Thick plate narrow surface double-drum defect control method and extra-thick plate blank continuous casting device

The thick slabs are processed through four-stage heating and rolling processes, combined with the narrow-side copper plate design of the extra-thick slab continuous casting device, the double drum defect problem is solved, the cutting of the steel plate is reduced and the material of the thick plate is improved Rate.

CN118976783APending Publication Date: 2024-11-19NORTHEASTERN UNIV CHINA
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411055195.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

During the thick plate rolling process, double-drum defects lead to a large depth of the drum joint in the middle of the narrow surface of the steel plate, affecting the material yield and production efficiency.

Method used

The thick slab with a convex structure on narrow surfaces is treated by four-stage heating technology and rough rolling and finishing rolling technology. The temperature gradient is controlled by preheating, heating and homogenizing sections, and the vertical rolling and horizontal rolling technology is combined to reduce the double drum-shaped middle part. The depth of the drum joint and the narrow-sided copper plate working surface design in the extra-thick slab continuous casting device is formed to form a convex structure to reduce the drum joint depth.

Benefits of technology

Effectively reduce the amount of edge cutting of steel plates, improve the material yield of thick plates, reduce internal stress and defects, and improve product quality and production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118976783A_ABST
    Figure CN118976783A_ABST
Patent Text Reader

Abstract

The invention provides a thick plate narrow face double-drum defect control method and an extra-thick plate blank continuous casting device. The method comprises the steps that a thick plate blank with the narrow face provided with an outwards-protruding structure is produced; a four-section heating process is adopted for machining the thick plate blank with the narrow face provided with the outwards-protruding structure; roughly rolling a thick plate blank with a convex structure on the narrow surface to obtain an intermediate blank; performing finish rolling on the intermediate billet to obtain a target steel plate; wherein the thick plate blank with the convex structure on the narrow surface processed by adopting the four-section heating process comprises a preheating section, a heating section I, a heating section II and a soaking section, and the thick plate blank with the convex structure on the narrow surface is heated by adopting the four-section heating process; wherein rough rolling of the thick plate blank with the narrow face provided with the convex structure comprises first-stage longitudinal rolling; second-stage transverse rolling; third-stage longitudinal rolling; wherein the step of finish rolling of the intermediate billet comprises fourth-stage longitudinal rolling. By producing the thick plate blank with the convex structure on the narrow surface and cooperating with a four-section heating process, a rough rolling process and a finish rolling process, the depth of a drum seam in the middle of a double-drum shape after the thick plate blank is rolled can be reduced, so that the edge cutting amount of a steel plate is reduced, and the yield of the thick plate is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of metal casting, and specifically relates to a method for controlling defects of thick plate narrow surface double drums and a continuous casting device for extra-thick slabs. Background Art

[0002] Double-drum deformation is a defect parallel to the rolling direction that occurs at the edge during the rolling process of extra-thick slabs. This type of defect is located on the narrow side of the steel plate, and the narrow side of the steel plate is double-drum shaped. After rolling, the depth of the drum seam in the middle of the narrow side of the steel plate caused by the double-drum defect ranges from 30 to 80 mm. In the actual production process, it is necessary to trim the edge at the deepest position of the drum seam, which leads to a decrease in the yield rate and production efficiency of the thick plate, causing huge economic losses to the enterprise. Therefore, eliminating the double-drum defect is an important aspect of improving the yield rate of thick plates. Summary of the invention

[0003] Therefore, the technical problem to be solved by the present application is to provide a method for controlling the narrow side double-drum defects of thick plates and a continuous casting device for ultra-thick slabs, which can reduce the depth of the narrow side double-drum gap of the thick slab after rolling, reduce the trimming amount of the steel plate, and improve the yield rate of the thick plate.

[0004] In order to solve the above problems, the present application provides a method for controlling the defects of thick plate narrow surface double drums, comprising:

[0005] Produce thick slabs with convex structures on the narrow side;

[0006] A four-stage heating process is used to process thick slabs with convex structures on the narrow side;

[0007] Rough rolling of thick slab with convex structure on narrow side to obtain intermediate slab;

[0008] Finish rolling the intermediate billet to obtain the target steel plate;

[0009] The thickness of the thick slab with the narrow side having the convex structure is 300 mm to 600 mm, and the convex height of the thick slab with the narrow side having the convex structure is 5 mm to 50 mm.

[0010] Optionally, a four-stage heating process is used to process a thick slab with a convex structure on a narrow side, including:

[0011] The preheating section heats the thick slab with a convex structure on the narrow side;

[0012] Heating a thick slab having a convex structure on a heating narrow surface;

[0013] The second heating stage heats the thick slab with a convex structure on the narrow side;

[0014] The soaking section heats the thick slab whose narrow surface has a convex structure.

[0015] Optionally, when the thick slab with the narrow side having the convex structure is processed by the four-stage heating process, the thick slab with the narrow side having the convex structure is placed in a heating furnace for heating;

[0016] Among them, the furnace atmosphere temperature of the preheating section is 1000℃~1100℃, the furnace atmosphere temperature of the heating section is 1080℃~1180℃, the furnace atmosphere temperature of the heating section is 1150℃~1250℃, and the furnace atmosphere temperature of the soaking section is 1180℃~1230℃;

[0017] Among them, the heating rates of the preheating section, the first heating section, the second heating section and the soaking section are all greater than 15min / cm;

[0018] Among them, the soaking time of the soaking section is greater than 45 minutes;

[0019] Among them, after the thick slab with a convex structure on the narrow side is processed by a four-stage heating process, the steel-out temperature is 1150℃~1210℃, the temperature difference between the upper and lower surfaces is less than 15℃, and the temperature difference between the core and the surface is less than 25℃.

[0020] Optionally, the rough-rolled narrow side thick slab with a convex structure comprises:

[0021] The first stage is longitudinal rolling;

[0022] The second stage is cross rolling;

[0023] The third stage is longitudinal rolling.

[0024] Optionally, the first stage is longitudinal rolling with 1 to 4 passes, the second stage is transverse rolling with 2 to 10 passes, and the third stage is longitudinal rolling with 3 to 8 passes.

[0025] Optionally, the first and second cross-rolling passes in the second stage of cross-rolling are kept at temperature for 1 to 2 minutes.

[0026] Optionally, during the third stage of longitudinal rolling, the reduction ratio of at least two passes is greater than 15%.

[0027] Optional, finishing intermediate billet, including:

[0028] The fourth stage is longitudinal rolling.

[0029] Optionally, the number of finish rolling passes is less than ten, and the reduction ratio of each pass is controlled to be less than 13.5%.

[0030] In another aspect of the present application, there is provided an ultra-thick slab continuous casting device for producing any of the above-mentioned thick slabs with a narrow surface having an outward convex structure;

[0031] The ultra-thick slab continuous casting device comprises a crystallizer, the crystallizer comprises a pair of wide copper plates and a pair of narrow copper plates, the pair of wide copper plates each extend in one direction and are installed to face each other in a direction intersecting the extending direction, the pair of narrow copper plates each extend to intersect the wide copper plates, and the pair of narrow copper plates are installed to face each other, thereby sealing a portion between the pair of wide copper plates to form an internal space for solidifying molten steel into a thick slab;

[0032] The narrow copper plate has a first working surface and a second working surface on one side close to the thick plate blank, wherein two second working surfaces are provided, one second working surface is provided on one side of the first working surface, and the other second working surface is provided on the other side of the first working surface, and the first working surface is connected to the two second working surfaces respectively;

[0033] The cross-section of the first working surface is a concave arc, the midpoint of the concave arc coincides with the transverse center line of the first working surface, the two second working surfaces are symmetrically arranged with the transverse center line of the first working surface as the center of symmetry, and the two second working surfaces are also perpendicular to the wide copper plate.

[0034] Beneficial Effects

[0035] The thick plate narrow side double-drum defect control method and ultra-thick slab continuous casting device provided in the embodiments of the present invention, by producing thick slabs with a narrow side having an outward convex structure, and coordinating the four-stage heating process, rough rolling and finishing rolling processes, can make the depth of the double-drum middle drum seam of the thick slab after rolling shallower, thereby reducing the trimming amount of the steel plate and improving the yield rate of the thick plate. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 A flowchart of a method for controlling double-drum defects on a narrow surface of a thick plate according to an optional embodiment of the present application;

[0037] Figure 2 A flowchart of a method for controlling double-drum defects on a narrow surface of a thick plate according to another optional embodiment of the present application;

[0038] Figure 3 This is a schematic structural diagram of a crystallizer of an optional embodiment of the present application;

[0039] Figure 4 This is a schematic structural diagram of a narrow copper plate of an optional embodiment of the present application;

[0040] Figure 5 This is a schematic structural diagram of a guide support roller according to an optional embodiment of the present application.

[0041] The reference numerals are:

[0042] 1. Wide copper plate; 2. Narrow copper plate; 21. First working surface; 22. Second working surface; 3. Thick slab; 4. Guide support roller; 41. First section; 42. Second section. DETAILED DESCRIPTION

[0043] In the description of the present application, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention.

[0044] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.

[0045] In this application, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be an indirect connection through an intermediate medium, or it can be the internal communication of two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0046] The preferred embodiments of the present invention are described below in conjunction with the accompanying drawings. It should be understood that the preferred embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0047] See also Figure 1 and Figure 2 As shown, according to one aspect of an embodiment of the present application, a thick plate narrow surface double-drum defect control method is provided, which is applied to thick slab rolling thick plate production, and the thick slab can be a cast ingot with a thickness of 300mm to 600mm.

[0048] Among them, thick plate production includes: casting, casting molten steel into thick slabs 3; heating, placing the thick slabs 3 into a heating furnace and uniformly heating them to a suitable rolling temperature; and rolling, reducing the thickness of the thick slabs 3 and controlling the size, plate shape and performance of the thick slabs 3.

[0049] The double-drum defect control methods for thick plate narrow surface include:

[0050] Step S101: producing a thick slab 3 with a narrow side having a convex structure.

[0051] The molten steel may be condensed during the continuous casting stage and solidified into a thick slab 3 .

[0052] The thick slab 3 includes two opposite wide surfaces and two opposite narrow surfaces. The narrow surfaces of the thick slab 3 are two relatively narrow side surfaces in the width direction of the thick slab 3.

[0053] Specifically, the crystallizer includes a narrow copper plate, and the narrow surface of the thick plate blank 3 is formed under the action of the narrow copper plate.

[0054] Among them, the wall surface of the narrow copper plate close to the thick slab 3 is the working surface, which is used to provide support for the narrow surface of the thick slab 3 that is solidifying and maintain the shape of the narrow surface; it is also used to conduct the heat inside the thick slab 3 to achieve cooling and solidification of the thick slab 3.

[0055] Specifically, the working surface can be recessed in the direction away from the thick slab 3 to form an inner concave structure, so that the narrow surface of the thick slab 3 after solidification presents an outer convex structure, reducing the depth of the double-drum middle drum seam on the narrow surface of the thick slab 3 after rolling.

[0056] The working surface may be concave in the direction away from the thick slab 3, or only the middle part of the working surface may be concave. It should be noted that when only the middle part of the working surface is concave, the depth of the double-drum-shaped drum seam on the narrow surface of the thick slab 3 after rolling can be reduced.

[0057] The middle portion of the working surface may be a region close to a transverse center line of the working surface in the width direction of the working surface.

[0058] Among them, the recessed area of ​​the working surface can be a smooth curved surface, which can avoid cracks on the narrow surface of the thick slab 3, and at the same time reduce the wear of the working surface when the thick slab 3 descends during the continuous casting process, thereby extending the service life of the narrow copper plate.

[0059] The depression of the working surface can be 5 mm to 50 mm. For example, if the depression of the working surface is 5 mm, the height of the convexity in the middle of the narrow surface of the solidified thick slab 3 is 5 mm; if the depression of the working surface is 25 mm, the height of the convexity in the middle of the narrow surface of the solidified thick slab 3 is 25 mm; if the depression of the working surface is 50 mm, the height of the convexity in the middle of the narrow surface of the solidified thick slab 3 is 50 mm.

[0060] After being pulled out of the crystallizer, the thick slab 3 enters the secondary cooling zone, which is provided with a guide support mechanism and a spray assembly, which can further cool the thick slab 3, accelerate the solidification speed of the molten steel, and form a solid thick slab 3 with a certain strength and shape as soon as possible.

[0061] Step S201: using a four-stage heating process to process a thick slab 3 having a narrow surface with a convex structure.

[0062] The four-stage heating process is used to process the thick slab 3 having a convex structure on the narrow side, which is to heat the thick slab 3 after the second cooling zone.

[0063] In this embodiment, the thick slab 3 is heated by a heating furnace.

[0064] Specifically, when heating the thick slab 3 with a convex structure on the narrow side, a four-stage heating process is used. The four-stage heating process can make the temperature gradient inside the thick slab 3 relatively small, make the temperature of the entire casting uniform, facilitate the rolling and cutting processes in the subsequent processing, and improve the processing efficiency and quality.

[0065] Step S301: Rough rolling a thick slab 3 with a narrow surface having a convex structure to obtain an intermediate slab.

[0066] The rough-rolled narrow surface of the thick slab 3 having a convex structure is used to initially reduce the thickness of the thick slab 3 .

[0067] Specifically, the rough rolling of the thick slab 3 with a convex structure on the narrow side includes multiple passes of large reduction rolling. Through the large reduction, the thickness of the thick slab 3 is quickly and significantly reduced, the coarse grains in the cast structure are broken, and the metal grains are initially refined, thereby improving the internal structure of the thick plate, making the deformation of the metal in the thickness direction more uniform, reducing the internal stress and defects caused by uneven deformation, preparing for the subsequent finishing process, and helping to improve the efficiency of finishing and product quality.

[0068] Step S401: Finish rolling the intermediate billet to obtain the target steel plate.

[0069] The intermediate blank is the slab obtained in step S301.

[0070] The target steel plate may be a thick plate with no double-bulge defects on the narrow side or a shallow double-bulge gap.

[0071] Among them, the finishing rolling intermediate billet is used to accurately control the size, plate shape and performance of the thick plate billet 3.

[0072] Specifically, the finishing rolling of the intermediate billet includes multiple passes of small reduction rolling. Through a small reduction, the thickness, width and length of the thick plate can be controlled with high precision. On the basis of rough rolling, the metal grains are further refined, thereby improving the mechanical properties and overall quality of the thick plate, reducing surface defects such as cracks and pitting, and making the surface of the thick plate smoother and flatter.

[0073] It can be understood that in the present application, by producing a thick slab 3 with a narrow side having an outward convex structure, and coordinating the four-stage heating process, rough rolling and finishing rolling processes, the depth of the double-drum middle drum seam of the thick slab 3 after rolling can be made shallower, thereby reducing the trimming amount of the steel plate and improving the yield rate of the thick plate.

[0074] See also Figure 2 As shown, the above step S201 uses a four-stage heating process to process the thick slab 3 with a narrow surface having a convex structure, including:

[0075] Step S2011: The preheating section heats the thick slab 3 whose narrow surface has a convex structure.

[0076] The preheating stage heats the thick slab 3 with the narrow surface having the convex structure in the heating furnace.

[0077] The furnace atmosphere temperature of the preheating section of the thick slab 3 with the convex structure on the narrow side can be 1000°C to 1100°C.

[0078] Step S2012: heating a section of thick slab 3 having a convex structure on a heated narrow surface.

[0079] The heating of a thick slab 3 having a narrow heating surface and a convex structure is also carried out in the heating furnace.

[0080] The furnace atmosphere temperature of the heating section of the thick slab 3 having the convex structure on the narrow side may be 1080°C to 1180°C.

[0081] Step S2013: Heating in the second stage: heating the thick slab 3 having a convex structure on the narrow side.

[0082] The second stage of heating the thick slab 3 with a narrow surface having a convex structure is also carried out in the heating furnace.

[0083] The furnace atmosphere temperature of the second heating stage of the thick slab 3 with the convex structure on the narrow side can be 1150-1250°C.

[0084] Step S2014: The soaking section heats the thick slab 3 whose narrow surface has a convex structure.

[0085] The heating of the thick slab 3 with the narrow surface having the convex structure in the soaking section is also carried out in the heating furnace.

[0086] The furnace atmosphere temperature of the soaking section of the thick slab 3 with the convex structure on the narrow side can be 1180°C to 1230°C.

[0087] It is understandable that the preheating section, the first heating section, the second heating section and the soaking section of the thick slab 3 with a convex structure on the narrow side are carried out in the same heating furnace. In the present application, the thick slab 3 with a convex structure on the narrow side is heated in stages by the same heating furnace, which can ensure that the temperature of the thick slab 3 is uniform, facilitates the rolling and cutting processes in the subsequent processing, and improves the processing efficiency and quality.

[0088] In the above steps S2011, S2012, S2013 and S2014, the heating rate of the thick slab 3 with the narrow side having the convex structure is greater than 15 min / cm.

[0089] It can be understood that in the present application, the thick slab 3 with a narrow surface having an outward convex structure uses a four-stage heating process, which helps to reduce the internal temperature gradient of the thick slab 3, make the structure more uniform, and reduce the performance difference caused by uneven temperature; at the same time, it can shorten the heating time, reduce the residence time of the thick slab 3 in the heating furnace, and reduce the reaction time between the surface of the thick slab 3 and the atmosphere in the furnace, thereby reducing the generation of iron oxide scale; at the same time, it can also speed up production efficiency and reduce energy consumption.

[0090] In the above step S2014, the soaking time of the soaking section of the thick slab 3 with the convex structure on the narrow side is greater than 45 minutes.

[0091] It can be understood that, in the present application, it is possible to ensure that the temperature inside the thick slab 3 is uniform, which helps to reduce the uneven deformation and internal stress concentration caused by temperature differences during the subsequent rolling process.

[0092] Among them, in this embodiment, after the above step S2014, the steel tapping temperature of the thick slab 3 is 1150℃~1210℃, and the temperature difference between the upper and lower surfaces of the thick slab 3 does not exceed 15℃, and the temperature difference between the core and surface of the thick slab 3 does not exceed 25℃.

[0093] See also Figure 2 As shown, the above step S301, rough rolling the thick slab 3 with a narrow surface having a convex structure, includes:

[0094] Step S3011: first stage longitudinal rolling.

[0095] During the first stage of longitudinal rolling, the thick slab 3 can be effectively compressed and thinned in the thickness direction to a great extent, so that the thick slab 3 undergoes plastic deformation.

[0096] In the first stage of longitudinal rolling, 1 to 4 longitudinal rolling passes may be performed.

[0097] Step S3012: Second stage cross rolling.

[0098] Among them, during the second stage transverse rolling, the width of the thick slab 3 can be effectively extended.

[0099] In the second stage of cross-rolling, 2 to 10 cross-rolling passes may be performed.

[0100] Step S3013: the third stage of longitudinal rolling.

[0101] Among them, during the third stage longitudinal rolling, the thick slab 3 can be further compressed and thinned in the thickness direction.

[0102] Among them, during the third stage of longitudinal rolling, longitudinal rolling can be performed for 3 to 8 times.

[0103] It can be understood that in the present application, when rough-rolling the thick slab 3 with a convex structure on the narrow side, a longitudinal-transverse-longitudinal process is adopted, and rolling in different directions makes the deformation of the thick slab 3 more sufficient and uniform, promotes grain refinement and uniform distribution, thereby reducing the depth of the double-drum middle drum seam on the narrow side of the thick slab 3 after rolling, reducing the trimming amount of the steel plate, and improving the yield rate of the thick plate.

[0104] Among them, in this embodiment, during the first stage of longitudinal rolling, the longitudinal rolling is performed once; during the second stage of transverse rolling, the transverse rolling is performed three times; during the third stage of longitudinal rolling, the longitudinal rolling is performed three times.

[0105] In the above step S3012, during the second stage of cross-rolling, the first cross-rolling pass and the second cross-rolling pass are kept at temperature for 1 to 2 minutes.

[0106] Specifically, in this embodiment, during the second stage of cross-rolling, the interval between the first cross-rolling pass and the second cross-rolling pass is 2 minutes.

[0107] It is understandable that in the present application, by setting an interval time between the first and second cross-rolling passes during the second stage of cross-rolling, the edge temperature of the thick slab 3 can be reduced, thereby inhibiting the metal flow at the edge of the thick slab 3.

[0108] In the above step S3013, during the third stage of longitudinal rolling, the reduction ratio of at least two passes is greater than 15%.

[0109] It can be understood that in the present application, during the third stage of longitudinal rolling, at least two longitudinal rolling passes have a large reduction rate, which can quickly and significantly reduce the thickness of the thick slab 3, break up the coarse grains in the cast structure, and initially refine the metal grains, thereby improving the internal structure of the thick plate, making the deformation of the metal in the thickness direction more uniform, reducing the internal stress and defects caused by uneven deformation, preparing for the subsequent finishing process, and helping to improve the efficiency of finishing and product quality.

[0110] See also Figure 2 As shown, the above step S401, finish rolling the intermediate billet to obtain the target steel plate, includes:

[0111] Step S4011: the fourth stage of longitudinal rolling.

[0112] The fourth stage of longitudinal finishing rolling can effectively compress and thin the thick slab 3 in the thickness direction to a great extent, causing the thick slab 3 to undergo plastic deformation.

[0113] Among them, when finishing rolling the intermediate billet obtained by rough rolling, longitudinal rolling can be performed less than ten times.

[0114] Specifically, in this embodiment, when finish rolling the intermediate billet obtained by rough rolling, eight longitudinal rolling passes are performed.

[0115] In the above step S4011, the reduction ratio of each pass is less than 13.5%.

[0116] It is understandable that in the present application, during the fourth stage of longitudinal rolling, each longitudinal rolling pass has a small reduction rate, which can achieve high-precision control of the thickness, width and length of the thick plate. On the basis of rough rolling, the metal grains are further refined, thereby improving the mechanical properties and comprehensive quality of the thick plate, reducing surface defects such as cracks, pitting, etc., and making the surface of the thick plate smoother and flatter.

[0117] Another aspect of the present application embodiment is shown in Figure 3 and Figure 4As shown, a super thick slab continuous casting device is provided, which is used to produce any of the above-mentioned thick slabs 3 with a narrow side having an outward convex structure; the super thick slab continuous casting device includes a crystallizer, the crystallizer includes a pair of wide copper plates 1 and a pair of narrow copper plates 2, the pair of wide copper plates 1 each extend in one direction and are installed to face each other in a direction intersecting the extending direction, the pair of narrow copper plates 2 are respectively extended to intersect with the wide copper plates 1, and the pair of narrow copper plates 2 are installed to face each other, thereby sealing the part between the pair of wide copper plates 1 to form an internal space for solidifying molten steel into the thick slab 3; the narrow copper plates 2 are close to the thick slab 3. One side of the copper plate 1 has a first working surface 21 and a second working surface 22, two second working surfaces 22 are arranged, one second working surface 22 is arranged on one side of the first working surface 21, and the other second working surface 22 is arranged on the other side of the first working surface 21, and the first working surface 21 is connected to the two second working surfaces 22 respectively; the cross section of the first working surface 21 is a concave arc, the midpoint of the concave arc coincides with the transverse center line of the first working surface 21, and the two second working surfaces 22 are symmetrically arranged with the transverse center line of the first working surface 21 as the symmetry center, and the two second working surfaces 22 are also perpendicular to the wide copper plate 1. By setting the first working surface 21 where the narrow copper plate 2 contacts the thick slab 3 as a concave structure, the production of thick slab 3 with a narrow surface having a convex structure can be achieved, thereby making the depth of the double-drum seam of the thick slab 3 shallower after rolling, reducing the trimming amount of the steel plate, and thus improving the yield rate of the thick plate; at the same time, by setting the second working surfaces 22 on both sides of the first working surface 21 as a straight structure, the corners of the thick slab 3 produced by the extra-thick slab continuous casting device are right-angle structures, which can avoid cracks at the corners of the thick slab 3 when producing micro-alloyed steel containing NB, AI, and V.

[0118] Among them, the ultra-thick slab continuous casting device includes: a ladle, which stores molten steel refined in the steelmaking process; a tundish, which receives the molten steel through an injection nozzle connected to the ladle and temporarily stores the molten steel; a crystallizer, which receives the molten steel stored in the tundish and makes the molten steel initially solidify into a predetermined shape; an immersed water nozzle, which supplies the molten steel in the tundish to the crystallizer; and a secondary cooling zone, which is arranged below the crystallizer and is used to provide water spray cooling to the thick slab 3 pulled out of the crystallizer, to help the thick slab 3 to solidify quickly, so as to facilitate a series of molding processes.

[0119] In the embodiment of the present application, the crystallizer is used to produce a thick slab 3 whose narrow side has a convex structure and whose corners are free of defects. It should be noted that the thick slab 3 can be a thick slab 3 with a thickness of 300 mm to 600 mm. When the narrow side of the thick slab 3 has a convex structure, the depth of the double-drum drum seam of the thick slab 3 after rolling is relatively shallow.

[0120] The crystallizer includes a pair of wide copper plates 1, each of which extends in one direction and is spaced apart from each other in a direction intersecting or perpendicular to the extending direction; and a pair of narrow copper plates 2 arranged between the pair of wide copper plates 1, each of which extends in a direction intersecting or perpendicular to the wide copper plates 1, and is spaced apart from each other in a direction intersecting or perpendicular to the extending direction.

[0121] Specifically, in the embodiment of the present application, the extension direction of the pair of wide copper plates 1 is perpendicular to the extension direction of the pair of narrow copper plates 2. For example, the extension direction of the pair of wide copper plates 1 is defined as the X-axis direction, and the extension direction of the pair of narrow copper plates 2 is the Y-axis direction. At this time, the pair of wide copper plates 1 are spaced apart in the Y-axis direction, and the pair of narrow copper plates 2 are spaced apart in the X-axis direction. The pair of wide copper plates 1 and the pair of narrow copper plates 2 form an internal space for solidifying molten steel into a thick slab 3.

[0122] Specifically, a pair of wide copper plates and a pair of narrow copper plates are combined to form an inner cavity of a crystallizer to solidify molten steel into a thick slab 3 .

[0123] The short side structure includes a working surface, which may be a wall surface of the narrow copper plate 2 facing the inner space of the crystallizer, and the working surface is used to contact the solidified thick slab 3.

[0124] The working surface includes a first working surface 21 and a second working surface 22, and the first working surface 21 and the second working surface 22 extend along the height direction of the narrow copper plate 2. It can be understood that the height direction of the narrow copper plate 2 can be the length direction of the thick plate blank 3.

[0125] There are two second working surfaces 22, which are arranged on both sides of the first working surface 21 along the width direction of the narrow copper plate 2 and are respectively connected to the first working surface 21. It can be understood that the width direction of the narrow copper plate 2 can be the thickness direction of the thick plate blank 3.

[0126] Specifically, the first working surface 21 is located in the middle of the narrow copper plate 2, and the second working surface 22 is located at the edge of the narrow copper plate 2. The first working surface 21 is smoothly connected with the two second working surfaces 22, which can reduce the probability of double-drum shape defects in the thick slab 3 during rolling.

[0127] The first working surface 21 is recessed in a direction away from the thick slab 3 to form an inner concave structure, so that the portion of the thick slab 3 that contacts the first working surface 21 after solidification presents an outer convex structure.

[0128] The depression of the first working surface 21 can be 5 mm to 50 mm. For example, the depression of the first working surface 21 is 5 mm, and the height of the convex part of the narrow surface of the thick slab 3 after solidification is 5 mm; the depression of the first working surface 21 is 25 mm, and the height of the convex part of the narrow surface of the thick slab 3 after solidification is 25 mm; the depression of the first working surface 21 is 50 mm, and the height of the convex part of the narrow surface of the thick slab 3 after solidification is 50 mm.

[0129] Specifically, the cross section of the first working surface 21 is a concave arc, which can reduce the wear of the narrow copper plate 2 when the solidified shell moves downward during the continuous casting process, thereby extending the service life of the narrow copper plate 2.

[0130] The second working surface 22 is a plane, so that the portion of the solidified thick slab 3 that contacts the second working surface 22 is a straight structure.

[0131] Specifically, the second working surface 22 is perpendicular to the wide copper plate 1, so that the ultra-thick slab continuous casting device can prepare a thick slab 3 with a right-angle structure at the corner, avoiding cracks at the corner when the thick slab 3 contains NB, AI, V micro-alloyed steel. It can be understood that the corner of the thick slab 3 can be a thick slab 3 corresponding to the angle at the intersection of the wide copper plate 1 and the narrow copper plate 2.

[0132] The narrow copper plate 2 also includes a top surface and a bottom surface, the top surface is flush with the upper opening of the crystallizer, and the bottom surface is flush with the lower opening of the crystallizer. It can be understood that the upper opening of the crystallizer can be the end where the molten steel enters the inner space of the crystallizer, and the lower opening of the crystallizer can be the end where the thick slab 3 leaves the inner space of the crystallizer.

[0133] The narrow copper plate 2 further includes a side surface, which may be a wall surface in contact with the wide copper plate 1 , and two side surfaces are provided, which are arranged opposite to each other.

[0134] In some possible implementations provided in this application, see Figure 5As shown, the continuous casting device of the extra-thick slab 3 also includes a guiding support mechanism, which is arranged at the lower mouth of the narrow copper plate 2; the guiding support mechanism includes a guiding support roller 4, which includes a first section 41, and the first section 41 includes two reduced diameter sections, and the diameters of the two reduced diameter sections gradually decrease in the direction facing each other, so that the roller surface of the guiding support roller 4 contacting the thick slab 3 presents a concave arc with the same cross-section as the first working surface 21, so as to support the thick slab 3 of the narrow surface convex part formed under the action of the first working surface 21; the guiding support roller 4 also includes a second section 42, and two second sections 42 are provided, and the two second sections 42 are arranged on both sides of the first section 41 along the axial direction of the first section 41, and the first section 41 is respectively connected to the two second sections 42, and the two second sections 42 are cylindrical, so that the two second sections 42 are suitable for supporting the thick slab 3 of the narrow surface straight part formed under the action of the two second working surfaces 22. By arranging a guiding support mechanism at the lower mouth of the crystallizer, support can be provided for the thick slab 3 pulled out of the crystallizer, maintaining the narrow surface of the thick slab 3 with an outward convex structure, and preventing the thick slab 3 that is not completely solidified from deforming; at the same time, it is beneficial to reduce defects such as bulging and concavity of the thick slab 3, and improve the surface quality and internal quality of the thick slab 3.

[0135] A spraying area is arranged below the narrow copper plate 2, a frame is arranged in the spraying area, and a guide support mechanism is installed on the frame.

[0136] Specifically, the guide support mechanism includes a guide support roller 4, which may be a foot roller rotatably disposed on the frame.

[0137] The guide support roller 4 includes a first section 41 and a second section 42 which are coaxially arranged, two second sections 42 are arranged, the first section 41 is arranged between the two second sections 42, and the two ends of the first section 41 are respectively connected to the two second sections 42. In addition, it can be understood that the guide support roller 4 can also be made of an integral molding.

[0138] Specifically, the first section 41 is roughly hourglass-shaped, and the first section 41 includes two reduced diameter sections, and the diameters of the two reduced diameter sections gradually decrease in the directions facing each other, so that the first section 41 can adapt to the bulge in the middle of the narrow surface of the thick slab 3; the second section 42 is roughly cylindrical, and the second section 42 is connected to the end of the reduced diameter section with a large end face area, and the diameter of the second section 42 is the same as the diameter of the end of the reduced diameter section with a large end face area, so that the second section 42 can adapt to the corner of the right-angle structure of the thick slab 3.

[0139] The length of the first section 41 is the same as the width of the first working surface 21 .

[0140] In one embodiment, the length of the second section 42 is less than the width of the second working surface 22; in another embodiment, the length of the second section 42 is the same as the width of the second working surface 22. In this embodiment, the length of the second section 42 is less than the width of the second working surface 22.

[0141] Specifically, in this embodiment, the length of the second section 42 is 0 mm to 20 mm less than the width of the second working surface 22. It should be noted that the thick slab 3 has a lower angle temperature and greater hardness and does not require support, thereby reducing the production cost of the guide support mechanism.

[0142] Among them, in this embodiment, when the height of the narrow copper plate 2 is 800mm~1000mm, the width is 300mm~600mm, the thickness is 35mm~55mm, the width of the second working surface 22 can be 0mm~150mm, and the length of the second section 42 can be 0mm~130mm.

[0143] It is easy for those skilled in the art to understand that, under the premise of no conflict, the above-mentioned advantageous methods can be freely combined and superimposed.

[0144] The above are only preferred embodiments of the present application and are not intended to limit the present application. Any modifications, equivalent replacements and improvements made within the spirit and principles of the present application shall be included in the protection scope of the present application. The above are only preferred implementations of the present application. It should be pointed out that for ordinary technicians in this technical field, several improvements and variations can be made without departing from the technical principles of the present application, and these improvements and variations should also be regarded as the protection scope of the present application.

Claims

1. A method for controlling double-drum defects on the narrow side of thick plates, characterized in that: include: Producing thick slabs (3) with convex structures on the narrow side; A four-stage heating process is used to process a thick slab (3) having a narrow surface with a convex structure; Rough rolling of a thick slab (3) with a narrow surface having a convex structure to obtain an intermediate slab; Finish rolling the intermediate billet to obtain the target steel plate; The thickness of the thick slab (3) with a narrow surface having an outward convex structure is 300 mm to 600 mm, and the convex height of the thick slab (3) with a narrow surface having an outward convex structure is 5 mm to 50 mm.

2. The thick plate narrow surface double-drum defect control method according to claim 1 is characterized in that: A four-stage heating process is used to process a thick slab (3) having a narrow surface with a convex structure, comprising: The preheating section heats the thick slab (3) whose narrow surface has a convex structure; Heating a thick slab (3) having a heating narrow surface with a convex structure; The second heating stage heats the thick slab (3) whose narrow surface has a convex structure; The soaking section heats a thick slab (3) having a narrow surface with an outwardly convex structure.

3. The thick plate narrow surface double-drum defect control method according to claim 2 is characterized in that: When the thick slab (3) with a narrow surface having a convex structure is processed by a four-stage heating process, the thick slab (3) with a narrow surface having a convex structure is placed in a heating furnace for heating; Among them, the furnace atmosphere temperature of the preheating section is 1000℃~1100℃, the furnace atmosphere temperature of the heating section is 1080℃~1180℃, the furnace atmosphere temperature of the heating section is 1150℃~1250℃, and the furnace atmosphere temperature of the soaking section is 1180℃~1230℃; Among them, the heating rates of the preheating section, the first heating section, the second heating section and the soaking section are all greater than 15min / cm; Among them, the soaking time of the soaking section is greater than 45 minutes; Among them, after the thick slab (3) with a convex structure on the narrow side is processed by a four-stage heating process, the steel-out temperature is 1150°C to 1210°C, the temperature difference between the upper and lower surfaces is less than 15°C, and the temperature difference between the core and the surface is less than 25°C.

4. The thick plate narrow surface double-drum defect control method according to claim 1 is characterized in that: A thick slab (3) having a rough-rolled narrow surface and a convex structure, comprising: The first stage is longitudinal rolling; The second stage is cross rolling; The third stage is longitudinal rolling.

5. The method for controlling the defects of the narrow surface of thick plates according to claim 4 is characterized in that: The first stage is longitudinal rolling with 1 to 4 passes, the second stage is transverse rolling with 2 to 10 passes, and the third stage is longitudinal rolling with 3 to 8 passes; The number of passes for rough rolling the thick slab (3) with a narrow surface having a convex structure is less than nine passes.

6. The method for controlling the defects of the narrow surface of thick plate by double drums according to claim 5 is characterized in that: The first and second cross-rolling passes in the second stage of cross-rolling are kept at temperature for 1 to 2 minutes.

7. The method for controlling the defects of the thick plate narrow surface by double drums according to claim 4 is characterized in that: During the third stage of longitudinal rolling, the reduction ratio of at least two passes is greater than 15%.

8. The thick plate narrow surface double-drum defect control method according to claim 1 is characterized in that: Finishing rolling intermediate billet, including: The fourth stage is longitudinal rolling.

9. The method for controlling the defects of the narrow surface of thick plates according to claim 8 is characterized in that: The number of passes of the finish rolling is ten or less, and the reduction ratio of each pass is controlled to be 13.5% or less.

10. A super thick slab continuous casting device, characterized in that: Used for producing a thick slab (3) with a convex structure on a narrow side according to any one of claims 1 to 9; The ultra-thick slab continuous casting device comprises a crystallizer, the crystallizer comprising a pair of wide copper plates (1) and a pair of narrow copper plates (2), the pair of wide copper plates (1) each extending in one direction and being installed to face each other in a direction intersecting the extending direction, the pair of narrow copper plates (2) respectively extending to intersect with the wide copper plates (1), and the pair of narrow copper plates (2) being installed to face each other, thereby sealing a portion between the pair of wide copper plates (1) to form an internal space for solidifying molten steel into a thick slab (3); The narrow copper plate (2) has a first working surface (21) and a second working surface (22) on one side close to the thick plate blank (3); two second working surfaces (22) are provided, one second working surface (22) is provided on one side of the first working surface (21), and the other second working surface (22) is provided on the other side of the first working surface (21); the first working surface (21) is connected to the two second working surfaces (22) respectively; The cross section of the first working surface (21) is a concave arc, the midpoint of the concave arc coincides with the transverse center line of the first working surface (21), the two second working surfaces (22) are symmetrically arranged with the transverse center line of the first working surface (21) as the symmetry center, and the two second working surfaces (22) are also perpendicular to the wide copper plate (1).

Citation Information

Patent Citations

  • Rolling method for eliminating edge line defects in silicon steel production

    CN109261718A

  • Wide and thick plate with low trimming loss and production method thereof

    CN112474801A

  • Method and structure for improving rollover of tail of plate blank on rough rolling vertical roll

    CN116900065A

  • Continuous casting equipment and continuous casting method

    CN117961017A

  • Ingot mould with large broad-thick ratio used for directly rolling thick plate

    CN2216877Y