Composite sheet for packaging cheese at normal temperature
Through the composite of modified graphene and ethylene-vinyl alcohol copolymer, the problem of degradation of barrier properties of existing cheese packaging materials under high humidity is solved, and excellent barrier properties of water vapor, oxygen and light are achieved. It is suitable for daily cheese packaging. Improves the overall performance of the material.
Patent Information
- Application Number
- CN202410962357.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-19
AI Technical Summary
The existing cheese packaging materials have deteriorated barrier properties under high humidity and have failed to effectively consider the impact of ambient temperature and light on cheese storage, which limits its application prospects.
Graphene is modified by modifying carboxylated UV-0 monomer with ultraviolet absorption function with branched UV absorber and compounding it with ethylene-vinyl alcohol copolymer, and prepared by multi-layer coextrusion and casting film formation process Composite sheets, enhanced interface compatibility and barrier properties.
It significantly improves the moisture barrier, oxygen and light performance of the composite sheet, complies with hygiene indicators, is suitable for daily cheese packaging, and improves the comprehensive performance of the material.
Smart Images

Figure CN118977445A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of research and development of cheese packaging materials, in particular to a composite sheet material for packaging cheese at room temperature. Background Art
[0002] At present, the packaging materials commonly used for cheese on the market include polyethylene, polypropylene, polyvinyl chloride, polystyrene, multi-layer composite materials, etc. Among them, multi-layer composite materials are widely used in the market due to their excellent barrier properties, good mechanical properties, strong compressive resistance and other advantages, and have good development prospects.
[0003] Conventional multilayer composite materials for cheese packaging usually use ethylene-vinyl alcohol copolymer as the barrier layer. However, there are a large number of hydroxyl groups in traditional ethylene-vinyl alcohol copolymer, and the barrier performance decreases under high humidity conditions. In addition, conventional multilayer composite materials usually only focus on blocking the effects of water vapor and oxygen on cheese, while factors such as ambient temperature and light that also affect the storage time of cheese are not taken into consideration, which limits their actual use in the field of cheese packaging.
[0004] At present, the method to improve the water vapor and oxygen barrier performance of materials is mainly nano-composite modification. For example, the patent with publication number CN117601532A discloses a nano-modified high barrier antibacterial biaxially stretched nylon film and its preparation method. The water vapor and oxygen barrier performance of the material can be significantly improved through the interaction between graphene oxide nanosheets and nylon resin; the method to improve the light barrier performance of materials is mainly to add light-blocking agents. For example, the patent with publication number CN117447817A prepares a PET material with excellent light-blocking performance by compounding a light-blocking agent with polyethylene terephthalate (PET).
[0005] The search found that graphene nanosheets have good barrier properties for small molecules because of their relatively high aspect ratio, which can provide a longer propagation path for penetrating molecules. When compounded with polymers, they can significantly improve the barrier properties of composite materials. However, the interface compatibility between graphene nanosheets and polymers is poor, so they are often surface modified to improve the comprehensive performance of composite materials. In addition, benzophenone, benzotriazole, and triazine compounds are common ultraviolet absorbers that can inhibit light and effectively protect food and materials from damage by ultraviolet rays. Summary of the invention
[0006] The invention provides a composite sheet for packaging cheese at room temperature. A graphene component is modified by using a carboxylated UV-0 monomer with an ultraviolet absorption function and a branched ultraviolet absorber, and the modified graphene is compounded with an ethylene-vinyl alcohol copolymer. On the one hand, the interface compatibility between the graphene and the ethylene-vinyl alcohol copolymer matrix is enhanced, and on the other hand, the technical goal of improving the light-blocking performance of the polymer material is achieved. On this basis, a multi-layer co-extrusion and cast film-forming process is adopted to prepare a composite sheet for packaging cheese at room temperature, which has excellent barrier properties and mechanical properties.
[0007] A process for preparing a composite sheet comprises the following steps:
[0008] Step 1: setting a five-layer co-extruded film, the structure of which is: support layer, adhesive layer, barrier layer, adhesive layer, support layer;
[0009] Step 2: Compounding the functionalized modified graphene containing UV-0 groups with ethylene-vinyl alcohol copolymer to prepare a GO&EVOH composite material;
[0010] Step 3: Using GO&EVOH composite material as the raw material of the barrier layer, low-density polyethylene resin as the raw material of the support layer, and maleic anhydride grafted low-density polyethylene resin as the raw material of the adhesive layer, a multi-layer co-extrusion and cast film forming process is adopted to prepare a composite sheet.
[0011] Preferably, the functionalized modified graphene is functionalized modified graphene I, and the preparation method of the functionalized modified graphene I is:
[0012] Step S2-1: 2,4-dihydroxybenzophenone and methyl 4-chlorobutyrate undergo a nucleophilic substitution reaction to generate a methyl ester UV-0 monomer; the methyl ester UV-0 monomer undergoes a hydrolysis reaction under alkaline conditions to generate a carboxylated UV-0 monomer; wherein the molar ratio of 2,4-dihydroxybenzophenone to methyl 4-chlorobutyrate is (1.01-1.05):1;
[0013] Step S2-2: Based on the esterification reaction mechanism, the hydroxylated graphene is modified using a carboxylated UV-0 monomer to obtain functionalized modified graphene I.
[0014] Preferably, the functionalized modified graphene is functionalized modified graphene II, and the preparation method of the functionalized modified graphene II is:
[0015] Step S3-1: generating a branched ultraviolet absorber by a nucleophilic substitution reaction between 2,4-dihydroxybenzophenone and cyanuric chloride; wherein the molar ratio of 2,4-dihydroxybenzophenone to cyanuric chloride is (3.01-3.05):1;
[0016] Step S3-2: The branched ultraviolet absorber and the functionalized modified graphene I are compounded through the interaction between the benzene rings to obtain the functionalized modified graphene II.
[0017] Preferably, the preparation process parameters of the barrier layer are set as follows: the temperatures of zones 1-3 of the screw extruder are 170-190°C, 180-200°C, and 200-220°C, respectively; the flow channel temperature is 190-210°C; and the rotation speed is 30-60 r / min.
[0018] The thickness of a composite sheet prepared according to the above process is 50 to 200 μm.
[0019] Preferably, the oxygen permeability of the composite sheet is 0.1 to 0.3 [cm 3 / (m 2 ·24h·0.1MPa)], water vapor transmission rate is 0.2~0.4[g / (m 2 ·24h)], light transmittance is 10-35%.
[0020] The composite sheet prepared according to the above process is used in the packaging of cheese at room temperature.
[0021] Beneficial Effects
[0022] The present invention first designs a novel composite sheet structure, and then develops a novel barrier interlayer, wherein the barrier interlayer is obtained by compounding modified graphene containing ultraviolet absorbing groups and ethylene-vinyl alcohol copolymer, and then adopts multi-layer co-extrusion and cast film forming processes to prepare the composite sheet;
[0023] The experimental results show that the composite sheet prepared by the present invention has excellent barrier properties (water vapor, oxygen and light), meets the hygiene indicators, and can be used in room temperature cheese packaging. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a product structure diagram of the composite sheet;
[0025] Among them, the number 1 is a barrier layer, the numbers 2-1 and 2-2 are adhesive layers, and the numbers 3-1 and 3-2 are support layers. DETAILED DESCRIPTION
[0026] Experimental example:
[0027] Research and development experiment 1: Synthesis of carboxylated UV-0 monomers, the synthesis route of which is: a nucleophilic substitution reaction is performed by 1 molar equivalent of 2,4-dihydroxybenzophenone and 1 molar equivalent of methyl 4-chlorobutyrate to generate a methyl ester UV-0 monomer; the methyl ester UV-0 monomer undergoes a hydrolysis reaction under alkaline conditions to generate a carboxylated UV-0 monomer, the chemical structure of which is:
[0028]
[0029] The nuclear magnetic resonance hydrogen spectrum of the carboxylated UV-0 monomer is characterized as follows: 1 H NMR (CDCl3, 400MHz) δ: 2.05-2.10 (m, 2H), 2.54-2.56 (t, 2H), 4.04-4.07 (t, 2H), 6.54-7.71 (m, 8H);
[0030] The specific experimental steps for preparing the carboxylated UV-0 monomer are as follows: 2.2 g of 2,4-dihydroxybenzophenone, 5 mL of 2 mol / L sodium hydroxide aqueous solution and 20 mL of acetone are added to a three-necked flask, stirred at room temperature until completely dissolved, and added dropwise to 10 mL of 4-chlorobutyric acid methyl ester solution (prepared by 1.4 g of 4-chlorobutyric acid methyl ester and 10 mL of acetone) under the protection of nitrogen, heated to 60° C. and refluxed for 4 h, washed with deionized water and ethanol in turn, dried over anhydrous magnesium sulfate, filtered, and recrystallized with ethanol after reduced pressure distillation to obtain a methyl ester UV-0 monomer; then, 1.6 g of methyl ester UV-0 monomer, 1.0 g of sodium hydroxide and 20 mL of deionized water are added to a two-necked flask, heated to 70° C. and stirred for 2 h, the solution pH was adjusted to 1 with concentrated hydrochloric acid, cooled to room temperature, washed with deionized water, and dried to obtain a carboxylated UV-0 monomer;
[0031] Research and development experiment 2: Synthesis of branched UV absorbers, the synthesis route of which is: through a nucleophilic substitution reaction between 3 molar equivalents of 2,4-dihydroxybenzophenone and 1 molar equivalent of cyanuric chloride, a branched UV absorber is generated, and its chemical structure is:
[0032]
[0033] The nuclear magnetic resonance hydrogen spectrum of the branched ultraviolet absorber is characterized by: 1 H NMR (CDCl3, 400MHz) δ: 6.42 (s, 3H), 7.46-7.73 (m, 21H);
[0034] The specific experimental steps for preparing the branched ultraviolet absorber are as follows: 0.9 g of cyanuric chloride and 20 mL of acetone are added to a three-necked flask, and stirred in an ice-water bath until completely dissolved. 50 mL of 2,4-dihydroxybenzophenone solution (prepared from 3.4 g of 2,4-dihydroxybenzophenone and 50 mL of acetone) and 15 mL of 2 mol / L sodium hydroxide aqueous solution (prepared from 0.2 g of sodium hydroxide and 20 mL of deionized water) are fully mixed and then slowly added dropwise to the three-necked flask. The reaction is stirred in an ice bath at 0°C for 5 h, filtered, washed with deionized water and ethanol in turn, and dried to obtain a branched ultraviolet absorber.
[0035] Embodiment 1:
[0036] (1) Preparation of functional modified graphene I: Based on the esterification reaction mechanism, carboxylated UV-0 monomer was used to modify hydroxylated graphene to obtain functional modified graphene I. The specific experimental steps are as follows: under nitrogen protection and mechanical stirring, 1 g of carboxylated UV-0 monomer, 5 g of hydroxylated graphene and 50 mL of N,N-dimethylformamide were added to a two-necked bottle, ultrasonicated for 30 min, 0.5 g of concentrated sulfuric acid was added dropwise, the temperature was raised to 60 ° C and stirred for 3 h, washed with anhydrous ethanol, filtered, rotary evaporated, and vacuum dried to obtain functional modified graphene I;
[0037] Preparation of functionalized modified graphene II: The branched ultraviolet absorber and the functionalized modified graphene I are compounded through the interaction between the benzene rings to obtain functionalized modified graphene II. The specific experimental steps are as follows: under nitrogen protection and mechanical stirring, 0.5 g of branched ultraviolet absorber, 5 g of functionalized modified graphene I and 50 mL of N, N-dimethylformamide are added to a two-necked bottle, ultrasonicated for 1 h, heated to 50 ° C and stirred for 2 h, washed with anhydrous ethanol, filtered, rotary evaporated, and vacuum dried to obtain functionalized modified graphene II;
[0038] (2) Preparation of GO&EVOH composite material I, the preparation method is: functionalized modified graphene I is uniformly dispersed in ethylene-vinyl alcohol copolymer (EVOH) to prepare GO&EVOH composite material I, the specific experimental steps are: 5g ethylene-vinyl alcohol copolymer resin and 100mL N,N-dimethylformamide are added to a two-necked bottle, the temperature is raised to 60°C and stirred until completely dissolved, then 10mL functionalized modified graphene I dispersion (prepared by 0.5g functionalized modified graphene I and 10mL N,N-dimethylformamide) is added dropwise to the two-necked bottle, the temperature is maintained at 60°C and stirred for 3h, and after cooling, it is poured into a polytetrafluoroethylene mold, and dried in an oven at 80°C, 100°C, and 120°C for 12h to obtain GO&EVOH composite material I;
[0039] GO&EVOH composite material II was prepared, and its preparation method was as follows: functionalized modified graphene II was uniformly dispersed in ethylene-vinyl alcohol copolymer to prepare GO&EVOH composite material II, and its specific experimental steps were as follows: 5g ethylene-vinyl alcohol copolymer resin and 100mL N,N-dimethylformamide were added to a two-necked bottle, and the temperature was raised to 60°C and stirred until all dissolved under mechanical stirring, and then 10mL functionalized modified graphene II dispersion (prepared by 0.5g functionalized modified graphene II and 10mL N,N-dimethylformamide) was dripped into the two-necked bottle, and the stirring reaction was maintained at 60°C for 3h, and after cooling, it was poured into a polytetrafluoroethylene mold, and dried in an oven at 80°C, 100°C, and 120°C for 12h, respectively, to obtain GO&EVOH composite material II;
[0040] Among them, ethylene-vinyl alcohol copolymer resin was purchased from Dongguan Kaisi Li Plastic Raw Materials Co., Ltd., with the specifications of E105B, Mn~10000, and ethylene content of 44%; graphene nanosheets were purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., with the product number G139804, and the specifications or purity were: >99.5%, thickness 4~20nm, and diameter 5~10μm.
[0041] The preparation method of hydroxylated graphene is as follows: 1 g of graphene nanosheets and 100 mL of deionized water are added to a round-bottom flask, ultrasonicated for 1 h to form a graphene nanosheet dispersion, 0.1 mol / L hydrochloric acid solution is added dropwise to adjust the pH to 3, and the temperature is raised to 35° C. under mechanical stirring, and 10 mL of ferrous chloride solution (prepared with 0.9 g of ferrous chloride and 10 mL of deionized water) and 10 mL of 30 wt% hydrogen peroxide solution are added dropwise to the flask in sequence, and the reaction is continued by stirring for 30 min, and the residual iron ions are washed away with 0.1 mol / L hydrochloric acid solution, and the iron ions are detected by potassium thiocyanate solution to determine whether they are completely removed, and then H is washed away with deionized water. + and Cl - , pH test paper and silver nitrate solution were used to detect H + and Cl - Whether it is completely removed, vacuum dried to obtain hydroxylated graphene.
[0042] Embodiment 2:
[0043] Preparation of composite sheet: A composite sheet with a thickness of 100 μm was prepared using a five-layer co-extrusion film casting unit. Figure 1 As shown, the symmetrical membrane structure of the composite sheet is: support layer 3-1, adhesive layer 2-1, barrier layer 1, adhesive layer 2-2, support layer 3-2, based on the mass ratio of the membrane structure of 35:5:20:5:35;
[0044] The raw materials of the above-mentioned adhesive layer are all maleic anhydride grafted low-density polyethylene resin, which is purchased from Dongguan Taotao Plastic Raw Materials Co., Ltd., with specifications of: 4288, Mn~130000;
[0045] The raw materials of the above supporting layers are all low-density polyethylene resins purchased from CNOOC Shell Petrochemical Co., Ltd., with specifications of: 2420H, Mn-180000, MFR 2.0-2.5g / 10min;
[0046] The process parameters of the screw extruder corresponding to the barrier layer were set as follows: the temperatures of zones 1-3 were 180°C, 200°C, and 210°C, respectively, the flow channel temperature was 205°C, and the rotation speed was 40 r / min;
[0047] The process parameters of the screw extruder corresponding to the bonding layer were set as follows: the temperatures of zones 1-3 were 115°C, 145°C, and 160°C, respectively, the flow channel temperature was 150°C, and the rotation speed was 15 r / min;
[0048] The process parameters of the screw extruder corresponding to the support layer were set as follows: the temperatures of zones 1-3 were 110°C, 140°C, and 160°C, respectively, the flow channel temperature was 150°C, and the rotation speed was 30 r / min;
[0049] Composite sheets I and II were prepared in sequence according to the above method, wherein the raw materials of barrier layer 1 are shown in Table 1 below;
[0050] Table 1 Raw materials of barrier layer in composite sheet
[0051] Composite sheet type Barrier layer raw materials Composite sheet Ⅰ GO&EVOH Composite MaterialⅠ Composite sheet Ⅱ GO&EVOH Composite Material Ⅱ Comparative Example EVOH
[0052] Performance Test:
[0053] 1. Barrier performance test:
[0054] (1) Water vapor barrier performance: The water vapor permeability test of the sample is carried out in accordance with GB / T 1037-2021 "Determination of water vapor permeability of plastic films and sheets - Cup weight gain and weight loss method". The specific test steps are as follows: a 30 cm circular film sample is placed in a glass desiccator at an ambient temperature of 25°C and anhydrous calcium chloride is used as a desiccant for 72 hours, and then the water vapor barrier performance is tested using a W3 / 060 water vapor permeability tester;
[0055] (2) Oxygen barrier performance: The oxygen permeation rate of the sample was tested in accordance with GB / T 1038-2000 "Plastic Film and Sheeting Gas Permeability Test Method - Pressure Difference Method". The specific test steps are as follows: a 30 cm circular film sample was placed in a glass desiccator at an ambient temperature of 25°C and anhydrous calcium chloride was used as a desiccant for 72 hours. After that, the oxygen barrier performance was tested using a Y110 oxygen permeability tester;
[0056] (3) Light blocking performance: Lambda 950 UV-visible spectrophotometer was used to test the light transmittance of the samples in accordance with GB / T2410-2008 “Determination of light transmittance and haze of transparent plastics”. The test wavelength range was 250-800 nm, and the light transmittance of the samples at 380 nm was recorded.
[0057] 2. Mechanical properties test:
[0058] The tensile strength of the samples was tested using an Instron 5565 universal tensile testing machine. The specific test steps were as follows: a 30 mm × 5 mm sample was fixed on the tensile testing machine, and a tensile test was performed at a tensile rate of 5 mm / min, and the longitudinal and transverse tensile strengths were recorded respectively;
[0059] 3. Hygienic performance
[0060] The hygienic properties of the samples were tested according to GB / T 5009.60-2003 "Analysis Method for Hygienic Standards of Polyethylene, Polystyrene and Polypropylene Molding Products for Food Packaging", and the physical and chemical indicators of the experimental results were based on GB / T5009.58-2003 "Analysis Method for Hygienic Standards of Polyethylene Resins for Food Packaging";
[0061] The above experimental results are shown in Tables 2-4 below.
[0062] Table 2 Barrier performance test results of each composite sheet
[0063]
[0064]
[0065] Table 3 Mechanical properties test results of each composite sheet
[0066]
[0067] Table 4 Hygienic performance test results of each composite sheet
[0068]
[0069] By analyzing the performance test results, the following conclusions can be drawn: the composite sheet prepared by modifying ethylene-vinyl alcohol copolymer with functionalized modified graphene has achieved beneficial technical effects of significantly improved water barrier, oxygen barrier and light barrier properties; and compared with functionalized modified graphene I, functionalized modified graphene II has a better effect on improving the light barrier properties of the final prepared composite sheet product.
Claims
1. A process for preparing a composite sheet, characterized in that: The steps include: Step 1: a five-layer co-extruded film is provided, wherein the structure is: a support layer (3-1), an adhesive layer (2-1), a barrier layer (1), an adhesive layer (2-2), and a support layer (3-2); Step 2: Compounding the functionalized modified graphene containing UV-0 groups with ethylene-vinyl alcohol copolymer to prepare a GO&EVOH composite material; Step 3: Using GO&EVOH composite material as the raw material of the barrier layer, low-density polyethylene resin as the raw material of the support layer, and maleic anhydride grafted low-density polyethylene resin as the raw material of the adhesive layer, a multi-layer co-extrusion and cast film forming process is adopted to prepare a composite sheet.
2. The process for preparing a composite sheet according to claim 1, characterized in that: The functionalized modified graphene is functionalized modified graphene I, and the preparation method of the functionalized modified graphene I is: Step S2-1: generating a methyl ester UV-0 monomer by a nucleophilic substitution reaction between 2,4-dihydroxybenzophenone and methyl 4-chlorobutyrate; The methyl ester UV-0 monomer undergoes a hydrolysis reaction under alkaline conditions to generate a carboxylated UV-0 monomer; wherein the molar ratio of 2,4-dihydroxybenzophenone to methyl 4-chlorobutyrate is (1.01-1.05):1; Step S2-2: Based on the esterification reaction mechanism, the hydroxylated graphene is modified using a carboxylated UV-0 monomer to obtain functionalized modified graphene I.
3. The process for preparing a composite sheet according to claim 1, characterized in that: The functionalized modified graphene is functionalized modified graphene II, and the preparation method of the functionalized modified graphene II is: Step S3-1: generating a branched ultraviolet absorber by a nucleophilic substitution reaction between 2,4-dihydroxybenzophenone and cyanuric chloride; wherein the molar ratio of 2,4-dihydroxybenzophenone to cyanuric chloride is (3.01-3.05):1; Step S3-2: The branched ultraviolet absorber and the functionalized modified graphene I are compounded through the interaction between the benzene rings to obtain the functionalized modified graphene II.
4. The process for preparing a composite sheet according to claim 1, characterized in that: The preparation process parameters of the barrier layer (1) are set as follows: the temperatures of the screw extruder zones 1-3 are 170-190° C., 180-200° C., and 200-220° C., respectively; the flow channel temperature is 190-210° C.; and the rotation speed is 30-60 r / min.
5. A composite sheet prepared by the process according to any one of claims 1 to 4, characterized in that: The thickness of the composite sheet is 50-200 μm.
6. A composite sheet according to claim 5, characterized in that: The oxygen permeability of the composite sheet is 0.1 to 0.3 [cm 3 / (m 2 ·24h·0.1MPa)], water vapor transmission rate is 0.2~0.4[g / (m 2 ·24h)], light transmittance is 10-35%.
7. Use of a composite sheet prepared according to the process according to any one of claims 1 to 4 in packaging cheese at room temperature.