All-solid-state secondary battery

By combining a vacuum-sealed structure with inorganic materials, the degradation problem of the electrode junction in all-solid-state batteries at high temperatures was solved, achieving stable charge and discharge performance in high-temperature environments.

CN118974998APending Publication Date: 2024-11-15NIPPON ELECTRIC GLASS CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202380032269.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-11-02
Filing Date
2023-06-07
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In all-solid-state batteries, the organic materials at the junction of the electrode terminals and the current collector, as well as the battery casing, deteriorate under high-temperature conditions, leading to increased internal resistance and affecting charge and discharge performance.

Method used

It adopts a vacuum-sealed structure, using low-melting-point glass as the sealing layer, combined with a solid electrolyte layer, positive electrode layer and negative electrode layer made of inorganic materials, to ensure that the internal space is in a vacuum state, preventing material expansion and peeling off of the joints.

Benefits of technology

Even at temperatures above 150°C, it maintains good output and cycle characteristics, prevents internal resistance from increasing, and ensures battery stability and performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118974998A_ABST
    Figure CN118974998A_ABST
Patent Text Reader

Abstract

Provided is an all-solid-state secondary battery capable of achieving good cycle characteristics even when used at a high temperature of 150 DEG C or higher for a certain period of time. The all-solid-state secondary battery (1) has a solid electrolyte layer (2), a positive electrode layer (3), and a negative electrode layer (4). The all-solid-state secondary battery (1) has: a first collector layer (5) provided on the main surface of the positive electrode layer (3) on the opposite side from the side on which the solid electrolyte layer (2) is disposed; a second current collector layer (6) provided on the main surface of the negative electrode layer (4) on the opposite side from the side on which the solid electrolyte layer (2) is disposed; and a sealing layer (7) that is provided between the outer peripheral edge (5a) of the first current collector layer (5) and the outer peripheral edge (6a) of the second current collector layer (6), and that seals the positive electrode layer (3) and the negative electrode layer (4). An internal space (8) surrounded by the first current collector layer (5), the second current collector layer (6), and the sealing layer (7) is vacuum.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an all-solid-state secondary battery. Background Art

[0002] Lithium-ion secondary batteries have established themselves as an indispensable high-capacity and lightweight power source in mobile devices, electric vehicles, etc. However, in existing lithium-ion secondary batteries, flammable organic electrolytes are mainly used as electrolytes, so there are concerns about dangers such as fire. As a solution to this problem, all-solid-state batteries such as all-solid-state lithium-ion batteries that use solid electrolytes (also called solid electrolytes) instead of organic electrolytes are being developed.

[0003] However, in all-solid-state batteries, organic materials such as resins are used in the joints between the electrode terminals and the current collectors and in the outer casing of the battery. In addition, gases such as air are contained inside the laminated outer casing in which all-solid-state battery elements are enclosed. (For example, see Patent Document 1).

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2015-79719 Summary of the invention

[0007] Technical problem to be solved by the invention

[0008] When using all-solid-state batteries in a high-temperature environment, for example, above 150°C, there is a problem that the joints between the electrode terminals and the current collectors, organic materials such as the resin used in the battery's outer casing deteriorate, or the gas remaining inside the laminated outer casing enclosing the all-solid-state battery elements expands, causing the joints between the components of the all-solid-state battery (for example, between the electrode terminals and the current collectors) to peel off, and the internal resistance of the all-solid-state battery to increase, which greatly reduces the discharge capacity that can be charged and discharged.

[0009] An object of the present invention is to provide an all-solid-state secondary battery that can achieve good output characteristics and cycle characteristics even when used at a high temperature of 150° C. or higher for a certain period of time.

[0010] Technical solutions for solving technical problems

[0011] The all-solid-state secondary battery of the present invention has a solid electrolyte layer, a positive electrode layer and a negative electrode layer, and the all-solid-state secondary battery is characterized in that it has: a first collector layer arranged on the main surface of the positive electrode layer on the opposite side of the side where the solid electrolyte layer is arranged; a second collector layer arranged on the main surface of the negative electrode layer on the opposite side of the side where the solid electrolyte layer is arranged; and a sealing layer arranged between the outer periphery of the first collector layer and the outer periphery of the second collector layer, and sealing the positive electrode layer and the negative electrode layer, and the internal space surrounded by the first collector layer, the second collector layer and the sealing layer is a vacuum.

[0012] In the present invention, it is preferred that the sealing layer contain low melting point glass having a softening point of 500° C. or less.

[0013] In the present invention, it is preferred that the sealing layer contains Bi2O3-B2O3 glass.

[0014] In the present invention, it is preferred that the positive electrode layer comprises a positive electrode active material composed of a crystallized glass, wherein the crystallized glass contains a x A crystal represented by MP2O7, wherein 1≤x≤2, and M is at least one element selected from Fe, Ni, Co, Mn and Cr.

[0015] In the present invention, it is preferred that the negative electrode layer contains a negative electrode active material composed of hard carbon.

[0016] In the present invention, it is preferred that the solid electrolyte layer contains a solid electrolyte which is at least one selected from the group consisting of β-alumina, β″-alumina, and NASICON crystal.

[0017] Effects of the Invention

[0018] According to the present invention, it is possible to provide an all-solid-state secondary battery that can achieve good output characteristics and cycle characteristics even when used at a high temperature of 150° C. or higher for a certain period of time. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 It is a schematic front cross-sectional view showing an all-solid-state secondary battery according to an embodiment of the present invention.

[0020] Figure 2 yes Figure 1 Schematic top cross-sectional view of section AA.

[0021] Figure 3 It is a schematic front cross-sectional view showing an all-solid-state secondary battery according to an embodiment of the present invention.

[0022] Figure 4 It is a graph showing the results of the charge and discharge test of Example 1. DETAILED DESCRIPTION

[0023] Hereinafter, preferred embodiments will be described. However, the following embodiments are merely illustrative, and the present invention is not limited to the following embodiments. In addition, in each of the drawings, components having substantially the same function are sometimes referred to with the same reference numerals.

[0024] (All-solid-state secondary battery)

[0025] Figure 1 This is a schematic cross-sectional view showing an all-solid-state secondary battery according to an embodiment of the present invention. Figure 2 yes Figure 1 A schematic top cross-sectional view of the AA section of FIG. Figure 1 , 2 As shown, the all-solid-state secondary battery 1 includes a solid electrolyte layer 2, a positive electrode layer 3, a negative electrode layer 4, a first collector layer 5, a second collector layer 6 and a sealing layer 7. As the all-solid-state secondary battery 1, an all-solid-state lithium ion secondary battery, an all-solid-state sodium ion secondary battery, an all-solid-state magnesium ion secondary battery, etc. can be cited. Hereinafter, an all-solid-state sodium ion secondary battery is used as an example for explanation, but the following embodiments can be applied to a general all-solid-state secondary battery.

[0026] In the present embodiment, the solid electrolyte layer 2 is composed of a sodium ion conductive oxide. The solid electrolyte layer 2 has a first main surface 2a and a second main surface 2b facing each other.

[0027] A positive electrode layer 3 is provided on the first main surface 2a of the solid electrolyte layer 2. The positive electrode layer 3 contains a positive electrode active material capable of absorbing and detaching (releasing) sodium. In addition, a first collector layer 5 is provided on the main surface 3a of the positive electrode layer 3 on the opposite side of the side on which the solid electrolyte layer 2 is provided. In addition, in order to improve the electronic conductivity at the interface between the positive electrode layer 3 and the first collector layer 5, it is preferred to form a thin film of metal aluminum or the like on the surface of the positive electrode layer 3 in advance by sputtering, vacuum evaporation, etc. In addition, when the thin film is a sputtered film formed by sputtering, it is excellent in adhesion to the positive electrode layer 3, so it is preferred.

[0028] A negative electrode layer 4 is provided on the second main surface 2b of the solid electrolyte layer 2. The negative electrode layer 4 contains a negative electrode active material capable of absorbing and releasing sodium. In addition, a second collector layer 6 is provided on the main surface 4a of the negative electrode layer 4 on the opposite side to the side on which the solid electrolyte layer 2 is provided. In addition, in order to improve the electronic conductivity at the interface between the negative electrode layer 4 and the second collector layer 6, it is preferred to form a thin film of metal aluminum or the like on the surface of the negative electrode layer 4 in advance by sputtering, vacuum evaporation, etc. In addition, when the thin film is a sputtered film formed by sputtering, it is excellent in adhesion to the negative electrode layer 4, so it is preferred.

[0029] A sealing layer 7 is provided between the outer peripheral edge 5a of the first collector layer 5 and the outer peripheral edge 6a of the second collector layer 6. A solid electrolyte layer 2, a positive electrode layer 3 and a negative electrode layer 4 are arranged in the internal space 8 surrounded by the first collector layer 5, the second collector layer 6 and the sealing layer 7. In addition, the internal space 8 surrounded by the first collector layer 5, the second collector layer 6 and the sealing layer 7 is a vacuum. Therefore, even when used at a high temperature of more than 150°C for a certain period of time, the internal space 8 of the battery will not expand, and an all-solid-state secondary battery 1 capable of achieving good output characteristics and cycle characteristics can be provided. In addition, the vacuum mentioned here means a pressure state below 1000Pa, and the higher the vacuum degree of the internal space 8 of the battery, the better the battery characteristics. The vacuum degree of the internal space 8 of the battery is preferably below 500Pa, and more preferably below 100Pa. In addition, by making the internal space 8 of the battery evacuated, the two current collector layers are always pressurized from the outside at atmospheric pressure, and the contact state between the positive electrode layer 3 and the first current collector layer 5, and between the negative electrode layer 4 and the second current collector layer 6 can be maintained stably for a long time. Figure 1 In the embodiment, the sealing layer 7 is arranged between the lower surface of the outer edge 5a of the first collector layer 5 and the upper surface of the outer edge 6a of the second collector layer 6, but the sealing layer 7 can also be arranged in a manner of contacting with the side surface of the outer edge 5a of the first collector layer 5 and the side surface of the outer edge 6a of the second collector layer 6, or the sealing layer 7 can be arranged in a manner of contacting with the side surface of the outer edge 5a of the first collector layer 5 and the upper surface of the outer edge 6a of the second collector layer 6, or the sealing layer 7 can be arranged in a manner of contacting with the lower surface of the outer edge 5a of the first collector layer 5 and the side surface of the outer edge 6a of the second collector layer 6.

[0030] In addition to the above structures, Figure 3As shown, in order to suppress the short circuit caused by the contact between the end of the solid electrolyte layer 2 formed with the positive electrode layer 3 and the negative electrode layer 4 and the first collector layer 5 or the second collector layer 6, an insulating component 9 can also be provided in the internal space 8 of the battery. The insulating component 9 is preferably in the form of a thin sheet. The thickness of the insulating component 9 is preferably 50 μm or less, more preferably 30 μm or less, preferably 0.5 μm or more, and more preferably 1 μm or more. The insulating component 9 preferably has a heat resistance of 150°C or more. The insulating component 9 is preferably composed of an inorganic material such as ceramics and glass, but a resin can also be used as long as it has a heat resistance of 150°C or more. As the insulating component 9 made of inorganic materials such as ceramics and glass, ceramic sheets, glass sheets, ceramic fiber nonwoven fabrics, glass fiber nonwoven fabrics, ceramic wool, glass wool, etc. formed of powders and fibers of aluminum oxide, zirconium oxide, aluminum nitride, silicon nitride, and glass can be used; as the insulating component 9 made of resin, ceramic sheets, glass sheets, ceramic fiber nonwoven fabrics, glass fiber nonwoven fabrics, ceramic wool, glass wool, etc. formed of powders and fibers of aluminum oxide, zirconium oxide, aluminum nitride, silicon nitride, and glass can be listed; polyphenylene sulfide, polyimide resin, polytetrafluoroethylene, polyamide-imide, silicone resin, allyl resin, etc. can be listed. In addition, in Figure 3 In the embodiment, the insulating member 9 is provided in both the internal space 8 between the solid electrolyte layer 2 and the first current collector layer 5 and the internal space 8 between the solid electrolyte layer 2 and the second current collector layer 6, but may be provided in only one of them.

[0031] In this embodiment, it is more preferred that the solid electrolyte layer 2, the positive electrode layer 3, the negative electrode layer 4, the first collector layer 5, the second collector layer 6 and the sealing layer 7 constituting the all-solid-state secondary battery 1 are all formed of inorganic substances, and it is more preferred that all components constituting the all-solid-state secondary battery 1 are formed of inorganic substances. "Formed of inorganic substances" means that it does not contain organic substances such as resins (for example, less than 0.1wt%) except for impurities, and is composed of inorganic substances such as metals, ceramics, and glass.

[0032] In the above embodiment, the capacity ratio of the negative electrode layer 3 to the positive electrode layer 4 (negative electrode layer / positive electrode layer) is preferably less than 1.10, more preferably less than 0.80, and further preferably less than 0.60. When the capacity ratio of the negative electrode layer 3 to the positive electrode layer 4 (negative electrode layer / positive electrode layer) is below the above upper limit, the charge and discharge efficiency of the all-solid-state secondary battery 1 can be further improved, and further high energy density can be achieved. In addition, the capacity ratio of the negative electrode layer 4 to the positive electrode layer 3 (negative electrode layer / positive electrode layer) is preferably greater than 0.10, more preferably greater than 0.30, and further preferably greater than 0.40. When the capacity ratio of the negative electrode layer 4 to the positive electrode layer 3 (negative electrode layer / positive electrode layer) is greater than the above lower limit, the excessive precipitation of metallic sodium in the negative electrode layer 4 can be suppressed, and short circuit is less likely.

[0033] In addition, the capacity ratio of the negative electrode layer 3 to the positive electrode layer 4 (negative electrode layer / positive electrode layer) can be adjusted by, for example, the types of materials constituting the positive electrode layer 3 and the negative electrode layer 4, the positive electrode active material, the ratio of the negative electrode active material, and the thickness of the negative electrode layer 3 relative to the positive electrode layer 4.

[0034] For example, in the above-mentioned embodiment, when the positive electrode layer 3 includes a positive electrode active material composed of crystallized glass and the negative electrode layer 4 includes a negative electrode active material composed of hard carbon, the thickness ratio of the negative electrode layer 4 to the positive electrode layer 3 (negative electrode layer / positive electrode layer) is preferably 0.50 or less, more preferably 0.35 or less, and further preferably 0.25 or less, wherein the crystallized glass contains a material composed of the general formula Na x Crystals represented by MP2O7 (1≤x≤2, M is at least one element selected from Fe, Ni, Co, Mn and Cr). When the thickness ratio of the negative electrode layer 4 to the positive electrode layer 3 (negative electrode layer / positive electrode layer) is below the above upper limit, the charge and discharge efficiency of the all-solid-state sodium ion secondary battery can be further improved, and further high energy density can be achieved.

[0035] In addition, the thickness ratio of the negative electrode layer 4 to the positive electrode layer 3 (negative electrode layer / positive electrode layer) is preferably 0.025 or more, more preferably 0.050 or more, and further preferably 0.150 or more. When the thickness ratio of the negative electrode layer 4 to the positive electrode layer 3 (negative electrode layer / positive electrode layer) is above the above lower limit, the precipitation of metallic sodium in the negative electrode layer 4 can be further suppressed, and short circuit is more difficult. In addition, the cycle characteristics can be further improved.

[0036] In addition, the thickness of the positive electrode layer 3 is preferably 50 μm or more, more preferably 200 μm or more, preferably 1000 μm or less, more preferably 600 μm or less. In addition, the thickness of the negative electrode layer 4 is preferably 10 μm or more, more preferably 40 μm or more, preferably 200 μm or less, more preferably 150 μm or less, and further preferably 100 μm or less.

[0037] In addition, in the present invention, as described above, it is preferred that at the end of charging, metallic sodium is precipitated inside the negative electrode layer 4. In this case, the safety of the all-solid-state sodium ion secondary battery can be further improved.

[0038] In addition, in the present invention, each capacity of the positive electrode layer 3 and the negative electrode layer 4 can be calculated by multiplying the weight of the active material carried (supported) by the positive electrode layer 3 and the negative electrode layer 4 by the theoretical capacity of the active material. Alternatively, half cells (using metal Na at the opposite electrodes) are made for the positive electrode layer 3 and the negative electrode layer 4, respectively, and each half cell is charged and discharged, thereby measuring each capacity of the positive electrode layer 3 and the negative electrode layer 4. In addition, when measuring each capacity of the positive electrode layer 3 and the negative electrode layer 4 of an all-solid-state sodium ion secondary battery (finished product), the all-solid-state sodium ion secondary battery is decomposed to separate the positive electrode layer 3 and the negative electrode layer 4, and after making half cells, each half cell is charged and discharged, thereby measuring each capacity of the positive electrode layer 3 and the negative electrode layer 4.

[0039] Hereinafter, the details of each layer constituting the all-solid-state secondary battery 1 of the present invention will be described.

[0040] (Solid electrolyte layer 2)

[0041] The solid electrolyte constituting the solid electrolyte layer 2 is preferably formed of an ion conductive material such as a sodium ion conductive oxide. As the sodium ion conductive oxide, there can be cited a compound containing at least one element selected from Al, Y, Zr, Si and P, Na, and O. As a specific example thereof, there can be cited β-alumina or NASICON crystals with excellent sodium ion conductivity. Preferably, the sodium ion conductive oxide is β-alumina or β"-alumina. They have better sodium ion conductivity.

[0042] There are two types of β-alumina crystals: β-alumina (theoretical composition formula: Na2O·11Al2O3) and β”-alumina (theoretical composition formula: Na2O·5.3Al2O3). β”-alumina is a metastable substance, so it is usually used to add Li2O and MgO as stabilizers. Compared with β-alumina, β”-alumina has a higher sodium ion conductivity, so it is preferred to use β”-alumina alone or a mixture of β”-alumina and β-alumina, and it is more preferred to use Li2O stabilized β”-alumina (Na 1.7 Li 0.3 Al 10.7 O 17 ) or MgO stabilized β"-alumina ((Al 10.32 Mg 0.68 O 16 )(Na 1.68 O)).

[0043] As NASICON crystal, Na3Zr2Si2PO4 can be cited. 12 、Na 3.2 Zr 1.3 Si 2.2 P 0.7O 10.5 、Na3Zr 1.6 Ti 0.4 Si2PO 12 、Na3Hf2Si2PO 12 、Na 3.4 Zr 0.9 Hf 1.4 Al 0.6 Si 1.2 P 1.8 O 12 、Na3Zr 1.7 Nb 0.24 Si2PO 12 、Na 3.6 Ti 0.2 Y 0.7 Si 2.8 O9、Na3Zr 1.88 Y 0.12 Si2PO 12 、Na 3.12 Zr 1.88 Y 0.12 Si2PO 12 、Na 3.6 Zr 0.13 Yb 1.67 Si 0.11 P 2.9 O 12 As NASICON crystals, especially Na 3.12 Zr 1.88 Y 0.12 Si2PO 12 It is preferred because of its excellent sodium ion conductivity.

[0044] The solid electrolyte layer 2 can be manufactured by mixing raw material powders, shaping the mixed raw material powders, and then firing them. For example, it can be manufactured by slurrying the raw material powders to make a green sheet, and then firing the green sheet. Alternatively, it can be manufactured by a sol-gel method.

[0045] The thickness of the solid electrolyte layer 2 is preferably in the range of 5 μm to 1000 μm, more preferably in the range of 10 μm to 200 μm, and particularly preferably in the range of 20 μm to 100 μm. If the thickness of the solid electrolyte layer 2 is too thin, the mechanical strength is reduced and easily damaged, so it is easy to cause an internal short circuit. When the thickness of the solid electrolyte layer 2 is too thick, the sodium ion conduction distance accompanying charge and discharge becomes longer, so the internal resistance becomes higher, and the discharge capacity and operating voltage are easily reduced. In addition, the energy density per unit volume of the all-solid-state sodium ion secondary battery is also easily reduced.

[0046] (Positive electrode layer 3)

[0047] The positive electrode active material contained in the positive electrode layer 3 is not particularly limited, but is preferably a positive electrode active material composed of crystallized glass, wherein the crystallized glass contains a general formula of Na x M y P2O z (1≤x≤2.8, 0.95≤y≤1.6, 6.5≤z≤8, M is at least one element selected from Fe, Ni, Co, Mn and Cr). Among them, a positive electrode active material composed of a crystallized glass is more preferred, and the crystallized glass contains a general formula Na x Crystals represented by MP2O7 (1≤x≤2, M is at least one element selected from Fe, Ni, Co, Mn and Cr). As such positive electrode active material crystals, for example, Na2FeP2O7, Na2CoP2O7, Na2NiP2O7, etc. can be used.

[0048] Wherein, in the present invention, crystallized glass refers to a glass in which a precursor glass containing an amorphous phase is heated (fired) to separate out crystals (crystallization). The amorphous phase can be completely transformed into a crystalline phase, or a residual amorphous phase can be obtained. In addition, one crystal can be separated out, or more than two crystals can be separated out. For example, crystallized glass can be judged to be a crystallized glass according to the peak angle represented by powder X-ray diffraction (XRD).

[0049] In addition, the positive electrode layer 3 may contain a sodium ion conductive solid electrolyte and a conductive auxiliary agent. The ratio of each material in the positive electrode layer 3 may be, for example, 60% to 99.9% of the positive electrode active material, 0% to 30% of the sodium ion conductive solid electrolyte, and 0.1% to 10% of the conductive auxiliary agent in terms of mass %.

[0050] In addition, the sodium ion conductive solid electrolyte can use, for example, the substance described in the solid electrolyte layer 2 column. The sodium ion conductive solid electrolyte is preferably used in a powdered form. The average particle size of the powder of the sodium ion conductive solid electrolyte is preferably 0.05 μm or more and 3 μm or less, more preferably 0.05 μm or more and less than 1.8 μm, further preferably 0.05 μm or more and 1.5 μm or less, particularly preferably 0.1 μm or more and 1.2 μm or less, and most preferably 0.1 μm or more and 0.7 μm or less.

[0051] In addition, as a conductive aid, for example, conductive carbon can be used. As conductive carbon, for example, acetylene black, carbon black, Ketjen black, vapor-grown carbon fiber conductive aid (VGCF), carbon nanotubes, etc. can be cited. The conductive aid is preferably a carbon-based conductive aid composed of the above-mentioned materials.

[0052] The positive electrode layer 3 can be formed, for example, by forming an electrode material layer containing a positive electrode active material precursor and, as required, a sodium ion conductive solid electrolyte powder and a conductive aid on the first main surface 2a of the solid electrolyte layer 2, and firing the electrode material layer. The electrode material layer can be obtained, for example, by applying (i.e., coating) a paste containing a positive electrode active material precursor and, as required, a solid electrolyte powder and a conductive aid (i.e., the paste contains a positive electrode active material precursor, and, as required, contains a solid electrolyte powder and a conductive aid) and drying. The paste may contain a binder, a plasticizer (plasticizer) or a solvent, etc. as required. In addition, the electrode material layer may also be a powder compact.

[0053] The drying temperature of the paste is not particularly limited, and can be, for example, 30° C. to 150° C. The drying time of the paste is not particularly limited, and can be, for example, 5 minutes to 600 minutes.

[0054] The firing atmosphere is preferably a reducing atmosphere. The firing temperature (maximum temperature) can be, for example, 400° C. to 600° C., and the holding time at the temperature can be, for example, 5 minutes to less than 3 hours.

[0055] Positive electrode active material precursor:

[0056] The positive electrode active material precursor (positive electrode active material precursor powder) is preferably composed of an amorphous oxide material that generates active material crystals by firing. When the positive electrode active material precursor powder is composed of an amorphous oxide material, active material crystals can be generated during firing, softening and flowing to form a dense positive electrode layer 3. In addition, when the positive electrode layer 3 contains a solid electrolyte, the positive electrode active material and the solid electrolyte can also be integrated. Alternatively, when the positive electrode layer 3 is in contact with the solid electrolyte layer 2, the two can be integrated. As a result, it is preferred because an ion conduction path can be formed better. In addition, in the present invention, "amorphous oxide material" is not limited to completely amorphous oxide materials, but also includes materials containing a portion of crystals (for example, a crystallinity of less than 10%).

[0057] The positive electrode active material precursor powder preferably contains Na2O 25% to 55%, Fe2O3+Cr2O3+MnO+CoO+NiO 10% to 30% and P2O5 25% to 55% in terms of mole % of the following oxides. The reasons for limiting the composition are described below. In the following description of the content of each component, "%" means "mole %" unless otherwise specified.

[0058] Na2O is composed of the general formula Na x M y P2O z(M is at least one transition metal element selected from Cr, Fe, Mn, Co and Ni, 1≤x≤2.8, 0.95≤y≤1.6, 6.5≤z≤8) The main component of the active material crystal represented by the content of Na2O is preferably 25% to 55%, more preferably 30% to 50%. When the content of Na2O is within the above range, the charge and discharge capacity can be further increased.

[0059] Fe2O3, Cr2O3, MnO, CoO and NiO are also composed of the general formula Na x M y P2O z The main component of the active material crystal represented by . The content of Fe2O3+Cr2O3+MnO+CoO+NiO is preferably 10% to 30%, and more preferably 15% to 25%. When the content of Fe2O3+Cr2O3+MnO+CoO+NiO is above the above lower limit, the charge and discharge capacity can be further increased. On the other hand, when the content of Fe2O3+Cr2O3+MnO+CoO+NiO is below the above upper limit, it is possible to prevent undesirable crystals of Fe2O3, Cr2O3, MnO, CoO or NiO from precipitating. In addition, in order to further improve the cycle characteristics, it is preferred to actively contain Fe2O3. The content of Fe2O3 is preferably 1% to 30%, more preferably 5% to 30%, further preferably 10% to 30%, and particularly preferably 15% to 25%. The content of each component of Cr2O3, MnO, CoO and NiO is preferably 0% to 30%, more preferably 10% to 30%, and further preferably 15% to 25%. In addition, when at least two components selected from Fe2O3, Cr2O3, MnO, CoO and NiO are contained, the total amount is preferably 10% to 30%, and more preferably 15% to 25%.

[0060] P2O5 is also composed of the general formula Na x M y P2O z The main component of the active material crystal represented by P2O5 is preferably 25% to 55%, more preferably 30% to 50%. When the content of P2O5 is within the above range, the charge and discharge capacity can be further increased.

[0061] In addition to the above-mentioned components, the positive electrode active material precursor powder may also contain V2O5, Nb2O5, MgO, Al2O3, TiO2, ZrO2 or Sc2O3. These components have the effect of improving electrical conductivity (electronic conductivity), and the high-speed charge and discharge characteristics are easily improved. The content of the above-mentioned components is preferably 0% to 25% in total, and more preferably 0.2% to 10%. When the content of the above-mentioned components is below the above-mentioned upper limit, it is difficult to produce heterogeneous crystals that do not contribute to the battery characteristics, and the charge and discharge capacity can be further increased.

[0062] In addition, the positive electrode active material precursor powder may contain SiO2, B2O3, GeO2, Ga2O3, Sb2O3 or Bi2O3 in addition to the above-mentioned components. By containing these components, the glass forming ability is further improved, and it is easy to obtain a more homogeneous positive electrode active material precursor powder. The content of the above-mentioned components is preferably 0% to 25% in total, and more preferably 0.2% to 10%. Because these components do not contribute to battery characteristics, if their content is too much, there is a tendency for the charge and discharge capacity to decrease.

[0063] The positive electrode active material precursor powder is preferably prepared by melting and molding the batches of raw materials. According to this method, it is easy to obtain an amorphous positive electrode active material precursor powder with excellent homogeneity, so it is preferred. Specifically, the positive electrode active material precursor powder can be manufactured as described below.

[0064] First, the raw materials are modulated in a manner to obtain a batch batch of raw materials in a desired composition. Next, the obtained batch batch of raw materials is melted. The melting temperature is appropriately adjusted so that the raw material batch is uniformly melted. For example, the melting temperature is preferably above 800°C, more preferably above 900°C. The upper limit of the melting temperature is not particularly limited, but if the melting temperature is too high, it will lead to energy loss, evaporation of sodium components, etc., and therefore it is preferably below 1500°C, more preferably below 1400°C.

[0065] The obtained molten material is then formed into a film by a method which is not particularly limited, and for example, the molten material may be flowed between a pair of cooling rolls and formed into a film while being rapidly cooled, or may be flowed into a casting mold and formed into an ingot.

[0066] Next, the obtained molded body is crushed to obtain a positive electrode active material precursor powder. The average particle size of the positive electrode active material precursor powder is preferably 0.01 μm or more and less than 0.7 μm, more preferably 0.03 μm or more and 0.6 μm or less, further preferably 0.05 μm or more and 0.6 μm or less, and particularly preferably 0.1 μm or more and 0.5 μm or less.

[0067] Adhesives:

[0068] Binders are materials used to integrate raw materials (raw material powders) with each other. Examples of binders include cellulose derivatives such as carboxymethyl cellulose, hydroxypropyl methyl cellulose, hydroxypropyl cellulose, ethyl cellulose, hydroxyethyl cellulose, and hydroxymethyl cellulose, or water-soluble polymers such as polyvinyl alcohol; thermosetting resins such as thermosetting polyimide, phenolic resin, epoxy resin, urea resin, melamine resin, unsaturated polyester resin, and polyurethane; polycarbonate resins such as polypropylene carbonate; and polyvinylidene fluoride.

[0069] (Negative electrode layer 4)

[0070] The negative electrode active material contained in the negative electrode layer 4 is not particularly limited, and for example, carbon electrode materials such as hard carbon and soft carbon can be used. The carbon electrode material is preferably hard carbon. However, the negative electrode active material may also include alloy-based negative electrode active materials such as tin, bismuth, lead, and phosphorus that can absorb sodium, or metallic sodium. In addition, the negative electrode layer 4 is preferably not a negative electrode layer composed of a single phase of metallic sodium.

[0071] The negative electrode layer 4 may further include a sodium ion conductive solid electrolyte and a conductive aid. The ratio of each material in the negative electrode layer 4 may be, for example, 60% to 95% of the negative electrode active material, 5% to 35% of the sodium ion conductive solid electrolyte, and 0% to 5% of the conductive aid in terms of mass %. Among them, the sodium ion conductive solid electrolyte may be, for example, the substance described in the solid electrolyte layer column. The conductive aid may be, for example, the conductive aid described in the positive electrode layer 3 column.

[0072] Hereinafter, as an example, a method for forming the negative electrode layer 4 including a carbon electrode material as a negative electrode active material and a sodium ion conductive solid electrolyte will be described.

[0073] Negative electrode layer 4 formation method:

[0074] First, prepare a paste containing a carbon electrode material precursor and a sodium ion conductive solid electrolyte. When preparing the paste, first, prepare a sodium ion conductive solid electrolyte precursor. In addition, at this stage, it is preferred to prepare a sodium ion conductive solid electrolyte precursor solution. Specific examples of sodium ion conductive solid electrolyte precursors and solutions thereof are described later. In addition, prepare a carbon electrode material precursor (a precursor of a carbon electrode material composed of hard carbon). Appropriate sugars, biomass or polymers, etc. can be used in the carbon electrode material precursor.

[0075] Next, the sodium ion conductive solid electrolyte precursor solution and the carbon electrode material precursor are mixed and then dried. Thus, a powder of a mixture of the sodium ion conductive solid electrolyte precursor and the carbon electrode material precursor is obtained. Next, the powder of the above mixture is crushed and then mixed with a conductive auxiliary agent and a binder in an organic solvent. The organic solvent can use, for example, N-methyl-2-pyrrolidone. Thus, a paste is obtained.

[0076] Next, apply the paste to the second main surface 2b of the solid electrolyte layer 2. In this way, a lamination process is performed to laminate the solid electrolyte layer 2 and the paste as the electrode material layer. Next, the laminate of the solid electrolyte layer 2 and the paste is fired, for example, under an N2 atmosphere at a temperature exceeding 600°C and below 1300°C. In addition, the above-mentioned firing can be carried out in an inactive atmosphere. For example, the above-mentioned firing can be carried out in an Ar, Ne or He atmosphere, or can also be carried out in a vacuum. In addition, the firing can also be carried out in a reducing atmosphere containing H2. When firing in an inactive atmosphere or a reducing atmosphere, the initial charge and discharge efficiency of the negative electrode active material can be further improved, so it is preferred. In addition, as long as the carbon electrode is not oxidized or oxidatively decomposed during firing, a small amount of oxygen may also be contained in the atmosphere. The oxygen concentration can be, for example, below 1000 ppm, but is not limited to this. As described above, the negative electrode layer 4 can be produced.

[0077] Carbon electrode material precursor:

[0078] When sugar is used as a carbon electrode material precursor, for example, sucrose, cellulose, D-glucose, sucrose, etc. can be cited. When biomass is used as a carbon electrode material precursor, for example, corn stalks, sorghum stalks, pine cones, mangosteen, nut shells, rice husks, dandelions, the core of grain straw, ramie fiber, cotton, kelp, coconut endocarp, etc. can be cited. When a polymer is used as a carbon electrode material precursor, for example, PAN (polyacrylonitrile), asphalt, PVC (polyvinyl chloride) nanofibers, polyaniline, sodium polyacrylate, tires (tire polymers), phosphorus-doped PAN, etc. can be cited.

[0079] Sodium ion conductive solid electrolyte precursor and solution thereof:

[0080] When the sodium conductive solid electrolyte is β-alumina, the sodium conductive solid electrolyte precursor can be obtained by mixing aluminum nitrate, sodium nitrate, and lithium nitrate, for example. At this time, the ratio of the above materials is adjusted to achieve the target composition ratio of the sodium ion conductive solid electrolyte.

[0081] In the sodium ion conductive solid electrolyte, NASICON type crystal, Na5XSi4O 12In the case of a sodium-conductive solid electrolyte precursor solution (X is a transition metal element of Group 3, preferably at least one element selected from rare earth elements), a solution containing sodium element and transition metal element, and carbonate ions constituting the sodium-conductive solid electrolyte can be listed as a sodium-conductive solid electrolyte precursor solution. In addition, in the solution, the sodium element is contained in the form of sodium ions, and the transition metal element is contained in the form of transition metal ions. The sodium-ion-conductive solid electrolyte precursor is composed of, for example, a gelled product or a dried product of the sodium-ion-conductive solid electrolyte precursor solution. Moreover, the above-mentioned sodium-ion-conductive solid electrolyte is composed of a sintered product of the sodium-ion-conductive solid electrolyte precursor.

[0082] Furthermore, the sodium ion conductive solid electrolyte precursor solution may contain nitrate ions instead of carbonate ions.

[0083] In the sodium ion conductive solid electrolyte precursor solution, it is preferred that the carbonate ions are bidentately (bidentate) coordinated to the transition metal element. In this case, the transition metal element is likely to exist stably in the solution.

[0084] In addition, as a counter ion of the sodium ion, it is preferable to contain NR 4+ (In the formula, each R is independently one or more substituents selected from H, CH3, C2H5 and CH2CH2OH.) In this way, the transition metal element can easily exist stably in the solution.

[0085] The sodium ion conductive solid electrolyte precursor solution can be obtained by, for example, mixing water glass (sodium silicate), sodium tripolyphosphate, and an aqueous zirconium carbonate ammonia solution.

[0086] As the binder, the binder described in the section of the positive electrode layer 3 can be used.

[0087] (First current collector layer 5 and second current collector layer 6)

[0088] There is no particular limitation on the materials of the first collector layer 5 and the second collector layer 6, and metal materials such as aluminum, titanium, silver, copper, stainless steel or alloys thereof can be used respectively. The above-mentioned metal materials can be used alone or in combination of two or more. In addition, their alloys refer to alloys containing at least one of the above-mentioned metals. The thickness of the first collector layer 5 and the second collector layer 6 is not particularly limited, and can be set in the range of 10μm to 1000μm, respectively. The first collector layer 5 and the second collector layer 6 are preferably larger than the solid electrolyte layer 2, the positive electrode layer 3, and the negative electrode layer 4 so that the outer periphery 5a and the outer periphery 6a can be formed. Figure 1 In the embodiment, the width of the first current collector layer 5 and the second current collector layer 6 extending from the solid electrolyte layer 2 is preferably 0.2 mm to 20 mm, and more preferably 0.5 mm to 10 mm.

[0089] (Sealing layer 7)

[0090] The sealing layer 7 is a layer provided to maintain the vacuum of the internal space 8 in the all-solid-state secondary battery 1. The glass used in the sealing layer 7 preferably has a softening point of 500° C. or less, more preferably 470° C. or less, and further preferably 450° C. or less, from the viewpoint that the glass has thermal stability, chemical stability, can maintain a vacuum, and is easy to handle as a powder state or paste. For example, Bi2O3-B2O3 glass can be used.

[0091] As a glass composition, the bismuth-based glass preferably contains, in mol%, 25 to 60% of Bi2O3, 10 to 35% of B2O3, and 1 to 40% of CuO+MnO, but is not limited to this composition.

[0092] Hereinafter, a method for forming the sealing layer 7 will be described as an example.

[0093] Sealing layer 7 forming method:

[0094] First, the raw material powder prepared in a manner to obtain the desired glass composition is melted at 700-1000°C for 1-2 hours until a homogeneous glass is obtained. Next, the obtained molten glass is formed into a film shape, etc., and then crushed and classified to produce glass powder. The average particle size D50 of the glass powder is preferably about 1-20 μm. In order to match the thermal expansion coefficient with the first and second collector layers (5, 6) or to improve the mechanical strength of the sealing layer 7, various refractory filler powders can also be added to the glass powder and mixed to produce a sealing material.

[0095] The amount of the refractory filler powder added can be within a range that does not inhibit the fluidity of the glass powder, and can be up to 40% by volume.

[0096] As refractory filler, zircon, zirconium oxide, tin oxide, quartz, β-spodumene, cordierite, willemite, mullite, quartz glass, β-eucryptite, β-quartz, zirconium phosphate, zirconium tungstate phosphate, zirconium tungstate, NbZr (PO4)3 and other compounds with the basic structure of [AB2 (MO4)3] (A is Li, Na, K, Mg, Ca, Sr, Ba, Zn, Cu, Ni, Mn, etc., B is Zr, Ti, Sn, Nb, Al, Sc, Y, etc., M is P, Si, W, Mo, etc.) or their solid solution can be used. Zirconium phosphate, cordierite, willemite, zirconium tungstate phosphate are particularly preferred. These refractory fillers have the properties of low thermal expansion coefficient and high mechanical strength, and are good in compatibility with Bi2O3-B2O3 system glass powder.

[0097] Next, a vehicle is added to the sealing material for mixing, thereby preparing a sealing material paste. The vehicle is mainly composed of an organic solvent and a resin, and the resin is added for the purpose of adjusting the viscosity of the paste. In the case where the softening point of the sealing material is low and the degreasing process has problems, a high-viscosity organic solvent that does not contain resin can also be used. In addition, surfactants, thickeners, etc. can also be added as needed. In addition, in order to pre-remove trace amounts of moisture and organic matter attached to the surface of the glass powder and refractory filler powder, the glass powder and refractory filler powder can also be subjected to a vacuum treatment for a certain period of time near the glass transition temperature of the glass powder before mixing the glass powder and refractory filler powder with the vehicle.

[0098] The organic solvent preferably has a low boiling point (for example, a boiling point of 300°C or less), a small amount of residue after firing, and an organic solvent that does not deteriorate the glass, and its content is preferably 10 to 40% by mass. As the organic solvent, propylene carbonate, toluene, N,N'-dimethylformamide (DMF), 1,3-dimethyl-2-imidazolidinone (DMI), dimethyl carbonate, butyl carbitol acetate (BCA), isoamyl acetate, dimethyl sulfoxide, acetone, methyl ethyl ketone, etc. are preferably used. In addition, as the organic solvent, higher alcohols are more preferably used. Since higher alcohols have viscosity themselves, pastes can be formed even without adding resin to the carrier. In addition, pentanediol and its derivatives, specifically diethylpentanediol (C9H 20 O2) also has excellent viscosity, so it can be used as a solvent.

[0099] The resin preferably has a low decomposition temperature, produces little residue after firing, and is unlikely to deteriorate the glass, and its content is preferably 0.1 to 20% by mass. As the resin, nitrocellulose, polyethylene glycol derivatives, polyethylene carbonate, acrylate (acrylic resin), etc. are preferably used.

[0100] Next, use a dispenser, screen printer or other coating machine to apply the sealing material paste to the sealing parts of the outer periphery (5a, 6a) of the first collector layer 5 and the second collector layer 6, dry it at a temperature at which the organic solvent evaporates, degrease and soften the sealing material and flow it, and in order to bond with the collector material, perform glaze treatment at a temperature above the softening point of the glass contained in the sealing material. In addition, in order to fully degrease, the temperature at which the resin decomposes may be maintained for a certain time before rising to a temperature above the softening point of the glass contained in the sealing material. Then, bring the other sealed objects into contact, and again perform heat treatment in a vacuum above the softening point of the glass contained in the sealing material, thereby causing the glass powder to soften and flow, and the two are sealed. Among them, it is also possible that after the sealing material paste is only applied to the sealing parts of the outer periphery of either the first collector layer 5 or the second collector layer 6, bring the other sealed objects into contact, and perform heat treatment in a vacuum above the softening point of the glass contained in the sealing material, thereby causing the glass powder to soften and flow, and the two are sealed. In addition, when performing heat treatment in a vacuum, in order to clarify and remove bubbles caused by dissolved gas inside the glass and air layers remaining at the interfaces between powder glasses, a certain amount of inert gas such as N2 can be introduced near the softening point, thereby performing re-pressurization treatment until it reaches atmospheric pressure.

[0101] (Example)

[0102] Hereinafter, the present invention will be described in more detail based on specific examples. The present invention is not limited to the following examples at all, and can be implemented by appropriately changing the scope of the present invention.

[0103] (Example 1)

[0104] (a) Preparation of Solid Electrolyte Layer 2

[0105] The raw material was pre-calcined and crushed at 1200°C to produce β-alumina powder so as to have the composition of β"-alumina that becomes the solid electrolyte. The β-alumina powder was crushed with a ball mill, and a binder and a solvent were mixed to produce a paste. A green sheet was formed from the paste, and fired at 1550°C for 30 minutes to form a solid electrolyte layer 2 with a square side of 36 mm and a thickness of 0.1 mm.

[0106] (b) Preparation of positive electrode paste

[0107] As a glass composition, raw materials prepared in a molar ratio of 40Na2O-20Fe2O3-40P2O5 were melted in the air at 1200°C for 1 hour and cooled using a double roller to produce a glass film. The obtained glass film was mixed with 5 mm φ ZrO2 jade, 3 mm φ ZrO2 jade, and 1 mm φ ZrO2 jade in ethanol and pulverized in a ball mill for 60 hours to obtain a specific surface area of ​​11.1 m2 The obtained glass powder was further pulverized in ethanol together with φ0.3 mm ZrO2 jade using a planetary ball mill at 300 rpm for 5 hours, thereby obtaining a specific surface area of ​​32.1 m 2 / g of glass powder.

[0108] The obtained glass powder was 83% by mass, and β"-alumina (specific surface area of ​​45.2 m 2 / g) 13 mass % and 4 mass % of acetylene black (AB) as a conductive aid were mixed to prepare a positive electrode composite material powder. For the obtained positive electrode composite material powder 100 mass %, 15 mass % of polypropylene carbonate (PPC) as a binder was added, and N-methyl-2-pyrrolidone as a solvent was added in a manner such that the concentration of the positive electrode composite material powder became 50 mass %. It was mixed with a rotation and revolution mixer to prepare a positive electrode paste.

[0109] (c) Preparation of negative electrode paste

[0110] In order to obtain a composition ratio of Na3Zr2Si2PO 12 NASICON crystals, weigh water glass (sodium silicate: Na2O·3SiO2), ammonium zirconium carbonate aqueous solution ((NH4)2Zr(OH)2(CO3)2), sodium tripolyphosphate (Na5P3O 10 ) totaling 25 g. They were added to 150 g of pure water and stirred at 50 ° C for 24 hours using a hot stirrer. Thus, a sodium ion conductive solid electrolyte precursor solution (pH = 9.7) was obtained. Then, the solution was allowed to stand in a thermostatic bath at 5 ° C overnight to gel. In the above manner, a sodium ion conductive solid electrolyte precursor was obtained.

[0111] Sucrose, a hard carbon source of a carbon electrode material precursor, and a sodium ion conductive solid electrolyte precursor were mixed in a stirrer at a weight ratio of 4:1 for 1 hour to obtain a mixture. Then, the mixture was dried in a thermostatic bath at 60°C for 12 hours, and then vacuum dried at 100°C for 6 hours to obtain a powder of a mixture of a sodium ion conductive solid electrolyte precursor and a carbon electrode material precursor. Then, the powder of the mixture was crushed in an agate mortar to form a powder.

[0112] The powder of the mixture of the sodium ion conductive solid electrolyte precursor and the carbon electrode material precursor and the conductive aid (acetylene black) were weighed so that the weight ratio was 19:1, and mixed to obtain a mixed powder. For 60 parts by mass of the mixed powder, 40 parts by mass of hard carbon powder (average particle size D50 is 1 μm) were mixed to obtain a negative electrode composite material powder. Furthermore, for 100% by mass of the negative electrode composite material powder, 15% by mass of polypropylene carbonate (PPC) as a binder was added, and N-methyl-2-pyrrolidone was added as a solvent so that the concentration of the negative electrode composite material powder was 50% by mass. It was mixed with a rotation and revolution mixer to prepare a negative electrode paste.

[0113] (d) Formation of Negative Electrode Layer 4

[0114] The negative electrode paste was applied to the center of one main surface of the solid electrolyte layer 2 of 36 mm square and 0.1 mm thickness so that the thickness was 50 μm and the length of one side of the square was 34 mm. It was dried in a thermostatic bath at 60°C for 1 hour. Then, it was fired at 800°C for 2 hours in an N2 (99.99%) atmosphere to form the negative electrode layer 4. The load-bearing weight of the negative electrode layer 4 is calculated by (the weight of the stack after the negative electrode is formed) - (the weight of the solid electrolyte layer). The calculated load-bearing weight is multiplied by the ratio of the active material therein, 0.8, to calculate the weight of the hard carbon active material. In addition, the capacity of the hard carbon is set to 300 mAh / g per gram, and the capacity of the negative electrode layer 4 is calculated. As a result, the capacity of the negative electrode layer 4 is 0.49 mAh.

[0115] (e) Formation of positive electrode layer 3

[0116] The positive electrode paste is applied to the center of the main surface of the solid electrolyte layer 2 on the opposite side of the negative electrode layer 4 in such a manner that the thickness is 400μm and 34mm□. After drying in a thermostatic bath at 60°C for 2 hours, it is fired in an N2 / H2 (96 / 4 volume %) atmosphere at 500°C for 30 minutes to form a positive electrode layer 3. The load-bearing weight of the positive electrode layer 3 is obtained by (the weight of the laminate after the positive electrode is formed) - (the weight of the laminate before the positive electrode is formed). The weight of the Na2FeP2O7 active material is calculated by multiplying the calculated load-bearing weight by the ratio of the active material therein, 0.83. The capacity of the Na2FeP2O7 crystallized glass (Na2FeP2O7 active material) is set to a theoretical capacity of 97mAh / g per gram, and the capacity of the positive electrode layer 3 is calculated. As a result, the capacity of the positive electrode layer 3 is 1.4mAh.

[0117] (f) Preparation of sealing material paste

[0118] First, the raw material powder prepared in a glass composition of Bi2O3 43%, B2O3 22%, ZnO 23%, BaO 5%, CuO 6%, and Fe2O3 1% in mole % was melted at 1100°C for 2 hours until a homogeneous glass was obtained. Next, the obtained molten glass was formed into a film, etc., and then pulverized and classified to produce Bi2O3-B2O3 glass powder with an average particle size D50 of 10 μm. The softening point of the produced glass powder was 410°C, and the thermal expansion coefficient was 110×10 -7 / ℃ (30-300℃). In addition, the volume resistivity of the produced glass powder: Logρ (Ω·cm) is 10, showing good insulation properties. A resin composed of acrylic resin and an organic solvent composed of α-terpineol (terpineol) are added to the produced glass powder and adjusted to a viscosity suitable for screen printing and dispenser coating and kneaded to produce a sealing material paste.

[0119] The thermal expansion coefficient is a value measured using a TMA device in a temperature range of 30 to 300°C. As the measurement sample of the thermal expansion coefficient, a sample densely sintered at a temperature of 20°C above its softening point is used. The softening point is a value obtained by large-scale DTA. In DTA, the measurement atmosphere is air, the heating rate is 10°C / min, and the measurement starts from room temperature.

[0120] (g) Formation of Sealing Layer 7

[0121] Next, a 50 mm square, 100 μm thick SUS430 (thermal expansion coefficient: 107×10 -7 The sealing part of the outer peripheral edge 5a of the first collector layer 5 and the outer peripheral edge 6a of the second collector layer 6 formed by the first collector layer 5 and the second collector layer 6 is coated with a sealant paste using a dispenser, a screen printer or other coating machine in a manner such that the size is 44 mm□, the width is 2 mm, and the height is 1 mm, and then dried at 120°C for 15 minutes, and kept at 430°C in the atmosphere for 10 minutes, and glaze treatment is performed. Then, the solid electrolyte layer 2 formed with the positive electrode layer 3 and the negative electrode layer 4 is placed on the part surrounded by the sealing material of the first collector layer 5, and the second collector layer 6 is placed in a manner such that the sealing materials are in contact with each other, and a heat treatment is performed at 450°C for 20 minutes in a vacuum of 2 to 3 Pa, thereby forming a sealing layer 7, and a fully solid-state secondary battery 1 is manufactured.

[0122] (h) Charge and discharge test

[0123] Based on the positive electrode capacity, a constant current charge test was carried out in a constant temperature chamber at 60°C with a current value of 0.02C (50 hours of charge and discharge), and a constant current discharge test was carried out in constant temperature chambers at 60°C and 150°C with a current value of 0.02C (50 hours of charge and discharge).

[0124] [Evaluation results]

[0125] Figure 4 It is a graph showing the results of the charge and discharge test of Example 1.

[0126] like Figure 4 As shown, even when discharging at 150°C, stable output characteristics were obtained as at 60°C. In addition, charge and discharge tests were performed at 200°C, 250°C, and 300°C in the same manner as at 150°C, and the results confirmed that the same output characteristics were exhibited as at 150°C.

[0127] Description of Reference Numerals

[0128] 1…All-solid-state secondary battery

[0129] 2…Solid electrolyte layer

[0130] 3… Positive electrode layer

[0131] 4…Negative electrode layer

[0132] 5…1st current collector layer

[0133] 6…Second current collector layer

[0134] 7…Sealing layer

[0135] 8…Interior space.

Claims

1. An all-solid-state secondary battery, comprising a solid electrolyte layer, a positive electrode layer and a negative electrode layer, wherein the all-solid-state secondary battery is characterized in that: A first current collector layer provided on a main surface of the positive electrode layer on the opposite side to the side on which the solid electrolyte layer is disposed; A second current collector layer provided on a main surface of the negative electrode layer on the opposite side to the side on which the solid electrolyte layer is arranged; and a sealing layer provided between the outer periphery of the first current collector layer and the outer periphery of the second current collector layer and sealing the positive electrode layer and the negative electrode layer, An internal space surrounded by the first current collector layer, the second current collector layer, and the sealing layer is a vacuum.

2. The all-solid-state secondary battery according to claim 1, characterized in that: The sealing layer contains low-melting-point glass having a softening point of 500° C. or less.

3. The all-solid-state secondary battery according to claim 2, characterized in that: The sealing layer contains Bi2O3-B2O3 glass.

4. The all-solid-state secondary battery according to any one of claims 1 to 3, characterized in that: The positive electrode layer includes a positive electrode active material composed of a crystallized glass, wherein the crystallized glass contains a x A crystal represented by MP2O7, wherein 1≤x≤2, and M is at least one element selected from Fe, Ni, Co, Mn and Cr.

5. The all-solid-state secondary battery according to any one of claims 1 to 3, characterized in that: The negative electrode layer includes a negative electrode active material composed of hard carbon.

6. The all-solid-state secondary battery according to any one of claims 1 to 3, characterized in that: The solid electrolyte layer includes a solid electrolyte, and the solid electrolyte is at least one selected from β-alumina, β"-alumina, and NASICON crystal.

Citation Information

Cited By

  • Solid state structure battery and method of making the same

    CN122800718A