oxygen (O), nitrogen (N) and sulfur (S) contents were measured by CHNS-O elemental analysis.

[0058] Under the effect of a specific thermal treatment (e.g. by thermogravimetric analysis "TGA" under nitrogen up to 600°C), these elements can be released from the rCB in the form of vaporized water or volatile organic compounds (VOCs). The amount of extracted VOCs is also a characteristic of the rCB according to the invention. Advantageously, the content of extracted VOCs is between 0.2% and 20% by weight, preferably between 0.5% and 7% by weight, even more preferably between 0.5% and 4% by weight, relative to the total weight of the rCB.

[0059] The rCB according to the invention also contains inorganic ash. The inorganic ash consists at least mainly of SiO 2 The present invention is based on the present invention in the form of a silicon dioxide (SiO) and an elemental zinc present at least predominantly in its oxidized form ZnO (zinc oxide) and / or its sulfide form ZnS (zinc sulfide), preferably in its sulfide form ZnS. The application of a specific heat treatment (at least 950° C. in air by TGA analysis) allows the content of inorganic ash present in the rCB according to the invention to be quantified. Thus, the content of inorganic ash is advantageously between 4% and 50% by weight, preferably between 8% and 40% by weight, even more preferably between 10% and 30% by weight, relative to the total weight of the rCB.

[0060] The rCB according to the present invention may also contain other heteroelements, the element content of which is less than 1 wt %, preferably less than 0.5 wt %, and more preferably less than 0.2 wt %, relative to the total weight of the rCB. The heteroelements may be, for example, but not limited to, elements Al, Ca, Mg, Cl, Fe, K, Br, Co, Ti and P. The content of these elements can be measured by X-ray fluorescence.

[0061] Advantageously, the rCB according to the invention has a 30 m 2 / g to 150m 2 / g, preferably 50m 2 / g to 90m 2 / g, and more preferably 50m 2 / g to 75m 2 / g specific surface area.

[0062] Advantageously, the structural index, determined by the OAN analysis method according to standard ASTM D2414, is 55×10 -5 m 3 / kg to 110×10 -5 m 3 / kg, preferably 55×10 -5 m 3 / kg to 90×10 -5 m 3 / kg.

[0063] The carbon black (CB) contained in the recycled carbon black (rCB) may include several grades of commercial carbon black alone or as a mixture.

[0064] Recovered carbon black (rCB) can be obtained by a waste tire conversion process comprising at least the following stages:

[0065] a) feeding a waste tire based solid feedstock into a reaction zone in the presence of a liquid solvent comprising an aromatic compound to at least partially dissolve the solid feedstock, and thermally decomposing the at least partially dissolved solid feedstock at a temperature below 400° C. and a pressure below 1.5 MPa to obtain a gaseous effluent and a first liquid effluent comprising carbon black, wherein the weight ratio of the liquid solvent to the solid feedstock is greater than 3 weight / weight;

[0066] b) sending the first liquid effluent obtained in stage a) to a filtering and washing zone in the presence of a washing solvent to obtain a filtered and washed carbon black filter cake and a second liquid effluent, said stage b) being carried out at a temperature of 55° C. to 95° C.;

[0067] c) sending at least part of said gaseous effluent obtained at the end of stage a) to a fractionation zone, and sending at least part of the second liquid effluent obtained at the end of stage b) to a fractionation zone, so as to obtain at least a hydrocarbon fraction comprising an aromatics content greater than 30% by weight relative to the total weight of said hydrocarbon fraction, and also comprising:

[0068] - a content of C5-C10 hydrocarbon compounds of less than 20% by weight relative to the total weight of said hydrocarbon fraction; and

[0069] - a content of C40+ hydrocarbon compounds of less than 5% by weight relative to the total weight of said hydrocarbon fraction;

[0070] d) passing at least part of the hydrocarbon fraction obtained at the end of stage c) to the reaction zone as liquid solvent for stage a);

[0071] e) drying the filtered and washed carbon black cake obtained at the end of stage b) at a temperature ranging from 50° C. to 200° C. to recover the carbon black.

[0072] Unless stated otherwise, all variants and embodiments described above can be combined with one another.

[0073] 3. Preparation of rCB

[0074] Another subject of the present invention is a method for preparing rCB according to the invention starting from waste tires. Said preparation method is a conversion method, more specifically a waste tire solvolysis method, in combination with a method according to one embodiment of the present invention with reference to Figure 1 , the method comprises at least the following stages:

[0075] a) feeding a solid feedstock 100 based on waste tires into a reaction zone 80 in the presence of a liquid solvent 760 comprising an aromatic compound to at least partially dissolve the solid feedstock, and thermally decomposing the at least partially dissolved solid feedstock at a temperature below 400° C., preferably 365° C. to 395° C., and more preferably 380° C. to 395° C., and at a pressure below 1.5 MPa, preferably 0.2 to 1.2 MPa, to obtain at least a gaseous effluent 310 and a first liquid effluent 320 comprising rCB according to the present invention, the weight ratio of the liquid solvent 760 to the solid feedstock 100 being greater than 3 weight / weight;

[0076] b) sending the liquid effluent 320 obtained in stage a) to a filtration and washing zone 40 in the presence of a washing solvent to obtain a filtered and washed rCB cake 430 and a second liquid effluent 410 according to the invention, said stage b) being carried out at a temperature of 55°C to 95°C, preferably 60°C to 90°C, still more preferably 65°C to 85°C;

[0077] c) sending at least part, preferably all, of said gaseous effluent 310 obtained at the end of stage a) to a fractionation zone 70, and sending at least part, preferably all, of the second liquid effluent 410 obtained at the end of stage b) to a fractionation zone 70, in order to obtain at least a hydrocarbon fraction 730 comprising an aromatics content greater than 30% by weight, preferably greater than 40% by weight, relative to the total weight of said hydrocarbon fraction, and comprising:

[0078] - a content of C5-C10 hydrocarbon compounds of less than 20% by weight, preferably less than 10% by weight, more preferably from 1% to 8% by weight, relative to the total weight of the hydrocarbon fraction 730; and

[0079] - a content of C40+ hydrocarbon compounds of less than 5% by weight, preferably less than 3% by weight, more preferably less than 1% by weight, still more preferably less than 0.5% by weight, relative to the total weight of the hydrocarbon fraction 730;

[0080] d) sending at least part of the hydrocarbon fraction 730 obtained at the end of stage c) to the reaction zone 80 as liquid solvent 760 for stage a);

[0081] e) drying the filtered and washed rCB cake 430 according to the invention obtained at the end of stage b) in a drying zone 50 at a temperature ranging from 50° C. to 200° C., preferably for a time sufficient for the content of washing solvent in the dried cake to be less than 0.5% by weight relative to the total weight of said dried cake.

[0082] Advantageously, the drying time is between 10 minutes and 36 hours, more preferably between 1 hour and 15 hours, in order to recover the rCB 520 according to the invention.

[0083] According to a basic aspect of the process according to the invention, a recycled hydrocarbon fraction is used as liquid solvent 760 for reaction zone 80 (i.e. stage d) of the process according to the invention), said hydrocarbon fraction comprising a high content of aromatic compounds, a low content of C40+ compounds (vacuum residue) and a not too high content of C5-C10 hydrocarbon compounds (gasoline), and which, when a solvent / solid feedstock weight ratio greater than or equal to 3 weight / weight, preferably from 3 weight / weight to 10 weight / weight, more preferably from 4 weight / weight to 7 weight / weight, is used, which allows better dissolution and decomposition of the solid feedstock 100, thereby maximizing the yield of rCB while limiting the presence of carbon-based residues in said rCB.

[0084] The solid raw material 100 used in the context of the present invention is advantageously based on tires obtained by processing waste tires, which can come from any source, such as light vehicles (LV) or heavy goods vehicles (HGV). The solid raw material can advantageously be provided in the form of tire particles, i.e. in the form of particles with a size less than 6 mm. Preferably, the solid raw material 100 is substantially free of textile fibers and wires, and / or ground tire materials with a characteristic size of typically 1 cm to 20 cm, i.e. ground tire lumps. Therefore, according to a preferred embodiment of the present invention, the solid raw material 100 is fed into a pre-treatment unit 10 to remove textile fibers and wires 110 from the solid raw material 100. Such pre-treatment units are well known to those skilled in the art and can be composed of various types of grinders (i.e. rotary shears, pulverizers, granulators, rechippers), magnetic separators, or vibrating screens, separation tables.

[0085] According to stage a) of the conversion process, the rubber contained in the solid raw material 100 dissolves upon contact with the liquid solvent 760 and then thermally decomposes. The origin and composition of the liquid solvent 760 will be described in detail below. Stage a) is preferably carried out at a temperature below 400° C., preferably between 365° C. and 395° C., more preferably between 380° C. and 395° C., at a pressure below 1.5 MPa, preferably between 0.2 and 1.2 MPa. At the end of stage a), at least a gaseous effluent 310 and a first liquid effluent 320 comprising the rCB according to the invention and optionally solid matter 210 contained in the waste tire, such as metal wires or textile fibers, are obtained, which are released and separated from the liquid effluent 320 obtained at the end of this stage.

[0086] The first liquid effluent 320 comprising the rCB according to the invention is then sent to a filtering and washing zone 40 (i.e. stage b) of the preparation process according to the invention) to recover a filtered and washed rCB cake 430 according to the invention and a second liquid effluent 410. This stage is carried out at a temperature of 55° C. to 95° C., preferably 60° C. to 90° C., still more preferably 65° C. to 85° C. In one embodiment according to the invention, the viscosity of the second liquid effluent 410 measured at 100° C., measured according to standard ASTM D3236, is less than 10 cP, preferably less than 5 cP, more preferably less than 3 cP.

[0087] The filtering and washing unit may comprise any device capable of filtering the rCB particles according to the invention contained in the first liquid effluent 320. For example, such a device may be provided in the form of a rotary filter, preferably operated at a temperature of 55° C. to 95° C., preferably 60° C. to 90° C., still more preferably 65° C. to 85° C. During stage b), the rCB filter cake according to the invention is washed with a washing solvent.

[0088] In one embodiment according to the invention, the washing solvent used during stage b) is a solvent 800 external to the process, such as Figure 1 The solvent may be selected from toluene or xylene, preferably xylene.

[0089] In another embodiment according to the invention, the washing solvent used during stage b) consists at least partly of the light fraction 720 obtained at the end of stage c). Figure 2 , a portion of the light fraction 720 can be sent to the distillation column 90 via the pipeline 725. The remaining part 735 of the light fraction is sent out of the process according to the invention as an upgradeable product. At the outlet of the distillation column 90, a light fraction 910 comprising aromatic compounds is obtained, whose final boiling point is less than or equal to 200° C., preferably less than 150° C., which can be used at least partially as a washing solvent for the filtration / washing zone 40. The heavier fraction 920 can be sent out of the process as an upgradeable product 920.

[0090] The filtered and washed rCB cake 430 according to the invention is sent to a drying unit 50 operated at a temperature of 50° C. to 200° C., preferably 50° C. to 150° C., to recover rCB 520 according to the invention (i.e. stage e) of the process according to the invention). Advantageously, the vapor effluent 510 comprising the washing solvent produced by the drying unit 50 is recycled in the washing / filtration unit 40.

[0091] According to the invention, the gaseous effluent 310 obtained at the end of stage a) and the second liquid effluent 410 obtained at the end of stage b) are sent to a fractionation unit 70 (i.e. stage c) of the process according to the invention) to produce at least a hydrocarbon fraction 730 comprising an aromatics content greater than 30% by weight relative to the total weight of said hydrocarbon fraction 730 and also comprising at least:

[0092] - a content of C5-C10 hydrocarbon compounds of less than 20% by weight, preferably less than 10% by weight, more preferably from 1% to 8% by weight, relative to the total weight of the hydrocarbon fraction 730; and

[0093] - a content of C40+ hydrocarbon compounds of less than 5% by weight, preferably less than 3% by weight, more preferably less than 1% by weight, still more preferably less than 0.5% by weight, relative to the total weight of said hydrocarbon fraction 730.

[0094] Advantageously, the hydrocarbon fraction 730 also comprises a content of C10-C20 hydrocarbon compounds ranging from 20% to 65% by weight, preferably from 30% to 65% by weight and more preferably still from 45% to 65% by weight relative to the total weight of said hydrocarbon fraction.

[0095] Advantageously, the hydrocarbon fraction 730 also comprises a content of C20-C40 hydrocarbon compounds ranging from 30% to 80% by weight, preferably from 30% to 70% by weight and more preferably still from 30% to 55% by weight relative to the total weight of said hydrocarbon fraction.

[0096] Advantageously, the hydrocarbon fraction 730 has an initial boiling point of 50°C to 325°C, preferably 50°C to 250°C, and a final boiling point of 350°C to 520°C, preferably 350°C to 450°C.

[0097] Advantageously, the fractionation zone 70 can also obtain a non-condensable gas 710, a light fraction 720 (whose final boiling point is preferably 250°C to 325°C) and a heavy fraction 740 (whose initial boiling point is preferably 350°C to 450°C).

[0098] Advantageously, the light fraction 720 may be fed at least partly as a washing solvent to the washing and filtering zone 40 to obtain a filtered and washed rCB cake 430 according to the invention.

[0099] Advantageously, the light fraction 720 comprises a content of C10-hydrocarbon compounds greater than 60% by weight relative to the total weight of the light fraction 720 .

[0100] Advantageously, the heavy fraction 740 comprises a C40+ hydrocarbon compound content greater than 60% by weight relative to the total weight of the heavy fraction 740 .

[0101] According to the invention, a fraction of the hydrocarbon fraction 730 is at least partially fed to the reaction zone 80 of stage a) as liquid solvent 760, and another part 750 is advantageously fed out of the process according to the invention as an upgraded product. The weight ratio of the flow rate of the liquid solvent 760 injected into the reaction zone 80 to the solid raw material 100 is greater than or equal to 3 weight / weight (w / w), preferably 3 weight / weight to 10 weight / weight, more preferably 4 weight / weight to 7 weight / weight. In particular, one of the characteristics of the liquid solvent 760 is that it contains an aromatic compound content greater than 30 weight % relative to the total weight of the liquid solvent 760, so that the solid raw material 100 can be effectively dissolved and the viscosity of the reaction medium in the reaction zone 80 can be effectively reduced. Another advantage of the process according to the invention is that, considering the limited production of gas and light hydrocarbons in the reaction zone 80 and the low content of C10- hydrocarbon compounds in the hydrocarbon fraction 730, the use of such a solvent can maintain the liquid form when the pressure in the reactor is limited to a level below 1.5 MPa.

[0102] For a better understanding of the present invention, the following description (as an application example) relates to a method for converting waste tires that can maximize the yield of rCB while limiting the presence of carbon-based residues in the rCB. Figure 2, the solid raw material 100 is fed into a pretreatment unit 10 so as to remove textile fibers and metal wires 110 from the solid raw material 100. The solid raw material substantially free of textile fibers and metal wires is then fed into a reaction zone 80 so that the waste tire can be thermally degraded, the reaction zone 80 comprising a first stirred reactor 20 fed with a liquid solvent 760, in order to promote the dissolution of tire particles or ground tire materials contained in the solid raw material 100. The weight ratio of liquid solvent / solid raw material is greater than or equal to 3 weight / weight, preferably 3 weight / weight to 10 weight / weight, more preferably 4 weight / weight to 7 weight / weight. The temperature in the reactor 20 is preferably 200° C. to 300° C., preferably 250° C. to 290° C. In the first stirred reactor 20, the ground material or particles are dissolved. The time required for this dissolution is preferably 30 minutes to 2 hours. The rubber mass and the future rCB according to the invention gradually released from the rubber are kept in suspension by mechanical agitation or hydrodynamic agitation, for example by upward liquid flow generated by reflux, by forced convection, or by any other means capable of keeping the medium subjected to agitation. The metal wires that may still be present in the solid raw materials and will not dissolve settle out and are discharged from the bottom of the first stirred reactor 20 through the pipeline 210. Under these conditions, the temperature is too low to significantly start the carbon-carbon cracking reaction, and only the crosslinking bonds between polymers (such as SS bonds related to rubber vulcanization) can be significantly cracked. The liquid fraction 220 obtained containing the suspended residual solid matter is introduced into the second stirred reactor 30, in which the thermal degradation reaction is carried out under moderate temperature conditions, i.e. at a temperature of less than or equal to 400°C, preferably 365°C to 395°C, and more preferably 380°C to 395°C, and for a limited time (corresponding to the residence time of the liquid fraction in the reactor 30), preferably 30 minutes to 2 hours, preferably 45 minutes to 90 minutes. The heat required for the thermal degradation reaction can be provided by an exchanger on the pump circulation (not shown) around the second stirred reactor 30, or by any other means, such as an exchanger on the reactor wall or an exchanger or oven on the reactor raw material upstream. The stirring in the second stirred reactor 30 is maintained by a mechanical stirring system or a pump circulation system or any other means known to those skilled in the art. Preferably, the pressure of the reactor is maintained at a level lower than 1.5 MPa by a control valve (not shown).

[0103] At the end of the reaction in the second stirred reactor 30, a first liquid effluent 320 containing suspended rCB particles according to the invention and a gaseous effluent 310 are obtained. Subsequently, the first liquid effluent 320 is sent to a filtration and washing zone 40, which comprises a rotary filter 41 and an intermediate fractionation unit 42 (see Figure 2). The rotary filter 41 is preferably operated at a temperature of 50°C to 200°C, and a rCB filter cake according to the present invention and a liquid fraction 425 can be obtained. Subsequently, the filter cake is washed with a washing solvent 800 (such as toluene or xylene, preferably xylene) at a temperature of 55°C to 95°C, preferably 60°C to 90°C, and more preferably 65°C to 85°C, so that the filtered and washed rCB 430 according to the present invention can be recovered. After the filtering / washing stage, the washing stream 405 can be sent to the intermediate fractionation unit 42 to obtain a fraction 610 and a fraction 415, which can be at least partially recycled as a make-up washing solvent upstream of the rotary filter 41 through a pipeline, and the fraction 415 can be sent to the fractionation zone 70 as a second liquid effluent 410 together with the liquid fraction 425. The filtered and washed rCB 430 according to the invention is then fed to a drying unit 50 which is operated at a temperature of 50° C. to 200° C., advantageously for a period of time sufficient to render the content of washing solvent in the dried cake less than 0.5% by weight relative to the total weight of the dried cake. The filtered, washed and dried rCB 520 according to the invention can then advantageously be granulated (granulated) with water to form granules of a few millimeters, for example in order to facilitate its transport and upgrading. The rCB thus produced can, after a stage of subsequent treatment and packaging of the substance according to the use and application, be used again as a reinforcing agent in the elastomer industry or as a pigment for other applications, for example in inks, plastics or paints. The residual washing solvent can be recovered at the outlet of the drying unit 50 and at least partially recovered via the pipeline 510.

[0104] The gaseous effluent 310 discharged from the reaction zone 80 via the second reactor 30 and the second liquid effluent 410 produced from the washing / filtration zone 40 are then introduced into the fractionation zone 70. The fractionation zone 70 may be composed of a heat exchanger, a gas-liquid separator drum, a distillation column comprising a top outlet, a bottom outlet and a side stream outlet, or a series of several distillation columns (e.g. a series of distillation columns operating at atmospheric pressure comprising a top outlet and a bottom outlet, followed by a distillation column operating under a low vacuum). The fractionation zone 70 may in particular produce a hydrocarbon fraction 730 comprising an aromatic compound content greater than 30% by weight, preferably greater than 40% by weight, relative to the total weight of the hydrocarbon fraction 730, and further comprising:

[0105] - a content of C5-C10 hydrocarbon compounds of less than 20% by weight, preferably less than 10% by weight, more preferably from 1% to 8% by weight, relative to the total weight of the hydrocarbon fraction 730; and

[0106] - a content of C40+ hydrocarbon compounds of less than 5% by weight, preferably less than 3% by weight, more preferably less than 1% by weight, still more preferably less than 0.5% by weight, relative to the total weight of the hydrocarbon fraction 730;

[0107] At least a portion of the solvent can be recycled as liquid solvent 760 in the reaction zone 80, and another portion 750 can be used for product upgrading. Preferably, the hydrocarbon fraction is fed into the first reactor 20 of the reaction zone 80 as the liquid solvent.

[0108] The fractionation zone 70 can also obtain non-condensable gas 710, light fraction 720 and heavy fraction 740, wherein the final boiling point of the light fraction 720 is preferably 250° C. to 325° C., and the initial boiling point of the heavy fraction 740 is preferably 350° C. to 450° C. Advantageously, the light fraction 720 can be at least partially fed as a washing solvent to the washing and filtering device 41 of the washing and filtering zone 40 to obtain the filtered and washed rCB filter cake 430 according to the present invention.

[0109] During the start-up of the plant, in the absence of a stable production of a middle distillate, the hydrocarbon fraction 730, an input solvent can be used temporarily, preferably consisting of a content of more than 40% by weight of aromatic molecules relative to the total weight of the fraction. Thus, this fraction can consist, for example, of the conversion effluent from a FCC (fluid catalytic cracking) catalytic cracking process, for example of middle distillates (light cycle oil (LCO)) or heavy distillates (heavy cycle oil (HCO)).

[0110] Example

[0111] The following examples illustrate preferred embodiments of the method and rCB production according to the present invention, but do not limit the scope thereof. Figure 2 The same as described in .

[0112] Example 1 (according to the present invention)

[0113] In a first embodiment consistent with the present invention, waste tire particles (solid raw material) are used, which are produced by a granulator using a grinder, which comes from heavy truck tires, and the particles produced by grinding have a size close to 2 mm. The tire particles are produced by the pretreatment unit 10 and do not contain textile fibers and metal fibers. Subsequently, the particles are continuously sent to the dissolution reactor, where they are mixed with a liquid solvent produced by recycling the hydrocarbon fraction 730 from the fractionation zone 70. A part of the hydrocarbon fraction 730 is used as a liquid solvent 760, and its composition is shown in Table 1 below. The amount of solid raw material treated is 100 kg / h. The amount of solvent recycled in the reactor 20 is 500 kg / h, corresponding to a solvent / particle weight ratio equal to 5 w / w. In the reactor 20, the temperature is maintained at 290°C, which makes it possible to dissolve the particles. The liquid fraction and the future rCB suspended are then introduced into the reactor 30, where the temperature is maintained at 385°C for one hour. At the outlet of the reactor 30, a first liquid effluent 320 and a gaseous effluent 310 are recovered, and the gaseous effluent 310 is all sent to the fractionation zone 70. The first liquid effluent 320 is sent to the rotary filter 41 operated at 80°C. The filtered rCB is washed with xylene at a temperature of 80°C. The second liquid effluent 410 collected at the outlet of the washing and filtering zone 40 is all sent to the fractionation zone 70. The filtered and washed rCB 430 is sent to the drying unit 50, which is operated at 150°C for 24 hours, so that the filtered, washed and dried rCB 520 can be recovered.

[0114] Example 2 (not in accordance with the present invention)

[0115] In Example 2 not in accordance with the present invention, the stages and operating conditions of the conversion process are identical to those of Example 1, except that the content of C40+ hydrocarbon compounds (vacuum residue or VR) in the liquid solvent 760 is outside the range according to the present invention and the stage of washing the recovered carbon black (rCB) is carried out at a temperature of 50°C.

[0116] The operating conditions for Examples 1 and 2 are summarized in Table 1 below.

[0117] Table 1

[0118]

[0119]

[0120] The main characteristics of the rCB obtained according to Examples 1 and 2 are summarized in Tables 2 and 3 below.

[0121] Table 2

[0122]

[0123] Table 3

[0124]

Claims

1. Recycled carbon black (rCB) comprising carbon black, inorganic ash and carbon-based residues resulting from the decomposition of pneumatic rubber and / or elastomer residues, characterized in that The carbon-based residue content determined by the percentage of the C1 peak area measured by X-ray photoelectron spectroscopy is less than or equal to 1% of the C1 peak area, wherein the percentage of the C1 peak area is calculated relative to the total area of ​​the C0 to C5 peaks.

2. The recovered carbon black according to claim 1, characterized in that The recycled carbon black comprises 50 wt % to 98 wt % of elemental carbon, relative to the total weight of the recycled carbon black.

3. The recovered carbon black according to any one of claims 1 and 2, characterized in that The recycled carbon black contains 0.2 wt % to 4 wt % of elemental oxygen, relative to the total weight of the recycled carbon black.

4. The recovered carbon black according to any one of claims 1 to 3, characterized in that The recycled carbon black contains 0.2 wt % to 3 wt % of elemental hydrogen, relative to the total weight of the recycled carbon black.

5. The recovered carbon black according to any one of claims 1 to 4, characterized in that The recycled carbon black comprises 0.05 wt % to 1 wt % of elemental nitrogen, relative to the total weight of the recycled carbon black.

6. The recovered carbon black according to any one of claims 1 to 5, characterized in that The recycled carbon black comprises 0.5 wt % to 6 wt % of elemental sulfur, relative to the total weight of the recycled carbon black.

7. The recovered carbon black according to any one of claims 1 to 6, characterized in that The recycled carbon black comprises 0.2 wt % to 20 wt % of extracted volatile organic compounds, relative to the total weight of the recycled carbon black.

8. The recovered carbon black according to any one of claims 1 to 7, characterized in that The content of inorganic ash is 4 wt % to 50 wt % relative to the total weight of the recycled carbon black.

9. The recovered carbon black according to any one of claims 1 to 8, characterized in that The recovered carbon black has 30m 2 / g to 150m 2 / g specific surface area.

10. The recycled carbon black according to any one of claims 1 to 9, characterized in that The structural index determined by the OAN analysis method according to standard ASTM D2414 is 55×10 -5 m 3 / kg to 110×10 -5 m 3 / kg.

11. The recycled carbon black according to any one of claims 1 to 10, characterized in that The carbon-based residue content calculated as the percentage of the C1 peak area measured by photoelectron spectroscopy is 0.001% to 0.05% of the C1 peak area, wherein the percentage of the C1 peak area is calculated relative to the total area of ​​C0 to C5 peaks.

12. A process for converting waste tires to obtain recovered carbon black (rCB) according to any one of claims 1 to 11, said process comprising at least the following stages: a) feeding a waste tire based solid feedstock (100) into a reaction zone (80) in the presence of a liquid solvent (760) comprising an aromatic compound to at least partially dissolve the solid feedstock, and thermally decomposing the at least partially dissolved solid feedstock at a temperature below 400° C. and a pressure below 1.5 MPa to obtain a gaseous effluent (310) and a first liquid effluent (320) comprising carbon black, wherein the weight ratio of the liquid solvent (760) to the solid feedstock (100) is greater than 3 weight / weight; b) sending the first liquid effluent (320) obtained in stage a) to a filtering and washing zone (40) in the presence of a washing solvent to obtain a filtered and washed carbon black filter cake (430) and a second liquid effluent (410), said stage b) being carried out at a temperature of 55° C. to 95° C.; c) sending at least part of the gaseous effluent (310) obtained at the end of stage a) to a fractionation zone (70), and sending at least part of the second liquid effluent (410) obtained at the end of stage b) to a fractionation zone (70), so as to obtain at least a hydrocarbon fraction (730) comprising an aromatics content greater than 30% by weight relative to the total weight of the hydrocarbon fraction, and also comprising: - a content of C5-C10 hydrocarbon compounds of less than 20% by weight relative to the total weight of said hydrocarbon fraction; and - a content of C40+ hydrocarbon compounds of less than 5% by weight relative to the total weight of said hydrocarbon fraction; d) sending at least part of the hydrocarbon fraction (730) obtained at the end of stage c) to the reaction zone (80) as liquid solvent (760) for stage a); e) drying the filtered and washed carbon black cake (430) obtained at the end of stage b) at a temperature ranging from 50°C to 200°C to recover the carbon black.

13. The method according to claim 12, wherein stage a) comprises the following sub-stages: a1) introducing the solid raw material (100) and the liquid solvent (760) into a first stirred reactor (20) to at least partially dissolve the solid raw material (100); a2) feeding the at least partially dissolved solid feedstock obtained at the end of stage a1) into a second stirred reactor (30) in order to thermally decompose the solid feedstock at a temperature of less than or equal to 400° C. and obtain a liquid effluent containing suspended carbon black particles.

14. The method according to any one of claims 12 and 13, wherein the content of aromatic compounds in the hydrocarbon fraction (730) is greater than 40% by weight relative to the total weight of the fraction.

15. The method according to any one of claims 12 to 14, wherein the content of C40+ hydrocarbon compounds in the hydrocarbon fraction (730) is less than 3% by weight relative to the total weight of the fraction.