High-melting-point high-uniformity Ni-Fe-W-Al alloy and preparation method thereof
Through the mixed smelting of nickel, iron, tungsten and separate smelting of aluminum, combined with the multi-layered smelting container design, the crystal segregation and uniformity problems in Ni-Fe-W-Al alloy are solved, and high melting point and high uniformity are achieved Alloy preparation improves the quality and utilization of the ingot.
Patent Information
- Application Number
- CN202411295108.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-15
- Publication Date
- 2024-11-19
AI Technical Summary
There are large crystal segregation phenomena and poor uniformity in the existing Ni-Fe-W-Al alloy preparation methods, resulting in low utilization of ingots.
Nickel, iron and tungsten are used as a mixed component for melting, aluminum is used as a separate component for melting, and then mixed and melting is carried out to avoid burning aluminum and the formation of intermetallic compounds, thereby improving component uniformity.
The Ni-Fe-W-Al alloy obtained by this method has high uniformity and small component deviation, which improves the purity of the product and the utilization rate of the ingot.
Smart Images

Figure CN118979167A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of new materials, and in particular to a high-melting-point and high-uniformity Ni-Fe-W-Al alloy and a preparation method thereof. Background Art
[0002] The magnetic recording medium includes a substrate, a soft magnetic bottom layer located on the substrate, and a double seed layer. The double seed layer includes a first seed layer containing a first concentration of NiFe and multiple additional metal elements, and the second seed layer contains segregants and a second concentration of NiFe different from the first concentration and multiple additional metal elements, and the additional elements include: W, Al, Cr, Ta, Mo and combinations thereof. The first seed layer can be on the soft magnetic bottom layer, and the second seed layer is on the first seed layer. The composition of the double seed layer requires: Ni in the range of 50% to 75% by atomic percentage; Fe in the range of 15% to 35% by atomic percentage; W in the range of 2% to 12% by atomic percentage; and Al in the range of 0.5% to 3% by atomic percentage, and has high composition uniformity. The double seed layer designed with this composition can provide a small grain size and a good crystallographic texture for the magnetic recording medium. The alloy target material for magnetron sputtering required to prepare the seed layer has a uniform composition, a grain size controlled within a certain range, and a large magnetic permeability.
[0003] The alloy of this composition requires: (1) high purity (greater than or equal to 99.95%) and oxygen content less than 150 ppm; (2) high composition uniformity (controlled within 0.3 at%).
[0004] In the previous experiments, we used a four-component blending smelting method for preparation. The obtained product had a more obvious segregation phenomenon and poor product uniformity, which led to low ingot utilization.
[0005] The technical problem solved in this case is how to further improve the product uniformity of Ni-Fe-W-Al alloy and how to solve the large crystal segregation phenomenon existing in existing products. Summary of the invention
[0006] The purpose of the present invention is to provide a method for preparing a high-melting-point and high-uniformity Ni-Fe-W-Al alloy, in which nickel, iron and tungsten are smelted as a mixed component, aluminum is smelted as a single component, and then mixed and smelted, which can avoid the aluminum burning phenomenon that occurs in the traditional four-component blending smelting process, and at the same time, aluminum liquid is added in the later stage, which can avoid the uneven distribution of components or even segregation caused by the combination of aluminum and nickel and iron elements to form intermetallic compounds. The product obtained by the method of the present invention has the advantages of good uniformity and small component deviation.
[0007] At the same time, the present invention also provides a Ni-Fe-W-Al alloy with high melting point and high uniformity prepared based on the method.
[0008] To achieve the above objectives, this application discloses:
[0009] A method for preparing a high melting point and high uniformity Ni-Fe-W-Al alloy comprises the following steps:
[0010] Step 1: Smelting Ni, Fe and W to obtain a first molten metal;
[0011] Step 2: Smelting Al to obtain a second molten metal;
[0012] Step 3: Mixing and smelting the first molten metal and the second molten metal to obtain a third molten metal;
[0013] Step 4: Casting the third molten metal to obtain Ni-Fe-W-Al alloy.
[0014] The present invention smelts Ni, Fe and W separately, and then adds aluminum liquid into the metal liquid for smelting and casting, thereby avoiding aluminum burning caused by long-term smelting, and improving product uniformity and reducing product segregation.
[0015] In the above-mentioned preparation method, in step 1, in the smelting container, the tungsten single substance is divided into multiple portions, and the multiple portions of tungsten single substance are distributed at different depths in the smelting container.
[0016] As another core invention of the present invention, tungsten is divided into multiple layers and arranged in the smelting container in step 1, so as to achieve sufficient and effective melting dispersion between tungsten and nickel and iron.
[0017] The melting point of tungsten is very high, and it is impractical to completely melt tungsten, which not only consumes a lot of energy but also reduces the life of the smelting container. The present invention disperses tungsten and melts it by melting iron and nickel, which not only saves energy but also effectively shortens the melting time.
[0018] In the present invention, iron and nickel are filled in the form of metal blocks to avoid oxidation; tungsten is added in the form of powder to shorten the melting time and reduce energy consumption.
[0019] Preferably, in step 1, a plurality of metal single layers are filled from top to bottom in the smelting container; between two adjacent tungsten single layers there is a nickel single layer and / or an iron single layer, or between two adjacent tungsten single layers there is a mixed single layer composed of a mixture of nickel and iron.
[0020] More preferably, the metal single-substance layer includes a tungsten single-substance layer, an iron single-substance layer, and a nickel single-substance layer; the tungsten single-substance layer, the iron single-substance layer, and the nickel single-substance layer are arranged alternately.
[0021] In the above preparation method, the molar percentage of each element in the Ni-Fe-W-Al alloy is:
[0022] Nickel: 50-75%;
[0023] Iron: 15-35%;
[0024] Tungsten: 2-12%;
[0025] Aluminum: 0.5~3%.
[0026] The corresponding mass ratio is:
[0027] Nickel: iron: tungsten: aluminum = 28~42: 8.8~20.5: 3.7~22: 0.14~0.81.
[0028] In the above preparation method, the smelting process of step 1 is:
[0029] In a vacuum environment, Ni, Fe, and W are heated to 1600-1650°C and kept at this temperature for 30-60 minutes;
[0030] After all the materials in the furnace are melted, electromagnetic stirring is performed for 10 to 20 minutes;
[0031] After the electromagnetic stirring is completed, the temperature is lowered to 1530-1570° C. to obtain the first molten metal.
[0032] In the above preparation method, the smelting process of step 3 is:
[0033] The second molten metal is added to the first molten metal at 1530-1570° C. with electromagnetic stirring for 10-20 minutes.
[0034] In the above preparation method, the casting process of step 4 is:
[0035] The smelting temperature is raised to 1600-1650°C again, and casting is performed at a speed of 2-3 kg / s, with the casting time for each 100 kg of the third molten metal not exceeding 60 seconds.
[0036] In the above-mentioned preparation method, the purity of nickel, iron, tungsten and aluminum is not less than 99.95wt%.
[0037] At the same time, the present invention also discloses a Ni-Fe-W-Al alloy with high melting point and high uniformity, which is prepared by any of the above-mentioned preparation methods.
[0038] This application has at least the following beneficial effects:
[0039] The present invention melts nickel, iron and tungsten as a mixed component, melts aluminum as a single component, and then performs mixed melting, which can avoid the aluminum burning phenomenon that occurs in the traditional four-component blending melting process. At the same time, adding aluminum liquid in the later stage can avoid the uneven distribution of components or even segregation caused by the combination of aluminum and nickel and iron elements to form intermetallic compounds. The product obtained by the method of the present invention has the advantages of good uniformity and small component deviation. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 This is the metallographic structure diagram of Example 1 of the present invention. DETAILED DESCRIPTION
[0041] The present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. In the description of the present invention, it should be noted that, if no specific conditions are specified in the embodiments, the conditions are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0042] The nickel and iron used in all the embodiments and comparative examples of the present invention are metal blocks, which are metal particles with a diameter of 0.5 to 2 cm. The tungsten is purchased tungsten powder; and the aluminum is an aluminum block.
[0043] Example 1
[0044] The Ni—Fe—W—Al ingot prepared in this embodiment is composed of the following elements in atomic percentage: Ni: 69%, Fe: 25%, W: 5%, Al: 1%.
[0045] The mass of the alloy ingot prepared in this embodiment is 200 kg, and the manufacturing method is as follows:
[0046] (1) Ingredients: According to the design requirements of the above alloy target composition, weigh the raw material Ni (purity ≥ 99.95%), raw material Fe (purity ≥ 99.95%), raw material W (purity ≥ 99.95%) and raw material Al (purity ≥ 99.95%).
[0047] (2) Feeding: Put the weighed nickel, iron and tungsten metals into the alumina crucible, and put the Al metal into the hopper of the vacuum induction melting furnace.
[0048] The arrangement of materials in the alumina crucible from top to bottom is:
[0049] Nickel single layer, tungsten single layer, iron single layer, tungsten single layer, nickel single layer, tungsten single layer, iron single layer, nickel single layer; when filling, nickel and iron should be filled as tightly as possible to allow the tungsten to be spread flat.
[0050] (3) Melting and casting:
[0051] Vacuum degree is >2.0×10 -2 Pa, heat Ni, Fe, and W to 1650°C and keep them at this temperature for 50 min;
[0052] After all the materials in the furnace are melted, electromagnetic stirring is carried out for 10 minutes; the power of the electromagnetic stirring is switched between 35kwh and 60kwh for 5 to 6 times.
[0053] After the electromagnetic stirring is completed, the temperature starts to drop to 1550°C and aluminum liquid is added;
[0054] After adding the aluminum liquid, smelt for 20 minutes, and then start the electromagnetic stirring for 10 minutes. The power of the electromagnetic stirring is switched between 35kwh and 60kwh 5 to 6 times.
[0055] Then, the temperature was raised to 1600° C. and casting was performed at a speed of 2.5 kg / s.
[0056] (4) Sawing: The shrinkage cavity on the top surface of the ingot is removed by sawing, and the removed part is retained as recycled material.
[0057] (5) Polishing: The oxide scale on the cylindrical surface of the sawn ingot is removed by turning.
[0058] The properties of the alloy ingot prepared in this embodiment are shown in Table 1. The microscopic metallographic structure thereof is as follows: Figure 1 shown.
[0059] Embodiment 2:
[0060] The Ni—Fe—W—Al ingot prepared in this embodiment is composed of the following elements in atomic percentage: Ni: 72%, Fe: 22%, W: 5%, Al: 1%.
[0061] The alloy ingot prepared in this embodiment has a mass of 100 kg and the manufacturing method is as follows:
[0062] (1) Ingredients: According to the design requirements of the above alloy target composition, weigh the raw material Ni (purity ≥ 99.95%), raw material Fe (purity ≥ 99.95%), raw material W (purity ≥ 99.95%) and raw material Al (purity ≥ 99.95%).
[0063] (2) Feeding: Put the weighed nickel, iron and tungsten metals into the alumina crucible, and put the Al metal into the hopper of the vacuum induction melting furnace.
[0064] The arrangement of materials in the alumina crucible from top to bottom is:
[0065] Nickel single layer, tungsten single layer, iron single layer, tungsten single layer, nickel single layer, tungsten single layer, iron single layer, nickel single layer; when filling, nickel and iron should be filled as tightly as possible to allow the tungsten to be spread flat.
[0066] (3) Melting and casting:
[0067] Vacuum degree>2.0×10 -2 Pa, heat Ni, Fe, and W to 1630°C and keep them at this temperature for 60 min;
[0068] After all the materials in the furnace are melted, electromagnetic stirring is carried out for 15 minutes; the power of the electromagnetic stirring is switched between 35kwh and 60kwh 7 to 8 times.
[0069] After the electromagnetic stirring is completed, the temperature starts to drop to 1550°C and aluminum liquid is added;
[0070] After adding the aluminum liquid, smelt for 20 minutes, and then start the electromagnetic stirring for 10 minutes. The power of the electromagnetic stirring is switched between 35kwh and 60kwh 5 to 6 times.
[0071] Then, the temperature was raised to 1620° C. and casting was performed at a speed of 2 kg / s.
[0072] (4) Sawing: The shrinkage cavity on the top surface of the ingot is removed by sawing, and the removed part is retained as recycled material.
[0073] (5) Polishing: The oxide scale on the cylindrical surface of the sawn ingot is removed by turning.
[0074] The properties of the alloy ingot prepared in this example are shown in Table 1.
[0075] Example 3
[0076] The Ni—Fe—W—Al ingot prepared in this embodiment is composed of the following elements in atomic percentage: Ni: 50%, Fe: 35%, W: 12%, Al: 3%.
[0077] The alloy ingot prepared in this embodiment has a mass of 100 kg and the manufacturing method is as follows:
[0078] (1) Ingredients: According to the design requirements of the above alloy target composition, weigh the raw material Ni (purity ≥ 99.95%), raw material Fe (purity ≥ 99.95%), raw material W (purity ≥ 99.95%) and raw material Al (purity ≥ 99.95%).
[0079] (2) Feeding: Put the weighed nickel, iron and tungsten metals into the alumina crucible, and put the Al metal into the hopper of the vacuum induction melting furnace.
[0080] The arrangement of materials in the alumina crucible from top to bottom is:
[0081] First, mix the nickel and iron blocks evenly, and then arrange them in the form of nickel-iron mixed single layer, tungsten single layer, nickel-iron mixed single layer, tungsten single layer, nickel-iron mixed single layer, tungsten single layer, nickel-iron mixed single layer, tungsten single layer, and nickel-iron mixed single layer. When filling, fill the nickel and iron as tightly as possible to allow the tungsten to be laid flat.
[0082] (3) Melting and casting:
[0083] Vacuum degree is >2.0×10 -2 Pa, heat Ni, Fe, and W to 1630°C and keep them at this temperature for 30 min;
[0084] After all the materials in the furnace are melted, electromagnetic stirring is carried out for 20 minutes; the power of the electromagnetic stirring is switched between 35kwh and 60kwh for 9 to 10 times.
[0085] After the electromagnetic stirring is completed, the temperature starts to drop to 1530°C and aluminum liquid is added;
[0086] After adding the aluminum liquid, smelting was carried out for 10 minutes, and then electromagnetic stirring was started for 20 minutes. The power and frequency of the electromagnetic stirring were switched back and forth between 35kwh and 55kwh for 9 to 10 times.
[0087] Then, the temperature was raised to 1650° C. and casting was performed at a speed of 3 kg / s.
[0088] (4) Sawing: The shrinkage cavity on the top surface of the ingot is removed by sawing, and the removed part is retained as recycled material.
[0089] (5) Polishing: The oxide scale on the cylindrical surface of the sawn ingot is removed by turning.
[0090] The properties of the alloy ingot prepared in this example are shown in Table 1.
[0091] Example 4
[0092] The Ni—Fe—W—Al ingot prepared in this embodiment is composed of the following elements in atomic percentage: Ni: 75%, Fe: 15%, W: 7%, Al: 3%.
[0093] The alloy ingot prepared in this embodiment has a mass of 100 kg and the manufacturing method is as follows:
[0094] (1) Ingredients: According to the design requirements of the above alloy target composition, weigh the raw material Ni (purity ≥ 99.95%), raw material Fe (purity ≥ 99.95%), raw material W (purity ≥ 99.95%) and raw material Al (purity ≥ 99.95%).
[0095] (2) Feeding: Put the weighed nickel, iron and tungsten metals into the alumina crucible, and put the Al metal into the hopper of the vacuum induction melting furnace.
[0096] The arrangement of materials in the alumina crucible from top to bottom is:
[0097] First, mix the nickel and iron blocks evenly, and then arrange them in the form of nickel-iron mixed single layer, tungsten single layer, nickel-iron mixed single layer, tungsten single layer, nickel-iron mixed single layer, tungsten single layer, nickel-iron mixed single layer, tungsten single layer, and nickel-iron mixed single layer. When filling, fill the nickel and iron as tightly as possible to allow the tungsten to be laid flat.
[0098] (3) Melting and casting:
[0099] Vacuum degree is >2.0×10 -2 Pa, heat Ni, Fe, and W to 1650°C and keep them at this temperature for 60 min;
[0100] After all the materials in the furnace are melted, electromagnetic stirring is carried out for 10 minutes; the power of the electromagnetic stirring is switched between 35kwh and 60kwh for 5 to 6 times.
[0101] After the electromagnetic stirring is completed, the temperature starts to drop to 1570°C and aluminum liquid is added;
[0102] After adding the aluminum liquid, smelt for 10 minutes, and then start the electromagnetic stirring for 15 minutes. The power of the electromagnetic stirring is switched between 35kwh and 60kwh, 7 to 8 times.
[0103] Then, the temperature was raised to 1600° C. and casting was performed at a speed of 2 kg / s.
[0104] (4) Sawing: The shrinkage cavity on the top surface of the ingot is removed by sawing, and the removed part is retained as recycled material.
[0105] (5) Polishing: The oxide scale on the cylindrical surface of the sawn ingot is removed by turning.
[0106] The properties of the alloy ingot prepared in this example are shown in Table 1.
[0107] Comparative Example 1
[0108] The Ni—Fe—W—Al ingot prepared in this comparative example is composed of the following elements in atomic percentage: Ni: 63%, Fe: 28%, W: 7%, Al: 2%.
[0109] The mass of the alloy ingot prepared in this comparative example is 200 kg, and the manufacturing method is as follows:
[0110] (1) Ingredients: According to the design requirements of the above alloy target composition, weigh the raw material Ni (purity ≥ 99.95%), raw material Fe (purity ≥ 99.95%), raw material W (purity ≥ 99.95%) and raw material Al (purity ≥ 99.95%).
[0111] (2) Feeding: Mix the weighed nickel, iron and tungsten metals evenly and put them into an alumina crucible, and put the Al metal into the hopper of the vacuum induction melting furnace.
[0112] (3) Melting and casting:
[0113] Vacuum degree>2.0×10 -2 Pa, heat Ni, Fe, and W to 1650°C and keep them at this temperature for 50 min;
[0114] After all the materials in the furnace are melted, electromagnetic stirring is carried out for 10 minutes; the power of the electromagnetic stirring is switched between 35kwh and 60kwh for 5 to 6 times.
[0115] After the electromagnetic stirring is completed, the temperature starts to drop to 1550°C and aluminum liquid is added;
[0116] After adding the aluminum liquid, smelt for 20 minutes, and then start the electromagnetic stirring for 10 minutes. The power of the electromagnetic stirring is switched between 35kwh and 60kwh 5 to 6 times.
[0117] Then, the temperature was raised to 1600° C. and casting was performed at a speed of 2.5 kg / s.
[0118] (4) Sawing: The shrinkage cavity on the top surface of the ingot is removed by sawing, and the removed part is retained as recycled material.
[0119] (5) Polishing: The oxide scale on the cylindrical surface of the sawn ingot is removed by turning.
[0120] The properties of the alloy ingot prepared in this comparative example are shown in Table 1.
[0121] Comparative Example 2
[0122] The Ni—Fe—W—Al ingot prepared in this comparative example is composed of the following elements in atomic percentage: Ni: 64%, Fe: 27%, W: 6%, Al: 3%.
[0123] The mass of the alloy ingot prepared in this comparative example is 200 kg, and the manufacturing method is as follows:
[0124] (1) Ingredients: According to the design requirements of the above alloy target composition, weigh the raw material Ni (purity ≥ 99.95%), raw material Fe (purity ≥ 99.95%), raw material W (purity ≥ 99.95%) and raw material Al (purity ≥ 99.95%).
[0125] (2) Adding materials: Mix the weighed nickel, iron, tungsten and aluminum metals evenly and put them into an alumina crucible.
[0126] (3) Melting and casting:
[0127] Vacuum degree is >2.0×10 -2 Pa, heat Ni, Fe, W, and Al to 1650°C and keep them at this temperature for 50 min;
[0128] After all the materials in the furnace are melted, electromagnetic stirring is carried out for 10 minutes; the power of the electromagnetic stirring is switched between 35kwh and 60kwh for 5 to 6 times.
[0129] Then casting was carried out at a speed of 2.5 kg / s.
[0130] (4) Sawing: The shrinkage cavity on the top surface of the ingot is removed by sawing, and the removed part is retained as recycled material.
[0131] (5) Polishing: The oxide scale on the cylindrical surface of the sawn ingot is removed by turning.
[0132] The properties of the alloy ingot prepared in this comparative example are shown in Table 1.
[0133] Comparative Example 3
[0134] The Ni—Fe—W—Al ingot prepared in this comparative example is composed of the following elements in atomic percentage: Ni: 72%, Fe: 22%, W: 5%, Al: 1%.
[0135] The mass of the alloy ingot prepared in this comparative example is 200 kg, and the manufacturing method is as follows:
[0136] (1) Ingredients: According to the design requirements of the above alloy target composition, weigh the raw material Ni (purity ≥ 99.95%), raw material Fe (purity ≥ 99.95%), raw material W (purity ≥ 99.95%) and raw material Al (purity ≥ 99.95%).
[0137] (2) Feeding: weigh the nickel, iron, tungsten and aluminum metals in multiple layers and place them in an alumina crucible;
[0138] Specifically, the distribution of single layers from top to bottom is: nickel single layer, aluminum single layer, iron single layer, tungsten single layer, nickel single layer, aluminum single layer, iron single layer, tungsten single layer, nickel single layer, aluminum single layer, iron single layer, tungsten single layer, nickel single layer, aluminum single layer, iron single layer, tungsten single layer, nickel single layer.
[0139] (3) Melting and casting:
[0140] Vacuum degree is >2.0×10 -2Pa, heat Ni, Fe, W, and Al to 1650°C and keep them at this temperature for 50 min;
[0141] After all the materials in the furnace are melted, electromagnetic stirring is carried out for 10 minutes; the power of the electromagnetic stirring is switched between 35kwh and 60kwh for 5 to 6 times.
[0142] Then casting was carried out at a speed of 2.5 kg / s.
[0143] (4) Sawing: The shrinkage cavity on the top surface of the ingot is removed by sawing, and the removed part is retained as recycled material.
[0144] (5) Polishing: The oxide scale on the cylindrical surface of the sawn ingot is removed by turning.
[0145] The properties of the alloy ingot prepared in this comparative example are shown in Table 1.
[0146] Performance Testing
[0147] Inspection items include composition deviation, purity, ingot utilization, and actual density;
[0148] The composition deviation is obtained by sampling different parts of the same alloy ingot and analyzing the alloy composition. The alloy composition analysis is carried out using X-ray fluorescence spectrometer (XRF) and inductively coupled plasma-mass spectrometer (ICP-MS).
[0149] The purity was determined by ICP-MS.
[0150] The actual density is determined according to GB / T1423-1996 (test method for density of precious metals and their alloys).
[0151] Ingot utilization calculation method:
[0152] L=W2 / W1*100%
[0153] Wherein, L is the utilization rate of the ingot, W1 is the weight of the ingot after being cast out of the furnace, and W2 is the weight of the ingot after being sawn and polished.
[0154] The test results are shown in Table 1 below;
[0155] Table 1 Test results
[0156] Case purity Composition deviation Ingot Utilization Rate Measured density Example 1 99.98% <0.10at% 80% <![CDATA[9.267g / cm 3 ]]> Example 2 99.98% <0.09at% 85% <![CDATA[9.266g / cm 3 ]]> Example 3 99.97% <0.08at% 82% <![CDATA[9.265g / cm 3 ]]> Example 4 99.99% <0.10at% 81% <![CDATA[9.266g / cm 3 ]]> Comparative Example 1 99.98% <0.7at% 79% <![CDATA[9.265g / cm 3 ]]> Comparative Example 2 99.97% <1.0at% 82% 9.267g / cm3 Comparative Example 3 99.96% <0.3at% 80% 9.268g / cm3
[0157] Result analysis:
[0158] 1. It can be seen from Examples 1 to 4 that by adopting the method of the present invention, tungsten can enter the melt in the form of solid solution, thereby improving the purity of the reaction product, reducing the component deviation, and improving the uniformity of the product; by smelting the aluminum liquid separately, the aluminum burnout can be reduced, the uniformity of the product can be improved, and the product segregation phenomenon can be reduced.
[0159] 2. It can be seen from Comparative Examples 1 and 2 that if nickel, iron and tungsten are blended and smelted, the composition deviation will increase and the availability of the ingot will be reduced; tungsten powder is easy to settle to the bottom of the crucible after blending, which makes it difficult for some tungsten to fully dissolve, which is the main reason for the deviation; in Comparative Example 2, there is also aluminum burnout, which further increases the deviation. It can be seen from Comparative Example 3 that the deviation caused by the blending of Comparative Example 2 can be reduced by multi-layer superposition, and the main reason is that the loss of tungsten is suppressed. At the same time, in Comparative Examples 1 and 2, there is also single substance segregation, which causes the final composition to deviate greatly from the design value.
[0160] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A method for preparing a high melting point and high uniformity Ni-Fe-W-Al alloy, characterized in that: The steps include: Step 1: Smelting Ni, Fe, and W to obtain a first molten metal; Step 2: Smelting Al to obtain a second molten metal; Step 3: Mixing and smelting the first molten metal and the second molten metal to obtain a third molten metal; Step 4: Casting the third molten metal to obtain Ni-Fe-W-Al alloy; In step 1, in the smelting container, the tungsten element is divided into multiple portions, and the multiple portions of tungsten element are distributed at different depths in the smelting container.
2. The preparation method according to claim 1, characterized in that In step 1, a plurality of metal single-substance layers are filled from top to bottom in the smelting container; between two adjacent tungsten single-substance layers there is a nickel single-substance layer and / or an iron single-substance layer, or between two adjacent tungsten single-substance layers there is a mixed single-substance layer composed of a mixture of nickel and iron.
3. The preparation method according to claim 2, characterized in that The metal single substance layer includes a tungsten single substance layer, an iron single substance layer, and a nickel single substance layer; the tungsten single substance layer, the iron single substance layer, and the nickel single substance layer are arranged alternately.
4. The preparation method according to claim 1, characterized in that In the Ni-Fe-W-Al alloy, the molar percentage of each element is: Nickel: 50-75%; Iron: 15-35%; Tungsten: 2-12%; Aluminum: 0.5~3%.
5. The preparation method according to claim 1, characterized in that The smelting process of step 1 is: In a vacuum environment, heat Ni, Fe, and W to 1600-1650°C and keep warm for 30-60 minutes; After all the materials in the furnace are melted, electromagnetic stirring is performed for 10 to 20 minutes; After the electromagnetic stirring is completed, the temperature is lowered to 1530-1570° C. to obtain the first molten metal.
6. The preparation method according to claim 5, characterized in that The smelting process of step 3 is: The second molten metal is added to the first molten metal at 1530-1570° C. with electromagnetic stirring for 10-20 minutes.
7. The preparation method according to claim 6, characterized in that The casting process of step 4 is: The melting temperature is raised to 1600-1650°C again, and casting is performed at a speed of 2-3 kg / s.
8. The preparation method according to any one of claims 1 to 7, characterized in that The purity of nickel, iron, tungsten and aluminum is no less than 99.95 wt%.
9. A high melting point and high uniformity Ni-Fe-W-Al alloy, characterized in that: The preparation method is as described in any one of claims 1 to 8.