Low-emission polypropylene material and preparation method thereof
By using deodorizing masterbatch and titanate sol in polypropylene materials, the problems of high VOC content and mechanical properties attenuation of polypropylene are solved, low emanation and efficient catalytic degradation are achieved, and the stability of the material is improved. performance and performance.
Patent Information
- Application Number
- CN202411186143.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-19
AI Technical Summary
Polypropylene materials produce high content of volatile organic compounds (VOCs) during use, resulting in bad odor emission and mechanical properties attenuated after aging. It is difficult for the prior art to achieve uniform dispersion of nanotitanium dioxide to catalyze the degradation of VOCs.
Using deodorizing masterbatch and titanate sol as titanium dioxide precursor, nanotitanium dioxide is generated through in-situ reaction through the extrusion process, combined with extracting deodorant, and completely reduce the VOC content, and improve catalytic activity and mechanical properties through two-dimensional flake structure titanium dioxide. .
It effectively reduces the VOC content and bad odor emission of polypropylene materials, maintains good mechanical properties, avoids the problems of uneven mixing of deodorants and early boiling, and achieves nano-scale dispersion and efficient catalytic degradation.
Smart Images

Figure CN118978768A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, in particular to a low-emission polypropylene material and a preparation method thereof. Background Art
[0002] Polypropylene has become the largest, most frequently used and fastest growing plastic variety due to its low density, light volume, wide design space, environmental friendliness, excellent performance and low manufacturing cost. However, polypropylene plastics will produce a large number of small molecules during the polymerization, modification and use process, emitting various bad odors and damaging the physical and mental health of consumers.
[0003] For the bad smell of polypropylene, the current manufacturers can reduce the volatile organic compound (VOC) content of polypropylene by optimizing the synthesis process, but this material is expensive and is mainly used in medical devices. A process for reducing the VOC of polypropylene is to perform extraction and devolatilization (for example, see patent CN107090128B) or add porous adsorbent (for example, see patent CN111040295B) during the processing, but the polypropylene produced in this way will still release VOCs in the later use process due to factors such as aging (especially light aging) of polypropylene and saturation of adsorbent, produce bad smell, and mechanical properties will also decay rapidly after aging. In addition, extraction and devolatilization is to mix the extraction deodorant with the polypropylene melt during the extrusion process, and the VOC in the polypropylene matrix is affinity coated by the extraction deodorant, and the polypropylene matrix is taken out, and then discharged by negative pressure, and the VOC with bad smell is removed. However, liquid deodorant is difficult to mix evenly with polypropylene, and the phenomenon of returning material will occur at the feeding port due to the boiling of the deodorant during the extrusion process. Therefore, it is necessary to prepare the deodorant in the form of a masterbatch and add it to avoid uneven mixing and premature boiling and volatilization of the deodorant. Another process for reducing the VOC of polypropylene is to add titanium dioxide to polypropylene during processing (for example, see patent application CN114163731A). Titanium dioxide absorbs light energy to produce holes and electrons with extremely strong oxidizing and reducing abilities, and has excellent catalytic degradation effects on small organic molecules. Therefore, titanium dioxide, as a photocatalyst, has a good photocatalytic degradation of VOC effects. However, when titanium dioxide is added to a plastic substrate as a photocatalyst, it will face the problem of how to achieve dispersion. Nanoscale titanium dioxide has many exposed active atoms and high catalytic activity, so nano titanium dioxide is generally selected as a photocatalyst. However, nano titanium dioxide cannot be uniformly dispersed in a polypropylene melt by traditional melt blending. First, because of the poor polarity of polypropylene and titanium dioxide, titanium dioxide tends to agglomerate together during the blending process. In addition, the high viscosity of the polypropylene melt makes it difficult to insert it between titanium dioxide nanoparticles and wet and coat the surface of the nanoparticles. Agglomerated titanium dioxide is difficult to exert efficient catalytic effect and has a weak catalytic degradation effect on VOCs.
[0004] In view of the above problems, it is necessary to develop a low-emission polypropylene material and a preparation method thereof which can effectively reduce the VOC content and bad odor emission of polypropylene, and still have a low VOC content and bad odor emission after aging, and maintain good mechanical properties. Summary of the invention
[0005] The main purpose of the present invention is to provide a low-emission polypropylene material and a preparation method thereof, so as to solve the problems in the prior art that polypropylene has a high VOC content, emits a bad odor, and is more likely to emit VOC and bad odor after aging and has attenuated mechanical properties.
[0006] In order to achieve the above object, the present invention provides a low-emission polypropylene material on one hand, wherein the raw materials of the low-emission polypropylene material comprise the following components:
[0007] Polypropylene,
[0008] A deodorizing masterbatch comprising an extractive deodorizing agent and a polypropylene carrier, and
[0009] The titanium dioxide precursor comprises a titanate sol.
[0010] Further, based on 100 parts by weight of the total weight of the raw materials, the raw materials of the low-emission polypropylene material include the following components:
[0011] 80-90 parts of the polypropylene,
[0012] 2-5 parts of the deodorizing masterbatch, and
[0013] 5-15 parts of the titanium dioxide precursor.
[0014] Further, based on 100 parts by weight of the total weight of the deodorizing masterbatch, the deodorizing masterbatch comprises 50-70 parts of the extractive deodorizing agent and 30-50 parts of the polypropylene carrier.
[0015] Furthermore, the titanate sol comprises titanate, a catalyst and a solvent.
[0016] Further, based on 100 parts by weight of the total weight of the titanate sol, the titanate sol comprises 40-70 parts of the titanate, 10-15 parts of the catalyst and 20-55 parts of the solvent.
[0017] Furthermore, the polypropylene includes any one of homopolymer polypropylene, copolymer polypropylene and random copolymer polypropylene; and the polypropylene carrier includes open-cell foamed polypropylene.
[0018] Furthermore, the extractive deodorant comprises water and isobutanol.
[0019] Furthermore, the titanate includes any one of tetrabutyl titanate, tetraethyl titanate, and isopropyl titanate; the catalyst includes any one of formic acid and acetic acid; and the solvent includes any one of ethanol and isopropyl titanate.
[0020] Another aspect of the present invention provides a method for preparing the low-emission polypropylene material described above, the method comprising the following steps:
[0021] 1) mixing and dispersing titanate, a catalyst and a solvent to obtain the titanate sol;
[0022] 2) mixing water and isobutyl alcohol to obtain the extraction deodorant, and then mixing the extraction deodorant and the polypropylene carrier to obtain a deodorizing masterbatch;
[0023] 3) adding the polypropylene, the titanate sol and the deodorizing masterbatch into an extruder for extrusion to obtain the low-emission polypropylene material;
[0024] Wherein, the titanate sol reacts to generate nano titanium dioxide during the extrusion process.
[0025] Furthermore, the nano titanium dioxide has a two-dimensional flake structure.
[0026] By applying the technical solution of the present invention, the deodorizing masterbatch and nano titanium dioxide are used to jointly reduce the VOC content in polypropylene. Among them, the present invention can completely discharge the small molecular substances in polypropylene from the polypropylene matrix through the deodorizing masterbatch, which is different from the porous adsorption deodorization process that only temporarily adsorbs the organic small molecules in the porous carrier instead of completely discharging the organic small molecules, and can reduce the risk of desorption and emission of organic small molecules from the porous substance in the later stage. In addition, the extraction deodorant is added in the form of a masterbatch, which avoids the problem of uneven mixing with polypropylene and premature boiling and volatilization of the deodorant causing loss of deodorant performance. The present invention introduces highly active nano titanium dioxide into polypropylene, which can catalytically degrade small molecular organic matter generated by aging of polypropylene during the use of polypropylene, and reduce the release of harmful substances during the use of polypropylene. The present invention introduces nano titanium dioxide into the polypropylene matrix through the in-situ reaction of titanium dioxide precursor. Unlike the traditional blending process, the titanium dioxide generated by the in-situ reaction is evenly dispersed, and nano-level dispersion is achieved in the polypropylene matrix without agglomeration, thereby improving the catalytic degradation performance of titanium dioxide on VOC. In addition, in the present invention, the titanium dioxide generated by the in-situ reaction has a limiting effect on the growth of the titanium dioxide in the polypropylene melt during the extrusion process, so that the obtained titanium dioxide presents a two-dimensional sheet structure. The two-dimensional sheet structure can expose more active atoms for catalyzing VOC degradation. In addition, the two-dimensional structure is entangled with the polymer chain segments, which can effectively limit the slippage of the polypropylene chain segments and enhance the mechanical properties of the polypropylene. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0028] Figure 1This is an electron microscope photograph of the low-emission polypropylene material prepared in Example 1.
[0029] Figure 2 This is the XRD pattern of the low-emission polypropylene material prepared in Example 1.
[0030] Figure 3 This is a transmission electron microscope image of the low-emission polypropylene material prepared in Example 1.
[0031] Figure 4 This is an electron microscope photograph of the low-emission polypropylene material prepared in Comparative Example 1. DETAILED DESCRIPTION
[0032] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.
[0033] As described in the background technology, polypropylene in the prior art has the problems of high VOC content, bad odor, and more likely to emit VOC and bad odor after aging, and mechanical properties decay. In order to solve the above technical problems, the present application provides a low-emission polypropylene material, the raw materials of which include the following components:
[0034] Polypropylene,
[0035] A deodorizing masterbatch comprising an extractive deodorizing agent and a polypropylene carrier, and
[0036] The titanium dioxide precursor comprises a titanate sol.
[0037] Polypropylene products often release a large amount of VOC molecules and emit bad odors during the extrusion granulation process due to catalyst residues in the polymerization process and oligomers produced by incomplete polymerization. The high temperature and strong shear environment during polypropylene extrusion will cause a large amount of VOC to be released from the polymer matrix, so the extrusion process is very suitable for polypropylene deodorization modification.
[0038] The present invention uses two substances, a deodorizing masterbatch and nano titanium dioxide, to jointly reduce the VOC content in polypropylene. Among them, the present invention can completely discharge the small molecular substances in polypropylene from the polypropylene matrix through the deodorizing masterbatch, which is different from the porous adsorption deodorization process that only temporarily adsorbs the organic small molecules in the porous carrier instead of completely discharging the organic small molecules, and can reduce the risk of desorption and emission of organic small molecules from the porous substance in the later stage. In addition, the extraction deodorant is added in the form of a masterbatch, which avoids the problem of uneven mixing with polypropylene and premature boiling and volatilization of the deodorant causing loss of deodorant performance. The present invention introduces highly active nano titanium dioxide into polypropylene, which can catalytically degrade small molecular organic matter generated by aging of polypropylene during the use of polypropylene, and reduce the release of harmful substances during the use of polypropylene. The present invention introduces nano titanium dioxide into the polypropylene matrix through the in-situ reaction of titanium dioxide precursor. Unlike the traditional blending process, the titanium dioxide generated by the in-situ reaction is evenly dispersed, and nano-level dispersion is achieved in the polypropylene matrix without agglomeration, thereby improving the catalytic degradation performance of titanium dioxide on VOC. In addition, in the present invention, the titanium dioxide generated by the in-situ reaction has a limiting effect on the growth of the titanium dioxide in the polypropylene melt during the extrusion process, so that the obtained titanium dioxide presents a two-dimensional sheet structure. The two-dimensional sheet structure can expose more active atoms for catalyzing VOC degradation. In addition, the two-dimensional structure is entangled with the polymer chain segments, which can effectively limit the slippage of the polypropylene chain segments and enhance the mechanical properties of the polypropylene.
[0039] In a preferred embodiment, based on 100 parts by weight of the total weight of the raw materials, the raw materials of the low-emission polypropylene material comprise the following components:
[0040] 80-90 parts of the polypropylene,
[0041] 2-5 parts of the deodorizing masterbatch, and
[0042] 10-15 parts of the titanium dioxide precursor.
[0043] In a preferred embodiment, based on 100 parts by weight of the total weight of the deodorizing masterbatch, the deodorizing masterbatch comprises 50-60 parts of the extractive deodorizing agent and 30-50 parts of the polypropylene carrier.
[0044] In a preferred embodiment, the titanate sol comprises titanate, a catalyst and a solvent.
[0045] In a preferred embodiment, based on 100 parts by weight of the total weight of the titanate sol, the titanate sol comprises 10-20 parts of the titanate, 0.5-1 parts of the catalyst and 5-10 parts of the solvent.
[0046] In a preferred embodiment, the polypropylene includes any one of homopolymer polypropylene, copolymer polypropylene and random copolymer polypropylene; and the polypropylene carrier includes open-cell foamed polypropylene.
[0047] At present, there are many types of polypropylene materials, and various types of polypropylene are widely used in all walks of life. The low-emission polypropylene of the present invention has universality and is applicable to all types of polypropylene materials at present. The polypropylene material includes any one of homopolymer polypropylene, copolymer polypropylene, and random copolymer polypropylene. Among them, homopolymer polypropylene has poor impact resistance (brittle), poor toughness, poor dimensional stability, easy aging, and poor long-term heat stability, while copolymer polypropylene has good comprehensive performance, high strength, high rigidity, good heat resistance, good dimensional stability, excellent low-temperature toughness (good flexibility), good transparency, and high gloss. Therefore, preferably, the polypropylene of the present invention is block copolymer polypropylene and random copolymer polypropylene. More preferably, the block copolymer polypropylene is any one of Yanshan Petrochemical K8303, Yangzi Petrochemical J340, and Qilu Petrochemical EPS30R. More preferably, the random copolymer polypropylene is any one of Yanshan Petrochemical BR4400, Zhenhai Refining and Chemical M26ET, and Qilu Petrochemical QPR01.
[0048] The extraction deodorant is processed into a deodorant masterbatch and a suitable substrate needs to be selected. Other matrix polymers cannot be introduced into polypropylene, and the deodorant cannot be ineffective during the processing of the deodorant masterbatch. Therefore, a polypropylene carrier is selected as the substrate. Preferably, the polypropylene carrier is an open-cell foamed polypropylene. Preferably, the open-cell foamed polypropylene has an open porosity of 70-92% and a bulk density of 60-200 kg / m 3 More preferably, the open-cell foamed polypropylene is any one of PP1020, PP1010 and PP1005 produced by Nanjing Xuzhi Materials Co., Ltd.
[0049] In a preferred embodiment, the extractive deodorant comprises water and isobutanol.
[0050] The extraction deodorant must have good affinity with VOC, and the boiling point of the deodorant must match the processing temperature. If the boiling point is too low, it is easy to volatilize during the mixing stage, resulting in a reduction in effective ingredients. If the boiling point is too high, it cannot be discharged through the negative pressure exhaust port of the extruder, and it will remain in the polypropylene matrix. Therefore, it is preferred to use a mixture of water and isobutanol as the extraction deodorant. The extraction deodorant in the present invention contains any ratio of water and isobutanol. Preferably, the ratio of water to isobutanol in the extraction deodorant is 30:70-70:30.
[0051] The preferred ratio of water and isobutanol in the above-mentioned extraction deodorant is conducive to further improving the performance of the extraction deodorant. When the water content is too high, the surface energy of water is high and it is a polar substance, resulting in a relatively low interfacial compatibility and devolatilization efficiency, especially for some non-polar organic matter; when the water content is too low, the organic matter evaporates quickly, and the effective residence extraction time is relatively short. In addition, a high isobutanol content will lead to a high organic vapor content, which poses a certain risk of fire.
[0052] In a preferred embodiment, the titanate includes any one of tetrabutyl titanate, tetraethyl titanate, and isopropyl titanate; the catalyst includes any one of formic acid and acetic acid; and the solvent includes any one of ethanol and isopropyl titanate.
[0053] The above preferred titanate, catalyst and solvent are conducive to further improving the devolatilization performance. Among them, the above small molecule organic titanate has high reaction activity and high sol-gel rate; formic acid and acetic acid as organic acid catalysts can effectively release hydrogen ions, but they are not as fast as inorganic acids, resulting in too fast reaction rate of the system; solvents ethanol and isopropanol have good compatibility with titanate substances.
[0054] Another aspect of the present invention provides a method for manufacturing the low-emission polypropylene material, comprising the following steps:
[0055] 1) mixing and dispersing titanate, a catalyst and a solvent to obtain the titanate sol;
[0056] 2) mixing water and isobutyl alcohol to obtain the extraction deodorant, and then mixing the extraction deodorant and the polypropylene carrier to obtain a deodorizing masterbatch;
[0057] 3) adding the polypropylene, the titanate sol and the deodorizing masterbatch into an extruder for extrusion to obtain the low-emission polypropylene material;
[0058] Wherein, the titanate sol reacts to generate nano titanium dioxide during the extrusion process.
[0059] As described above, in the method for preparing low-emission polypropylene material of the present invention, the extracting deodorant is added in the form of a masterbatch to avoid uneven mixing of the deodorant and premature boiling and volatilization problems, and to avoid high-temperature processing leading to loss of deodorant performance. In the preparation of low-emission polypropylene, the in-situ generation of nano titanium dioxide can solve the dispersion problem of titanium dioxide in the polypropylene melt, and the high temperature and high pressure environment of the polypropylene melt can be used to limit the production of titanium dioxide to obtain more efficient catalytic activity. Titanium dioxide is prepared by a sol-gel method. In combination with the polypropylene melt processing process, titanate sol is first mixed with polypropylene particles so that the titanate sol is uniformly dispersed in the polypropylene, and then the high temperature and high pressure devolatilization environment in extrusion is used to perform a hydrothermal reaction to generate nano titanium dioxide in situ. The present invention introduces nano titanium dioxide into the polypropylene matrix through an in-situ reaction. Unlike the traditional blending process, the titanium dioxide generated by the in-situ reaction is uniformly dispersed, and nano-level dispersion is achieved in the polypropylene matrix without agglomeration. In addition, the method of the present invention is simple and efficient, does not require additional equipment modification, and is suitable for all processing plants.
[0060] In a preferred embodiment, the nano titanium dioxide has a two-dimensional sheet structure. Preferably, the nano titanium dioxide has a lateral size of 5-10 micrometers and a thickness of 5-30 nanometers.
[0061] In the present invention, the titanium dioxide generated by the in-situ reaction has a limiting effect on the growth of the titanium dioxide by the polypropylene melt during the extrusion process. The titanium dioxide finally obtained presents a two-dimensional sheet structure. The two-dimensional sheet structure can expose more active atoms for catalyzing the degradation of VOCs. In addition, the two-dimensional structure is entangled with the polymer chain segments, which can effectively limit the slippage of the polypropylene chain segments and enhance the polypropylene.
[0062] In a preferred embodiment, the extruder in step 3) is a twin-screw extruder. Preferably, the aspect ratio of the twin-screw extruder is 42-51, and the vacuum degree is ≤-0.08MPa. Preferably, the temperature of the twin-screw extruder is: 80-100°C in zone 1, 140-170°C in zone 2, 180-200°C in zone 3, 180-200°C in zone 4, 180-200°C in zone 5, 180-200°C in zone 6, 180-200°C in zone 7, 180-200°C in zone 8, 180-200°C in zone 9, 180-200°C in zone 10, 180-200°C in zone 11, and the die head is 170-190°C; the screw speed is 250-330rpm.
[0063] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.
[0064] The polypropylene used in the following examples is K8303 from Yanshan Petrochemical and M26ET from Zhenhai Refining and Chemical; the open-cell foamed polypropylene is PP1020 and PP1010 from Nanjing Xuzhi Material Technology Co., Ltd.; the photocatalyst titanium dioxide is purchased from Shanghai Yifu Industrial Co., Ltd.; and other reagents are purchased from Aladdin Chemical Reagents.
[0065] Example 1
[0066] The low-emission polypropylene material was prepared according to the following steps:
[0067] S1: 6 kg of tetraethyl titanate, 1.3 kg of acetic acid, and 2.7 kg of ethanol were dispersed by ultrasonic stirring for 5 min to obtain a titanate sol;
[0068] S2: 5 kg of water and 5 kg of isobutanol were uniformly mixed to obtain an extractive deodorant; 7 kg of the extractive deodorant and 3 kg of PP1020 were stirred and mixed under a negative pressure of -0.08 MPa for 30 min, and the deodorizing masterbatch was obtained after the pressure was released;
[0069] S3: 8kg of polypropylene K8303, 0.5kg of deodorizing masterbatch and 1.5kg of titanate sol were uniformly mixed and then put into a twin-screw extruder;
[0070] S4: Extrusion is carried out under the following conditions: the extruder temperature is: 90°C for zone 1, 140°C for zone 2, 180°C for zone 3, 200°C for zone 4, 200°C for zone 5, 200°C for zone 6, 200°C for zone 7, 200°C for zone 8, 200°C for zone 9, 200°C for zone 10, 200°C for zone 11, the die head is 180°C, the screw speed is 330rpm, the aspect ratio of the twin screw is 44, the vacuum degree is -0.09MPa, and a low-emission polypropylene product is obtained.
[0071] The low-emission polypropylene obtained in this example was confirmed to have a titanium dioxide structure by XRD testing, and then the sample was injection molded into a 100 g specimen and heated at 1 m 3 Light aging tests were carried out in a closed chamber with five different sunlight intensities.
[0072] Figure 1 is an electron microscope photograph of the low-emission polypropylene material prepared in Example 1. Figure 1 It can be seen that the titanium dioxide generated in the low-emission polypropylene material prepared according to Example 1 is evenly dispersed without agglomeration, the particles are uniform, and the active surfaces are more exposed. Figure 2 is the XRD pattern of the low-emission polypropylene material prepared in Example 1. Figure 2 In the figure, the peak at 25.3° corresponds to (101), the peak at 38° corresponds to (004), the peak at 47.7° corresponds to (105), and the peak at 54.8° corresponds to (204), which are consistent with the characteristic peaks of titanium dioxide. Figure 3is a transmission electron microscope image of the low-emission polypropylene material prepared in Example 1. Figure 3 It can be seen that the obtained titanium dioxide presents a two-dimensional flake structure.
[0073] Example 2
[0074] The low-emission polypropylene material was prepared according to the following steps:
[0075] S1: 1.5 kg of tetrabutyl titanate, 0.4 kg of formic acid, and 1 kg of ethanol were dispersed by ultrasonic stirring for 5 min to obtain a titanate sol;
[0076] S2: 7 kg of water and 3 kg of isobutanol were uniformly mixed to obtain an extractive deodorant; 6 kg of the extractive deodorant and 4 kg of PP1010 were stirred and mixed under a negative pressure of -0.08 MPa for 30 min, and the deodorizing masterbatch was obtained after the pressure was released;
[0077] S3: 9 kg of polypropylene M226E, 0.5 kg of deodorizing masterbatch and 0.5 kg of titanate sol were uniformly mixed and then put into a twin-screw extruder;
[0078] S4: Extrusion is performed under the following conditions: the extruder temperature is: 100°C for zone 1, 140°C for zone 2, 200°C for zone 3, 200°C for zone 4, 200°C for zone 5, 200°C for zone 6, 200°C for zone 7, 200°C for zone 8, 200°C for zone 9, 200°C for zone 10, 200°C for zone 11, the die is 190°C, the screw speed is 300rpm. The aspect ratio of the twin screw is 51, the vacuum degree is -0.1MPa, and a low-emission polypropylene product is obtained.
[0079] The low-emission polypropylene obtained in this example was confirmed to have a titanium dioxide structure by XRD testing, and then the sample was injection molded into a 100 g specimen and heated at 1 m 3 Light aging tests were carried out in a closed chamber with five different sunlight intensities.
[0080] Example 3
[0081] S1: 3.9 kg of isopropyl titanate, 0.9 kg of acetic acid, and 6.0 kg of isopropyl alcohol were dispersed by ultrasonic stirring for 5 min to obtain a titanate sol;
[0082] S2: 5 kg of water and 5 kg of isobutyl alcohol are uniformly mixed to obtain an extractive deodorant; and 5 kg of the above-mentioned extractive deodorant and 5 kg of PP1010 are stirred and mixed under a negative pressure of -0.08 MPa for 30 minutes, and the deodorizing masterbatch is obtained after the pressure is released;
[0083] S3: 9 kg of polypropylene M226E, 0.1 kg of deodorizing masterbatch and 0.3 kg of titanate sol were uniformly mixed and then put into a twin-screw extruder;
[0084] S4: Extrusion is performed under the following conditions: the extruder temperature is: 100°C for zone 1, 140°C for zone 2, 200°C for zone 3, 200°C for zone 4, 200°C for zone 5, 200°C for zone 6, 200°C for zone 7, 200°C for zone 8, 200°C for zone 9, 200°C for zone 10, 200°C for zone 11, the die is 190°C, the screw speed is 300rpm. The aspect ratio of the twin screw is 51, the vacuum degree is -0.1MPa, and a low-emission polypropylene product is obtained.
[0085] The low-emission polypropylene sample obtained in this example was injection molded into a 100 g specimen and placed in a 1 m 3 Light aging tests were carried out in a closed chamber with five different sunlight intensities.
[0086] Comparative Example 1
[0087] The preparation steps of this comparative example are the same as those of Example 1, except that step S1 is not performed, and in step S3, no titanate sol is added, and 0.69 kg of commercially available nano titanium dioxide photocatalyst is directly added (0.69 g is calculated according to the molar amount of tetrabutyl titanate in Example 1).
[0088] Figure 4 This is an electron microscope photo of the low-emission polypropylene material prepared in Comparative Example 1. Figure 1 and Figure 4 It can be found that compared with the low-emission polypropylene material prepared in Example 1, the titanium dioxide in the polypropylene material prepared in Comparative Example 1 aggregates and is not well dispersed.
[0089] Comparative Example 2
[0090] The preparation steps of this comparative example are the same as those of Example 2, except that step S1 is not performed, and in step S3, 9 kg of polypropylene M226E and 1.45 kg of deodorizing masterbatch are added instead of titanate sol.
[0091] Comparative Example 3
[0092] The preparation steps of this comparative example are the same as those of Example 1, except that in step S2, only water and isobutanol are mixed to obtain an extraction deodorant without preparing a deodorizing masterbatch, and in step S3, 0.5 kg of the extraction deodorant is added instead of the deodorizing masterbatch.
[0093] Comparative Example 4
[0094] The preparation steps of this comparative example are the same as those of Example 1, except that step S2 is not performed, and in step S3, 9 kg of polypropylene M226E and 2 kg of titanate sol are added instead of adding the deodorizing masterbatch.
[0095] The specific performance tests are as follows:
[0096] The low-emission polypropylene strips prepared in Examples 1-3 and Comparative Examples 1-4 were subjected to light aging tests in a test chamber, and the gas in the test chamber was extracted at the same time, and the formaldehyde and TVOC contents were tested by the headspace method. The mechanical properties test of polypropylene refers to GB / T1040.2-2006. The specific test results are shown in Table 1.
[0097] Table 1 VOC content and mechanical properties of low emission polypropylene
[0098]
[0099]
[0100] It can be seen from Table 1 that the formaldehyde and TVOC contents of the polypropylene material prepared by the method of the present invention are lower than the national standards; by comparing Comparative Example 1 with Example 1, it can be seen that the titanium dioxide generated in situ has an enhancing effect on polypropylene, and the titanium dioxide generated by the in situ reaction has a higher and more lasting catalytic activity; by comparing Comparative Example 2 with Example 2, it can be seen that in the absence of the titanium dioxide photocatalyst, polypropylene will release a large amount of VOC under the action of photoaging, and the mechanical properties will also decay rapidly; by comparing Comparative Examples 3-4 with Example 1, it can be seen that by preparing the extract deodorant in the form of a masterbatch and adding it to the polypropylene material, the release of formaldehyde and VOC can be reduced.
[0101] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the terms used in this way can be interchangeable where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those described herein, for example.
[0102] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A low-emission polypropylene material, characterized in that: The raw materials of the low-emission polypropylene material include the following components: Polypropylene, A deodorizing masterbatch comprising an extractive deodorizing agent and a polypropylene carrier, and The titanium dioxide precursor comprises a titanate sol.
2. The low-emission polypropylene material according to claim 1, characterized in that: Based on 100 parts by weight of the total weight of the raw materials, the raw materials of the low-emission polypropylene material include the following components: 80-90 parts of the polypropylene, 2-5 parts of the deodorizing masterbatch, and 5-15 parts of the titanium dioxide precursor.
3. The low-emission polypropylene material according to claim 1, characterized in that: Based on 100 parts by weight of the total weight of the deodorizing masterbatch, the deodorizing masterbatch comprises 50-70 parts of the extractive deodorizing agent and 30-50 parts of the polypropylene carrier.
4. The low-emission polypropylene material according to claim 1, characterized in that: The titanate sol comprises titanate, a catalyst and a solvent.
5. The low-emission polypropylene material according to claim 4, characterized in that: The titanate sol includes 40-70 parts of the titanate, 10-15 parts of the catalyst and 20-55 parts of the solvent, based on 100 parts by weight of the total weight of the titanate sol.
6. The low-emission polypropylene material according to any one of claims 1 to 3, characterized in that: The polypropylene includes any one of homopolymer polypropylene, copolymer polypropylene and random copolymer polypropylene; the polypropylene carrier includes open-cell foamed polypropylene.
7. The low-emission polypropylene material according to any one of claims 1 to 3, characterized in that: The extractive deodorant comprises water and isobutyl alcohol.
8. The low-emission polypropylene material according to claim 4 or 5, characterized in that: The titanate ester includes any one of tetrabutyl titanate, tetraethyl titanate, and isopropyl titanate; the catalyst includes any one of formic acid and acetic acid; and the solvent includes any one of ethanol and isopropyl titanate.
9. A method for preparing the low-emission polypropylene material according to any one of claims 1 to 8, characterized in that: The method comprises the following steps: 1) mixing and dispersing titanate, a catalyst and a solvent to obtain the titanate sol; 2) mixing water and isobutyl alcohol to obtain the extraction deodorant, and then mixing the extraction deodorant and the polypropylene carrier to obtain a deodorizing masterbatch; 3) adding the polypropylene, the titanate sol and the deodorizing masterbatch into an extruder for extrusion to obtain the low-emission polypropylene material; Wherein, the titanate sol reacts to generate nano titanium dioxide during the extrusion process.
10. The method according to claim 9, characterized in that The nano titanium dioxide has a two-dimensional sheet structure.