Fluorine-containing copolymer, preparation method thereof and application of fluorine-containing copolymer as lithium battery binder

By using the fluorine-containing copolymer generated by the copolymerization reaction as a binder in lithium batteries, the problem of poor adhesion of polyvinylidene fluoride in lithium batteries is solved, and the bonding performance of the electrode and the stability of the battery are significantly improved.

CN118978627APending Publication Date: 2024-11-19INNER MONGOLIA WANHAO FLUOROCHEM +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411176256.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The polyvinylidene fluoride materials used in existing lithium battery adhesives have problems such as poor adhesion, poor water wetting and poor adhesion of current collector substrates in the treatment and application, resulting in the occurrence of extreme sheets during the use of lithium batteries. Problems such as cracking, chip loss, layering, and debonding affect the stability and life of the battery.

Method used

By copolymerizing the first polymerized monomer with the second modified monomer, a fluorine-containing copolymer is generated and used as a binder in a lithium battery, specific polymerization reaction conditions and additives are used to improve the bonding performance.

Benefits of technology

It significantly improves the bonding performance of the lithium battery electrode, enhances the peel strength of the positive electrode sheet and the negative electrode sheet, alleviates the problems of cracking and powder loss of the electrode sheet, and improves the stability and service life of the lithium battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978627A_ABST
    Figure CN118978627A_ABST
Patent Text Reader

Abstract

The invention provides a fluorine-containing copolymer as well as a preparation method and application thereof, and the method comprises the following step: carrying out copolymerization reaction on a first polymeric monomer and a second modified monomer to generate the fluorine-containing copolymer. When the fluorine-containing copolymer is used as a binder for manufacturing a lithium ion battery, the cracking and powder falling conditions of a pole piece can be effectively relieved, the binding power between slurry and a current collector can be greatly improved, and the strict requirement of the lithium battery on the binder can be met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the field of polymer materials, and specifically relates to a fluorine-containing copolymer, a preparation method of the fluorine-containing copolymer, and application of the fluorine-containing copolymer as a binder for lithium batteries. Background Art

[0002] In recent years, with the rapid development of electric vehicles and energy storage systems, higher requirements have been put forward for lithium batteries, especially power lithium batteries. People hope that lithium batteries have higher energy density, power density, cycle life and safety of use. Positive electrode materials, negative electrode materials, diaphragms, and electrolytes are the core of lithium batteries, and binders, as one of the key auxiliary materials, are the main medium that combines electrode active materials, conductive agents and electrode current collectors. Binders can make the components inside the electrode have integrity and form a stable electrode structure, which is conducive to alleviating the volume deformation of the electrodes of lithium-ion batteries during the charging and discharging process, preventing the detachment of active materials, thereby maintaining the mechanical integrity of the electrodes and improving the electrochemical performance of the battery. In addition, if the binder has higher adhesion, the amount of binder can be reduced in the process of manufacturing the battery, which is conducive to the preparation of higher capacity batteries.

[0003] Fluorine-containing polymers, such as polyvinylidene fluoride, are widely used as binders in commercial lithium batteries due to their high dielectric constant, stable electrochemical window, and easy slurry formation. However, these favorable properties also make polyvinylidene fluoride difficult to handle and limit its application. For example, polyvinylidene fluoride polymer lacks functional groups on the main chain, so its polarity is small, it is difficult to provide sites for subsequent chemical modification, it is difficult to be wetted by water, and it has poor adhesion to the battery's current collector substrate. These defects will inevitably lead to poor adhesion based on polyvinylidene fluoride, and when used to manufacture lithium batteries, larger binders have to be used, which will inevitably lead to a decrease in the capacity of the lithium battery. But even so, the battery will still have problems such as cracking of the pole piece, chipping, delamination, and debonding during use, which has a negative impact on the stability and life of the battery.

[0004] In the prior art, various enterprises and scientific research institutions have invested a lot of manpower and material resources in research and development in order to overcome the above-mentioned defects, but have not achieved satisfactory results.

[0005] Therefore, to date, people are still eager to develop a fluorinated copolymer that can be used as a lithium battery binder and a preparation method thereof. This technology should be able to synthesize a fluorinated copolymer with high adhesion in a low-cost and simple manner, which is conducive to the preparation of electrode plates with excellent performance with a small amount, thereby further improving the stability, capacity and service life of lithium-ion batteries. Summary of the invention

[0006] The inventors of the present application have unexpectedly developed a fluorine-containing copolymer and a preparation method and application thereof through extensive research, successfully solving the technical problems that have long been urgently needed to be solved in the prior art.

[0007] The first aspect of the present application provides a method for preparing a fluorine-containing copolymer, the method comprising: copolymerizing a first polymerizable monomer with a second modified monomer to generate the fluorine-containing copolymer;

[0008] The first polymerizable monomer has a structure shown in Formula I:

[0009]

[0010] In Formula I, R 1 and R 2 Each is independently selected from: H, F, C1-C4 alkyl, fluorinated C1-C4 alkyl, C2-C4 alkenyl, fluorinated C2-C4 alkenyl, C1-C4 alkoxy, fluorinated C1-C4 alkoxy; R3 and R4 are each independently selected from F, fluorinated C1-C4 alkyl, fluorinated C2-C4 alkenyl, fluorinated C1-C4 alkoxy;

[0011] The second modified monomer has a structure shown in Formula II:

[0012]

[0013] In Formula II, R 5 and R 6 Each is independently selected from H, F, C1-C6 alkyl, fluorinated C1-C6 alkyl, C1-C6 alkoxy, fluorinated C1-C6 alkoxy, C2-C6 alkenyl, fluorinated C2-C6 alkenyl; R 7 is selected from F, fluorinated C1-C6 alkyl, fluorinated C1-C6 alkoxy, fluorinated C2-C6 alkenyl; R 8 Selected from hydroxy, C1-C12 alkoxy, fluorinated C1-C12 alkoxy, C3-12 cycloalkoxy, hydroxy C3-12 cycloalkoxy, fluorinated C3-12 cycloalkoxy, hydroxy fluorinated C3-12 cycloalkoxy, C6-C12 aryloxy, fluorinated C6-C12 aryloxy, C4-C12 heteroaryloxy, fluorinated C4-C12 heteroaryloxy.

[0014] According to an embodiment of one aspect of the present application, the weight ratio of the first polymerized monomer to the second modified monomer is 99.9:1 to 80:20.

[0015] According to another embodiment of one aspect of the present application, the first polymerized monomer is selected from one or more of the following: vinylidene fluoride, trifluoroethylene, 1,1-difluoropropylene, 1,1,3-trifluoropropylene, hexafluoroisobutylene, hexafluorobutadiene, hexafluoro-2-butene, 1,1-difluoro-2-fluoromethoxyethylene, and 1,1-difluoro-2-perfluoromethoxyethylene.

[0016] According to another embodiment of one aspect of the present application, the second modifying monomer is selected from one or more of the following: 2-(trifluoromethyl)acrylic acid, methyl 2-(trifluoromethyl)acrylate, ethyl 2-(trifluoromethyl)acrylate, propyl 2-(trifluoromethyl)acrylate, tert-butyl 2-(trifluoromethyl)acrylate, methyl pentafluoromethylacrylate, 2-(trifluoromethyl)acrylate-2,2,2-trifluoroethyl ester, 2-(trifluoromethyl)acrylate-4-hydroxycyclohexyl ester, 2-(trifluoromethyl)acrylate-tetrahydro-2H-pyran-2-yl ester, 2-(trifluoromethyl)-acrylate-3,3,3-trifluoropropyl ester, and 2-(trifluoromethyl)acrylate-4,4,4-trifluorobutyl ester.

[0017] According to another embodiment of one aspect of the present application, the method includes: during the polymerization of the first polymerizable monomer in the reactor, the second modified monomer is added into the reactor all at once, in batches or continuously, so that the first polymerizable monomer and the second modified monomer undergo copolymerization to generate the fluorine-containing copolymer.

[0018] According to another embodiment of one aspect of the present application, the method uses one or more additives selected from the following: dispersants, initiators, chain transfer agents. According to another embodiment of one aspect of the present application, the dispersant is selected from one or more of the following: methyl hydroxymethyl cellulose, methyl hydroxyethyl cellulose, methyl hydroxypropyl cellulose, ethyl hydroxymethyl cellulose, ethyl hydroxyethyl cellulose, polyvinyl alcohol. According to another embodiment of one aspect of the present application, the initiator is selected from one or more of the following: diethylhexyl peroxydicarbonate, tert-butyl peroxyneodecanoate, diisopropyl peroxydicarbonate, dodecyl peroxide, dibenzoyl peroxide, tert-butyl peroxy-2-ethylhexanoate. According to another embodiment of one aspect of the present application, the chain transfer agent is selected from one or more of the following: ethyl acetate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, ethylene carbonate, diethyl malonate, acetone, methyl propionate, ethyl propionate, diethyl succinate.

[0019] A second aspect of the present application provides a fluorine-containing copolymer, wherein the fluorine-containing copolymer comprises a first copolymerization unit and a second copolymerization unit:

[0020] The first copolymerized unit is derived from the first polymerized monomer shown in formula I:

[0021]

[0022] In Formula I, R 1 and R 2 Each is independently selected from: H, F, C1-C4 alkyl, fluorinated C1-C4 alkyl, C2-C4 alkenyl, fluorinated C2-C4 alkenyl, C1-C4 alkoxy, fluorinated C1-C4 alkoxy; R3 and R4 are each independently selected from F, fluorinated C1-C4 alkyl, fluorinated C2-C4 alkenyl, fluorinated C1-C4 alkoxy;

[0023] The second copolymerized unit is derived from the second modified monomer shown in formula II:

[0024]

[0025] In Formula II, R 5 and R 6 Each is independently selected from H, F, C1-C6 alkyl, fluorinated C1-C6 alkyl, C1-C6 alkoxy, fluorinated C1-C6 alkoxy, C2-C6 alkenyl, fluorinated C2-C6 alkenyl; R 7 is selected from F, fluorinated C1-C6 alkyl, fluorinated C1-C6 alkoxy, fluorinated C2-C6 alkenyl; R 8 Selected from hydroxy, C1-C12 alkoxy, fluorinated C1-C12 alkoxy, C3-12 cycloalkoxy, hydroxy C3-12 cycloalkoxy, fluorinated C3-12 cycloalkoxy, hydroxy fluorinated C3-12 cycloalkoxy, C6-C12 aryloxy, fluorinated C6-C12 aryloxy, C4-C12 heteroaryloxy, fluorinated C4-C12 heteroaryloxy.

[0026] According to one embodiment of the second aspect of the present application, the weight ratio of the first copolymerization unit to the second copolymerization unit is 99.9:1 to 80:20.

[0027] According to another embodiment of the second aspect of the present application, the fluorine-containing copolymer is prepared by the method of the present application.

[0028] The third aspect of the present application provides a binder for a lithium battery, wherein the binder comprises a fluorine-containing copolymer prepared by the method of the present application.

[0029] A fourth aspect of the present application provides an electrode for a lithium battery, wherein the electrode is manufactured using the binder of the present invention.

[0030] A fifth aspect of the present application provides a lithium battery, which comprises at least two electrodes, at least one of which is manufactured using the binder of the present invention.

[0031] In the following specific implementation section, the technical solution of the present application is described in conjunction with the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 Infrared spectrum of a fluorinated copolymer prepared according to a specific embodiment of the present application. DETAILED DESCRIPTION

[0033] "Range" disclosed herein is in the form of lower limit and upper limit. It can be one or more lower limits, and one or more upper limits respectively. A given range is defined by selecting a lower limit and an upper limit. The selected lower limit and upper limit define the boundaries of a particular range. All ranges that can be defined in this way are inclusive and combinable, i.e. any lower limit can be combined with any upper limit to form a range. For example, a range of 60-120 and 80-110 is listed for a particular parameter, and it is understood that a range of 60-110 and 80-120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3, 4 and 5 are listed, the following ranges can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5.

[0034] In the present invention, unless otherwise specified, the numerical range "ab" represents an abbreviation of any real number combination between a and b, where a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" have been listed in this document, and "0-5" is just an abbreviation of these numerical combinations.

[0035] In the present invention, unless otherwise specified, all embodiments and preferred embodiments mentioned herein can be combined with each other to form a new technical solution.

[0036] In the present invention, unless otherwise specified, all technical features and preferred features mentioned herein can be combined with each other to form a new technical solution.

[0037] In the present invention, unless otherwise specified, all steps mentioned herein may be performed sequentially or randomly, but are preferably performed sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0038] In the present invention, if there is no special explanation, the "including" mentioned herein means open or closed. For example, the "including" may mean that other components not listed may also be included, or only the listed components may be included.

[0039] In the present invention, when describing the spatial relationship of a specific component or object relative to other components or objects, the terms "inside", "outside", "above", "below", etc. are used to indicate that the former is located inside, outside, above or below the latter, and the two may be in direct contact, or be separated by a certain distance or separated by a third component or object.

[0040] It should be emphasized that what is shown in the drawings and described below are only some specific embodiments of the present invention, and the protection scope of the present invention is not limited to these specific embodiments. The protection scope of the present invention is defined by the claims of the present invention, and may include any technical solution within the scope of the claims, including but not limited to further improvements and substitutions to these specific embodiments.

[0041] The fluorine-containing copolymer of the present application includes a first polymerizable monomer and a second modified monomer undergoing copolymerization to generate the fluorine-containing copolymer. According to a specific embodiment of the present application, the fluorine-containing copolymer of the present invention is a "binary fluorine-containing copolymer", and the monomers used to prepare the fluorine-containing copolymer only include the first polymerizable monomer and the second modified monomer described above, and do not include any other copolymerizable monomers.

[0042] According to one embodiment of the present application, the first polymerizable monomer has a structure shown in Formula I:

[0043]

[0044] In Formula I, R 1 and R 2 Each is independently selected from: H, F, C1-C4 alkyl, fluorinated C1-C4 alkyl, C2-C4 alkenyl, fluorinated C2-C4 alkenyl, C1-C4 alkoxy, fluorinated C1-C4 alkoxy; R3 and R4 are each independently selected from F, fluorinated C1-C4 alkyl, fluorinated C2-C4 alkenyl, fluorinated C1-C4 alkoxy.

[0045] Throughout this application, when a group is described as "fluorinated", it means that at least one hydrogen atom connected to a carbon atom in the group is replaced by a fluorine atom. For example, a fluorinated group can be substituted by one, two, three, four, five, six, seven, eight, nine, ten, eleven, twelve, thirteen, fourteen, fifteen, sixteen or more fluorine atoms. The fluorination rate of the fluorinated group can be at least 5%, or at least 10%, or at least 20%, or at least 30%, or at least 40%, or at least 50%, or at least 60%, or at least 70%, or at least 80%, or at least 90%, or it is perfluorinated.

[0046] According to one embodiment of the present application, the first polymerizable monomer is a C2-C6 olefin containing at least two fluorine atoms. According to a specific embodiment of the present application, the first polymerizable monomer is selected from one or more of the following: vinylidene fluoride, trifluoroethylene, 1,1-difluoropropylene, 1,1,3-trifluoropropylene, hexafluoroisobutylene, hexafluorobutadiene, hexafluoro-2-butene, 1,1-difluoro-2-fluoromethoxyethylene, 1,1-difluoro-2-perfluoromethoxyethylene. More specifically, the first polymerizable monomer is vinylidene fluoride, i.e., 1,1-difluoroethylene.

[0047] According to another embodiment of the present application, the second modified monomer has a structure shown in Formula II:

[0048]

[0049] In Formula II, R 5 and R 6 Each is independently selected from H, F, C1-C6 alkyl, fluorinated C1-C6 alkyl, C1-C6 alkoxy, fluorinated C1-C6 alkoxy, C2-C6 alkenyl, fluorinated C2-C6 alkenyl; R 7 is selected from F, fluorinated C1-C6 alkyl, fluorinated C1-C6 alkoxy, fluorinated C2-C6 alkenyl; R 8 is selected from hydroxy, C1-C12 alkoxy, fluorinated C1-C12 alkoxy, C3-12 cycloalkoxy, hydroxy C3-12 cycloalkoxy, fluorinated C3-12 cycloalkoxy, hydroxy fluorinated C3-12 cycloalkoxy, C6-C12 aryloxy, fluorinated C6-C12 aryloxy, C4-C12 heteroaryloxy, fluorinated C4-C12 heteroaryloxy. For example, in Formula II, R 5 and R 6 Each is independently selected from H, F, C1-C4 alkyl, fluorinated C1-C4 alkyl, C1-C4 alkoxy, fluorinated C1-C4 alkoxy, C2-C4 alkenyl, fluorinated C2-C4 alkenyl; R 7is selected from F, fluorinated C1-C4 alkyl, fluorinated C1-C4 alkoxy, fluorinated C2-C4 alkenyl; R 8 Selected from hydroxy, C1-C6 alkoxy, fluorinated C1-C6 alkoxy, C3-C6 cycloalkoxy, hydroxy C3-C6 cycloalkoxy, fluorinated C3-C6 cycloalkoxy, hydroxy fluorinated C3-C6 cycloalkoxy, C6-C10 aryloxy, fluorinated C6-C10 aryloxy, C4-C10 heteroaryloxy, fluorinated C4-C10 heteroaryloxy.

[0050] According to a specific embodiment of the present application, the second modified monomer is 2-(trifluoromethyl) acrylic acid or 2-(trifluoromethyl) acrylic acid ester, such as alkyl ester, fluoroalkyl ester, cycloalkyl ester, fluorocycloalkyl ester, aryl ester, fluoroaryl ester, heteroaryl ester, fluoroheteroaryl ester. For example, the second modified monomer is selected from one or more of the following: 2-(trifluoromethyl) acrylic acid, methyl 2-(trifluoromethyl) acrylic acid, ethyl 2-(trifluoromethyl) acrylic acid, propyl 2-(trifluoromethyl) acrylic acid, tert-butyl 2-(trifluoromethyl) acrylic acid, methyl pentafluoromethylacrylate, 2-(trifluoromethyl) acrylic acid-2,2,2-trifluoroethyl ester, 2-(trifluoromethyl) acrylic acid-4-hydroxycyclohexyl ester, 2-(trifluoromethyl) acrylic acid-tetrahydro-2H-pyran-2-yl ester, 2-(trifluoromethyl)-acrylic acid-3,3,3-trifluoropropyl ester, 2-(trifluoromethyl) acrylic acid-4,4,4-trifluorobutyl ester. According to a more specific example, the second modifying monomer is 2-(trifluoromethyl)acrylic acid, methyl 2-(trifluoromethyl)acrylate or methyl pentafluoromethacrylate, wherein methyl pentafluoromethacrylate refers to (difluoromethyl) 2-(trifluoromethyl)acrylate.

[0051] According to one embodiment of the present application, the weight ratio of the first polymerized monomer to the second modified monomer is 99.9:0.1 to 80:20, for example, it can be 99:1 to 82:18, or 98:2 to 85:15, or 95:5 to 88:12, or 92:8 to 90:10, or it can be within the ratio range obtained by combining any two of the above end values.

[0052] According to one embodiment of the present application, the copolymerization reaction of the first polymerizable monomer and the second modifying monomer is performed by suspension polymerization.

[0053] According to a specific embodiment of the present application, the copolymerization reaction can be carried out in a reaction vessel under suitable reaction conditions with a first polymerizable monomer and a second modifying monomer. According to an exemplary embodiment of the present application, the first polymerizable monomer and the second modifying monomer are in the form of gas, liquid or solid, respectively, for example, the first polymerizable monomer is in the form of gas, and the second modifying monomer is in the form of liquid or solid.

[0054] In the case where the first polymerizable monomer is a gas and the second modifying monomer is a liquid or a solid, the first monomer can be charged into the reactor as a gas, and the second monomer can be added into the reactor as a liquid or a solution (a solution formed by dissolving a liquid or a solid in water), and the reactor can also be additionally filled with water and optional other components; as the polymerization reaction proceeds, the first polymerizable monomer and the second modifying monomer are polymerized to form a polymer, and the intermediate polymer is dispersed in the water in the reactor to form an aqueous dispersion.

[0055] According to one embodiment of the present application, the first polymerizable monomer and the second modifying monomer are added into the reactor at one time before the reaction starts.

[0056] According to another embodiment of the present application, the first polymerizable monomer is divided into several portions, a portion of which is added to the reactor before the reaction begins, and the remaining portion is added to the reactor in batches or continuously during the reaction; the second modifying monomer is added to the reactor in a one-time, step-by-step or continuous manner after the polymerization reaction begins.

[0057] According to one embodiment of the present application, the first polymerizable monomer is charged into the reactor in the form of gas so that the reactor obtains a target pressure. After the reaction starts, the second modified monomer is added to the reactor in a one-time, step-by-step or continuous manner; and the first polymerizable monomer is continuously replenished during the reaction so that the pressure in the reactor is maintained at the above-mentioned target pressure until the required amount of the first polymerizable monomer reacts.

[0058] According to one embodiment of the present application, the target pressure of the first polymerization monomer during the reaction process can be 4.0-8.5 MPa, for example 4.5-8.0 MPa, or 5.0-7.5 MPa, or 5.5-7.0 MPa, or 6.0-6.5 MPa, or within the numerical range obtained by combining any two of the above end values.

[0059] According to one embodiment of the present application, the water added to the reactor, the total amount of the first polymerized monomer and the second modified monomer added to the reactor, and the amount of various optional additives added to the reactor are selected so that the concentration of the aqueous dispersion formed after the reaction can be 1-70% by weight, for example, 2-65% by weight, or 5-60% by weight, or 8-55% by weight, or 10-50% by weight, or 15-40% by weight, or 20-35% by weight, or 25-30% by weight, or within the numerical range obtained by combining any two of the above end values.

[0060] The copolymerization reaction can be carried out at a temperature of 35-110°C, for example, 36-100°C, or 37-90°C, or 38-80°C, or 38-75°C, 40-70°C, or 45-65°C, or 50-60°C, or within the numerical range obtained by combining any two of the above end values.

[0061] The water used in the polymerization reaction may be distilled water, double distilled water, deionized water, etc.

[0062] According to one embodiment of the present application, one or more of the following additives may be used as needed: a dispersant, a chain transfer agent, and an initiator. One or more of the additives may be added to the reactor in a one-time, batch, or continuous form before the reaction and / or during the reaction, for example, in the form of an aqueous solution.

[0063] According to one embodiment of the present application, the dispersant is modified cellulose or polyvinyl alcohol, for example, the dispersant can be selected from one or more of the following: methyl hydroxymethyl cellulose, methyl hydroxyethyl cellulose, methyl hydroxypropyl cellulose, ethyl hydroxymethyl cellulose, ethyl hydroxyethyl cellulose, polyvinyl alcohol. According to another embodiment of the present application, based on the weight of the water in the reactor as 100 parts by weight, the amount of the dispersant added is 0.03-1.5 parts by weight, for example, 0.05-1.2 parts by weight, or 0.1-1.0 parts by weight, or 0.2-0.8 parts by weight, or 0.3-0.7 parts by weight, or 0.4-0.5 parts by weight, or within the numerical range obtained by combining any two of the above end values.

[0064] According to one embodiment of the present application, the chain transfer agent is selected from one or more of the following: ethyl acetate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, ethylene carbonate, diethyl malonate, acetone, methyl propionate, ethyl propionate, diethyl succinate. According to another embodiment of the present application, based on the weight of the water in the reactor as 100 parts by weight, the content of the chain transfer agent is 0.003-1.5 parts by weight, for example, 0.005-1.4 parts by weight, or 0.01-1.3 parts by weight, or 0.05-1.2 parts by weight, or 0.1-1.1 parts by weight, or 0.2-1.0 parts by weight, or 0.4-0.9 parts by weight, or 0.5-0.8 parts by weight, or 0.6-0.7 parts by weight, or within the numerical range obtained by combining any two of the above end values.

[0065] According to one embodiment of the present application, the initiator is selected from one or more of the following: diethylhexyl peroxydicarbonate, tert-butyl peroxyneodecanoate, diisopropyl peroxydicarbonate, dodecyl peroxide, dibenzoyl peroxide, tert-butyl peroxy-2-ethylhexanoate. According to another embodiment of the present application, based on the weight of the water in the reactor as 100 parts by weight, the content of the initiator is 0.05-2.0 parts by weight, for example, 0.08-1.8 parts by weight, or 0.10-1.6 parts by weight, or 0.15-1.5 parts by weight, or 0.50-1.4 parts by weight, or 0.60-1.3 parts by weight, or 0.7-1.2 parts by weight, or 0.8-1.1 parts by weight, or 0.9-1.0 parts by weight, or within the numerical range obtained by combining any two of the above end values.

[0066] According to one embodiment of the present application, the aqueous dispersion prepared by copolymerization reaction can be dried, washed, and other steps to obtain a fluorine-containing polymer product.

[0067] According to one embodiment of the present application, the weight average molecular weight (Mw) of the fluorinated copolymer prepared by the present invention can be 5000 to 3,000,000 g / mol, for example, 6000 to 2,000,000 g / mol, or 8000 to 1,500,000 g / mol, or 10,000 to 1,000,000 g / mol, or 20,000 to 900,000 g / mol, or 50,000 to 850,000 g / mol, or 80,000 to 800,000 g / mol, or 100,000 to 750,000 g / mol, preferably 700,000 to 850,000 g / mol, or within the numerical range obtained by combining any two of the above end values.

[0068] According to one embodiment of the present application, the polydispersity (also known as molecular weight distribution, Mw / Mn) of the fluorinated copolymer prepared by the present invention can be 1.5-3.5, for example, 1.8-3.2, or 2.0-3.0, or 2.2-2.8, or 2.3-2.7, or within the numerical range obtained by combining any two of the above end values.

[0069] According to one embodiment of the present application, the first polymerized monomer and the second modified monomer are covalently connected to each other through the "carbon-carbon double bonds" contained in each of them during the polymerization process to form the main chain of the product fluorinated copolymer. Therefore, in the present application, the main chain of the fluorinated copolymer comprises a first polymerized unit derived from the first polymerized monomer and a second polymerized unit derived from the second modified monomer.

[0070] According to a specific embodiment of the present application, the method of the present invention comprises the following steps: (1) adding water, dispersant and chain transfer agent into a reactor, evacuating the reactor, and then replacing the oxygen content in the reactor with nitrogen until the oxygen content is less than 150ppm; (2) heating the reactor to 38-75°C, introducing the first polymerization monomer in gaseous state, raising the pressure in the reactor to 4.0-8.5Mpa, and injecting the chain transfer agent and initiator into the reactor through a metering pump to initiate the reaction; (3) after the reaction is initiated, continuously adding the second modified monomer into the reactor through a metering pump for copolymerization, and at the same time starting the compression pump to add the first polymerization monomer, so that the pressure in the reactor is kept stable at 4.0-8.5Mpa, and injecting the initiator into the reactor every 30-70 minutes; (4) ending the reaction, cooling and releasing the pressure to remove the remaining gas; (5) then releasing the water dispersion in the reactor, washing until the wastewater conductivity is reduced to below 2μs / cm, and drying to obtain a white solid powder, which is the fluorine-containing copolymer of the present invention.

[0071] According to one embodiment of the present application, the fluorinated copolymer of the present application can be used as a binder for preparing electrodes in lithium-ion batteries, and exhibits extremely excellent bonding properties, such as improving the peel strength of the positive electrode sheet and / or the negative electrode sheet, alleviating cracking and powdering of the electrode sheet, and greatly improving the bonding force between the electrode active slurry and the current collector, meeting the requirements of lithium batteries for the use of binders, and obtaining lithium batteries with higher stability.

[0072] Example

[0073] The preferred embodiments of the present invention are specifically listed in the following examples, but it should be understood that the protection scope of the present application is not limited thereto. Any equivalent changes or modifications made according to the essence of the present application should be included in the protection scope of the present application.

[0074] Example 1

[0075] Add 3.5 kg of deionized water to a 5L stainless steel horizontal reactor, weigh 3.2 g of hydroxypropyl methylcellulose, dissolve it in 100 g of deionized water, and add the obtained solution to the reactor. The reactor is sealed, evacuated and replaced with nitrogen, and the oxygen content in the reactor is lower than 150 ppm, and the temperature in the reactor is raised to 55 ° C by heating. After reaching the above-mentioned set temperature, vinylidene fluoride (VDF) is transported from the VDF storage tank to the sealed reactor by a membrane pump, so that the pressure in the reactor reaches 6.2 MPa, and 2.7 g of ethyl acetate and 1.3 g of diisopropyl peroxydicarbonate are added to the reactor by a metering pump, so that polymerization reaction begins in the reactor. 28.5 g of 2-(trifluoromethyl) acrylic acid is dissolved in deionized water in advance to prepare an aqueous solution with a concentration of 5% by weight. By observing the gauge pressure of the pressure gauge, when observing that the pressure in the reactor begins to decrease, the above-mentioned 2-(trifluoromethyl) acrylic acid aqueous solution prepared in advance is transported into the reactor at a speed of 90 grams per hour with a metering pump to make it participate in the reaction. During the entire reaction period, VDF gas is supplemented in the reactor at any time by the pressure automatic control system so that the pressure in the reactor is maintained at 6.2MPa. Calculated from the moment when the polyreaction starts, every 1 hour, diisopropyl peroxydicarbonate 4g is added to the reactor, and the addition of diisopropyl peroxydicarbonate is carried out five times. Polyreaction is carried out after 6.3 hours to terminate the reaction, and the whole polymerization process consumes 950 grams of vinylidene fluoride. The temperature of the reactor was lowered to room temperature, the reactor was depressurized, the polymer aqueous dispersion in the reactor was discharged from the reactor, the gas was removed in a degassing tank, the unreacted monomer was recovered, the polymer aqueous dispersion was transported to a washing tank, deionized water at a temperature of 80° C. was added thereto, stirred for 30 minutes, allowed to stand for stratification and the waste water was discarded, the washing was repeated until the waste water conductivity was less than 2 μs / cm, and the washed polymer aqueous dispersion was spray-dried to obtain a white powder product.

[0076] The white powder product was characterized by infrared spectrometer, and the infrared spectrum was measured as follows: Figure 1 As shown. Figure 1 It can be seen that in Example 1, a copolymer of VDF and 2-(trifluoromethyl)acrylic acid was prepared.

[0077] The properties of the white powder product were tested and the test results are listed in Table 1.

[0078] Example 2

[0079] Add 3.5 kg of deionized water to a 5L stainless steel horizontal reactor, weigh 3.2 g of hydroxypropyl methylcellulose, dissolve it in 100 g of deionized water, and add the obtained solution to the reactor. The reactor is sealed, evacuated and replaced with nitrogen, and the oxygen content in the reactor is lower than 150 ppm, and the temperature in the reactor is raised to 55 ° C by heating. After reaching the above-mentioned set temperature, vinylidene fluoride (VDF) is transported from the VDF storage tank to the sealed reactor by a membrane pump, so that the pressure in the reactor reaches 6.2 MPa, and 2.7 g of ethyl acetate and 1.3 g of diisopropyl peroxydicarbonate are added to the reactor by a metering pump, so that polymerization reaction begins in the reactor. 42.7 g of 2-(trifluoromethyl) acrylic acid is dissolved in deionized water in advance to prepare an aqueous solution with a concentration of 5% by weight. By observing the gauge pressure of the pressure gauge, when observing that the pressure in the reactor begins to decline, the above-mentioned 2-(trifluoromethyl) acrylic acid aqueous solution prepared in advance is transported into the reactor at a speed of 180 grams per hour with a metering pump, so that it participates in the reaction. During the whole reaction period, VDF gas is supplemented in the reactor at any time by the pressure automatic control system so that the pressure in the reactor is maintained at 6.2MPa. Calculated from the moment when the polyreaction starts, every 1 hour, diisopropyl peroxydicarbonate 4g is added to the reactor, and the addition of diisopropyl peroxydicarbonate is carried out five times. Polyreaction is carried out 7.1 hours later and the reaction is terminated, and the whole polymerization process consumes 950 grams of vinylidene fluoride. The temperature of the reactor was lowered to room temperature, the reactor was depressurized, the polymer aqueous dispersion in the reactor was discharged from the reactor, the gas was removed in a degassing tank, the unreacted monomer was recovered, the polymer aqueous dispersion was transported to a washing tank, deionized water at a temperature of 80° C. was added thereto, stirred for 30 minutes, allowed to stand for stratification and the waste water was discarded, the washing was repeated until the waste water conductivity was less than 2 μs / cm, and the washed polymer aqueous dispersion was spray-dried to obtain a white powder product.

[0080] The properties of the white powder product were detected and the characterization results are listed in Table 1.

[0081] Example 3

[0082] 3.5 kg of deionized water was added to a 5L stainless steel horizontal reactor, 3.2 g of hydroxypropyl methylcellulose was weighed, dissolved in 100 g of deionized water, and the obtained solution was added to the reactor. The reactor was sealed, evacuated and replaced with nitrogen, the oxygen content in the reactor was lower than 150 ppm, and the temperature in the reactor was raised to 55 ° C by heating. After reaching the above-mentioned set temperature, vinylidene fluoride (VDF) was transported from the VDF storage tank to the sealed reactor by a membrane pump, so that the pressure in the reactor reached 6.2 MPa, and 2.7 g of ethyl acetate and 1.3 g of diisopropyl peroxydicarbonate were added to the reactor by a metering pump, so that polymerization began to occur in the reactor. 28.5 g of methyl 2-(trifluoromethyl)acrylate was dissolved in deionized water in advance and prepared into an aqueous solution with a concentration of 5% by weight. By observing the gauge pressure of the pressure gauge, when it is observed that the pressure in the reactor begins to decrease, the above-mentioned pre-prepared 2-(trifluoromethyl) methyl acrylate aqueous solution is transported into the reactor at a speed of 90 grams per hour with a metering pump to participate in the reaction. During the entire reaction, VDF gas is supplemented in the reactor at any time by the pressure automatic control system so that the pressure in the reactor is maintained at 6.2MPa. Calculated from the moment when the polymerization reaction starts, every 1 hour, diisopropyl peroxydicarbonate 4g is added to the reactor, and the addition of diisopropyl peroxydicarbonate is carried out five times. The polymerization reaction ends after 6.5 hours, and the whole polymerization process consumes 950 grams of vinylidene fluoride. The temperature of the reactor was lowered to room temperature, the reactor was depressurized, the polymer aqueous dispersion in the reactor was discharged from the reactor, the gas was removed in a degassing tank, the unreacted monomer was recovered, the polymer aqueous dispersion was transported to a washing tank, deionized water at a temperature of 80° C. was added thereto, stirred for 30 minutes, allowed to stand for stratification and the waste water was discarded, the washing was repeated until the waste water conductivity was less than 2 μs / cm, and the washed polymer aqueous dispersion was spray-dried to obtain a white powder product.

[0083] The properties of the white powder product were detected and the characterization results are listed in Table 1.

[0084] Example 4

[0085] Add 3.5 kg of deionized water to a 5L stainless steel horizontal reactor, weigh 3.2 g of hydroxypropyl methylcellulose, dissolve it in 100 g of deionized water, and add the obtained solution to the reactor. Close the reactor, evacuate and replace with nitrogen, wait for the oxygen content in the reactor to be lower than 150 ppm, and heat the reactor to raise the temperature to 55 ° C. After reaching the above-mentioned set temperature, use a membrane pump to transport vinylidene fluoride (VDF) from the VDF storage tank to the closed reactor, so that the pressure in the reactor reaches 6.2 MPa, and use a metering pump to add 2.7 g of ethyl acetate and 1.3 g of diisopropyl peroxydicarbonate to the reactor, so that polymerization reaction begins in the reactor. Dissolve 28.5 g of methyl pentafluoromethacrylate in deionized water in advance to prepare an aqueous solution with a concentration of 5% by weight. By observing the gauge pressure of the pressure gauge, when it is observed that the pressure in the reactor begins to drop, the above-prepared aqueous solution of methyl pentafluoromethacrylate is transported into the reactor at a speed of 90 grams per hour with a metering pump to participate in the reaction. During the entire reaction period, VDF gas is added to the reactor at any time through the pressure automatic control system so that the pressure in the reactor is maintained at 6.2MPa. Calculated from the moment when the polymerization reaction starts, 4g of diisopropyl peroxydicarbonate is added to the reactor every 1 hour, and a total of five additions of diisopropyl peroxydicarbonate are performed. The polymerization reaction ends after 6.5 hours, and the entire polymerization process consumes a total of 950 grams of vinylidene fluoride. The temperature of the reactor was lowered to room temperature, the reactor was depressurized, the polymer aqueous dispersion in the reactor was discharged from the reactor, the gas was removed in a degassing tank, the unreacted monomer was recovered, the polymer aqueous dispersion was transported to a washing tank, deionized water at a temperature of 80° C. was added thereto, stirred for 30 minutes, allowed to stand for stratification and the waste water was discarded, the washing was repeated until the waste water conductivity was less than 2 μs / cm, and the washed polymer aqueous dispersion was spray-dried to obtain a white powder product.

[0086] The properties of the white powder product were detected and the characterization results are listed in Table 1.

[0088] Comparative Example 1

[0089] 3.5 kg of deionized water was added to a 5L stainless steel horizontal reactor, 3.2 g of hydroxypropyl methylcellulose was weighed, dissolved in 100 g of deionized water, and the obtained solution was added to the reactor. The reactor was closed, vacuumed and replaced with nitrogen, the oxygen content in the reactor was lower than 150 ppm, and the temperature in the reactor was raised to 55 ° C by heating. After reaching the above-mentioned set temperature, vinylidene fluoride (VDF) was transported from the VDF storage tank to the closed reactor with a membrane pump, so that the pressure in the reactor reached 6.2 MPa, and 2.7 g of ethyl acetate and 1.3 g of diisopropyl peroxydicarbonate were added to the reactor with a metering pump, so that polymerization began to occur in the reactor. During the entire reaction, VDF gas was supplemented in the reactor at any time by the pressure automatic control system, so that the pressure in the reactor was maintained at 6.2 MPa. Calculated from the moment when the polymerization reaction started, 4 g of diisopropyl peroxydicarbonate was added to the reactor every 1 hour, and a total of five diisopropyl peroxydicarbonate additions were performed. The polymerization reaction was terminated after 6.7 hours, and a total of 950 grams of vinylidene fluoride was consumed in the whole polymerization process. The temperature of the reactor was lowered to room temperature, the reactor was depressurized, the polymer aqueous dispersion in the reactor was discharged from the reactor, the gas was removed in the degassing tank, the unreacted monomer was recovered, the polymer aqueous dispersion was transported to a washing tank, deionized water at a temperature of 80° C. was added thereto, stirred for 30 minutes, allowed to stand for stratification and the waste water was discarded, and the washing was repeated until the waste water conductivity was less than 2 μs / cm, and the washed polymer aqueous dispersion was spray-dried to obtain a white powder product.

[0090] The properties of the white powder product were detected and the characterization results are listed in Table 1.

[0091] The test results show that the vinylidene fluoride copolymer prepared by the method of the present invention exhibits excellent peel strength due to the combination of modified monomers in the polymer main chain. When the polymer is used as a binder, it will inevitably effectively improve its bonding force with the electrode active material and the current collector, and the prepared lithium battery will inevitably have the advantages of high peel strength and high cycle capacity retention rate.

[0092] Table 1 Performance test of fluorine-containing polymers of Examples 1-4 and Comparative Example 1

[0093]

Claims

1. A method for preparing a fluorinated copolymer, the method comprising: Allowing the first polymerizable monomer to copolymerize with the second modified monomer to generate the fluorine-containing copolymer; The first polymerizable monomer has a structure shown in Formula I: In Formula I, R1 and R2 are each independently selected from: H, F, C1-C4 alkyl, fluorinated C1-C4 alkyl, C2-C4 alkenyl, fluorinated C2-C4 alkenyl, C1-C4 alkoxy, fluorinated C1-C4 alkoxy; R3 and R4 are each independently selected from: F, fluorinated C1-C4 alkyl, fluorinated C2-C4 alkenyl, fluorinated C1-C4 alkoxy; The second modified monomer has a structure shown in Formula II: In formula II, R5 and R6 are each independently selected from H, F, C1-C6 alkyl, fluorinated C1-C6 alkyl, C1-C6 alkoxy, fluorinated C1-C6 alkoxy, C2-C6 alkenyl, fluorinated C2-C6 alkenyl; R7 is selected from F, fluorinated C1-C6 alkyl, fluorinated C1-C6 alkoxy, fluorinated C2-C6 alkenyl; R8 is selected from hydroxyl, C1-C12 alkoxy, fluorinated C1-C12 alkoxy, C3-12 cycloalkyloxy, hydroxyl C3-12 cycloalkyloxy, fluorinated C3-12 cycloalkyloxy, hydroxyl fluorinated C3-12 cycloalkyloxy, C6-C12 aryloxy, fluorinated C6-C12 aryloxy, C4-C12 heteroaryloxy, fluorinated C4-C12 heteroaryloxy.

2. The method according to claim 1, characterized in that The weight ratio of the first polymerizable monomer to the second modifying monomer is 99.9:1 to 80:

20.

3. The method according to claim 1 or 2, characterized in that The first polymerizable monomer is selected from one or more of the following: vinylidene fluoride, trifluoroethylene, 1,1-difluoropropylene, 1,1,3-trifluoropropylene, hexafluoroisobutylene, hexafluorobutadiene, hexafluoro-2-butene, 1,1-difluoro-2-fluoromethoxyethylene, and 1,1-difluoro-2-perfluoromethoxyethylene.

4. The method according to claim 1 or 2, characterized in that: The second modifying monomer is selected from one or more of the following: 2-(trifluoromethyl)acrylic acid, methyl 2-(trifluoromethyl)acrylate, ethyl 2-(trifluoromethyl)acrylate, propyl 2-(trifluoromethyl)acrylate, tert-butyl 2-(trifluoromethyl)acrylate, methyl pentafluoromethacrylate, 2-(trifluoromethyl)acrylate-2,2,2-trifluoroethyl ester, 2-(trifluoromethyl)acrylate-4-hydroxycyclohexyl ester, 2-(trifluoromethyl)acrylate-tetrahydro-2H-pyran-2-yl ester, 2-(trifluoromethyl)-acrylate-3,3,3-trifluoropropyl ester, and 2-(trifluoromethyl)acrylate-4,4,4-trifluorobutyl ester.

5. The method according to claim 1 or 2, characterized in that: The method comprises: during the polymerization of the first polymerizable monomer in the reactor, adding the second modifying monomer into the reactor all at once, in batches or continuously, so that the first polymerizable monomer and the second modifying monomer undergo copolymerization reaction to generate the fluorine-containing copolymer.

6. The method according to claim 1 or 2, characterized in that: The method uses one or more additives selected from the group consisting of: dispersants, initiators, chain transfer agents; The dispersant is selected from one or more of the following: methyl hydroxymethyl cellulose, methyl hydroxyethyl cellulose, methyl hydroxypropyl cellulose, ethyl hydroxymethyl cellulose, ethyl hydroxyethyl cellulose, polyvinyl alcohol; The initiator is selected from one or more of the following: diethylhexyl peroxydicarbonate, tert-butyl peroxyneodecanoate, diisopropyl peroxydicarbonate, dodecyl peroxide, dibenzoyl peroxide, tert-butyl peroxy-2-ethylhexanoate; The chain transfer agent is selected from one or more of the following: ethyl acetate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, ethylene carbonate, diethyl malonate, acetone, methyl propionate, ethyl propionate, and diethyl succinate.

7. A fluorine-containing copolymer, comprising a first copolymerization unit and a second copolymerization unit: The first copolymerized unit is derived from the first polymerized monomer shown in formula I: In Formula I, R1 and R2 are each independently selected from: H, F, C1-C4 alkyl, fluorinated C1-C4 alkyl, C2-C4 alkenyl, fluorinated C2-C4 alkenyl, C1-C4 alkoxy, fluorinated C1-C4 alkoxy; R3 and R4 are each independently selected from: F, fluorinated C1-C4 alkyl, fluorinated C2-C4 alkenyl, fluorinated C1-C4 alkoxy; The second copolymerized unit is derived from the second modified monomer shown in formula II: In formula II, R5 and R6 are each independently selected from H, F, C1-C6 alkyl, fluorinated C1-C6 alkyl, C1-C6 alkoxy, fluorinated C1-C6 alkoxy, C2-C6 alkenyl, fluorinated C2-C6 alkenyl; R7 is selected from F, fluorinated C1-C6 alkyl, fluorinated C1-C6 alkoxy, fluorinated C2-C6 alkenyl; R8 is selected from hydroxy, C1-C12 alkoxy, fluorinated C1-C12 alkoxy, C3-12 cycloalkyloxy, hydroxy C3-12 cycloalkyloxy, fluorinated C3-12 cycloalkyloxy, hydroxy fluorinated C3-12 cycloalkyloxy, C6-C12 aryloxy, fluorinated C6-C12 aryloxy, C4-C12 heteroaryloxy, fluorinated C4-C12 heteroaryloxy; The weight ratio of the first copolymerization unit to the second copolymerization unit is 99.9:1 to 80:

20.

8. The fluorinated copolymer according to claim 7, characterized in that The fluorine-containing copolymer is prepared by the method according to any one of claims 1 to 6. 9 . A binder for a lithium battery, the binder comprising a fluorine-containing copolymer prepared by the method according to claim 1 , or the binder comprising a fluorine-containing copolymer according to claim 7 . 10 . A lithium battery comprising a positive electrode and a negative electrode, wherein at least one of the positive electrode and the negative electrode is prepared using the binder according to claim 9 .

Citation Information

Cited By

  • Graphene protective film and preparation method thereof

    CN119391315A