Photonic crystal radiation refrigeration device with colored structure and preparation method of photonic crystal radiation refrigeration device

By adopting a two-layer angle combination micro-circular three-dimensional grating and multi-layer film structure in photonic crystal radiation refrigeration devices, the problem of high energy consumption in traditional refrigeration technology and incompatible performance of color radiation cooling devices is solved, and the rainbow color characteristics and high efficiency are achieved The infrared radiation cooling effect is suitable for environmental protection and energy saving needs.

CN118980190AActive Publication Date: 2024-11-19NANJING UNIV OF AERONAUTICS & ASTRONAUTICS

Patent Information

Application Number
CN202411089707.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-19
Estimated Expiration
2044-08-09

AI Technical Summary

Technical Problem

Traditional steam compression refrigeration, steam absorption refrigeration, and adsorption refrigeration technologies have high energy demand and lead to global warming. The existing color radiation cooling devices have color appearance and are incompatible with high cooling performance, dyes have a hazard to the environment and stable color. The problem of poor performance is difficult to meet the needs of new environmentally friendly and energy-saving refrigeration.

Method used

Photonic crystal radiation refrigeration device using a micro-circular three-dimensional grating with a top double-layer angle combination and a bottom multi-layer film structure colored, is prepared by photolithography-coating-peeling process using a high reflectivity metal layer, a dielectric layer and a substrate. A micro-sphere grating with iridescent color characteristics and low absorption in the visible light range is formed to achieve high reflectivity and high emissivity.

Benefits of technology

It realizes the color daytime radiation cooling effect with low absorption in the visible light range, improves infrared radiation regulation performance, has good material stability, and controllable material usage. It is suitable for buildings and automobiles and can achieve average temperature drop in mid-latitude areas. 6.1~7.7℃.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118980190A_ABST
    Figure CN118980190A_ABST
Patent Text Reader

Abstract

The invention discloses a photonic crystal radiation refrigeration device with a colored structure and a preparation method thereof.The device comprises a double-layer micro-circular-truncated-cone three-dimensional grating located at the top and a multi-layer film structure located at the bottom, and the included angles between the generatrix of the micro-circular-truncated-cone three-dimensional grating on the upper layer and the bottom face and the included angles between the generatrix of the micro-circular-truncated-cone three-dimensional grating on the lower layer and the bottom face are different. The bottom multilayer film structure comprises a metal layer, a dielectric layer and a substrate from bottom to top. The preparation method comprises the following steps: spin-coating a layer of photoresist on a substrate, pre-baking, carrying out contact exposure under a mask, post-baking, developing in a solution to obtain a substrate with a micro-grating complementary structure constructed on the surface, evaporating a layer of MgF2 on the surface to obtain a substrate with a MgF2 microstructure deposited on the surface, and then carrying out surface SiO2 deposition and bottom dielectric layer deposition to obtain the micro-grating substrate with the MgF2 microstructure deposited on the surface. And finally, depositing a metal layer. By means of angle combination, emissivity wave crests and wave troughs of two microstructure angles can be neutralized, and the wide-spectrum infrared radiation regulation and control effect is achieved; a good color effect is achieved in different light environments; the average reflectivity and the average emissivity of the infrared band are both 0.9 or above, and the average temperature is reduced by 6.1-7.7 DEG C compared with the environment temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a refrigeration device and a preparation method thereof, and in particular to a structure-colored photonic crystal radiation refrigeration device and a preparation method thereof. Background Art

[0002] With the continuous development of global industrialization, energy crisis and global warming have become two major problems that cannot be ignored in today's world. At the same time, the quality of life of residents in many emerging economies has been unprecedentedly improved, and people's demand for air conditioning and refrigeration has increased significantly. Traditional technologies such as steam compression refrigeration, steam absorption refrigeration, and adsorption refrigeration have high energy requirements and will discharge waste heat into the atmosphere, thereby causing global warming and the intensification of the urban heat island effect. They can no longer fully meet the needs of new environmentally friendly and energy-saving refrigeration.

[0003] Radiative cooling is a passive cooling technology. Due to its unique thermodynamic mechanism, it can release the heat energy of an object to the largest cold object - space without any additional energy input. Passive radiative cooling technology is attracting more and more attention due to its environmental protection and energy-free characteristics. To achieve daytime passive radiative cooling, it is necessary to meet the conditions of high reflection in the solar spectrum band (0.3-2.5μm) and high emission in the infrared band (2.5-20μm). This optical property of spectrally selective absorption is achieved through micro-nano engineering of specific materials and coatings. Many reported radiative coolers have achieved good results in cooling performance, but whether it is photonic crystal film or polymer film, in order to maximize the broadband high reflectivity of the solar spectrum band, most of them have a white or mirror-like appearance. This single color tone is a visual aesthetic disadvantage for some consumer-oriented industries, such as architecture and automotive applications, where a colorful appearance can be more attractive.

[0004] However, some colored radiation cooling devices in the industry currently have problems such as the incompatibility of colored appearance with high cooling performance, environmental hazards of dyes, and poor color stability. The development of a colored daytime radiation cooler with low absorption in the visible light range using structural coloring has great application prospects. Summary of the invention

[0005] Purpose of the invention: The purpose of the present invention is to provide a structurally colored photonic crystal radiation cooling device with low absorption in the visible light range;

[0006] The second object of the present invention is to provide a method for preparing the above-mentioned structurally colored photonic crystal radiation cooling device.

[0007] Technical solution: The structurally colored photonic crystal radiation cooling device described in the present invention includes a top double-layer angle-combined micro-cone three-dimensional grating and a bottom multilayer film structure, wherein the bottom multilayer film structure includes a metal layer, a dielectric layer and a substrate from bottom to top.

[0008] Among them, the double-layer angle-combined micro-cone three-dimensional grating includes an upper cone and a lower cone, the angles between the lower cone busbar and the upper cone busbar and the bottom surface are 30° to 40° and 60° to 70° respectively, and the grating period is 4 to 7 μm.

[0009] The metal layer is a material with stable physical and chemical properties and high reflectivity, such as at least one of Ag, Au, Al, etc., and the dielectric layer material is Si 3 N 4 and / or HfO 2 ; The substrate is SiO 2 Substrate.

[0010] The method for preparing the above-mentioned structure-colored photonic crystal radiation cooling device comprises the following steps:

[0011] (1) Cleaning and drying the substrate;

[0012] (2) Spin-coating a layer of photoresist on the substrate, performing pre-baking, then performing contact exposure under a mask, and then performing post-baking; after post-baking, developing in a solution to obtain a substrate with a micro-grating complementary structure constructed on the surface;

[0013] (3) A layer of MgF is evaporated on the surface of the substrate with a micro-grating complementary structure. 2 After completion, the residual photoresist is removed by immersing in a degumming solution to obtain a surface with MgF 2 Microstructured substrates;

[0014] (4) Using ion enhanced chemical vapor deposition, MgF 2 Microstructured substrate with surface SiO 2 The structure-colored photonic crystal radiation cooling device is manufactured by depositing a top layer and a bottom dielectric layer, and then evaporating a metal layer on the dielectric layer.

[0015] Wherein, in step (1), the substrate is SiO 2 Substrate; for SiO 2 The substrate was placed in an ethanol solution for ultrasonic cleaning, and then taken out and dried.

[0016] Wherein, in step (2), the photoresist is NR77-6000PY negative photoresist; the photoresist spin coating speed is 4500-5000 rpm; the pre-baking is performed on a hot plate at 90-120°C for 120-150 s; the post-baking is performed on a hot plate at 90-120°C for 90-120 s; and the contact exposure time is 0.4-0.5 s.

[0017] Wherein, in step (2), the developer is a 2.38% TMAH aqueous solution, and the development time is 5 to 6 seconds.

[0018] Wherein, in step (3), MgF 2 The vapor deposition thickness is 1.6 to 2 μm.

[0019] Wherein, in step (4), SiO 2 The deposition thickness of MgF 2 The thickness is consistent, the deposition thickness of the dielectric layer is 0.5-1.2 μm, and the deposition thickness of the metal layer is greater than 100 nm.

[0020] In step (4), MgF 2 The microstructured substrate was transferred to a plasma enhanced chemical vapor deposition device for surface SiO 2 The substrate is then transferred to a vacuum evaporation device for deposition of a metal layer.

[0021] Deposition of MgF 2 The main function of MgF is to prepare the required surface microstructure without affecting the spectral performance. 2 The deposition stability and controllability are much greater than that of SiO 2 , so it is easier to form the target microstructure.

[0022] Beneficial effects: Compared with the prior art, the present invention achieves the following significant effects:

[0023] (1) The present invention is SiO 2 The three-dimensional micro-grating with the angle combination on the top can neutralize the emissivity peaks and valleys of the two micro-structure angle micro-structures, greatly reducing the bulk SiO 2 In the impedance mismatch of the atmospheric window band, the dielectric layer can further enhance the infrared emissivity and achieve a wide-spectrum infrared radiation regulation effect; while the bottom metal reflective layer can achieve high reflectivity of the solar spectrum;

[0024] (2) The raw materials used in the present invention are all common materials, which are abundant and easily available;

[0025] (3) The present invention adopts a photolithography-coating-stripping preparation process, and the period of the prepared micro-truncated cone grating is 4 to 7 μm, the line width is relatively large, and a high preparation success rate can be obtained by reasonably controlling the exposure and development time;

[0026] (4) The micro-truncated cone grating prepared by the present invention has a height of 1.6 to 2 μm, good structural stability, and controllable material dosage;

[0027] (5) The structurally colored photonic crystal radiation cooling device prepared by the present invention utilizes the multiple interference of micro-gratings to form a rainbow color feature with a silver reflective layer, has a good color effect under different light environments, and has no obvious absorption peak in the visible light band;

[0028] (6) The average reflectivity of the structure-colored photonic crystal radiation cooling device prepared by the present invention in the solar band and the average emissivity in the infrared band are both above 0.9;

[0029] (7) The structurally colored photonic crystal radiation cooling device prepared by the present invention can achieve an average temperature reduction of 6.1 to 7.7°C compared to the ambient temperature in mid-latitude areas with an air temperature of 25°C. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 The basic structure of the photonic crystal radiation cooling device with structural coloring in Example 1 of the present invention;

[0031] Figure 2 SiO is obtained in step (4) of Example 1 of the present invention. 2 SEM image of the complementary micro-grating structure constructed on the substrate surface;

[0032] Figure 3 This is a SEM image of the photonic crystal radiation cooling device prepared in Example 1 of the present invention;

[0033] Figure 4 The spectral characterization curve of the structure-colored photonic crystal radiation cooling device prepared in Example 1 of the present invention and the multilayer film structure under the same deposition conditions;

[0034] Figure 5 The structure-colored photonic crystal radiation cooling device prepared in Example 1 of the present invention is compared with the SiO 2 Comparison of emissivity of substrates in the local infrared band;

[0035] Figure 6 The theoretical radiative cooling power curve of the structure-colored photonic crystal radiative cooling device prepared in Example 1 of the present invention under different non-radiative heat transfer coefficients;

[0036] Figure 7The color diagram of the structure-colored photonic crystal radiation cooling device prepared in Example 1 of the present invention at different angles under strong sunlight;

[0037] Figure 8 Detailed changes in the emissivity of different angle combinations calculated in Example 2 of the present invention;

[0038] Fig. 9 This is a SEM image of the radiation cooling device prepared in Example 3 of the present invention;

[0039] Fig.10 Detailed changes in the emissivity at different periods and microstructure heights calculated in Example 4 of the present invention;

[0040] Fig.11 Detailed changes in the emissivity of different dielectric layer thicknesses calculated in Example 5 of the present invention;

[0041] Fig.12 This is a SEM image of the hole structure when the development time is less than 5 seconds in Example 6 of the present invention. DETAILED DESCRIPTION

[0042] The present invention is described in further detail below.

[0043] Example 1

[0044] This embodiment provides a structure-colored photonic crystal radiation cooling device, including a double-layer micro-cone three-dimensional grating at the top and a multi-layer film structure at the bottom, wherein the busbars of the micro-cone three-dimensional gratings at the top and bottom layers are at different angles with the bottom surface, and the bottom multi-layer film structure includes a metal layer, a dielectric layer and a substrate from bottom to top. The basic structure is as follows Figure 1 As shown, Figure 1 Middle left picture: SiO 2 Double-layer micro-truncated cone three-dimensional grating array, with a multi-layer film structure underneath; Figure 1 Right picture in A: The upper part is SiO 2 Double-layer micro-truncated cone 3D grating, the lower part in A is MgF 2 layer, covered with SiO 2 The interior of the double-layer micro-truncated cone 3D grating; B is SiO 2 Substrate, C and D are Si 3 N 4 and Ag film. The angle between the upper micro-truncated cone 3D grating busbar and the bottom surface of this embodiment is 70°, the angle between the lower micro-truncated cone 3D grating busbar and the bottom surface is 40°, the period of the double-layer micro-truncated cone 3D grating structure is 5μm, and the average reflectivity of the solar spectrum and the average emissivity of the atmospheric window are calculated to be 0.929 and 0.931 respectively. The preparation process includes the following steps:

[0045] (1) The selected size is 30×30×0.5mm 3 SiO 2 The substrate is ultrasonically cleaned in an ethanol solution, taken out, rinsed with deionized water, and then dried;

[0046] (2) In SiO 2 A layer of NR77-6000PY negative photoresist was spin-coated on the substrate, and then pre-baked on a hot plate at 120°C for 120 seconds. The spin-coating parameters are shown in Table 1 below:

[0047] Table 1

[0048] step Speed / rpm Spinning time / s <![CDATA[Acceleration / rpm·s -1 > 1 4000 1 4000 2 5000 40 4000 3 0 3 2000

[0049] (3) A photolithography machine was used to perform contact exposure for 0.4 s under the mask, with a mask period of 5 μm, followed by post-baking on a hot plate at 120° C. for 90 s. The micro-cone angle combinations obtained under these parameters were 40° and 70°.

[0050] (4) Soak in 2.38% TMAH aqueous solution for 6 seconds to obtain SiO 2 SEM images of micro-grating complementary structures constructed on the substrate surface, such as Figure 2 As shown;

[0051] (5) Deposit 1.6 μm thick MgF at an evaporation rate of 0.15 nm / s 2 After degumming in Remover PG solution at 75°C, SiO2 with the same thickness was deposited at a speed of 0.88 nm / s. 2 , Si with a thickness of 1 μm is deposited on the back 3 N 4 The thickness is 100nmAg, and the speed is 0.3nm / s and 0.2nm / s respectively. The SEM image of the prepared photonic crystal radiation cooling device is obtained, as shown in Figure 3 shown.

[0052] Figure 4 The spectral characterization curve of the prepared structure-colored photonic crystal radiation cooling device and the multilayer film structure under the same deposition conditions. The multilayer film structure under the same deposition conditions is used as a comparison. The average reflectivity of the solar spectrum band is 0.95, and the average infrared emissivity is 0.95; according to Kirchhoff's law, the emissivity is equal to the absorptivity, that is, ε=A=1–T–R. Average reflectivity of the solar spectrum band and infrared average emissivity It can be calculated according to the following formula:

[0053]

[0054] Among them, refers to the standard solar spectrum irradiance AM1.5G (Global tilted irradiation AM1.5), R(λ) refers to the spectral reflectance of the sample, and I bb (T,λ) refers to the standard black body spectral radiation intensity when the temperature is T, ε(T,λ) refers to the sample spectral emissivity, and other bands can be calculated by changing the integration interval. The Planck coefficient h=6.626×10 -34 J s, speed of light c = 2.998 × 10 8 ms -1 , Stefan-Boltzmann constant k = 1.381×10 -23 JK -1 .

[0055] Figure 5 The fabricated structure-colored photonic crystal radiative cooling device is comparable to the SiO2 coated with silver only. 2 The emissivity comparison of the substrate in the local infrared band shows that the bulk SiO 2 The impedance mismatch is greatly reduced and the emissivity is greatly improved.

[0056] Figure 6 The theoretical radiative cooling power curve of the fabricated structure-colored photonic crystal radiative cooling device under different non-radiative heat transfer coefficients. It can be seen from the figure that the net cooling power per unit area is expected to be 147.1 Wm -2 Theoretical radiative cooling power P cooling It can be calculated according to the following formula:

[0057] P cooling (T cool )=P rad (T cool )-P solar -P atm (T amb )-P cond+conv (T cool ,T amb )

[0058] Among them, P solar is the solar radiation power absorbed by the radiation cooler surface, P rad is the thermal radiation power absorbed by the surface, P atm is the atmospheric radiation power absorbed by the surface, P cond+conv is the non-radiative heat transfer power, T cool is the surface temperature of the radiation cooler, T amb is the ambient air temperature. Specifically:

[0059]

[0060] ε atm =1-t(λ)1 / cosθ

[0061] P cond+conv (T cool ,T amb )=h c (T amb -T cool )

[0062] Where Ω is the solid angle, θ is the zenith angle, and the atmospheric emissivity ε atm =1-t(λ) 1 / cosθ , t is the spectral transmittance, h c is the non-radiative heat transfer coefficient.

[0063] Figure 7 Color map of the photonic crystal that colors the structure under strong sunlight at different angles, showing red, yellow, green and blue as the angle changes.

[0064] Example 2

[0065] Based on Example 1, the angle combination of the top double-layer microstructure is modified. Figure 8 The detailed changes in the emissivity of the angle combinations of 30° and 60°, 30° and 70°, 40° and 60°, and 40° and 70° are shown. This set of data is based on the control of the bottom diameter of the micro-cone structure, and the average emissivity calculated is 0.900, 0.913, 0.919, and 0.931. It can be seen that when the angle range between the lower and upper truncated cone generatrix and the bottom surface is 30° to 40° and 60° to 70°, respectively, the obtained radiation cooling device has a good infrared broadband emission effect, among which the 40°-70° combination has the best effect.

[0066] Example 3

[0067] During the preparation process, modifying the photoresist spin coating speed and exposure time can accurately control the undercut angle of the cavity complementary structure and the height of the vertical part of the cavity bottom, thereby achieving different angle combinations of the double-layer microstructure. Based on the preparation process of Example 1, the photoresist spin coating speed was modified to 4500rpm, and the exposure time was modified to 0.4s. The SEM image of the prepared radiation cooling device is as follows: Fig. 9 shown.

[0068] Example 4

[0069] Based on Example 1, the periodic size and height of the top microstructure array are modified to perform calculations respectively. Fig.10The detailed changes in emissivity when the period is 4μm, 5μm, 6μm, 7μm and the height is 2μm. It can be seen that the emissivity will first increase and then decrease with the increase of the period, but it can perfectly cover the working band and has a good average emissivity, and the effect is best at 5μm. The microstructure array height can achieve good broadband emission effects in the range of 1.6 to 2μm.

[0070] Example 5

[0071] Based on Example 1, the thickness of the dielectric layer is modified, and the calculation result of the infrared emissivity of the atmospheric window is as follows: Fig.11 As shown. When the thickness is 0.5μm, 1μm and 1.2μm, the emission characteristics are slightly different, but they all have good performance, and the average emissivity can reach above 0.9. The dielectric layer material has strong transmittance in the solar spectrum band. When the thickness reaches 1.2μm, the average reflectivity of the solar spectrum of the cooler is still 0.926, so that both reflectivity and emissivity performance can be guaranteed.

[0072] Example 6

[0073] On the basis of Example 1, the developing time was modified. When the developing time was less than 5 s, the colloid in the unexposed area did not react sufficiently with the developer, and a clear cavity structure could not be obtained. In this state, the SEM image was as follows: Fig.12 As shown; when the development time is higher than 6s, the colloid in the unexposed area reacts with the developer. The longer the development time, the stronger the overdevelopment effect, which will destroy the complete hole structure and cause partial or overall structure shedding. The best development time is 5-6s, which can obtain an ideal hole structure.

Claims

1. A structurally colored photonic crystal radiation cooling device, characterized in that: It includes a double-layer micro-cone three-dimensional grating at the top and a multi-layer film structure at the bottom, wherein the busbars of the micro-cone three-dimensional gratings in the upper and lower layers have different angles with the bottom surface, and the bottom multi-layer film structure includes a metal layer, a dielectric layer and a substrate from bottom to top.

2. The structurally colored photonic crystal radiation cooling device according to claim 1, characterized in that: The angle between the three-dimensional grating busbar of the upper micro-cone and the bottom surface is 60°~70°, and the angle between the three-dimensional grating busbar of the lower micro-cone and the bottom surface is 30°~40°; the period of the double-layer micro-cone three-dimensional grating is 4~7μm.

3. The structurally colored photonic crystal radiation cooling device according to claim 1, characterized in that: The metal layer is at least one of Ag, Au and Al, and the dielectric layer material is Si3N4 and / or HfO2.

4. A method for preparing the structurally colored photonic crystal radiation cooling device as claimed in claim 1, characterized in that: The following steps are involved: (1) Cleaning and drying the substrate; (2) Spin-coating a layer of photoresist on the substrate, pre-baking, then performing contact exposure under a mask, and then post-baking; After post-baking, the substrate is developed in a developer to obtain a substrate having a micro-grating complementary structure constructed on the surface; (3) evaporating a layer of MgF2 on the surface of the substrate having a micro-grating complementary structure, and then immersing the substrate in a degumming solution to remove the residual photoresist to obtain a substrate having a MgF2 microstructure deposited on the surface; (4) Using ion enhanced chemical vapor deposition, SiO2 is deposited on the surface of a substrate with a MgF2 microstructure and a bottom dielectric layer is deposited. Then, a metal layer is evaporated on the dielectric layer to obtain a structurally colored photonic crystal radiation cooling device.

5. The method for preparing the structurally colored photonic crystal radiation cooling device according to claim 4, characterized in that: In step (2), the contact exposure time is 0.4 to 0.5 s.

6. The method for preparing the structurally colored photonic crystal radiation cooling device according to claim 4, characterized in that: In step (2), the developer is a 2.38% TMAH aqueous solution, and the development time is 5 to 6 seconds.

7. The method for preparing the structurally colored photonic crystal radiation cooling device according to claim 4, characterized in that: The MgF2 evaporation thickness in step (3) is 1.6 to 2 μm.

8. The method for preparing the structurally colored photonic crystal radiation cooling device according to claim 4, characterized in that: In step (2), the pre-baking temperature is 90-120° C. and the time is 120-150 seconds; the post-baking temperature is 90-120° C. and the time is 90-120 seconds.

9. The method for preparing the structurally colored photonic crystal radiation cooling device according to claim 4, characterized in that: In step (2), the photoresist spin coating speed is 4500-5000 rpm.

10. The method for preparing the structurally colored photonic crystal radiation cooling device according to claim 4, characterized in that: In step (4), the deposition thickness of SiO2 is consistent with the thickness of MgF2, the deposition thickness of the dielectric layer is 0.5-1.2 μm, and the deposition thickness of the metal layer is greater than 100 nm.

Citation Information

Patent Citations

  • Thick radiation sensitive devices

    CA2495304A1

  • Multi-component gas concentration measurement method based on photonic crystal groove waveguide

    CN103091268A

  • Polarization-controllable color radiation refrigeration metamaterial and preparation method and application thereof

    CN117073255A

  • RADIATION DEVICE

    DE3423895A1

  • Electromagnetic radiation transmitter / reflector device, apparatus and method therefor

    KR1020000022392A

Cited By

  • Radiation refrigeration cement-based material with metasurface as well as preparation method and application of radiation refrigeration cement-based material

    CN120004577A