Method for constructing compact hydrogen barrier film through segmented precise regulation and control of electrostatic-hydrogen-bond interaction

By adjusting the pH value of the polymer solution in segments, switching the dominant driving force in the self-assembly process, combining electrostatic and hydrogen bonding, an efficient and stable hydrogen barrier membrane is built, solving the problem of the hydrogen barrier membrane easily forming holes and The problem of structural instability achieves excellent hydrogen barrier performance.

CN118978731APending Publication Date: 2024-11-19CHINA UNIV OF PETROLEUM (EAST CHINA)
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202411252489.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The hydrogen barrier film caused by a single driving force in traditional layer-by-layer self-assembly technology is prone to form holes and unstable structure, making it difficult to build a dense and stable hydrogen barrier film.

Method used

By adjusting the pH value of the polymer solution in segments, changing the charge density of the polymer, thereby flexibly switching the dominant driving force during self-assembly, and using the combination of electrostatic and hydrogen bonding to build a dense hydrogen barrier membrane.

Benefits of technology

The hydrogen barrier membrane is achieved with high efficiency, stability and excellent performance, and the hydrogen transmittance is less than 40cm3·m-2·24h-1·0.1MPa-1, overcoming the limitations in a single driving force mode.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a strategy for constructing a compact hydrogen barrier film by utilizing two driving forces, namely electrostatic attraction and hydrogen-bond interaction, in stages in a layer-by-layer self-assembly process. According to the strategy, the limitation caused by a single driving force mode in a traditional layer-by-layer self-assembly process is overcome, the hydrogen-bond interaction is dominated in the early stage, the electrostatic interaction is dominated in the later stage, the problem that holes appear in a barrier layer due to repulsion among polymer molecular chains when the single electrostatic interaction is too strong is effectively avoided, and the compactness of an interlayer structure is ensured; meanwhile, in the initial stage of self-assembly, the binding force between the polymer and the lamellar material is also enhanced by introducing and strengthening the hydrogen bonds. According to the method, the polymer and the two-dimensional layered material are assembled layer by layer, the obtained compact barrier layer creates an extremely zigzag channel for hydrogen permeation, the diffusion process of hydrogen is slowed down, and hydrogen leakage in the storage and transportation process can be effectively inhibited. The method provides a new thought for preparing an efficient, stable and controllable hydrogen barrier film, and has a wide application prospect and a huge economic value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a preparation process of a gas barrier film, which is suitable for blocking hydrogen and inhibiting leakage of hydrogen during storage. Background Art

[0002] With the rapid development of society, economy and technology, the demand for clean energy has shown an unprecedented growth trend. Building an efficient, low-carbon and sustainable energy system has become an urgent need for the development of the times. Hydrogen energy has attracted much attention as the most ideal clean energy in the 21st century. The production of hydrogen is no longer a problem. However, safe and efficient hydrogen storage technology has not been effectively solved, which restricts the large-scale application of hydrogen energy.

[0003] The study found that by combining two-dimensional layered materials with a large aspect ratio with polymers through layer-by-layer self-assembly, a composite film with excellent hydrogen barrier properties can be obtained. However, traditional layer-by-layer self-assembly technology often focuses on a single driving force, such as electrostatic attraction, hydrogen bonding, and one of other forces. Electrostatic attraction is the most common driving force in the layer-by-layer self-assembly process, but if a single electrostatic attraction is used as the driving force, when the charge density of the polymer is too large, there will be a significant repulsive force between the polymer's own molecular chains, which will cause the molecular chain structure adsorbed on the film to be sparse, and the barrier layer is prone to form holes; hydrogen bonding, as an intramolecular and intermolecular interaction, has moderate strength, but its action distance is small, and relying on a single hydrogen bonding action is often not enough to build a dense and stable hydrogen barrier film.

[0004] In order to overcome this limitation, this scheme proposes a new idea: by adjusting the pH value of the polymer solution in stages to change the charge density of the polymer, the dominant driving force can be flexibly switched at different self-assembly stages. In the initial stage of self-assembly, hydrogen bonding is dominant, which enhances the interfacial bonding force between the polymer and the sheet material, prevents the agglomeration of the sheet material and makes it evenly dispersed. At this time, the charge density of the polyelectrolyte is low, the polymer molecular chain is in a random coil conformation, the single-layer film is thick and rough, and as the self-assembly process deepens, the large surface roughness is prone to defects, which is not conducive to the subsequent layer stacking; instead, electrostatic action is dominant, the solution charge density increases, the polymer molecular chain is fully extended, the single-layer film roughness decreases, and the film thickness decreases, which is conducive to the increase of the number of self-assembly layers to obtain a dense barrier layer. Through this strategy, we can make full use of the advantages of electrostatic attraction and hydrogen bonding to construct a more dense, stable and high-performance hydrogen barrier film, which is of great significance to the development of safe and efficient hydrogen storage technology and has great application potential. Summary of the invention

[0005] The purpose of the present invention is to flexibly change the dominant driving force in different stages of self-assembly, so as to overcome the problem that the barrier layer is easy to form a permeation channel and the structure is not stable enough due to the dominance of a single driving force in the traditional layer-by-layer self-assembly process. The present invention has the advantages of high efficiency, flexibility, strong repeatability and high stability.

[0006] The technical solution of the present invention is summarized as follows:

[0007] 1. A method for constructing a dense hydrogen barrier film by precisely controlling electrostatic-hydrogen bonding in sections, characterized in that it comprises the following steps:

[0008] Step 1: Pretreatment of substrate materials: cleaning and modification of the substrate materials;

[0009] Step 2: Solution preparation: prepare two self-assembly solutions, one is a dispersion of layered materials to ensure that they are evenly dispersed in the solvent; the other is a polyelectrolyte solution, selecting a polyelectrolyte with appropriate molecular structure and charge characteristics;

[0010] Step 3: regulating the charge density of the polyelectrolyte solution for the first time;

[0011] Step 4: Alternate assembly and drying: First, place the substrate material under the self-assembly device containing the polyelectrolyte solution. After the assembly is completed, immediately place the substrate material in a desktop glue machine and spin dry. Then, place the substrate material under the self-assembly device containing the sheet material dispersion. After the assembly is completed, immediately place the substrate material in a desktop glue machine and spin dry. Repeat the above operation 5 times to complete the self-assembly of the first 5 layers.

[0012] Step 5: regulating the charge density of the polyelectrolyte solution for a second time;

[0013] Step 6 Repeat step 4 to complete the 5-layer self-assembly.

[0014] 2. According to claim 1, a method for constructing a dense hydrogen barrier film by segmented and precise control of electrostatic-hydrogen bonding is characterized in that the base material used is a polymer film.

[0015] 3. According to claim 1, a method for constructing a dense hydrogen barrier film by segmented precise control of electrostatic-hydrogen bonding is characterized in that the modification of the base material is surface modification to enhance the bonding force between the base material and the barrier layer.

[0016] 4. According to claim 1, a method for constructing a dense hydrogen barrier membrane by segmented precise control of electrostatic-hydrogen bonding is characterized in that the polyelectrolyte solution is a polyethyleneimine solution, the two-dimensional layered material dispersion is a montmorillonite dispersion, the concentrations are all 1-3 mg / ml, and the solvents are all water.

[0017] 5. According to claim 1, a method for constructing a dense hydrogen barrier film by segmented precise control of electrostatic-hydrogen bonding is characterized in that the charge density of the polyethyleneimine solution is changed by adjusting the pH value of the polyethyleneimine solution, and the pH value of the polyethyleneimine solution is adjusted to 9.5 for the first time to complete the self-assembly of the first 5 layers.

[0018] 6. According to claim 1, a method for constructing a dense hydrogen barrier film by segmented precise control of electrostatic-hydrogen bonding is characterized in that the charge density of the polyethyleneimine solution is changed by adjusting the pH value of the polyethyleneimine solution, and the pH value of the polyethyleneimine solution is adjusted to 6.5 for the second time, and then 5 layers are self-assembled.

[0019] The present invention has the following excellent effects:

[0020] The present invention can break through the inherent limitation of the single driving force mode in the self-assembly process by regulating the driving force of the self-assembly process in sections and accurately regulating the membrane structure from a microscopic perspective, effectively alleviating the problem of holes in the barrier layer and unstable structure. The hydrogen barrier film prepared by this method has high hydrogen barrier performance. Under certain optimized conditions, the hydrogen permeability of the prepared hydrogen barrier film is less than 40cm 3 ·m -2 ·24h -1 0.1MPa -1 . Specific implementation methods

[0022] The base film material used is a commercial film.

[0023] Implementation Example 1

[0024] (1) Weigh 0.08 g of polyethyleneimine and dissolve it in 40 ml of deionized water, stir for 1 h to completely dissolve it to form a homogeneous solution, and adjust the pH to 9.5 for later use; weigh 0.04 g of montmorillonite and dissolve it in 40 ml of deionized water, sonicate at 250 W for 15 min, stir for 24 h, and set aside;

[0025] (2) adding the polyethyleneimine solution and the montmorillonite dispersion in step (1) into the atomizing nozzles of two self-assembly devices respectively, placing the substrate materials under the atomizing nozzles alternately, starting the atomization timing, and stopping the spraying after 10 seconds;

[0026] (3) Place the substrate material into a tabletop glue spinner and spin dry at 4000 rpm for 30 seconds;

[0027] (4) Repeat steps (2) and (3) 5 times to complete the self-assembly of the first 5 layers;

[0028] (5) re-adjusting the pH value of the polyethyleneimine solution in step (1) to 6.5;

[0029] (6) Repeat steps (2) and (3) 5 times to complete 5 layers of self-assembly.

[0030] The hydrogen permeation performance test was carried out using a high-pressure gas permeometer at 25°C and 0.1 MPa. The raw gas was high-purity hydrogen. The hydrogen permeation rate of the hydrogen barrier film prepared in this example was 53.24 cm 3 ·m -2 ·24h -1 0.1MPa -1 .

[0031] Implementation Example 2

[0032] (1) Weigh 0.08 g of polyethyleneimine and dissolve it in 40 ml of deionized water, stir for 1 h to completely dissolve it to form a homogeneous solution, and adjust the pH to 9.5 for later use; weigh 0.08 g of montmorillonite and dissolve it in 40 ml of deionized water, sonicate at 250 W for 15 min, stir for 24 h, and set aside;

[0033] (2) adding the polyethyleneimine solution and the montmorillonite dispersion in step (1) into the atomizing nozzles of two self-assembly devices respectively, placing the substrate materials under the atomizing nozzles alternately, starting the atomization timing, and stopping the spraying after 10 seconds;

[0034] (3) Place the substrate material into a tabletop glue spinner and spin dry at 4000 rpm for 30 seconds;

[0035] (4) Repeat steps (2) and (3) 5 times to complete the self-assembly of the first 5 layers;

[0036] (5) re-adjusting the pH value of the polyethyleneimine solution in step (1) to 6.5;

[0037] (6) Repeat steps (2) and (3) 5 times to complete 5 layers of self-assembly.

[0038] The hydrogen permeation performance test was carried out using a high-pressure gas permeometer at 25°C and 0.1 MPa. The raw gas was high-purity hydrogen. The hydrogen permeation rate of the hydrogen barrier film prepared in this example was 45.36 cm 3 ·m -2 ·24h -1 0.1MPa -1 .

[0039] Implementation Example 3

[0040] (1) Weigh 0.08 g of polyethyleneimine and dissolve it in 40 ml of deionized water, stir for 1 h to completely dissolve it to form a homogeneous solution, and adjust the pH to 9.5 for later use; weigh 0.12 g of montmorillonite and dissolve it in 40 ml of deionized water, sonicate at 250 W for 15 min, stir for 24 h, and set aside;

[0041] (2) adding the polyethyleneimine solution and the montmorillonite dispersion in step (1) into the atomizing nozzles of two self-assembly devices respectively, placing the substrate materials under the atomizing nozzles alternately, starting the atomization timing, and stopping the spraying after 10 seconds;

[0042] (3) Place the substrate material into a tabletop glue spinner and spin dry at 4000 rpm for 30 seconds;

[0043] (4) Repeat steps (2) and (3) 5 times to complete the self-assembly of the first 5 layers;

[0044] (5) re-adjusting the pH value of the polyethyleneimine solution in step (1) to 6.5;

[0045] (6) Repeat steps (2) and (3) 5 times to complete 5 layers of self-assembly.

[0046] The hydrogen permeation performance test was carried out using a high-pressure gas permeometer at 25°C and 0.1 MPa. The raw gas was high-purity hydrogen. The hydrogen permeation rate of the hydrogen barrier film prepared in this example was 32.12 cm 3 ·m -2 ·24h -1 0.1MPa -1 .

[0047] It can be seen that the hydrogen barrier film prepared by this method has good hydrogen barrier properties.

[0048] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for constructing a dense hydrogen barrier film by precisely controlling electrostatic-hydrogen bonding in sections, characterized in that: The following steps are involved: Step 1: Pretreatment of substrate materials: cleaning and modification of the substrate materials; Step 2: Solution preparation: prepare two self-assembly solutions, one is a dispersion of layered materials to ensure that they are evenly dispersed in the solvent; the other is a polyelectrolyte solution, selecting a polyelectrolyte with appropriate molecular structure and charge characteristics; Step 3: regulating the charge density of the polyelectrolyte solution for the first time; Step 4: Alternate assembly and drying: First, place the substrate material under the self-assembly device containing the polyelectrolyte solution. After the assembly is completed, immediately place the substrate material in a desktop glue machine and spin dry. Then, place the substrate material under the self-assembly device containing the sheet material dispersion. After the assembly is completed, immediately place the substrate material in a desktop glue machine and spin dry. Repeat the above operation 5 times to complete the self-assembly of the first 5 layers. Step 5: regulating the charge density of the polyelectrolyte solution for a second time; Step 6 Repeat step 4 to complete the 5-layer self-assembly.

2. According to claim 1, a method for constructing a dense hydrogen barrier film by segmented and precise control of electrostatic-hydrogen bonding is characterized in that: The substrate material used is a polymer film.

3. The method of constructing a dense hydrogen barrier film by segmented and precise control of electrostatic-hydrogen bonding according to claim 1 is characterized in that: The modification of the base material is surface modification to enhance the bonding force between the base material and the barrier layer.

4. The method of constructing a dense hydrogen barrier film by segmented and precise control of electrostatic-hydrogen bonding according to claim 1 is characterized in that: The polyelectrolyte solution is a polyethyleneimine solution, the two-dimensional layered material dispersion is a montmorillonite dispersion, the concentrations of both are 1-3 mg / ml, and the solvent is water.

5. The method of constructing a dense hydrogen barrier film by segmented and precise control of electrostatic-hydrogen bonding according to claim 1 is characterized in that: The charge density of the polyethyleneimine solution was changed by adjusting the pH value of the polyethyleneimine solution. The pH value of the polyethyleneimine solution was adjusted to 9.5 for the first time to complete the self-assembly of the first 5 layers.

6. The method of constructing a dense hydrogen barrier film by segmented and precise control of electrostatic-hydrogen bonding according to claim 1 is characterized in that: The charge density of the polyethyleneimine solution was changed by adjusting the pH value. The pH value of the polyethyleneimine solution was adjusted to 6.5 for the second time, and the 5-layer self-assembly was completed.

Citation Information

Patent Citations

  • Preparation method and application of mixed matrix composite membrane based on polyethyleneimine modified porous montmorillonite

    CN113750820A

  • Preparation method and application of mixed matrix composite membrane based on polyaniline intercalation modified acid activated montmorillonite

    CN113750822A

  • Method for preparing hydrogen barrier coating through ultrasonic atomization assisted layer-by-layer self-assembly

    CN114146880A

  • Preparation method of efficient GO / PLA layer-by-layer self-assembled barrier film

    CN116199924A

  • Nanocellulose-based high-transparency composite barrier film and preparation method thereof