Improved ethyl cellulose reinforcing agent, preparation method thereof and application of improved ethyl cellulose reinforcing agent in iron salt blue printing paper reinforcement

By improving the ethyl cellulose reinforcement, combined with organic solvents and antioxidants, the color changes and aging problems of iron salt drawings are solved, and effective protection of iron salt drawings is achieved, extending its preservation life and maintaining cultural information.

CN118979410AActive Publication Date: 2024-11-19SHAANXI NORMAL UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411108535.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-19
Estimated Expiration
2044-08-13

AI Technical Summary

Technical Problem

Existing paper reinforcement agents are ineffective for the color changes of iron salt drawings, and traditional methods cannot effectively protect the color changes and aging problems, making it difficult to solve.

Method used

Use modified ethyl cellulose reinforcement, composed of ethyl cellulose, organic solvent and antioxidant, and dissolves and heats and stirs through condensation and reflux to form a reinforcement agent, which is used to protect the iron salt drawings, inhibit color changes and improve water-efficacy sex.

Benefits of technology

Effectively inhibit the color changes of iron salt drawings, improve its mechanical properties and weather resistance, extend the storage life, avoid moisture damage to the structure, and maintain historical and cultural information.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979410A_ABST
    Figure CN118979410A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of archive protection, and relates to an improved ethyl cellulose reinforcing agent, a preparation method thereof and application of the improved ethyl cellulose reinforcing agent in iron salt blue printing paper reinforcement, the improved ethyl cellulose reinforcing agent is composed of ethyl cellulose, an organic solvent and an antioxidant; the mass-to-volume ratio of the ethyl cellulose to the organic solvent to the antioxidant is 0.9 g: 3ml: 15 [mu] L-50 [mu] L; the organic solvent is formed by mixing ethyl acetate, acetone and n-butyl alcohol in equal proportion. The improved ethyl cellulose reinforcing agent is formed by the ethyl cellulose, the organic solvent and the antioxidant, can inhibit the color change of the iron salt blue printing paper, has hydrophobic performance, and has a very good reinforcing and protecting effect on the iron salt blue printing paper.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of archive protection, and relates to an improved ethyl cellulose reinforcing agent, a preparation method thereof, and application in reinforcing iron salt sun-drying drawings. Background Art

[0002] Solar drawings are an important part of archives. Some important engineering drawings recorded on them are our indispensable archival wealth. Effectively preserving these solar drawings archives is one of the management tasks of archives. However, some solar drawings have a long history and are unstable in nature. Therefore, as long as the nature of solar drawings is studied and properly preserved, the use value and preservation life of solar drawings will be maximized. Although my country has carried out a lot of work in the restoration and preservation of other paper cultural relics for a long time, there is little research on the preservation of solar drawings archives. Many precious solar drawings archives have serious fading and blurred handwriting problems, which have not been thoroughly solved. Traditional methods have not effectively protected these solar drawings archives from the root; therefore, it is imperative to study new, efficient and practical methods for protecting solar drawings archives.

[0003] At present, diazonium salt sun-drying drawings are mainly used on the market, so most of them are aimed at the protection of this type of sun-drying drawings. However, there is no relevant literature on the reinforcement protection of iron salt sun-drying drawings, indicating that the protection of iron salt sun-drying drawings is a completely new direction.

[0004] Common paper reinforcement methods include mounting, silk screen reinforcement, and protective liquid reinforcement. Mounting is a traditional paper reinforcement method unique to my country, mostly used to protect precious calligraphy and paintings. Its process is complicated and requires high skills from technicians, so it is not suitable for the large-scale protection of conventional paper cultural relics archives; silk screen reinforcement is to use silk fabrics such as silk mesh to glue paper cultural relics, which is more suitable for reinforcing curled and fragile paper, and silk protein is easy to breed bacteria and cause secondary damage to paper cultural relics; protective liquid reinforcement refers to applying a reinforcement agent to the surface of the cultural relic to form a protective film, so that its mechanical properties, aging resistance and durability are improved, the operation process is simple and reversible.

[0005] Existing paper reinforcement agents include polymethyl methacrylate, fluororesin, ethyl cellulose, etc. Among them, polymethyl methacrylate is a thermoplastic polymer compound. When coated on the surface of paper cultural relics, it can form a colorless and transparent protective film with certain water resistance, but its reversibility is poor and it is easy to burn when exposed to fire; fluororesin reinforcement has the advantages of corrosion resistance, aging resistance, and light resistance, but fluororesin has a large molecular weight, resulting in poor permeability and wettability. The reinforcement agent is not easy to penetrate into the paper fibers, and it is easy to cause a concentration gradient on the surface and inside of the paper, which will cause the color of the drawings to change and accelerate the aging of the paper. Summary of the invention

[0006] In view of the technical problem that existing paper reinforcing agents may cause the color of drawings to change, the present invention provides an improved ethyl cellulose reinforcing agent, a preparation method thereof, and an application thereof in reinforcing iron salt-dried drawings.

[0007] The improved ethyl cellulose reinforcing agent formed by ethyl cellulose, an organic solvent and an antioxidant can inhibit the color change of iron salt sun-drying paper, has hydrophobicity, and has a good reinforcing and protecting effect on the iron salt sun-drying paper.

[0008] In order to achieve the above-mentioned purpose, the technical solution adopted by the present invention is:

[0009] An improved ethyl cellulose reinforcing agent consists of ethyl cellulose, an organic solvent and an antioxidant; the mass volume ratio of the ethyl cellulose, the organic solvent and the antioxidant is 0.9 g: 3 ml: 15 μL-50 μL.

[0010] It is further defined that the organic solvent is a mixture of equal volumes of ethyl acetate, acetone and n-butanol.

[0011] It is further defined that the antioxidant is diisooctyl benzene phosphite, pentaerythritol tetrakis(3,5-di-tert-butyl-4-hydroxy)phenylpropionate, n-octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, tris(2,4-di-tert-butyl)phosphite or triethylene glycol ether-di(3-tert-butyl-4-hydroxy-5-methylphenyl)propionate.

[0012] The preparation method of the improved ethyl cellulose reinforcing agent as described above comprises the following steps:

[0013] S1, mixing ethyl cellulose and an organic solvent, and completely dissolving the ethyl cellulose by condensation reflux method under stirring to obtain an ethyl cellulose solution;

[0014] S2. Add an antioxidant to the ethyl cellulose solution, heat and stir to mix evenly, and obtain a reinforcing agent.

[0015] It is further defined that in step S1, the condensation reflux temperature is 45°C to 55°C, and the stirring speed is 300r / min to 400r / min.

[0016] It is further defined that in step S2, the heating temperature is between 35°C and 40°C, and the stirring speed is between 200 r / min and 300 r / min.

[0017] The improved ethyl cellulose reinforcing agent provided by the invention is used in reinforcing and protecting iron salt sun-drying drawings.

[0018] It is further defined that the improved ethyl cellulose reinforcing agent allows the color difference value of the iron salt sun-dried paper after aging to reach a minimum of 1.74.

[0019] The beneficial effects of the technical solution of the present invention are:

[0020] 1. The improved ethyl cellulose reinforcement provided by the present invention can effectively inhibit the color change of iron salt sun-dried drawings through the interaction of ethyl cellulose, organic solvents and antioxidants. When used in iron salt sun-dried drawings, the color difference value of the iron salt sun-dried drawings after aging is as low as 1.74.

[0021] 2. The improved ethyl cellulose reinforcement agent provided by the present invention significantly enhances the hydrophobicity of the sundry paper sample after being treated, making it difficult for the structure to be destroyed by water molecules during long-term storage, avoiding a series of problems such as blurring, blurring, and smudging of the sundry paper content, thereby destroying the historical and cultural information it carries.

[0022] 3. In the present invention, ethyl cellulose can strengthen the hydrogen bonds between fibers, thereby improving the mechanical properties of paper, while the antioxidant DPOP can protect the paper under aging conditions and improve the weather resistance of the sun-bathed paper.

[0023] 4. The improved ethyl cellulose reinforcing agent provided by the present invention has a good effect in alleviating the reduction of the whiteness value of the sun-dried paper. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 TG curves of membranes with five groups of different reinforcement agents;

[0025] Figure 2 The whiteness changes of six groups of sun-dried paper with different treatments before and after aging;

[0026] Figure 3 The infrared spectra of six groups of differently treated sun-dried paper before and after aging (a is the infrared spectrum before and after ethyl cellulose treatment, b, c, d, e, f are the infrared spectra of sun-dried paper before and after aging (b: sample 1; c: sample 2; d: sample 3; e: sample 4; f: sample 5));

[0027] Figure 4 The scanning electron microscope images of six groups of differently treated sun-dried paper before and after aging (a1, a2 are sample 1; b1, b2 are sample 2; c1, c2 are sample 3; d1, d2 are sample 4; e1, e2 are sample 5);

[0028] Figure 5 The changes in folding endurance of six groups of differently treated sun-dried drawings before and after aging;

[0029] Figure 6 The changes in tensile strength of six groups of differently treated sun-dried drawings before and after aging;

[0030] Figure 7 The contact angle changes of six groups of differently treated sun-dried graphite sheets before and after aging;

[0031] Figure 8 The whiteness changes of different antioxidants coated on the sun-baked paper before and after aging. DETAILED DESCRIPTION

[0032] The technical solution protected by the present invention is now described in detail in conjunction with the accompanying drawings and embodiments. However, it is obvious that the described embodiments are part of the embodiments of the present application, rather than all of the embodiments. Based on the described embodiments of the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.

[0033] The invention provides a sun-drying paper reinforcing agent, which is composed of ethyl cellulose, an organic solvent and an antioxidant; the mass volume ratio of the ethyl cellulose, the organic solvent and the antioxidant is 0.9 g: 3 ml: 15 μL-50 μL.

[0034] Preferably, the organic solvent is a mixture of equal volumes of ethyl acetate, acetone and n-butanol.

[0035] In the present invention, the antioxidant is diisooctyl phosphite (antioxidant DPOP), pentaerythritol tetrakis(3,5-di-tert-butyl-4-hydroxy)phenylpropionate (antioxidant 1010), n-octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate (antioxidant 1076), tris(2,4-di-tert-butyl)phosphite (antioxidant 168), triethylene glycol ether-di(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate (antioxidant XH-245).

[0036] The present invention also provides a method for preparing an improved ethyl cellulose reinforcing agent, comprising the following steps:

[0037] S1. Mix ethyl cellulose and an organic solvent, and dissolve the ethyl cellulose completely by condensation reflux method under stirring to obtain an ethyl cellulose solution; in step S1, the condensation reflux temperature is 45° C. to 55° C., and the stirring speed is 300 r / min to 400 r / min.

[0038] S2. Add antioxidant to ethyl cellulose solution, heat and stir to mix evenly, and obtain reinforcing agent. The heating temperature is 35℃~40℃, and the stirring speed is 200r / min~300r / min.

[0039] The solar paper reinforcing agent obtained by the present invention can make the color difference value of the iron salt solar paper after aging reach a minimum of 1.74, can effectively inhibit the color change of the iron salt solar paper, has hydrophobicity, and also has good mechanical properties, heat resistance and anti-aging properties, and can be used as a reinforcing material in the iron salt solar paper.

[0040] The present invention is described in detail below with reference to specific embodiments.

[0041] It should be noted that, unless otherwise specified, the reagents and drugs used in the following examples and experiments are conventional commercially available products.

[0042] It should be noted that, unless otherwise specified, the operations used in the following examples and experiments are routine operations in the art.

[0043] In the following examples, the experimental drugs used are shown in Table 1.

[0044] Table 1 Experimental drugs

[0045]

[0046]

[0047] In the following examples, the experimental instruments used are shown in Table 2.

[0048] Table 2 Experimental instruments

[0049] Instrument Name model Manufacturer Electronic balance JM-B Yao City Jiming Weighing and Calibration Equipment Co., Ltd. Tungsten Filament Scanning Electron Microscope SU3500 Hitachi High-Technologies Corporation Video Optical Contact Angle Tester OCA20 DatapHysics Magnetic heating stirrer CJJ-6 Jiangsu Jintan Dadi Automation Instrument Factory Humidity and heat aging test chamber SDJ6025 Chongqing Galaxy Testing Instrument Co., Ltd. Sartorius Popular pH Meter PB-10 Shanghai Precision Scientific Instrument Co., Ltd. Folding endurance tester DC-MIT135B Sichuan Changjiang Papermaking Instrument Co., Ltd. Computer controlled universal material testing instrument QT-1136 Gaotai Testing Instrument Co., Ltd. Mid-infrared-far infrared spectrometer Frontier PerkinElmer Thermogravimetric Analyzer Themys one Setteram, France

[0050] Example 1

[0051] The iron salt sun-drying paper reinforcing agent provided in this embodiment includes the following raw materials: 1.8 g of ethyl cellulose powder, 20 mL of ethyl acetate, 20 mL of acetone, 20 mL of n-butanol reagent and 30 μL of antioxidant DPOP solution.

[0052] In this embodiment, the preparation method of the iron salt paper strengthening agent comprises the following steps:

[0053] S1. Take ethyl cellulose, an organic solvent and an antioxidant according to the stated mass proportions.

[0054] In this example, 1.8 g of ethyl cellulose powder, 20 mL of ethyl acetate, 20 mL of acetone, 20 mL of n-butanol reagent and 30 μL of antioxidant DPOP solution were weighed.

[0055] S2, weigh 1.8g of ethyl cellulose powder, weigh 20mL of ethyl acetate, 20mL of acetone, and 20mL of n-butanol reagent, put them into a three-necked flask, add a condensing reflux device, and stir evenly with a magnetic heating stirrer until the ethyl cellulose is completely dissolved;

[0056] In this embodiment, the water bath heating temperature is set at 50° C. and the stirring speed is 350 r / min.

[0057] S3. Measure 10 mL of the prepared ethyl cellulose solution into a 25 mL beaker, use a 100 μL pipette to take 30 μL of the antioxidant DPOP solution, add it to the ethyl cellulose solution, prepare a 0.3%-DPOP solution, place it on a magnetic heating stirrer and stir evenly. Set the bath heating temperature at 40°C and the stirring speed at 300 r / min until the mixture is evenly mixed to obtain a reinforcing agent.

[0058] Example 2

[0059] The iron salt sun-drying paper reinforcing agent provided in this embodiment includes the following raw materials: 1.8 g of ethyl cellulose powder, 20 mL of ethyl acetate, 20 mL of acetone, 20 mL of n-butanol reagent and 50 μL of antioxidant DPOP solution.

[0060] In this embodiment, the preparation method of the iron salt paper strengthening agent comprises the following steps:

[0061] S1. Take ethyl cellulose, an organic solvent and an antioxidant according to the stated mass proportions.

[0062] In this example, 1.8 g of ethyl cellulose powder, 20 mL of ethyl acetate, 20 mL of acetone, 20 mL of n-butanol reagent and 50 μL of antioxidant DPOP solution were weighed.

[0063] S2, weigh 1.8g of ethyl cellulose powder, weigh 20mL of ethyl acetate, 20mL of acetone, and 20mL of n-butanol reagent, put them into a three-necked flask, add a condensing reflux device, and stir evenly with a magnetic heating stirrer until the ethyl cellulose is completely dissolved;

[0064] In this embodiment, the water bath heating temperature is set at 50° C. and the stirring speed is 350 r / min.

[0065] S3. Measure 10 mL of the prepared ethyl cellulose solution into a 25 mL beaker, use a 100 μL pipette to take 50 μL of the antioxidant DPOP solution, add it to the ethyl cellulose solution, prepare a 0.5%-DPOP solution, place it in a magnetic heating stirrer and stir evenly. Set the bath heating temperature at 40°C and the stirring speed at 300 r / min until the mixture is evenly mixed to obtain a reinforcing agent.

[0066] Example 3

[0067] The iron salt sun-drying paper reinforcing agent provided in this embodiment includes the following raw materials: 1.8 g of ethyl cellulose powder, 20 mL of ethyl acetate, 20 mL of acetone, 20 mL of n-butanol reagent and 80 μL of antioxidant DPOP solution.

[0068] In this embodiment, the preparation method of the iron salt paper strengthening agent comprises the following steps:

[0069] S1. Take ethyl cellulose, an organic solvent and an antioxidant according to the stated mass proportions.

[0070] In this example, 1.8 g of ethyl cellulose powder, 20 mL of ethyl acetate, 20 mL of acetone, 20 mL of n-butanol reagent and 80 μL of antioxidant DPOP solution were weighed.

[0071] S2, weigh 1.8g of ethyl cellulose powder, weigh 20mL of ethyl acetate, 20mL of acetone, and 20mL of n-butanol reagent, put them into a three-necked flask, add a condensing reflux device, and stir evenly with a magnetic heating stirrer until the ethyl cellulose is completely dissolved;

[0072] In this embodiment, the water bath heating temperature is set at 50° C. and the stirring speed is 350 r / min.

[0073] S3. Measure 10 mL of the prepared ethyl cellulose solution into a 25 mL beaker, use a 100 μL pipette to take 80 μL of the antioxidant DPOP solution, add it to the ethyl cellulose solution, prepare a 0.8%-DPOP solution, place it on a magnetic heating stirrer and stir evenly. Set the bath heating temperature at 40°C and the stirring speed at 300 r / min until the mixture is evenly mixed to obtain a reinforcing agent.

[0074] Example 4

[0075] The iron salt sun-drying paper reinforcing agent provided in this embodiment includes the following raw materials: 1.8 g of ethyl cellulose powder, 20 mL of ethyl acetate, 20 mL of acetone, 20 mL of n-butanol reagent and 100 μL of antioxidant DPOP solution.

[0076] In this embodiment, the preparation method of the iron salt paper strengthening agent comprises the following steps:

[0077] S1. Take ethyl cellulose, an organic solvent and an antioxidant according to the stated mass proportions.

[0078] In this example, 1.8 g of ethyl cellulose powder, 20 mL of ethyl acetate, 20 mL of acetone, 20 mL of n-butanol reagent and 100 μL of antioxidant DPOP solution were weighed.

[0079] S2, weigh 1.8g of ethyl cellulose powder, weigh 20mL of ethyl acetate, 20mL of acetone, and 20mL of n-butanol reagent, put them into a three-necked flask, add a condensing reflux device, and stir evenly with a magnetic heating stirrer until the ethyl cellulose is completely dissolved;

[0080] In this embodiment, the water bath heating temperature is set at 50° C. and the stirring speed is 350 r / min.

[0081] S3. Measure 10 mL of the prepared ethyl cellulose solution into a 25 mL beaker, use a 100 μL pipette to take 100 μL of the antioxidant DPOP solution, add it to the ethyl cellulose solution to prepare a 1.0%-DPOP solution, place it on a magnetic heating stirrer and stir evenly. Set the bath heating temperature at 40°C and the stirring speed at 300 r / min until the mixture is evenly mixed to obtain a reinforcing agent.

[0082] Comparative Example 1

[0083] The coating material provided in this comparative example includes the following raw materials: 1.8 g of ethyl cellulose powder, 20 mL of ethyl acetate, 20 mL of acetone, and 20 mL of n-butanol reagent.

[0084] In this comparative example, the preparation method of the reinforcing agent comprises the following steps:

[0085] S1. Take ethyl cellulose, an organic solvent and an antioxidant according to the stated mass proportions.

[0086] In this example, 1.8 g of ethyl cellulose powder, 20 mL of ethyl acetate, 20 mL of acetone, 20 mL of n-butanol reagent and 30 μL of antioxidant DPOP solution were weighed.

[0087] S2. Weigh 1.8g of ethyl cellulose powder, weigh 20mL of ethyl acetate, 20mL of acetone, and 20mL of n-butanol reagent, put them into a three-necked flask, add a condensing reflux device, and stir evenly with a magnetic heating stirrer until the ethyl cellulose is completely dissolved.

[0088] In this embodiment, the water bath heating temperature is set at 50° C. and the stirring speed is 350 r / min.

[0089] In order to verify the performance advantages of the iron salt sun-dried paper reinforcing agent of the present invention, the following test was carried out using the iron salt sun-dried paper reinforcing agent provided in the examples and comparative examples.

[0090] Test 1: Thermogravimetric curve test of different iron salts for strengthening drawings

[0091] Test samples: the reinforcing agent of comparative example 1, wherein the antioxidant content is 0; the reinforcing agents of Examples 1 to 4, wherein the content of the antioxidant DPOP is 0.3%, 0.5%, 0.8% and 1.0%-DPOP, respectively. The reinforcing agents of comparative example 1 and Examples 1 to 4 are correspondingly recorded as sample 1, sample 2 to sample 5.

[0092] The test process is: take 5 ml of each of the above five samples, drop them into a 50*50*2mm square silicone mold, let it stand at a constant temperature of 25℃ for 48 hours, and then use tweezers to demould to obtain five different reinforcing agent films.

[0093] The thermal stability analysis was performed using the Themys one thermogravimetric analyzer from the French company Setram. 5 to 10 mg of sample film was weighed and placed in an α-Al2O3 crucible. The crucible was placed in the thermogravimetric analyzer with a heating rate of 20°C / min and a temperature range of 30°C to 600°C in an air atmosphere. The results are as follows: Figure 1 shown.

[0094] Figure 1 The TG curve in the middle is measured under air atmosphere. It can be seen from the TG curve that no matter how much the concentration of antioxidant DPOP is, there is a mass loss at about 300℃. The thermogravimetric curve trend of the blank control group with only ethyl cellulose added is similar to that of the four groups with antioxidant DPOP added. The antioxidant DPOP does not decompose other substances in this temperature range. The five experimental groups basically completed the mass loss at 550℃. The mass loss of the blank control group without antioxidant added was as high as 86.6% at 500℃, while the mass loss of 0.8%-DPO was more than 78%; and when the mass loss rate was the largest at 350℃, the mass loss of the blank control group without antioxidant added was as high as 78.2%, while the mass loss of 0.8%-DPO and 1.0%-DPOP was about 65%. Other concentrations of DPOP more or less play a role in reducing mass loss. It can be seen that the antioxidant DPOP contributes to the thermal stability of the reinforcing agent, among which the effects of 0.8%-DPOP and 1.0%-DPOP are more prominent than those of the other two groups.

[0095] Through comprehensive comparison, the reinforcing agent material of Example 1 (reinforcing agent 4) has good film-forming effect and is most suitable for use as a reinforcing agent in the protection of iron salt sun-drying drawings. It can improve the heat resistance of cultural relics and achieve the expected protection effect.

[0096] Test 2: Whiteness Characterization of Different Reinforcements

[0097] Test samples: Comparative Example 1, Sample 1, and Sample 2 to Sample 5 corresponding to Examples 1 to 4.

[0098] The experimental process is: prepare analytical grade ammonium ferric citrate and potassium ferrocyanide chemical reagents, beakers, glass rods, rubber-tipped droppers, brown reagent bottles, brushes, electronic balances with an accuracy of 0.1g, trays, acrylic plates, deionized water and other drugs and instruments. The entire experimental operation should be carried out in a dark room without sunlight. Preparation of photosensitive agent A and B liquid: Photosensitive agent A liquid: Take 40g of ammonium ferric citrate and dissolve it in 200mL of water to obtain a dark brown solution, and place it in a brown reagent bottle after the solid sample is completely dissolved; Photosensitive agent B liquid: Take 16g of potassium ferrocyanide and dissolve it in 200mL of water to obtain a yellow solution, and place it in a brown reagent bottle after the solid sample is completely dissolved; Take an appropriate amount of photosensitive agent A liquid and photosensitive agent B liquid and mix them in equal volumes to obtain a dark yellow-green photosensitive agent mixture with Prussian yellow as the component. Use a brush to dip an appropriate amount of the photosensitive agent mixture and evenly apply it on the surface of the paper in the order of vertical first and then horizontal. After the coating is completed, the paper coated with the photosensitive agent is placed in a dark or weak light condition to dry to obtain photosensitive paper. Use two acrylic plates to fix the photosensitive paper in the middle, put it in a dark box with ultraviolet light to expose for 10 minutes, and rinse the exposed paper with water for 10 minutes. The highlight area must be rinsed until it is white and there is no yellow-green color in the water. Put the drawing on a plastic sheet to dry to obtain the iron salt drying drawing.

[0099] Take 5 ml of each of the above samples and brush them evenly on the homemade iron salt sun-drying paper to prepare 5 groups of sun-drying paper simulation samples, which are then tested together with the untreated sun-drying paper samples.

[0100] According to the national standard GB / 22894-2008, 5 groups of simulated samples and original samples of sun-dried paper were subjected to accelerated aging test under damp heat. Aging conditions: set the temperature to 80℃, humidity to 65%, and time to 72h. After taking out the sun-dried paper samples, balance them in indoor environment for two days. The 5 groups of simulated samples of sun-dried paper and original samples of sun-dried paper after aging were tested.

[0101] Test method: Use a black tube to zero the WSB-2 digital whiteness meter (Shanghai Pingxuan Scientific Instrument Co., Ltd.), and then use a standard white board with a whiteness value of 81.5 for whiteness calibration. According to "Determination of CIE whiteness of paper and paperboard, D65 / 10°" (GB / T22880-2008), the whiteness meter is used to test the whiteness of the paper before and after reinforcement. The same sample is tested 10 times in parallel, and the relative error should be less than 5%. The results are as follows Figure 2 shown.

[0102] See also Figure 2As shown in the figure, the whiteness value before the wet heat accelerated aging treatment has no obvious relationship with whether the reinforcing agent is applied, but depends on the preparation and washing process of the photosensitive solution in the preparation process of the iron salt sun-drying paper; after the wet heat accelerated aging treatment, the whiteness of the iron salt sun-drying paper simulation samples decreased, among which the whiteness value of the untreated sun-drying paper sample decreased by 2.5%, and the whiteness values ​​of samples 1 to 5 decreased by 1.5%, 2%, 1.7%, 1.3%, and 2.3%, respectively, indicating that the reinforcing agent has a certain alleviating effect on the reduction of the whiteness value of the sun-drying paper, among which the alleviating effect on the reduction of whiteness after 0.8%-DPOP treatment is the best.

[0103] Experiment 3: Microscopic morphology test of thin films with different reinforcement coating materials

[0104] Test samples: Sample 1, Sample 2 to Sample 5 in Test 2. Prepared sun-drying paper simulation samples and sun-drying paper original samples, and five sets of sun-drying paper simulation samples and sun-drying paper original samples after aging.

[0105] Test method: The color difference is measured with an X-RiteVS-450 spectrophotometer, and the CIE L*a*b color coordinate system is used to characterize the color change of the solar paper sample before and after accelerated aging with damp heat. L*, a*, and b* are the measurements of brightness, hue, and color saturation, respectively. The smaller the measured color difference ΔE, the smaller the color change at the same point of the solar paper sample before and after aging. Conversely, it means that the color change is large. The CIE L*a*b color system color difference value calculation formula is as follows:

[0106] ΔE * =[(ΔL * ) 2 +(Δa * ) 2 +(Δb * ) 2 ] 1 / 2

[0107] Where: ΔL*=L 老化后 -L* 老化前 (ΔL* is the brightness difference)

[0108] Δa*=a 老化后 -a* 老化前 (Δa* is the red-green color deviation)

[0109] Δb*=b 老化后 -b* 老化前 (Δb* is the yellow-blue deviation)

[0110] The results are shown in Table 3.

[0111] Table 3 Color difference of the printed paper before and after aging

[0112] Sample name ΔE* Sample drawing 6.12 Sample 1 5.82 Sample 2 4.17 Sample 3 3.66 Sample 4 1.74 Sample 5 2.71

[0113] As shown in Table 3, after accelerated aging with wet heat, the color difference value of the untreated sundrying paper sample is 6.12, which is a significant color change; the color difference value of sample 1 with only ethyl cellulose added is 5.82, which is a slight color change, indicating that ethyl cellulose has basically no effect on protecting the color difference change of sundrying paper; the color difference values ​​of samples 2 and 3 are 4.17 and 3.66, which are slight color changes; the color difference values ​​of samples 4 and 5 are 1.74 and 2.71, which are very slight color changes. This shows that the antioxidant DPOP can inhibit the color change of iron salt sundrying paper, among which 0.8%-DPOP has the best effect.

[0114] Test 4: Infrared spectroscopy analysis

[0115] Test samples: the sundrying paper simulation samples and original sundrying paper samples prepared from samples 1 to 5 in Test 2, as well as five groups of sundrying paper simulation samples and original sundrying paper samples after aging.

[0116] Test method: The simulated sample 1 before and after reinforcement, and the samples 1 to 5 before and after the wet heat accelerated aging test were measured by a PE-Frontier mid-infrared-far-infrared spectrometer at 4000 -1 ~400cm -1 The infrared spectrum of the sample is measured within the range, and the results are as follows Figure 3 shown.

[0117] See also Figure 3 From the infrared spectrum of ethyl cellulose, we can see that the peak positions before and after coating are basically the same, the absorption peak intensity has changed, and no new functional groups have been generated, indicating that ethyl cellulose itself does not react with iron salt drying drawings, which is in line with the principle of cultural relics protection. -1 The absorption peak at 2900 cm is the OH stretching vibration peak. -1 The absorption peak at 1740 cm is the stretching vibration of CH and CH2 in the molecule. -1 The absorption peak at 1434 cm is the C=O stretching vibration peak. -1 and 1372cm -1 The absorption peak at 1020cm is the bending vibration peak of methylene. -1 The absorption peak at 880cm is the stretching vibration peak of CO. -1 917cm -1 The absorption peak is caused by the vibration absorption peak of the OC2H3 functional group of ethyl cellulose.

[0118] Figure 3 b, c, d, e, and f are infrared spectra of sun-dried paper reinforced with ethyl cellulose with different concentrations of DPOP before and after aging. It can be seen from the comparison that there is no obvious change in the peak position, 3400cm -1~3300cm -1 The peak is the OH stretching vibration peak. The peak intensity of sample 4 with 0.8%-DPOP decreases the least before and after aging, which means that the fiber bonding strength of the sundry paper decreases little after aging and the durability remains good. The reinforcement agent of this concentration acts on the sundry paper to ensure that it is least affected in a high temperature and high humidity environment, and to protect the information carried on the sundry paper from damage to the greatest extent.

[0119] Test 5: Microscopic morphology test

[0120] Test samples: sun-drying paper simulation samples prepared from samples 1 to 5 in Test 2 and five groups of sun-drying paper simulation samples after aging.

[0121] Test method: Samples 1 to 5 before and after heat aging were fixed on the cross-section test bench with conductive glue, and the surface was treated with gold spraying for 120s using an ion sputtering instrument. Then, the surface morphology of the samples was observed with a SU3500 tungsten filament scanning electron microscope at a certain magnification. The microscopic morphology of the samples at 200μm under the tungsten filament scanning electron microscope is as follows: Figure 4 As shown, where: a1: unaged sample 1, a2: aged sample 1; b1: unaged sample 2, b2: aged sample; c1: unaged sample 3, c2: aged sample 3; d1: unaged sample 4, d2: aged sample 4; e1: unaged sample 5, e2: aged sample 5.

[0122] Depend on Figure 4 It can be seen that the sun-dried paper fibers present a three-dimensional network structure, which are stacked and interlaced with each other, forming a large number of irregular gaps and holes on the surface, and Prussian blue pigment is attached to the fiber surface. After reinforcement, the Prussian blue pigment is tightly coated on the fiber, forming a thin film on the surface of the sun-dried paper, making it difficult for the pigment to fall off, and the reinforcement fills the gaps in the paper fibers to a certain extent, which helps to improve the mechanical properties of the sun-dried paper. After accelerated aging by wet heat, the unreinforced sun-dried paper in the environment of high temperature and high humidity has aggravated hydrolysis of paper cellulose and more fiber breakage, while the reinforced sun-dried paper has fewer fiber breakages and better film retention.

[0123] Test 6: Mechanical properties test

[0124] Test samples: the sundrying paper simulation samples and original sundrying paper samples prepared from samples 1 to 5 in Test 2, as well as five groups of sundrying paper simulation samples and original sundrying paper samples after aging.

[0125] Test method: Cut the simulated samples of samples 1 to 5 before and after accelerated aging with damp heat into paper strips with a width of (15±0.1) mm and a length of 130 mm, place them in an environment with a temperature of 25°C and a humidity of 35% for equilibration for 3 days, and then conduct paper tensile strength and folding endurance tests.

[0126] ①Tensile strength test

[0127] According to GB / T12914-2008 "Determination of tensile strength of paper and paperboard", the tensile strength of paper samples was tested by constant speed tensile method. The paper samples before and after accelerated aging were vertically clamped between two clamps, with a gauge length of 100mm and a constant tensile speed of 20mm / min. Ten groups of paper samples before and after accelerated aging were measured and the average value was taken.

[0128] ②Folding endurance test

[0129] According to GB / T457-2008 "Determination of folding resistance of paper and paperboard", the folding resistance of paper is tested using a paper folding resistance tester. The LB-MIT135 paper folding resistance tester is used to test the paper before and after aging, and the weight used is 4.91N. 10 groups of samples are tested before and after accelerated aging with damp heat and take the average value.

[0130] The folding endurance of samples 1 to 5 before and after the wet heat accelerated aging test is as follows: Figure 5 As shown, the tensile strength is Figure 6 shown.

[0131] Depend on Figure 5 It can be seen that the folding resistance of samples 1 to 5 after treatment is higher than that of the sun-dried paper sample, indicating that the mechanical properties of the samples are enhanced after ethyl cellulose film formation. After the wet heat accelerated aging treatment, the folding resistance of the paper decreased, among which the folding resistance of the sun-dried paper sample decreased by 56%, and the folding resistance of samples 1 to 5 decreased by 42.9%, 22.8%, 33.3%, 14.3%, and 25% respectively. The folding resistance of samples 1 to 5 decreased less than that of the sun-dried paper sample.

[0132] Depend on Figure 6 It can be seen that the tensile strength of samples 1 to 5 after treatment is higher than that of the sundry paper samples. After the wet heat accelerated aging treatment, the tensile strength of the sundry paper decreased, among which the tensile strength of the original sundry paper decreased by 1.28kN / m, and the tensile strength of samples 1 to 5 decreased by 1.05kN / m, 0.51kN / m, 0.65kN / m, 0.49kN / m, and 1.12kN / m respectively. The tensile strength of samples 1 to 5 decreased less than that of the original sundry paper.

[0133] It can be inferred from the changes in folding endurance and tensile strength that the overall mechanical properties of the treated samples 1 to 5 are better than those of the untreated sundrying paper. Ethyl cellulose can strengthen the hydrogen bonds between fibers, thereby improving the mechanical properties of paper, while the antioxidant DPOP can protect the paper under aging conditions and improve the weather resistance of the sundrying paper, among which 0.8%-DPOP has the best effect.

[0134] Test 7: Contact angle test

[0135] The contact angle refers to the angle between the solid-liquid interface. The larger the contact angle, the more hydrophobic the solid surface is; the smaller the contact angle, the more hydrophilic it is. For the protection of paper cultural relics, good hydrophobicity can prevent the cultural relics from being eroded by moisture in the preservation environment.

[0136] Test samples: the sundrying paper simulation samples and original sundrying paper samples prepared from samples 1 to 5 in Test 2, as well as five groups of sundrying paper simulation samples and original sundrying paper samples after aging.

[0137] Test method: The static contact angle of the sun-dried paper before and after accelerated aging with wet heat is measured by the sessile drop method in the video optical contact angle tester. A long strip of sun-dried paper sample is cut and placed on the sample table. Then 2 microliters of deionized water is dropped on the surface of the paper sample. The appropriate light intensity is adjusted and the lower droplet surface of the water drop is quickly photographed with a camera. The computer automatically performs fitting calculations and obtains the static contact angle value of the sample. Each sample is measured and 10 groups are averaged. The results are shown as follows: Figure 7 shown.

[0138] Depend on Figure 7 It can be seen that the contact angles of samples 1 to 5 are all larger than those of the sun-dried paper samples, increasing by 10.9°, 21.5°, 15°, 12.4°, and 6.6°, respectively. The contact angle of the sun-dried paper samples changed significantly after 60s, decreasing by 15.2°; while the contact angles of samples 1 to 5 after reinforcement treatment changed within 5° after 60s, indicating that the hydrophobicity of the sun-dried paper samples was significantly enhanced after being treated with ethyl cellulose reinforcement agent. After accelerated aging with wet heat, the bonding force between paper fibers decreased, the antioxidant was partially consumed, and the contact angles of each sample decreased. The contact angle of the sun-dried paper decreased by 12.1°; the contact angles of samples 1 to 5 decreased by 2.3°, 12.5°, 6.9°, 0.6°, and 5°, respectively; after 60s, the contact angle of the sun-dried paper sample decreased by 26.1°; the contact angles of samples 1 to 5 decreased by 2°, 1°, 6°, 2.4°, and 1.7°, respectively. From the test results, it can be seen that the ethyl cellulose reinforcement agent with DPOP has a significant protective effect on the sundry paper, which can effectively improve the hydrophobicity of the sundry paper itself, making it difficult for water molecules to destroy the structure during long-term storage, avoiding a series of problems such as blurring, blurring, and smudging of the sundry paper content, which damages the information it carries. Among them, the ethyl cellulose protective agent with 0.8%-DPOP has the smallest change in contact angle after wet heat aging treatment, and has the best protective effect on the sundry paper.

[0139] Test 8: Optimization test of antioxidants.

[0140] In order to select the best antioxidant from among several antioxidants, different types of antioxidants were dissolved in ethyl cellulose solution and prepared into reinforcing agents with a mass fraction of 0.8% according to the raw material ratio of Example 3.

[0141] The types of antioxidants selected are antioxidant DPOP, pentaerythritol tetrakis(3,5-di-tert-butyl-4-hydroxy)benzenepropionate (antioxidant 1010), n-octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate (antioxidant 1076), tris(2,4-di-tert-butyl) phosphite (antioxidant 168), and triethylene glycol ether-di(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate (antioxidant XH-245).

[0142] A batch of iron salt sun-dried paper was prepared again according to the method of Experiment 2; then the reinforcing agent prepared with different antioxidants was coated on the iron salt sun-dried paper, and a damp heat accelerated aging test was carried out, and the aging conditions were: the set temperature was 80℃, the humidity was 65%, and the time was 72h. After taking out the sun-dried paper samples, they were balanced in the indoor environment for two days. The iron salt sun-dried paper samples before and after damp heat accelerated aging were subjected to color difference and whiteness experiments.

[0143] (1) The color difference of the same position of the sun-dried paper before and after aging after different antioxidants were applied is shown in Table 4. The color difference of the untreated paper after aging is 6.38.

[0144] Table 4 Color difference of different antioxidants applied to the sun-dried paper before and after aging

[0145] Sample name ΔE* Antioxidant DPOP 1.92 Antioxidant 1010 3.29 Antioxidant 1076 6.33 Antioxidant 168 2.75 Antioxidant XH-245 5.01

[0146] It can be seen from Table 4 that the color difference of the iron salt sun-dried paper coated with antioxidant DPOP is the smallest at 1.92, and the color difference is the most significant data reflecting the change of the iron salt sun-dried paper before and after aging. The smaller the color difference change value, the smaller the color change of the sun-dried paper under high temperature and high humidity conditions, and the better the retention degree. It can be explained that the antioxidant DPOP has a significant alleviating effect on the chromaticity change of the iron salt sun-dried paper compared with the other four antioxidants.

[0147] (2) The whiteness of the same position of the printed paper before and after aging after different antioxidants were applied is as follows Figure 8 shown.

[0148] Depend on Figure 8 It can be seen that the whiteness of the simulated samples coated with different antioxidants on iron salt sun-bathed paper decreased after accelerated aging with damp heat, with antioxidant DPOP decreasing by 0.4%, antioxidant 1010 decreasing by 1.9%, antioxidant 1076 decreasing by 2.2%, antioxidant 168 decreasing by 2.0%, and antioxidant XH-245 decreasing by 2.0%. This indicates that antioxidant DPOP has the best effect in alleviating the reduction of whiteness after reinforcement treatment.

[0149] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. An improved ethyl cellulose reinforcing agent, characterized in that: The invention is composed of ethyl cellulose, an organic solvent and an antioxidant; the mass volume ratio of the ethyl cellulose, the organic solvent and the antioxidant is 0.9 g: 3 ml: 15 μL-50 μL.

2. The improved ethyl cellulose reinforcing agent according to claim 1, characterized in that The organic solvent is prepared by mixing ethyl acetate, acetone and n-butanol in equal volumes.

3. The improved ethyl cellulose reinforcing agent according to claim 1, characterized in that The antioxidant is diisooctyl benzene phosphite, pentaerythritol tetrakis(3,5-di-tert-butyl-4-hydroxy)phenylpropionate, n-octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, tris(2,4-di-tert-butyl)phosphite or triethylene glycol ether-di(3-tert-butyl-4-hydroxy-5-methylphenyl)propionate.

4. The method for preparing the improved ethyl cellulose reinforcing agent according to claim 1, characterized in that: The preparation method comprises the following steps: S1, mixing ethyl cellulose and an organic solvent, and completely dissolving the ethyl cellulose by condensation reflux method under stirring to obtain an ethyl cellulose solution; S2. Add an antioxidant to the ethyl cellulose solution, heat and stir to mix evenly, and obtain a reinforcing agent.

5. The preparation method according to claim 4, characterized in that: In the step S1, the condensation reflux temperature is 45°C to 55°C, and the stirring speed is 300r / min to 400r / min.

6. The preparation method according to claim 4, characterized in that: In step S2, the heating temperature is between 35°C and 40°C, and the stirring speed is between 200 r / min and 300 r / min.

7. Use of the improved ethyl cellulose reinforcing agent as claimed in claim 1 in reinforcing and protecting iron salt sun-drying drawings.

8. The use according to claim 7, characterized in that: The improved ethyl cellulose reinforcement agent makes the color difference value of the iron salt sun-dried drawings after aging reach a minimum of 1.74.

Citation Information

Patent Citations

  • Black and white photo development reinforcing agent

    CN102786847A

  • Environment-friendly low-cost method for reinforcing fragile paper by using cotton fiber silk screen

    CN103952948A

  • Paper Buddhist text crisp powder pigment layer repairing liquid and repairing method

    CN106120455A

  • Solidifying agent and / or stabilizer

    WO2002042557A1