Negative electrode for non-aqueous electrolyte secondary battery, and non-aqueous electrolyte secondary battery
By using the mixing of the second material with a high reaction potential and the first material of silicon in the negative electrode of the lithium-ion secondary battery, the negative electrode potential is improved, the early charging termination problem caused by the increase in silicon content is solved, and the voltage and capacity of the battery are increased Utilization.
Patent Information
- Application Number
- CN202380029789.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-25
- Filing Date
- 2023-03-08
- Publication Date
- 2024-11-15
AI Technical Summary
When increasing the negative silicon content of lithium-ion secondary battery, it is easy to cause the polarization of the negative electrode to increase, and the negative electrode potential during charging is lower than the lithium metal potential, resulting in the charging termination voltage earlier than expected and the capacity utilization decreases.
The negative electrode mixture layer using the negative electrode active material includes the second material with a high reaction potential and the first material of silicon. The silicon content Cs is set to more than 10%. The negative electrode potential is adjusted by mixing the potential to prevent early charging and increase the battery voltage. .
It effectively suppresses the drop in the closed circuit potential of the negative electrode, prevents early charging termination, and improves battery voltage and capacity utilization.
Smart Images

Figure CN118974965A_ABST
Abstract
Description
Technical Field
[0001] The present invention mainly relates to a negative electrode for a non-aqueous electrolyte secondary battery. Background Art
[0002] Non-aqueous electrolyte secondary batteries, especially lithium-ion secondary batteries, have high voltage and high energy density, and are therefore highly anticipated as power sources for small household applications, power storage devices, and electric vehicles. In the pursuit of higher energy density of batteries, the use of silicon-containing materials that alloy with lithium as negative electrode active materials with high theoretical capacity density is highly anticipated.
[0003] For example, Patent Document 1 proposes a method for producing a negative electrode material for a lithium ion secondary battery, in which substrate particles formed of a material containing silicon atoms are prepared, and a carbon coating is formed on the surface of the substrate particles to form a coated particle. As the substrate particles, silicon particles, particles having a composite structure in which silicon fine particles are dispersed in a silicon-based compound, and particles of the general formula SiO x Silicon oxide particles represented by (0.5≤x≤1.6) or a mixture thereof.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2016-91649 Summary of the invention
[0007] Problem that the invention aims to solve
[0008] In order to increase the capacity of non-aqueous electrolyte secondary batteries, it is effective to increase the silicon content in the negative electrode. However, when the silicon content is increased, the polarization of the negative electrode sometimes increases, and the negative electrode potential (closed circuit potential) during charging will be lower than the potential of lithium metal. In this case, the charge termination voltage will be reached earlier than expected, the potential of the positive electrode cannot be fully increased, and the capacity utilization rate will decrease.
[0009] Solutions for solving problems
[0010] One aspect of the present invention relates to a negative electrode for a non-aqueous electrolyte secondary battery. The present invention relates to a negative electrode for a non-aqueous electrolyte secondary battery as follows: the negative electrode has a negative electrode mixture layer containing a negative electrode active material, the negative electrode active material contains a first material containing silicon and a second material having a higher reaction potential with Li than silicon, and the content Cs of the silicon in the negative electrode mixture layer is 10% by mass or more.
[0011] Another aspect of the present invention relates to a nonaqueous electrolyte secondary battery including a positive electrode, the negative electrode described above, a separator disposed between the positive electrode and the negative electrode, and a nonaqueous electrolyte.
[0012] Effects of the Invention
[0013] According to the present invention, a decrease in the closed-circuit potential of the negative electrode can be suppressed, so that a phenomenon in which the charge end voltage is reached earlier than expected can be made less likely to occur.
[0014] The novel features of the present invention are described in the appended claims, but both the composition and content of the present invention should be fully understood from the following detailed description with reference to the accompanying drawings together with other objects and features of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 This is a longitudinal cross-sectional view of a nonaqueous electrolyte secondary battery according to one embodiment of the present invention.
[0016] Figure 2A Graph showing a charge curve of a battery of Reference Example R1 using a negative electrode not including the second material.
[0017] Figure 2B Graph showing the charge curve of a battery of Reference Example R2 in which the negative electrode of R1 is replaced with lithium metal.
[0018] Figure 3A is a graph showing the polarization behavior of graphite.
[0019] Figure 3B Graph showing polarization behavior of a first material including silicon.
[0020] Figure 3C Graph showing polarization behavior of a first material including silicon.
[0021] Figure 3D Graph showing polarization behavior of a first material including silicon.
[0022] Figure 3E Graph showing polarization behavior of a first material including silicon.
[0023] Figure 3F Graph showing polarization behavior of a first material including silicon.
[0024] Figure 4 It is a graph showing a charge curve of a negative electrode including a first material and a second material.
[0025] Figure 5 for Figure 4 An enlarged view of the curve at the end of charging.
[0026] Figure 6 This is a graph showing the relationship between the SOC of the test cell when the closed-circuit potential of the negative electrode reaches the potential of lithium metal and the content of the second material in the negative electrode mixture layer. DETAILED DESCRIPTION
[0027] Below, the embodiments of the present invention are illustrated, but the present invention is not limited to the examples described below. Specific numerical values, materials, etc. are sometimes listed in the following description, but other numerical values, materials, etc. can also be applied as long as the effects of the present invention can be obtained. It should be noted that in the present invention, the components other than the characteristic parts can also apply the components of the known non-aqueous electrolyte secondary battery and its negative electrode. In this specification, in the case of "the range of numerical value A to numerical value B", the range includes numerical value A and numerical value B. When multiple materials are listed, one can be selected from them for use alone, or two or more can be used in combination. In addition, the present invention includes a combination of the contents described in two or more claims arbitrarily selected from the multiple claims recorded in the attached claims. That is, as long as no technical contradiction occurs, the contents described in two or more claims arbitrarily selected from the multiple claims recorded in the attached claims can be combined.
[0028] Below, as an example of a non-aqueous electrolyte secondary battery, a lithium ion secondary battery is mainly described, but the non-aqueous electrolyte secondary battery of the present invention widely includes secondary batteries with liquid, gel or solid non-aqueous electrolytes, as long as they do not conflict with the main purpose of the invention. For example, the present invention can also be applied to all-solid-state secondary batteries, etc.
[0029] A nonaqueous electrolyte secondary battery generally includes an electrode group, a nonaqueous electrolyte, and a battery case that accommodates the electrode group and the nonaqueous electrolyte. The electrode group includes a positive electrode, a negative electrode, and a separator disposed between the positive electrode and the negative electrode.
[0030] The negative electrode of this embodiment has a negative electrode mixture layer containing a negative electrode active material. The negative electrode mixture layer is, for example, provided on the surface of a sheet-shaped negative electrode current collector. The negative electrode mixture layer is composed of a negative electrode mixture containing a negative electrode active material as a main component, and therefore can also be referred to as a negative electrode active material layer. The negative electrode mixture is a mixture containing a negative electrode active material as a main component, and may contain a binder, a conductive agent, etc. as optional components.
[0031] The negative electrode active material includes at least a first material and a second material. Both the first material and the second material are active materials that exhibit capacity through Faraday reaction. That is, the first material and the second material are active materials that absorb and release (or embed and deintercalate) lithium ions as the battery reaction proceeds. However, it is not necessary for the first material as a whole to be an active material, as long as at least a portion of the first material is composed of an active material. In addition, it is not necessary for the second material as a whole to be an active material, as long as at least a portion of the second material is composed of an active material. Here, the first material may include silicon that reacts with Li to form an alloy. The surface of silicon may be oxidized, for example, it may have a natural oxide film. The second material may include an active material having a higher reaction potential with Li than silicon.
[0032] Comparing the first material and the second material, the second material has a higher reaction potential with Li than the first material. By mixing the first material and the second material in the negative electrode mixture layer, the negative electrode potential becomes a mixed potential that is at least affected by the potential of the first material and the potential of the second material. Such a mixed potential is higher than the potential of the first material. As a result, even if the content of the first material in the negative electrode mixture layer (in other words, the content of silicon) is greatly increased, the negative electrode potential is not easy to reach the potential of lithium metal during charging. Therefore, the positive electrode potential can be fully increased when the battery voltage reaches the charge termination voltage, and the utilization rate of the capacity is improved.
[0033] When the content of the first material in the negative electrode mixture layer is greatly increased, the negative electrode potential will be excessively reduced earlier, thereby reaching the charge termination voltage earlier than expected. Specifically, this phenomenon will be manifested when the silicon content Cs in the negative electrode mixture layer is 10% by mass or more. In batteries that have been put into use in the past, this phenomenon has not been manifested because the silicon content Cs in the negative electrode mixture layer is small.
[0034] On the other hand, in order to realize the further high capacity of the nonaqueous electrolyte secondary battery, it is effective to make the silicon content Cs in the negative electrode mixture layer be 10 mass % or more, and it is expected to be 12 mass % or more, and it is further expected to be 20 mass % or more. At this time, it is found that in terms of increasing the positive electrode potential when the battery voltage reaches the charge termination voltage, it is effective to use the second material to increase the average potential of the negative electrode.
[0035] It should be noted that the charge termination voltage corresponds to the voltage (closed circuit voltage) of the battery in a fully charged state. On the other hand, the discharge termination voltage corresponds to the voltage (closed circuit voltage) of the battery in a fully discharged state. The amount of charge when a battery in a fully discharged state with a depth of discharge (DOD) of 100% is charged until it becomes a fully charged state (DOD = 0%) with a state of charge (SOC: depth of charge) of 100% is equivalent to the rated capacity. The charging and discharging of the non-aqueous electrolyte secondary battery is controlled by a prescribed control circuit. The control circuit controls the charging in such a way that the charging is stopped when a preset charge termination voltage (for example, 4.2V) is reached. The greater the polarization of the negative electrode, the easier it is for the battery voltage to rise, and therefore it is easy to reach the charge termination voltage earlier before a sufficient amount of electricity is charged. According to the present invention, this phenomenon can be suppressed.
[0036] The second material is a material that does not contain silicon that contributes to charging and discharging, and does not contribute to the high capacity of the negative electrode like the first material containing silicon (or silicon phase). Therefore, the second material is preferably used in an amount that does not damage the high capacity effect brought about by the first material. From the viewpoint of improving the effect of high capacity, it is preferred that the content C1 of the first material in the negative electrode mixture layer is greater than the content C2 of the second material in the negative electrode mixture layer. Specifically, the content C2 can be less than 0.5 times the content C1 (C2 / C1≤0.5).
[0037] The silicon content Cs in the negative electrode mixture layer can be made greater than the content C2. Specifically, the content Cs can be 1.5 times or more of the content C2 (Cs / C2≥1.5), or can be 2 times or more (Cs / C2≥2). The greater the content Cs of the silicon phase, the more favorable it is for high capacity. On the other hand, from the viewpoint of suppressing the polarization of the negative electrode while suppressing the deterioration of the negative electrode caused by the expansion and contraction of the silicon phase, the silicon content Cs can be limited to less than 30% by mass.
[0038] The content C2 of the second material in the negative electrode mixture layer is not particularly limited. A small amount of the second material is included in the negative electrode mixture layer, so that a mixed potential can be formed, and the effect of suppressing the decline of the negative electrode battery during charging can be obtained. On the other hand, the greater the content C2, the greater the effect of suppressing the decline of the negative electrode potential during charging. From the viewpoint of obtaining a more significant effect, the content C2 is preferably 0.5% by mass or more, and can be 3% by mass or more, or 5% by mass or more, or 10% by mass or more. On the other hand, the second material will not contribute to high capacity like the first material, so the content C2 can be, for example, 15% by mass or less, or 10% by mass or less.
[0039] The first material may contain silicon, and may be substantially composed of only silicon (or a silicon phase), or may be composite particles containing a material other than silicon. The first material may be used alone or in combination of two or more.
[0040] The first material may be a composite particle including a silicon phase and a matrix phase in which the silicon phase is dispersed. The matrix phase may be composed of a material having lithium ion conductivity. The matrix phase may include, for example, at least one selected from the group consisting of a silicon oxide phase and a carbon phase.
[0041] The silicon oxide phase contains Si and O, and may further contain a third element other than Si and O. The silicon oxide phase may be composed of SiO2, may be composed of lithium silicate, or may be composed of both.
[0042] The composite particles as the first material (composite particles including a silicon phase and a matrix phase in which the silicon phase is dispersed) may be, for example, in any of the following forms (a) to (c).
[0043] (a) A first composite particle including a silicon phase and a silicon dioxide (SiO 2 ) phase in which the silicon phase is dispersed.
[0044] (b) Second composite particles including a silicon phase and a lithium silicate phase in which the silicon phase is dispersed.
[0045] (c) Third composite particles including a silicon phase and a carbon phase in which the silicon phase is dispersed.
[0046] The first, second and third composite particles may include a silicon phase dispersed in a matrix phase and a second material dispersed in a matrix phase. That is, the first material and the second material may be combined to form any composite particle. In this case, it can be understood that the first material is composed only of a silicon phase, and the first material as a whole can be regarded as an active material (silicon phase).
[0047] The negative electrode mixture layer may be in any of the following forms (A) to (C), for example.
[0048] (A) A negative electrode mixture layer including a mixture of particles of a first material and particles of a second material.
[0049] (B) A negative electrode mixture layer comprising composite particles in which the first material and the second material are composited into particles (for example, the first, second and third composite particles described above).
[0050] (C) A negative electrode mixture layer comprising a mixture of composite particles in which the first material and the second material are composited into particles (e.g., the first, second, and third composite particles described above) and particles of a third material other than the composite particles (e.g., carbonaceous particles such as graphite, non-graphitizable carbon, and easily graphitizable carbon).
[0051] In the first material, the first composite particle (comprising a silicon dioxide (SiO2) phase and a silicon phase dispersed in the silicon dioxide (SiO2) phase) is excellent in terms of high stability and small volume change. It can be considered that the high stability is due to the small particle size of the silicon phase (or silicon particles) dispersed in the silicon dioxide phase, which makes it difficult to perform deep charging. Since the silicon dioxide phase has more sites that can irreversibly capture lithium ions, there is a tendency for the irreversible capacity to increase in the first material, but the structural stability is correspondingly high, and the volume change is easily suppressed.
[0052] The first composite particle can be synthesized, for example, by heating a raw silicon oxide in a non-oxidizing atmosphere to perform a disproportionation reaction. In the disproportionation reaction, silicon microparticles can be uniformly generated in the silicon dioxide phase. The average particle size of the silicon microparticles generated by the disproportionation reaction is, for example, less than 100 nm, and can be 5 nm to 50 nm. For example, 95 to 100% by mass of the matrix phase of the first composite particle can be composed of silicon dioxide. The overall composition of the first composite particle can be represented by the general formula SiO x (0<x<2) indicates.
[0053] The content of the silicon phase contained in the first composite particles may be, for example, 20% by mass to 60% by mass.
[0054] In the first material, the second composite particles (comprising a lithium silicate phase and a silicon phase dispersed in the lithium silicate phase) are excellent in that the irreversible capacity is small. When the second composite particles are used, excellent charge and discharge efficiency can be obtained. The effect is particularly significant in the initial stage of charge and discharge.
[0055] In the lithium silicate phase, in addition to Li, Si and O, as the third element, at least one selected from the group consisting of the first group elements (excluding Li) and the second group elements of the long period periodic table may be included. The first group elements and the second group elements may be, for example, K, Na, Mg, Ca, Sr, Ba, etc. The lithium silicate phase may further include Al, B, La, P, Zr, Ti, Fe, Cr, Ni, Mn, Cu, Mo, Zn, etc.
[0056] The ratio of the number of O atoms to the number of Si atoms in the lithium silicate phase (O / Si) is, for example, greater than 2 and less than 4. In this case, it is advantageous in terms of stability and lithium ion conductivity. The O / Si ratio may be greater than 2 and less than 3. The ratio of the number of Li atoms to the number of Si atoms in the lithium silicate phase (Li / Si) is, for example, greater than 0 and less than 4.
[0057] The composition of lithium silicate can be expressed by the general formula Li 2z SiO 2+z (0<z<2). From the viewpoint of stability of lithium silicate, ease of production, and lithium ion conductivity, z preferably satisfies 0<z<1, and more preferably z=1 / 2.
[0058] The second composite particles can be obtained, for example, by mixing lithium silicate and raw silicon, pulverizing the mixture with a mixer such as a ball mill while stirring, and then calcining the mixture in an inert atmosphere to obtain the second composite particles. Alternatively, the mixture can be sintered and the sintered body pulverized to obtain the second composite particles.
[0059] The content of the silicon phase contained in the second composite particles may be, for example, 35% by mass or more and 80% by mass or less. The content of the silicon phase in the second composite particles can be arbitrarily changed, so it is easy to design a high-capacity negative electrode.
[0060] In the first material, the third composite particle (comprising a carbon phase and a silicon phase dispersed in the carbon phase) is excellent in that the irreversible capacity is small. In addition, the carbon phase can exhibit capacity through a Faraday reaction with lithium ions, and therefore is advantageous for increasing the capacity in the first material.
[0061] The carbon phase may include crystalline carbon (graphite) or amorphous carbon (ie, non-crystalline carbon) having low crystallinity. The amorphous carbon may be, for example, hardly graphitizable carbon, easily graphitizable carbon, or other amorphous carbon.
[0062] The third composite particles can be obtained, for example, by mixing a carbon source and raw silicon, pulverizing the mixture with a mixer such as a ball mill while stirring, and then calcining the mixture in an inert atmosphere to obtain the third composite particles. Alternatively, the mixture may be sintered and the sintered body pulverized to obtain the third composite particles.
[0063] As the carbon source, for example, sugars, water-soluble resins, etc. can be used. For example, as the carbon source, carboxymethyl cellulose (CMC), polyvinyl pyrrolidone, cellulose, sucrose, etc. can be used. When the carbon source is mixed with the raw silicon, the carbon source and the raw silicon can be dispersed in a dispersion medium of a liquid organic matter such as alcohol.
[0064] The content of the silicon phase contained in the third composite particles may be, for example, 40% by mass or more and 80% by mass or less. The content of the silicon phase in the third composite particles can be arbitrarily changed, so it is easy to design a high-capacity negative electrode.
[0065] The average particle size of the silicon phase (or silicon particles) in the second composite particle or the third composite particle is, for example, 100 nm to 500 nm, 400 nm or 200 nm. The large average particle size of the silicon phase can easily increase the capacity of these composite particles.
[0066] The silicon phase dispersed in the matrix phase of the second composite particle or the third composite particle can be composed of a plurality of crystallites. The crystallite size can be, for example, less than 30 nm, or less than 25 nm. In this case, the volume change caused by the expansion and contraction of the silicon phase accompanying charging and discharging can be greatly reduced. The crystallite size is not particularly limited, for example, it can be more than 5 μm, or more than 10 nm. The crystallite size of the silicon phase is calculated from the half-value width of the diffraction peak attributable to the Si (111) plane of the X-ray diffraction (XRD) spectrum of the silicon phase according to the Scherrer formula.
[0067] The average particle size of the first, second and third composite materials can be, for example, 2 μm to 10 μm, or 4 μm to 7 μm. This makes it easy to relieve the stress caused by the volume change of the silicon phase accompanying charging and discharging. The average particle size refers to the particle size (volume average particle size) at which the volume cumulative value is 50% in the particle size distribution measured, for example, by a laser diffraction scattering method. The measuring device can be, for example, "LA-750" manufactured by HORIBA.
[0068] The contents of the silicon phase in the first, second, and third composite materials can be measured by, for example, Si-NMR.
[0069] The average particle size of the silicon phase in the first, second and third composite materials can be measured from a cross-sectional SEM (scanning electron microscope) photograph of the composite particles. Specifically, the average particle size of the silicon phase can be obtained by averaging the maximum diameters of any 100 silicon particles.
[0070] The second material may include an active material having a higher reaction potential with Li than silicon. However, from the viewpoint of effectively improving the mixed potential of the negative electrode during charging, the reaction potential of the second material with Li is preferably 0.5 V or more higher than the potential of lithium metal. Such a second material is usually a material other than a carbonaceous material, for example, a metal compound is promising. The second material may be used alone or in combination of two or more.
[0071] The metal compound that can be used as the second material can have a crystal structure such as a spinel structure, a perovskite structure, a layered rock salt structure, etc. Specifically, lithium-titanium composite oxides, lithium-manganese composite oxides, and lithium-containing transition metal oxides with a layered rock salt structure known as positive electrode active materials for lithium-ion secondary batteries can be used. Among them, the reaction potential of the lithium-titanium composite oxide with Li is about 1.5V to 1.6V relative to the potential of lithium metal, which is preferred in that it exhibits excellent performance as a negative electrode active material for non-aqueous electrolyte secondary batteries.
[0072] The lithium titanium composite oxide having a spinel crystal structure is, for example, composed of the general formula Li 4+z Ti5O 12 (0≤z≤1). Lithium-titanium composite oxides are also excellent in terms of high lithium ion acceptance and easy reduction of ion diffusion resistance in the negative electrode. The most typical material is Li4Ti5O 12 .
[0073] You can also use the general formula: Li v Ti 5-w M w O 12+t A lithium titanium composite oxide represented by (3≤v≤5, 0.005≤w≤1.5, -1≤t≤1). M is, for example, at least one selected from the group consisting of V, Mn, Fe, Co, Ni, Cu, Zn, Al, B, Mg, Ca, Sr, Ba, Zr, Nb, Mo, W, Bi, Na, K and rare earth elements.
[0074] From the viewpoint of ensuring the dispersibility in the negative electrode mixture layer and forming a uniform mixed potential, the average particle size of the lithium titanium composite oxide is, for example, 20 μm or less, or 10 μm or less. The average particle size of the lithium titanium composite oxide can be, for example, 0.4 μm or more, or 0.6 μm or more. Here, the average particle size also refers to the volume average particle size of the volume cumulative value 50% in the particle size distribution measured by the laser diffraction scattering method.
[0075] The negative electrode active material may further include carbonaceous particles in addition to the first material and the second material. Compared with the first material, the carbonaceous particles expand and contract less during charge and discharge, so it is easy to improve the cycle characteristics. In addition, compared with the second material, the carbonaceous particles have a low reaction potential with Li, which is conducive to high capacity.
[0076] The content of the carbonaceous particles (excluding the carbon phase as the matrix phase of the first material) in the negative electrode active material may be, for example, 70% to 90% by mass. This makes it easy to achieve both high capacity and cycle characteristics.
[0077] As carbonaceous particles, for example, graphite, easily graphitized carbon (soft carbon), difficultly graphitized carbon (hard carbon), etc. can be cited. Among them, graphite with excellent charge and discharge stability and small irreversible capacity is preferred. Graphite refers to a material with a graphite-type crystal structure, such as natural graphite, artificial graphite, graphitized mesophase carbon particles, etc. Carbon materials can be used alone or in combination of two or more.
[0078] Next, a lithium ion secondary battery as an example of a nonaqueous electrolyte secondary battery according to an embodiment of the present invention is summarized. The lithium ion secondary battery includes, for example, the following negative electrode, positive electrode, and nonaqueous electrolyte.
[0079] [negative electrode]
[0080] The negative electrode includes a negative electrode current collector and a negative electrode mixture layer. The negative electrode mixture layer can be formed, for example, by applying a negative electrode slurry obtained by dispersing a negative electrode mixture containing a negative electrode active material in a dispersion medium on the surface of the negative electrode current collector, and rolling the dried coating film. The negative electrode mixture layer can be formed on one surface of the negative electrode current collector or on both surfaces.
[0081] The negative electrode mixture contains a negative electrode active material as an essential component, and contains a binder, a conductive agent, a thickener, etc. as optional components.
[0082] The negative electrode current collector is in sheet form, and metal foil, mesh, net, stamping sheet, etc. can be used. The material of the negative electrode current collector includes stainless steel, nickel, nickel alloy, copper, copper alloy, etc. The thickness of the negative electrode current collector is not particularly limited, and is, for example, 1 μm to 50 μm, or 5 μm to 20 μm.
[0083] As the binder, a resin material can be used, for example, fluororesin, polyolefin resin, polyamide resin, polyimide resin, acrylic resin, vinyl resin, rubber-like material, etc. can be mentioned.
[0084] Examples of the conductive agent include carbon black and carbon nanotubes.
[0085] Examples of the thickener include carboxymethyl cellulose (CMC), modified forms of CMC (such as sodium salt), cellulose derivatives, polyvinyl alcohol, and polyethers.
[0086] Examples of the dispersion medium include water, alcohol, ether, and N-methyl-2-pyrrolidone (NMP).
[0087] [positive electrode]
[0088] The positive electrode contains a positive electrode active material that can electrochemically absorb and release lithium ions. The positive electrode, for example, includes a positive electrode collector and a positive electrode mixture layer. The positive electrode mixture layer can be formed by, for example, applying a positive electrode slurry obtained by dispersing a positive electrode mixture containing a positive electrode active material in a dispersion medium on the surface of the positive electrode collector, and rolling the dried coating. The positive electrode mixture layer can be formed on one surface of the positive electrode collector, or on both surfaces.
[0089] The positive electrode mixture contains a positive electrode active material as an essential component, and contains a binder, a conductive agent, etc. as optional components.
[0090] As the positive electrode active material, for example, a lithium-containing transition metal oxide can be used. For example, Li a CoO2、Li a NiO2、Li a MnO2、Li a Co b Ni 1-b O2、Li a Co b M 1-b O c , Li a Ni 1-b Mb c , Li a Mn2O4、Li a Mn 2-b M bO4, LiMPO4, Li2MPO4F (M is at least one selected from the group consisting of Na, Mg, Sc, Y, Mn, Fe, Co, Ni, Cu, Zn, Al, Cr, Pb, Sb, and B.) Here, a=0 to 1.2, b=0 to 0.9, and c=2.0 to 2.3. It should be noted that the value a representing the molar ratio of lithium increases or decreases due to charge and discharge.
[0091] Among them, Li is preferred a Ni b M 1-b A lithium nickel composite oxide represented by O2 (M is at least one selected from the group consisting of Mn, Co and Al, 0<a≤1.2, 0.3≤b≤1.) is preferred. From the viewpoint of high capacity, it is more preferred to satisfy 0.80≤b≤1. From the viewpoint of crystal structure stability, it is further preferred that Li2O3 contain Co and Al as M. a Ni b Co c Al d O2 (0<a≤1.2, 0.80≤b<1, 0<c<0.20, 0<d≤0.1, b+c+d=1).
[0092] As the binder and the conductive agent, for example, any of the materials listed for the negative electrode can be used. As the conductive agent, graphite such as natural graphite and artificial graphite can also be used.
[0093] The positive electrode current collector is in sheet form, and metal foil, mesh, net, stamping sheet, etc. can be used. Examples of the material of the positive electrode current collector include stainless steel, aluminum, aluminum alloy, titanium, etc. The thickness of the positive electrode current collector is not particularly limited, and is, for example, 1 μm to 50 μm, or 5 μm to 20 μm.
[0094] [Non-aqueous electrolyte]
[0095] The non-aqueous electrolyte may be a liquid electrolyte (electrolyte), a gel electrolyte, or a solid electrolyte. The gel electrolyte comprises a lithium salt and a matrix polymer or comprises a lithium salt, a non-aqueous solvent, and a matrix polymer. As the matrix polymer, a polymer material that absorbs a non-aqueous solvent and gels may be used. As polymer materials, fluororesins, acrylic resins, polyether resins, polyethylene oxides, etc. may be listed. The solid electrolyte may also be an inorganic solid electrolyte. As an inorganic solid electrolyte, for example, well-known materials in all-solid-state lithium-ion secondary batteries, etc. (e.g., oxide-based solid electrolytes, sulfide-based solid electrolytes, halide-based solid electrolytes, etc.) may be used.
[0096] The liquid electrolyte (electrolyte) contains, for example, a non-aqueous solvent and an electrolyte salt. The electrolyte salt contains at least a lithium salt. The concentration of the lithium salt in the non-aqueous electrolyte is preferably, for example, 0.5 mol / L or more and 2 mol / L or less.
[0097] As the non-aqueous solvent, for example, cyclic carbonate, chain carbonate, cyclic carboxylic acid ester, chain carboxylic acid ester, etc. can be used.
[0098] Examples of lithium salts include LiClO4, LiBF4, LiPF6, LiAlCl4, LiSbF6, LiSCN, LiCF3SO3, LiCF3CO2, LiAsF6, and imide salts. Examples of imide salts include lithium bis(fluorosulfonyl)imide (LiN(FSO2)2), lithium bis(trifluoromethanesulfonyl)imide (LiN(CF3SO2)2), and the like.
[0099] [Separator]
[0100] A separator may be provided between the positive electrode and the negative electrode. The separator has high ion permeability and has appropriate mechanical strength and insulation. As the separator, a microporous membrane, a woven fabric, a non-woven fabric, etc. may be used. The material of the separator includes, for example, polyolefins such as polypropylene and polyethylene.
[0101] [Lithium-ion secondary battery]
[0102] The lithium ion secondary battery may be in any form, for example, cylindrical, square, coin, button, laminated, etc. Figure 1 The structure of a cylindrical lithium ion secondary battery (secondary battery 10 ) will be described.
[0103] The secondary battery 10 includes an electrode group 18, an electrolyte (not shown), and a bottomed cylindrical battery can 22 for accommodating them. The sealing body 11 is pressed and fixed to the opening of the battery can 22 via a sealing gasket 21. As a result, the interior of the battery is sealed. The sealing body 11 includes a valve body 12, a metal plate 13, and an annular insulating member 14 sandwiched between the valve body 12 and the metal plate 13. The valve body 12 and the metal plate 13 are connected to each other at their respective center portions. The positive electrode lead 15a led out from the positive electrode 15 is connected to the metal plate 13. Therefore, the valve body 12 functions as an external terminal of the positive electrode. The negative electrode lead 16a led out from the negative electrode 16 is connected to the bottom inner surface of the battery can 22. An annular groove portion 22a is formed near the open end of the battery can 22. A first insulating plate 23 is arranged between one end surface of the electrode group 18 and the annular groove portion 22a. A second insulating plate 24 is disposed between the other end surface of the electrode group 18 and the bottom of the battery can 22. The electrode group 18 is formed by winding a strip-shaped positive electrode 15 and a strip-shaped negative electrode 16 with a separator 17 interposed therebetween.
[0104] Hereinafter, the present invention will be specifically described based on Examples and Comparative Examples, but the present invention is not limited to the following Examples.
[0105] 《Reference Example R1》
[0106] As the first material, second composite particles (average particle size 8 μm, silicon content 55 mass %) and third composite particles (average particle size 7 μm, silicon content 58 mass %) were prepared.
[0107] (Second composite particle)
[0108] The second composite particle contains a lithium silicate phase represented by Li2Si2O5 (z=0.5) and a silicon phase dispersed in the lithium silicate phase. The second composite particle is mixed with coal tar, the mixture is calcined at 800°C in an inert atmosphere, the surface of the second composite particle is covered with conductive carbon, and the average particle size is controlled by the subsequent pulverization conditions. The thickness of the conductive layer is estimated to be about 100nm. The average particle size of the silicon phase is about 100nm, and the crystallite size of the silicon phase is 15nm.
[0109] (Third composite particle)
[0110] The third composite material includes an amorphous carbon phase and a silicon phase dispersed in the amorphous carbon phase. The average grain size of the silicon phase is about 200 nm, and the crystallite size is 15 nm.
[0111] <Negative electrode active material>
[0112] The second composite particles, the third composite particles, and graphite were mixed at a mass ratio of 3:32:65 to prepare a negative electrode active material.
[0113] [Production of negative electrode]
[0114] A negative electrode mixture containing a negative electrode active material, a sodium salt of CMC, and styrene butadiene rubber (SBR) in a mass ratio of 97.5:1:1.5 is dispersed in water as a dispersion medium and stirred with a mixer to prepare a negative electrode slurry. The silicon content Cs in the negative electrode mixture (i.e., the negative electrode mixture layer formed later) is 19.7% by mass, and the content C1 of the first material (the total amount of the first composite particles and the second composite particles) is 34.1% by mass. The negative electrode slurry is applied to both sides of a copper foil, and after the coating is dried, it is rolled to form a negative electrode mixture layer on both sides of the copper foil, thereby obtaining a negative electrode.
[0115] [Production of positive electrode]
[0116] Lithium nickel composite oxide (LiNi 0.8 Co 0.18 Al 0.02O2), acetylene black and polyvinylidene fluoride are mixed in a mass ratio of 95:2.5:2.5, dispersed in NMP, and stirred with a mixer to prepare a positive electrode slurry. The positive electrode slurry is applied on both sides of an aluminum foil, and after the coating is dried, it is rolled to form a positive electrode mixture layer on both sides of the aluminum foil, thereby obtaining a positive electrode.
[0117] [Preparation of non-aqueous electrolyte]
[0118] The non-aqueous electrolyte was prepared by dissolving a lithium salt in a non-aqueous solvent. The non-aqueous solvent used was a mixed solvent containing ethylene carbonate (EC) and dimethyl carbonate (DMC) at a volume ratio of 30:70. The lithium salt used was LiPF6. The LiPF6 concentration was set to 1.1 mol / L.
[0119] [Manufacturing of lithium-ion secondary batteries]
[0120] A pole piece was installed on each electrode, and the positive electrode and the negative electrode were wound into a spiral shape with the pole piece located at the outermost periphery to prepare an electrode group. The electrode group was inserted into an outer casing made of an aluminum laminate film, vacuum dried at 60° C. for 12 hours, and then a non-aqueous electrolyte was injected, and the opening of the outer casing was sealed to obtain a battery R1 of Reference Example 1.
[0121] The battery R1 of the reference example R1 prepared above was subjected to predetermined pre-charge and discharge twice, and then charged by the following method.
[0122] For battery R1, at an ambient temperature of 25°C, constant current charging was performed at a current of 0.1C until the battery voltage reached 4.2V, and then constant voltage charging was performed at a constant voltage of 4.2V until the current reached 0.02C. The charging curve at this time is shown in Figure 2A .
[0123] 《Reference Example R2》
[0124] A single-electrode positive electrode battery R2 was obtained in the same manner as in Reference Example R1 except that the negative electrode was lithium metal with an electrode sheet attached thereto.
[0125] After the battery R2 of the reference example R2 prepared above was pre-charged and discharged twice, it was charged at a constant current of 0.1C at an ambient temperature of 25°C until the battery voltage reached 4.3V, and then charged at a constant voltage of 4.3V until the current reached 0.02C. The charging curve at this time is shown in Figure 2B .
[0126] Figure 2B In the end of charging, the voltage rise behavior corresponding to the structural change of the positive electrode active material can be observed. Figure 2AIt can be understood that at the end of charging, the battery voltage reached 4.2V earlier and the positive electrode potential did not rise to the expected level.
[0127] It should be noted that when the rated capacity is set to C (Ah), C (Ah) / X (h) represents the current value when charging or discharging the rated capacity in X hours. For example, 0.1C means the current value when charging the battery from DOD 100% to SOC 100% in X = 10 hours.
[0128] 《Reference Example C1》
[0129] [Production of negative electrode]
[0130] A negative electrode slurry was prepared in the same manner as Reference Example R1 except that only graphite was used as the negative electrode active material. The negative electrode slurry was applied on both sides of a copper foil, and the coating was dried and then rolled to form negative electrode mixture layers on both sides of the copper foil, thereby obtaining a negative electrode.
[0131] The negative electrode was cut into a 20 mm × 20 mm shape with a 5 mm × 5 mm protrusion, and the negative electrode mixture layer of the protrusion was peeled off to expose the copper foil. Then, the negative electrode tab lead was connected to the exposed portion of the negative electrode current collector, and a predetermined area around the negative electrode tab lead was covered with an insulating film.
[0132] [Fabrication of Counter Electrode]
[0133] A small electrode piece with a Ni mesh welded to the end was prepared, cut into a predetermined size, and the mesh portion was pressed onto a lithium metal foil with a thickness of 300 μm to prepare a counter electrode.
[0134] [Preparation of non-aqueous electrolyte]
[0135] LiPF6 was dissolved in a mixed solvent of ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) at a volume ratio of EC:EMC:DMC=4:1:15 to prepare a non-aqueous electrolyte. The LiPF6 concentration was set to 1.3 mol / L.
[0136] [Production of battery cells]
[0137] Use the above-mentioned negative electrode and two counter electrodes to make a negative electrode-restricted battery cell. Use a pair of counter electrodes to clamp the negative electrode so that the negative electrode mixture layer and the lithium metal foil are opposite to each other through the separator to obtain an electrode group. Next, fold the Al laminated film cut into a rectangle in half, and heat-seal the two ends of the long side to form a tube. Then, put the prepared electrode group into the tube from one side of the short side, align the end face of the Al laminated film with the position of the insulating film of each connector lead and perform heat sealing. Next, inject 0.3cm from the unheat-sealed short side of the tube. 3After the non-aqueous electrolyte was injected, it was left to stand for 3 minutes under a reduced pressure of 0.02 MPa, and then the operation of returning to atmospheric pressure was performed twice to allow the non-aqueous electrolyte to penetrate into the negative electrode mixture layer. Finally, the end face of the Al laminate film on the injection side was heat-sealed while reducing the pressure, thereby obtaining the evaluation battery cell C1. The production of the battery cell C1 was carried out in a dry air atmosphere with a dew point of less than -60°C.
[0138] [evaluate]
[0139] At an ambient temperature of 25°C, the battery cell was clamped with a pair of 10×5cm stainless steel clamps and fixed under pressure at 1MPa. Then, the lithium was charged in the negative electrode at a constant current of 0.1C until the battery cell voltage became 0.1V, and then the charging was continued until the expected capacity was reached. During the continuous charging process, the charging was interrupted at an appropriate time, stopped for 3 hours, and the open circuit voltage was measured.
[0140] 《Reference Example E1》
[0141] The second composite particles and graphite were mixed at a mass ratio of 20:80 to prepare a negative electrode active material. A negative electrode slurry was prepared in the same manner as Reference Example R1, and the negative electrode slurry was applied to both sides of a copper foil. After the coating was dried, it was rolled to form a negative electrode mixture layer on both sides of the copper foil, thereby obtaining a negative electrode. Then, a test battery cell E1 was prepared and evaluated in the same manner as Reference Example C1.
[0142] 《Reference Example E2》
[0143] The third composite particles and graphite were mixed at a mass ratio of 20:80 to prepare a negative electrode active material. A negative electrode slurry was prepared in the same manner as Reference Example R1, and the negative electrode slurry was applied to both sides of a copper foil. After the coating was dried, it was rolled to form a negative electrode mixture layer on both sides of the copper foil, thereby obtaining a negative electrode. Then, a test battery cell E2 was prepared and evaluated in the same manner as Reference Example C1.
[0144] 《Reference Example E3》
[0145] The second composite particles, the third composite particles and graphite were mixed at a mass ratio of 5:25:70 to prepare a negative electrode active material. A negative electrode slurry was prepared in the same manner as Reference Example R1, and the negative electrode slurry was applied to both sides of a copper foil. After the coating was dried, it was rolled to form a negative electrode mixture layer on both sides of the copper foil, thereby obtaining a negative electrode. Then, a test battery cell E3 was prepared and evaluated in the same manner as Reference Example C1.
[0146] "Reference Example E4"
[0147] The second composite particles and graphite were mixed at a mass ratio of 30:70 to prepare a negative electrode active material. A negative electrode slurry was prepared in the same manner as Reference Example R1, and the negative electrode slurry was applied to both sides of a copper foil. After the coating was dried, it was rolled to form a negative electrode mixture layer on both sides of the copper foil, thereby obtaining a negative electrode. Then, a test battery cell E4 was prepared and evaluated in the same manner as Reference Example C1.
[0148] 《Reference Example E5》
[0149] The third composite particles and graphite were mixed at a mass ratio of 30:70 to prepare a negative electrode active material. A negative electrode slurry was prepared in the same manner as Reference Example R1, and the negative electrode slurry was applied to both sides of a copper foil. After the coating was dried, it was rolled to form a negative electrode mixture layer on both sides of the copper foil, thereby obtaining a negative electrode. Then, a test battery cell E5 was prepared and evaluated in the same manner as Reference Example C1.
[0150] At Figure 3A The charging curve of the battery cell C1 is shown in Figure 3B to Figure 3F The charging curves of E1 to E5 are shown in FIG. Figure 3A to Figure 3E It can be understood that the polarization of the negative electrode of the battery cell C1 of reference example 2 is small, and the negative electrode potential (closed circuit potential) is higher than the potential of lithium metal when fully charged. On the other hand, it can be understood that the polarization of the negative electrode of the battery cells E1 to E5 of reference examples E1 to E5 is large, and the negative electrode potential (closed circuit potential) is lower than the potential of lithium metal when fully charged.
[0151] 《Example 1》
[0152] The second composite particles, the third composite particles, graphite and the second material (Li4Ti5O 12 ) are mixed in a mass ratio of 3:32:65:3 to prepare a negative electrode active material. Otherwise, a negative electrode slurry is prepared in the same manner as reference example R1, the negative electrode slurry is applied on both sides of a copper foil, and after the coating is dried, it is rolled to form a negative electrode mixture layer on both sides of the copper foil, thereby obtaining a negative electrode.
[0153] The silicon content Cs in the negative electrode mixture (i.e., the negative electrode mixture layer) was 19.1% by mass, the content C1 of the first material (the total amount of the first composite particles and the second composite particles) was 33.1% by mass, and the content C2 of the second material was 3% by mass. In addition, a test cell A1 was prepared and evaluated in the same manner as in Reference Example C1.
[0154] 《Example 2》
[0155] The second composite particles, the third composite particles, graphite and the second material (Li4Ti5O 12) are mixed in a mass ratio of 3:32:65:5 to prepare a negative electrode active material. Otherwise, a negative electrode slurry is prepared in the same manner as reference example R1, the negative electrode slurry is applied on both sides of a copper foil, and after the coating is dried, it is rolled to form a negative electrode mixture layer on both sides of the copper foil, thereby obtaining a negative electrode.
[0156] The silicon content Cs in the negative electrode mixture (i.e., the negative electrode mixture layer) was 18.8% by mass, the content C1 of the first material (the total amount of the first composite particles and the second composite particles) was 32.5% by mass, and the content C2 of the second material was 5% by mass. In addition, a test cell A2 was prepared and evaluated in the same manner as in Reference Example C1.
[0157] 《Example 3》
[0158] The second composite particles, the third composite particles, graphite and the second material (Li4Ti5O 12 ) are mixed in a mass ratio of 3:32:65:10 to prepare a negative electrode active material. Otherwise, a negative electrode slurry is prepared in the same manner as reference example R1, the negative electrode slurry is applied on both sides of a copper foil, and after the coating is dried, it is rolled to form a negative electrode mixture layer on both sides of the copper foil, thereby obtaining a negative electrode.
[0159] The silicon content Cs in the negative electrode mixture (i.e., the negative electrode mixture layer) was 17.9 mass %, the content C1 of the first material (the total amount of the first composite particles and the second composite particles) was 31.0 mass %, and the content C2 of the second material was 10 mass %. In addition, a test cell A3 was prepared and evaluated in the same manner as in Reference Example C1.
[0160] 《Example 4》
[0161] The second composite particles, the third composite particles, graphite and the second material (Li4Ti5O 12 ) are mixed in a mass ratio of 3:32:65:15 to prepare a negative electrode active material. Otherwise, a negative electrode slurry is prepared in the same manner as reference example R1, the negative electrode slurry is applied on both sides of a copper foil, and after the coating is dried, it is rolled to form a negative electrode mixture layer on both sides of the copper foil, thereby obtaining a negative electrode.
[0162] The silicon content Cs in the negative electrode mixture (i.e., the negative electrode mixture layer) was 17.1% by mass, the content C1 of the first material (the total amount of the first composite particles and the second composite particles) was 29.7% by mass, and the content C2 of the second material was 15% by mass. In addition, a test cell A4 was prepared and evaluated in the same manner as in Reference Example C1.
[0163] Comparative Example 1
[0164] The second composite particles, the third composite particles and graphite were mixed in a mass ratio of 3:32:65 without using the second material (Li4Ti5O 12 ), prepare a negative electrode active material, except that a negative electrode slurry is prepared in the same manner as Reference Example R1, the negative electrode slurry is applied on both sides of a copper foil, and after the coating is dried, it is rolled to form a negative electrode mixture layer on both sides of the copper foil, thereby obtaining a negative electrode.
[0165] The silicon content Cs in the negative electrode mixture (i.e., the negative electrode mixture layer) was 19.7% by mass, the content C1 of the first material (the total amount of the first composite particles and the second composite particles) was 34.1% by mass, and the content C2 of the second material was 0% by mass. In addition, a test cell A5 was prepared and evaluated in the same manner as in Reference Example C1.
[0166] At Figure 4 2 shows the charging curves of battery cells A1 to A5. Figure 4 In the figure, the solid line curve is the curve of the battery cell A5 which does not use the second material. The larger the SOC curve at the end of charging, the greater the content of the second material. That is, the curves of the battery cells A1 to A4 are sequentially assigned from the left to the right. Figure 5 Shown in Figure 4 This is an enlarged view of the final stage of charging. Figure 6 2 shows the relationship between the SOC of the test cell when the closed circuit potential of the negative electrode reaches the potential of lithium metal (negative potential inrush SOC (%)) and the content rate (addition amount (%)) of the second material in the negative electrode mixture layer.
[0167] according to Figure 6 It is understood that the SOC of the test cell when the closed circuit potential of the negative electrode reaches the potential of lithium metal varies according to the content C2 of the second material in the negative electrode mixture layer. In addition, the greater the content C2, the greater the effect of increasing the negative electrode potential at the end of charging.
[0168] Industrial Applicability
[0169] The nonaqueous electrolyte secondary battery including the negative electrode for a nonaqueous electrolyte secondary battery of the present invention is suitable for use as a main power source for mobile communication devices, portable electronic devices, etc., a vehicle-mounted power source, etc., but the use is not limited thereto.
[0170] The preferred embodiments of the present invention are described, but the disclosure thereof shall not be interpreted as restrictive. It is obvious to those skilled in the art that various modifications and changes can be clearly understood by reading the above disclosure. Therefore, the attached claims should be interpreted as including all modifications and changes that do not depart from the true spirit and scope of the present invention.
[0171] Description of Reference Numerals
[0172] 10: Secondary battery, 11: Sealing body, 12: Valve body, 13: Metal plate, 14: Insulating member, 15: Positive electrode plate, 15a: Positive electrode lead, 16: Negative electrode plate, 16a: Negative electrode lead, 17: Separator, 18: Electrode group, 21: Gasket, 22: Battery can, 22a: Groove, 23: First insulating plate, 24: Second insulating plate, 16: Negative electrode, 161: Negative electrode current collector, 162: Negative electrode mixture layer
Claims
1. A negative electrode for a non-aqueous electrolyte secondary battery, wherein: The negative electrode has a negative electrode mixture layer containing a negative electrode active material. The negative electrode active material includes a first material containing silicon and a second material having a higher reaction potential with Li than silicon. The silicon content Cs in the negative electrode mixture layer is 10 mass % or more.
2. The negative electrode for a non-aqueous electrolyte secondary battery according to claim 1, wherein A content C1 of the first material in the negative electrode mixture layer is greater than a content C2 of the second material in the negative electrode mixture layer.
3. The negative electrode for a non-aqueous electrolyte secondary battery according to claim 1, wherein A content Cs of the silicon in the negative electrode mixture layer is greater than a content C2 of the second material in the negative electrode mixture layer.
4. The negative electrode for a non-aqueous electrolyte secondary battery according to any one of claims 1 to 3, wherein A content C2 of the second material in the negative electrode mixture layer is 0.5 mass % or more.
5. The negative electrode for a non-aqueous electrolyte secondary battery according to any one of claims 1 to 4, wherein The second material includes a lithium-titanium composite oxide.
6. The negative electrode for a nonaqueous electrolyte secondary battery according to any one of claims 1 to 5, wherein The first material includes the silicon phase and a matrix phase in which the silicon phase is dispersed. The matrix phase includes at least one selected from the group consisting of a silicon oxide phase and a carbon phase.
7. The negative electrode for a non-aqueous electrolyte secondary battery according to claim 6, wherein The silicon oxide phase includes lithium silicate.
8. The negative electrode for a non-aqueous electrolyte secondary battery according to claim 6 or 7, wherein The second material is further dispersed in the matrix phase in which the silicon is dispersed.
9. The negative electrode for a non-aqueous electrolyte secondary battery according to any one of claims 1 to 8, wherein The negative electrode active material further includes carbonaceous particles. 10 . A nonaqueous electrolyte secondary battery comprising a positive electrode, the negative electrode according to claim 1 , a separator disposed between the positive electrode and the negative electrode, and a nonaqueous electrolyte.