Safe treatment and comprehensive utilization method for multiple components of coal gasification waste residues
Through foam flotation and multi-step treatment, porous carbon, calcium-rich filtrate and aerogel are obtained, which solves the problem of underutilization of coal gasified waste slag, realizes its effective application in carbon dioxide capture and sewage treatment, and improves resources Utilization and environmental security.
Patent Information
- Application Number
- CN202411040753.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-07-31
AI Technical Summary
The prior art fails to fully and comprehensively utilize porous carbon components and mineral elements in coal gasified waste slag, resulting in their occupation of land, polluting the environment, and lacking large-scale and effective utilization methods.
Floating fine carbon and tail ash were obtained by foam flotation method, and further treatment was obtained to obtain porous carbon material, calcium-rich filtrate and Al2O3-SiO2 aerogel for carbon dioxide capture and sewage treatment or building insulation materials.
Achieved the safe disposal and comprehensive utilization of carbon, calcium, aluminum and silicon in coal gasified waste slag, and prepared porous carbon, calcium-rich filtrate and aerogel for carbon dioxide capture and sewage treatment, which improved resource utilization and Environmental safety.
Smart Images

Figure CN118978156A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of solid waste resource utilization, and specifically relates to a method for safe treatment and comprehensive utilization of multi-component coal gasification waste residue. Background Art
[0002] Coal chemical industry belongs to new productivity. Gasification slag is a typical solid waste produced by coal chemical process. The annual output is large. If a large amount of storage is carried out, it will not only occupy land area, but also pollute the surrounding environment such as soil, atmosphere and water. However, there is no effective method for large-scale utilization. Gasification slag contains a large amount of unburned carbon and has well-developed pores. At the same time, gasification slag contains rich silicon, aluminum, calcium and other elements. Although there are reports that gasification slag can be used as porous materials for wastewater treatment and carbon dioxide capture after being treated, there is no literature report that can fully and comprehensively utilize the porous carbon components and mineral elements in gasification waste slag. Summary of the invention
[0003] The purpose of the present invention is to provide a method for safe treatment and comprehensive utilization of multi-component coal gasification waste slag, which can realize the effective utilization of carbon, calcium, aluminum, and silicon multi-components in the coal gasification waste slag. The prepared porous carbon and calcium-rich filtrate can be used for carbon dioxide capture, and Al2O3-SiO2 aerogel can be used as an adsorption material for sewage treatment or a building insulation material.
[0004] To achieve the above object, the technical solution adopted by the present invention is: a method for safe treatment and comprehensive utilization of multi-component coal gasification waste residue, comprising the following steps:
[0005] (1) The coal gasification fine slag is prepared into a slurry, and a certain amount of collector and frother are added and stirred to obtain flotation concentrate and flotation tailings;
[0006] (2) adding hydrochloric acid solution to the flotation refined carbon to leach metal elements, filtering to obtain acid-washed residual carbon and washing with deionized water until neutral, and obtaining an acidic filtrate;
[0007] (3) adding potassium hydroxide to the residual carbon obtained in step (2) to activate it to obtain a porous carbon material for CO2 capture;
[0008] (4) mixing the acidic filtrate obtained in step (2) with the flotation tailings obtained in step (1), adding hydrochloric acid solution, and filtering to obtain silicon-aluminum residue and filtrate;
[0009] (5) adding aqueous ammonia to the filtrate obtained in step (4) to adjust the pH to 8.5-9.5, filtering out the particulate matter in the filtrate to obtain a calcium-rich filtrate for CO2 capture;
[0010] (6) introducing CO2 gas into the calcium-rich filtrate obtained in step (5) to mineralize the calcium-rich filtrate and carbonate the calcium-rich filtrate;
[0011] (7) Adding sodium hydroxide to the silicon-aluminum residue obtained in step (4) for alkali melting activation, then adding trimethylchlorosilane and hexane, and then drying to obtain Al2O3-SiO2 aerogel.
[0012] Preferably, in step (1), the collector is diesel or methyl oleate, and the foaming agent is octanol; the concentration of the slurry is 100 g / L; the amounts of the collector and foaming agent are 7 kg / t coal gasification fine slag and 10 kg / t coal gasification fine slag, respectively.
[0013] Preferably, in step (1), the specific surface area of the coal gasification fine slag is 200m 2 / g; the ash components of the coal gasification fine slag include the following components: by weight percentage, 2.13% K2O, 1.98% Na2O, 50.94% SiO2, 18.92% Al2O3, 9.14% CaO, 9.96% Fe2O3, 3.57% MgO, and the rest are residual carbon and other impurities; the ignition loss of the coal gasification fine slag is 23.06%.
[0014] Preferably, in step (2), the concentration of the hydrochloric acid solution is 1.5-3 mol / L, the liquid-to-solid ratio of the flotation refined carbon to the hydrochloric acid solution is 15-30 mL / g, the leaching time is 30-60 min, and the leaching temperature is 60-90°C.
[0015] Preferably, in step (3), the mass ratio of residual carbon to potassium hydroxide is 1:(1-3); the activation temperature is 700-850° C., and the activation time is 60-120 min.
[0016] Preferably, in step (4), the concentration of the hydrochloric acid solution is 1.5-3 mol / L, the liquid-to-solid ratio is 15-30 mL / g, the leaching time is 30-60 min, and the leaching temperature is 60-90°C.
[0017] Preferably, in step (6), the mineralization reaction temperature is 30-60° C., and the reaction time is 30-60 min.
[0018] Preferably, in step (7), the activation temperature is 750-850° C. and the reaction time is 60-90 min.
[0019] Preferably, in step (7), the mass ratio between trimethylchlorosilane and hexane is (0.22-0.28):1.
[0020] Preferably, in step (7), drying is first performed at room temperature for 12-15 hours, and then dried at 75-85°C for 6-8 hours.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] The present invention can fully and comprehensively utilize the porous carbon components and mineral elements in coal-based solid waste, obtain flotation refined carbon and tailing ash by the method of foam flotation, wherein the flotation refined carbon is further activated by KOH to prepare porous carbon materials while recovering the mineral elements leached in the pickling process, the generated acidic waste liquid is further mixed with the tailing ash to extract mineral elements and obtain calcium-rich filtrate, and the remaining silicon-aluminum residue is activated by alkali to obtain silicon-aluminum solution, and Al2O3-SiO2 aerogel is obtained after aging. So far, the three materials of porous carbon, calcium-rich filtrate and Al2O3-SiO2 aerogel are successfully prepared, the prepared porous carbon and calcium-rich filtrate can be used for carbon dioxide capture, and Al2O3-SiO2 aerogel can be used as an adsorbent material for sewage treatment or a building insulation material, realizing a multi-component safe disposal and comprehensive utilization method of carbon, calcium, aluminum and silicon of coal gasification waste. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION
[0024] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0025] All raw materials and reagents in the examples of the present application were purchased on the market or prepared according to conventional methods well known to those skilled in the art.
[0026] The specific surface area of the coal gasification slag used in the following examples is 200m 2 / g; the ash components of the coal gasification fine slag include the following components: by weight percentage, 2.13% K2O, 1.98% Na2O, 50.94% SiO2, 18.92% Al2O3, 9.14% CaO, 9.96% Fe2O3, 3.57% MgO, and the rest are residual carbon and other impurities; the ignition loss of the coal gasification fine slag is 23.06%.
[0027] Example 1
[0028] like Figure 1 As shown, a method for safe treatment and comprehensive utilization of multi-component coal gasification waste residue comprises the following steps:
[0029] (1) The coal gasification fine slag is prepared into a slurry with a concentration of 100 g / L, and a certain amount of collector and frother are added and stirred. Based on the calculation of treating 1 t of coal gasification fine slag, the amount of collector diesel is 7 kg, and the amount of frother octanol is 10 kg; the flotation fine carbon yield is 37.62%, the ignition loss is 59.78%, the flotation tail ash yield is 62.38%, and the ignition loss is 4.78%;
[0030] (2) Adding 2 mol / L hydrochloric acid solution to the flotation concentrate to leach metal elements, the liquid-to-solid ratio of the flotation concentrate to the hydrochloric acid solution is 25 mL / g, the leaching time is 50 min, the leaching temperature is 80°C, the calcium ion leaching rate is 99%, and the specific surface area of the flotation residual carbon after pickling is 496 m 2 / g, filter to obtain the acid-washed carbon residue and rinse with deionized water until neutral, and obtain an acidic filtrate;
[0031] (3) Adding potassium hydroxide to the residual carbon obtained in step (2) to activate the porous carbon material for CO2 capture; the mass ratio between the residual carbon and potassium hydroxide is 1:2; the activation temperature is 800°C, and the activation time is 90 min; the specific surface area of the prepared porous carbon material is 1480 m 2 / g, the CO2 adsorption capacity reached 4.7mmol / g at 0℃, and the CO2 adsorption saturation time was 2min;
[0032] (4) the acidic filtrate obtained in step (2) is mixed with the flotation tailings obtained in step (1), and then a hydrochloric acid solution with a concentration of 2 mol / L is added, the liquid-to-solid ratio is 25 mL / g, the leaching time is 50 min, the leaching temperature is 80° C., and the silicon-aluminum residue and the filtrate are obtained by filtering; the calcium ion leaching rate is 99%;
[0033] (5) adding aqueous ammonia to the filtrate obtained in step (4) to adjust the pH to 8.5-9.5, filtering out the particulate matter in the filtrate to obtain a calcium-rich filtrate for CO2 capture;
[0034] (6) introducing CO2 gas into the calcium-rich filtrate obtained in step (5) for mineralization, the mineralization reaction temperature is 50°C, the reaction time is 50 min, and the calcium-rich filtrate is carbonated, and the carbonation efficiency is 97%;
[0035] (7) Sodium hydroxide was added to the silicon-aluminum residue obtained in step (4) for alkali melting activation, the activation temperature was 800°C, the reaction time was 75 min, and then trimethylchlorosilane and hexane were added, the mass ratio of trimethylchlorosilane to hexane was 0.26:1, and then dried at room temperature for 15 h, and then dried at 80°C for 7.5 h to obtain Al2O3-SiO2 aerogel, the specific surface area of the aerogel reached 650 m 2 / g.
[0036] Example 2
[0037] like Figure 1 As shown, a method for safe treatment and comprehensive utilization of multi-component coal gasification waste residue comprises the following steps:
[0038] (1) The coal gasification fine slag is prepared into a slurry with a concentration of 100 g / L, and a certain amount of collector and frother are added and stirred. Based on the calculation of treating 1 t of coal gasification fine slag, the amount of collector methyl oleate is 7 kg, and the amount of frother octanol is 10 kg; the flotation fine carbon yield is 37.62%, the ignition loss is 59.78%, the flotation tail ash yield is 62.38%, and the ignition loss is 4.78%;
[0039] (2) Adding 3 mol / L hydrochloric acid solution to the flotation concentrate to leach metal elements, the liquid-to-solid ratio of the flotation concentrate to the hydrochloric acid solution is 30 mL / g, the leaching time is 60 min, the leaching temperature is 90°C, the calcium ion leaching rate is 99.5%, and the specific surface area of the flotation residual carbon after pickling is 508 m 2 / g, filter to obtain the acid-washed carbon residue and rinse with deionized water until neutral, and obtain an acidic filtrate;
[0040] (3) Adding potassium hydroxide to the residual carbon obtained in step (2) to activate it to obtain a porous carbon material for CO2 capture; the mass ratio between the residual carbon and potassium hydroxide is 1:3; the activation temperature is 850°C, and the activation time is 120 min; the specific surface area of the prepared porous carbon material is 1210 m 2 / g, the CO2 adsorption capacity reached 4.4mmol / g at 0℃, and the CO2 adsorption saturation time was 2min;
[0041] (4) the acidic filtrate obtained in step (2) is mixed with the flotation tailings obtained in step (1), and then a hydrochloric acid solution having a concentration of 3 mol / L is added, the liquid-to-solid ratio is 30 mL / g, the leaching time is 60 min, the leaching temperature is 90° C., and the silicon-aluminum residue and the filtrate are obtained by filtering; the calcium ion leaching rate is 99.5%;
[0042] (5) adding aqueous ammonia to the filtrate obtained in step (4) to adjust the pH to 8.5-9.5, filtering out the particulate matter in the filtrate to obtain a calcium-rich filtrate for CO2 capture;
[0043] (6) introducing CO2 gas into the calcium-rich filtrate obtained in step (5) for mineralization, the mineralization reaction temperature is 60°C, the reaction time is 60 min, and the calcium-rich filtrate is carbonated, and the carbonation efficiency is 98%;
[0044] (7) Sodium hydroxide was added to the silicon-aluminum residue obtained in step (4) for alkali melting activation, the activation temperature was 850°C, the reaction time was 90 min, and then trimethylsilyl chloride and hexane were added, the mass ratio of trimethylsilyl chloride to hexane was 0.28:1, and then dried at room temperature for 15 h, and then dried at 85°C for 7.5 h to obtain Al2O3-SiO2 aerogel, the specific surface area of the aerogel reached 710 m 2 / g.
[0045] Example 3
[0046] like Figure 1 As shown, a method for safe treatment and comprehensive utilization of multi-component coal gasification waste residue comprises the following steps:
[0047] (1) The coal gasification fine slag is prepared into a slurry with a concentration of 100 g / L, and a certain amount of collector and frother are added and stirred. Based on the calculation of treating 1 t of coal gasification fine slag, the amount of collector diesel is 7 kg, and the amount of frother octanol is 10 kg; the flotation fine carbon yield is 37.62%, the ignition loss is 59.78%, the flotation tail ash yield is 62.38%, and the ignition loss is 4.78%;
[0048] (2) Adding 1.5 mol / L hydrochloric acid solution to the flotation concentrate to leach metal elements, the liquid-to-solid ratio of the flotation concentrate to the hydrochloric acid solution is 20 mL / g, the leaching time is 30 min, the leaching temperature is 60°C, the calcium ion leaching rate is 92%, and the specific surface area of the flotation residual carbon after pickling is 463 m 2 / g, filter to obtain the acid-washed carbon residue and rinse with deionized water until neutral, and obtain an acidic filtrate;
[0049] (3) Adding potassium hydroxide to the residual carbon obtained in step (2) to activate it to obtain a porous carbon material for CO2 capture; the mass ratio between the residual carbon and potassium hydroxide is 1:1; the activation temperature is 750°C, and the activation time is 60 min; the specific surface area of the prepared porous carbon material is 1015 m 2 / g, the CO2 adsorption capacity reached 3.7mmol / g at 0℃, and the CO2 adsorption saturation time was 2min;
[0050] (4) the acidic filtrate obtained in step (2) is mixed with the flotation tailings obtained in step (1), and then a hydrochloric acid solution with a concentration of 1.5 mol / L is added, the liquid-to-solid ratio is 20 mL / g, the leaching time is 30 min, the leaching temperature is 60° C., and the silicon-aluminum residue and the filtrate are obtained by filtering; the calcium ion leaching rate is 94%;
[0051] (5) adding aqueous ammonia to the filtrate obtained in step (4) to adjust the pH to 8.5-9.5, filtering out the particulate matter in the filtrate to obtain a calcium-rich filtrate for CO2 capture;
[0052] (6) introducing CO2 gas into the calcium-rich filtrate obtained in step (5) for mineralization, the mineralization reaction temperature is 45°C, the reaction time is 30 min, and the calcium-rich filtrate is carbonated, and the carbonation efficiency is 91%;
[0053] (7) Sodium hydroxide was added to the silicon-aluminum residue obtained in step (4) for alkali melting activation, the activation temperature was 750°C, the reaction time was 60 min, and then trimethylsilyl chloride and hexane were added, the mass ratio of trimethylsilyl chloride to hexane was 0.22:1, and then dried at room temperature for 12 h, and then dried at 75°C for 7.5 h to obtain Al2O3-SiO2 aerogel, the specific surface area of the aerogel reached 595 m 2 / g.
Claims
1. A method for safe treatment and comprehensive utilization of multi-component coal gasification waste residue, characterized in that: The following steps are involved: (1) The coal gasification fine slag is prepared into a slurry, and a certain amount of collector and frother are added and stirred to obtain flotation concentrate and flotation tailings; (2) adding hydrochloric acid solution to the flotation refined carbon to leach metal elements, filtering to obtain acid-washed residual carbon and washing with deionized water until neutral, and obtaining an acidic filtrate; (3) adding potassium hydroxide to the residual carbon obtained in step (2) to activate it to obtain a porous carbon material for CO2 capture; (4) mixing the acidic filtrate obtained in step (2) with the flotation tailings obtained in step (1), adding hydrochloric acid solution, and filtering to obtain silicon-aluminum residue and filtrate; (5) adding aqueous ammonia to the filtrate obtained in step (4) to adjust the pH to 8.5-9.5, filtering out the particulate matter in the filtrate to obtain a calcium-rich filtrate for CO2 capture; (6) introducing CO2 gas into the calcium-rich filtrate obtained in step (5) to mineralize the calcium-rich filtrate and carbonate the calcium-rich filtrate; (7) Adding sodium hydroxide to the silicon-aluminum residue obtained in step (4) for alkali melting activation, then adding trimethylchlorosilane and hexane, and then drying to obtain Al2O3-SiO2 aerogel.
2. A method for safe treatment and comprehensive utilization of multi-component coal gasification waste residue according to claim 1, characterized in that: In step (1), the collector is diesel or methyl oleate, and the foaming agent is octanol; the concentration of the slurry is 100 g / L; the amounts of the collector and foaming agent are 7 kg / t coal gasification fine slag and 10 kg / t coal gasification fine slag, respectively.
3. A method for safe treatment and comprehensive utilization of multi-component coal gasification waste residue according to claim 1 or 2, characterized in that: In step (1), the specific surface area of the coal gasification fine slag is 200m 2 / g; the ash components of the coal gasification fine slag include the following components: by weight percentage, 2.13% K2O, 1.98% Na2O, 50.94% SiO2, 18.92% Al2O3, 9.14% CaO, 9.96% Fe2O3, 3.57% MgO, and the rest are residual carbon and other impurities; the ignition loss of the coal gasification fine slag is 23.06%.
4. A method for safe treatment and comprehensive utilization of multi-component coal gasification waste residue according to claim 1 or 2, characterized in that: In step (2), the concentration of the hydrochloric acid solution is 1.5-3 mol / L, the liquid-to-solid ratio of the flotation refined carbon to the hydrochloric acid solution is 15-30 mL / g, the leaching time is 30-60 min, and the leaching temperature is 60-90°C.
5. A method for safe treatment and comprehensive utilization of multi-component coal gasification waste residue according to claim 1 or 2, characterized in that: In step (3), the mass ratio of residual carbon to potassium hydroxide is 1:(1-3); the activation temperature is 700-850° C., and the activation time is 60-120 min.
6. A method for safe treatment and comprehensive utilization of multi-component coal gasification waste residue according to claim 1 or 2, characterized in that: In step (4), the concentration of the hydrochloric acid solution is 1.5-3 mol / L, the liquid-to-solid ratio is 15-30 mL / g, the leaching time is 30-60 min, and the leaching temperature is 60-90° C.
7. A method for safe treatment and comprehensive utilization of multi-component coal gasification waste residue according to claim 1 or 2, characterized in that: In step (6), the mineralization reaction temperature is 30-60° C. and the reaction time is 30-60 min.
8. A method for safe treatment and comprehensive utilization of multi-component coal gasification waste residue according to claim 1 or 2, characterized in that: In step (7), the activation temperature is 750-850° C. and the reaction time is 60-90 min.
9. A method for safe treatment and comprehensive utilization of multi-component coal gasification waste residue according to claim 1 or 2, characterized in that: In step (7), the mass ratio between trimethylchlorosilane and hexane is (0.22-0.28):
1.
10. A method for safe treatment and comprehensive utilization of multi-component coal gasification waste residue according to claim 1 or 2, characterized in that: In step (7), the mixture is first dried at room temperature for 12-15 h, and then dried at 75-85° C. for 6-8 h.
Citation Information
Patent Citations
Coal gasification slag carbon ash separation and coal chemical industry wastewater combined treatment method
CN114956244A
Coal-based solid waste separation-smelting-material resource comprehensive utilization process method and application thereof
CN116812939A
Gradient recycling and quality-based utilization method of coal gasification slag
CN117548473A
Cited By
Coal gasification fine slag-based brain wrinkle-imitating aerogel porous material and application thereof
CN122582852A
Coal gasification fine slag-based imitation brain fold aerogel porous material and application
CN122582852B