Secondary battery

By setting up lithium supplement agents in the positive electrode sheet and optimizing its distribution parameters, the problem of lithium-ion secondary batteries taking into account compatibility and stability in lithium supplement technology is solved, and excellent long-cycle and rate performance is achieved, which is suitable for long-term use. Fast charging application.

CN118983544APending Publication Date: 2024-11-19SUNWODA MOBILITY ENERGY TECHNOLOGY CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411048361.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

While the existing lithium-ion secondary battery lithium replenishment technology improves the battery service life, it is difficult to take into account the compatibility and stability of the electrode sheet active materials and electrolytes, and negative phenomena such as gas production and lithium extraction are prone to occur, especially in a long time. Poor performance in the charging scenario.

Method used

The lithium supplement agent is installed in the positive electrode diaphragm of the positive electrode sheet, and the relationship range between the non-Faraday capacitance, spherical degree, particle dispersion and particle size distribution is optimized to improve the effective compaction density of the positive electrode sheet and reduce the electrolysis The contact reaction area of ​​the liquid reduces the risk of gas production and lithium extraction.

Benefits of technology

It realizes the excellent long-cycle performance and rate performance of the secondary battery, which is suitable for long-term fast charging scenarios, improves the safety and stability of the battery, and avoids overvoltage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004975732470000111
    Figure BDA0004975732470000111
  • Figure BDA0004975732470000121
    Figure BDA0004975732470000121
  • Figure BDA0004975732470000122
    Figure BDA0004975732470000122
Patent Text Reader

Abstract

The invention discloses a secondary battery, and belongs to the technical field of batteries. According to the secondary battery disclosed by the invention, the lithium supplementing agent is arranged in the positive pole diaphragm of the positive pole piece, and meanwhile, the effective compaction density of the positive pole piece is effectively improved by optimizing and regulating the non-Faraday capacitance of the positive pole piece and the relationship interval of the sphericity degree, the particle dispersity and the particle size distribution of the lithium supplementing agent, so that the effective compaction density of the positive pole piece is effectively improved while the electrolyte is fully infiltrated; and the contact reaction area with electrolyte is reduced, so that the lithium precipitation risk in the cycle process of the secondary battery is reduced, and the secondary battery has excellent long cycle performance and rate capability and is suitable for being applied to a long-time quick charge scene.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of battery technology, and in particular to a secondary battery. Background Art

[0002] Lithium replenishment technology for lithium-ion secondary batteries is to replenish additional lithium to the battery through physical or electrochemical means to compensate for the irreversible active lithium lost during the preparation and charge-discharge cycle, thereby achieving the purpose of extending the battery life. However, in the actual application process, in addition to considering the amount of lithium replenishment, the lithium replenishment method also needs to consider the compatibility and stability with components such as the electrode active material and the electrolyte. In other words, while improving the product's charge-discharge performance, it is also necessary to ensure that the product will not produce negative phenomena such as gas production and lithium precipitation. Summary of the invention

[0003] The purpose of the present application is to overcome the deficiencies of the prior art and provide a secondary battery. The secondary battery of the present application is based on setting a lithium supplement agent in the positive electrode membrane of the positive electrode plate, and at the same time, by optimizing and regulating the non-Faraday capacitance of the positive electrode plate and the relationship range of the sphericity, particle dispersion and particle size distribution of the lithium supplement agent, the effective compaction density of the positive electrode plate is effectively improved, and overpressure will not occur. The positive electrode material in the positive electrode plate is subjected to little stress during the processing process, and can be fully infiltrated with the electrolyte while reducing the contact reaction area with the electrolyte, thereby reducing the risk of gas production and lithium precipitation during the cycle, so that the secondary battery has excellent long cycle performance and rate performance, and is suitable for application in long-term fast charging scenarios.

[0004] To achieve the above-mentioned object, in a first aspect of the present application, the present application provides a secondary battery, comprising a positive electrode plate, wherein the positive electrode plate comprises a current collector and a positive electrode film, wherein the positive electrode film comprises a positive electrode material and a lithium supplement;

[0005] The positive electrode sheet satisfies: 1.8≤10×Cdl×Sp×N / Dv 99 ≤22;

[0006] Wherein, the Cdl nF is the non-Faraday capacitance of the positive electrode plate;

[0007] The Sp is the sphericity of the lithium supplement;

[0008] The N is the particle dispersion of the lithium supplement;

[0009] Dv 99 μm is the particle size corresponding to when the cumulative particle size distribution number of the lithium supplement reaches 99% based on the volume standard.

[0010] As an embodiment of the present application, the positive electrode material includes at least one of lithium iron phosphate, lithium manganese phosphate, lithium manganese iron phosphate, lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, and lithium nickel cobalt manganese oxide.

[0011] As an embodiment of the present application, the lithium supplement includes at least one of Li5FeO5, Li6CoO4, Li2NiO2, Li2MnO3, Li2MoO3, Li2DHBN, and Li2C2O4.

[0012] As an embodiment of the present application, the secondary battery satisfies at least one of the following conditions:

[0013] (1) 0.6nF ≤ Cdl nF ≤ 1.8nF;

[0014] (2) 0.5 ≤ Sp ≤ 0.9;

[0015] (3) 10≤N≤20;

[0016] (4) 6μm≤Dv 99 μm≤20μm

[0017] As an embodiment of the present application, the positive electrode material satisfies at least one of the following conditions:

[0018] (1) 0.1μm≤Dv' 10 μm≤0.5μm;

[0019] (2) 0.6μm≤Dv' 50 μm≤1.5μm;

[0020] (3) 1μm≤Dv' 99 μm≤10μm;

[0021] The Dv' 10 μm is the particle size corresponding to 10% of the cumulative particle size distribution of the positive electrode material based on the volume standard;

[0022] The Dv' 50 μm is the particle size corresponding to 50% of the cumulative particle size distribution of the positive electrode material based on the volume standard;

[0023] The Dv' 99 μm is the particle size corresponding to 99% of the cumulative particle size distribution of the positive electrode material based on the volume standard.

[0024] As an embodiment of the present application, the mass content of the lithium supplement agent in the positive electrode membrane is 0.3-5wt%.

[0025] As an embodiment of the present application, the secondary battery further comprises a negative electrode sheet, wherein the negative electrode sheet comprises a current collector and a negative electrode membrane;

[0026] The secondary battery satisfies: 0.1≤(H1-H2) / H2≤0.4;

[0027] The H1 μm is the thickness of the positive electrode membrane, and H2 μm is the thickness of the negative electrode membrane.

[0028] As an embodiment of the present application, the H1μm satisfies: 90μm≤H1μm≤250μm;

[0029] The H2 satisfies: 70 μm≤H2 μm≤180 μm.

[0030] As an implementation scheme of the present application, the positive electrode material is further provided with a coating layer, and the coating layer includes at least one of a carbon element, a metal oxide, and a solid electrolyte.

[0031] As an embodiment of the present application, the positive electrode sheet satisfies: 1.2≤C×Sp / Dv 99 ≤11.5; wherein C nm is the thickness of the coating layer

[0032] As an embodiment of the present application, 25 nm ≤ C nm ≤ 200 nm.

[0033] In a second aspect of the present application, the present application provides an electrical device, comprising the secondary battery, wherein the secondary battery serves as a power supply for the electrical device.

[0034] The beneficial effects of this application are:

[0035] The present application provides a secondary battery, which is based on setting a lithium supplement agent in a positive electrode film of a positive electrode plate, and optimizing and controlling the non-Faraday capacitance of the positive electrode plate and the relationship range of the sphericity, particle dispersion and particle size distribution of the lithium supplement agent, thereby effectively improving the effective compaction density of the positive electrode plate and preventing overpressure. The positive electrode material in the positive electrode plate is subjected to little stress during the processing process, and can be fully infiltrated with the electrolyte while reducing the contact reaction area with the electrolyte, thereby reducing the risk of gas production and lithium precipitation during the cycle, so that the secondary battery has excellent long cycle performance and rate performance, and has ideal fast charging performance. DETAILED DESCRIPTION

[0036] In order to make the purpose, technical solutions and advantages of the embodiments of the present application clearer, the technical solutions in the embodiments of the present application are described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.

[0037] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0038] In this application, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values ​​of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0039] The present application is further described below with specific embodiments:

[0040] The embodiment of the present application provides a secondary battery, including a positive electrode plate, wherein the positive electrode plate includes a current collector and a positive electrode film, and the positive electrode film contains a positive electrode material and a lithium supplement;

[0041] The positive electrode sheet satisfies: 1.8≤10×Cdl×Sp×N / Dv 99 ≤22;

[0042] Wherein, the Cdl nF is the non-Faraday capacitance of the positive electrode plate;

[0043] The Sp is the sphericity of the lithium supplement;

[0044] The N is the particle dispersion of the lithium supplement;

[0045] Dv 99 μm is the particle size corresponding to when the cumulative particle size distribution number of the lithium supplement reaches 99% based on the volume standard.

[0046] More preferably, 10×Cdl×Sp×N / Dv 99 A range of one or both of 1.8, 2, 3, 3.7, 4, 4.1, 4.5, 5, 5.4, 5.9, 6, 6.2, 7, 7.1, 7.4, 7.5, 8, 9, 9.2, 9.5, 9.6, 9.9, 10, 10.5, 11, 11.9, 12, 15, 18, 20, 22.

[0047] The improvement effect of existing lithium replenishment technology on secondary batteries involves multiple aspects. In addition to the adaptability of lithium replenishment materials, the type of lithium replenishment, the energy density of the overall electrode, the capacitance setting, etc. will also affect the lithium replenishment effect of the lithium replenishment and even the safety of the entire secondary battery. Therefore, based on the regulation of the sphericity, particle dispersion and particle size distribution range of the lithium replenishment agent and the non-Faraday capacitance of the overall electrode, the relationship ratio is established to achieve the dual effect of improving the safety and expansion performance of the secondary battery. The non-Faraday capacitance is the ability of the active material in the electrode to store charge in the electrolyte through physical adsorption or ion intercalation. The higher the non-Faraday capacitance, the higher the instantaneous charging power and instantaneous power output of the secondary battery. However, when controlling the size of the Faraday capacitance, the safety and stability of the positive electrode material and the lithium replenishment effect of the lithium replenisher must also be taken into account. On the other hand, the higher the sphericity of the lithium replenisher, the closer the particles of the lithium replenisher are to spherical, the lower the surface free energy of the particles and the more uniform the charge distribution, the lower the degree of particle aggregation, and the larger the contact area with the electrolyte, which in turn affects the electrochemical reaction and cycle stability of the battery. The particle size of the lithium replenisher is also related to its specific surface area. In theory, smaller particles have a larger specific surface area, and the lithium replenisher particles are also easier to release and replenish active lithium, but the probability of recrystallization of small particles of lithium replenisher will also increase. In addition, the particle size and dispersion of the lithium replenisher will also affect the compaction density of the electrode. Therefore, by optimizing 10×Cdl×Sp×N / Dv 99 When the range is between 1.8 and 26, the positive electrode plate in the obtained secondary battery can be fully wetted by the electrolyte, and the lithium replenisher on the plate can fully release the compensating lithium while ensuring safety and stability, so that the secondary battery has excellent rate performance and long cycle performance.

[0048] In some embodiments, the positive electrode material includes at least one of lithium phosphate and lithium transition metal oxide, for example, it can be at least one of lithium iron phosphate, lithium manganese phosphate, lithium manganese iron phosphate, lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, and nickel cobalt manganese oxide.

[0049] In some embodiments, the positive electrode material satisfies: 0.1 μm ≤ Dv' 10 μm≤0.5μm; Dv' 10 μm is the particle size corresponding to 10% of the cumulative particle size distribution of the positive electrode material based on the volume standard;

[0050] Further preferably, Dv' 10 μm is a range value of one or any two of 0.1 μm, 0.15 μm, 0.2 μm, 0.25 μm, 0.3 μm, 0.35 μm, 0.4 μm, 0.45 μm, and 0.5 μm.

[0051] In some embodiments, the positive electrode material satisfies: 0.6 μm ≤ Dv'10 μm≤1.5μm; Dv' 10 μm is the particle size corresponding to 10% of the cumulative particle size distribution of the positive electrode material based on the volume standard;

[0052] Further preferably, Dv' 50 μm is a range value of one or any two of 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, 1 μm, 1.2 μm, 1.3 μm, and 1.5 μm.

[0053] In some embodiments, the positive electrode material satisfies: 1 μm ≤ Dv' 99 μm≤10μm;

[0054] The Dv' 99 μm is the particle size corresponding to 99% of the cumulative particle size distribution of the positive electrode material based on the volume standard;

[0055] Further preferably, Dv' 99 μm is a range value of one or any two of 1 μm, 1.5 μm, 2 μm, 3 μm, 4 μm, 5 μm, 8 μm, 9.5 μm, and 10 μm.

[0056] Dv' of positive electrode material 10 、Dv' 50 、Dv' 99 When within the above range, the positive electrode material can have a suitable specific surface area, ensuring that the contact area between the electrolyte and the positive electrode material is moderate, which is beneficial to reducing the diffusion path of lithium ions and reducing the diffusion resistance of lithium ions, thereby making the battery have better electrochemical performance.

[0057] In some embodiments, the lithium supplement includes at least one of Li5FeO5, Li6CoO4, Li2NiO2, Li2MnO3, Li2MoO3, Li2DHBN, and Li2C2O4.

[0058] In some embodiments, the mass content of the lithium supplement agent in the positive electrode film is 0.3-5 wt %.

[0059] Further preferably, the mass content of the lithium supplement in the positive electrode membrane is in the range of one or any two of 0.3wt%, 0.5wt%, 0.8wt%, 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt%, 4.5wt%, 5wt%.

[0060] In some embodiments, the non-Faraday capacitance of the positive electrode plate satisfies:

[0061] 0.6nF≤Cdl nF≤1.8nF;

[0062] Further preferably, the non-Faraday capacitance Cdl nF of the positive electrode plate is in the range of one or any two of 0.6nF, 0.8nF, 1nF, 1.2nF, 1.4nF, 1.5nF, 1.8nF.

[0063] The non-faradaic capacitance of the positive electrode plate is related to the fast charging capability and service life of the secondary battery. When the non-faradaic capacitance is within the above range, the positive electrode material in the secondary battery can be protected from strong current attacks, have a long service life, and can enhance the relationship between the positive electrode material and the lithium replenisher, thereby improving the fast lithium deintercalation capability of the positive electrode material and the lithium replenishment performance of the lithium replenisher.

[0064] In some embodiments, the test method of the non-Faradaic capacitance of the positive electrode sheet in the secondary battery is as follows: two positive electrode sheets and a conventional electrolyte are assembled into a symmetrical battery, and then a first test is performed by cyclic voltammetry, with a test voltage of 0.05 to 3V and a scan rate of 0.1 to 2mV / s, and then according to the first test result, a potential interval of the straight section of the result curve is selected for a secondary test, with a test voltage of 2.5 to 2.7V and a scan rate of 0.1 to 20mV / s, and finally, the median U of the potential interval of any five specific scan rates in the second test (exemplarily, the specific scan rate can be five points of 0.1mV / s, 1mV / s, 5mV / s, 10mV / s and 20mV / s, or other scan rates) is selected, and the corresponding current value is obtained, and a scan rate-current scatter plot is obtained by plotting the five data and fitting a linear function, and the slope of the linear function is calculated, and the result obtained is the non-Faradaic capacitance value of the positive electrode sheet.

[0065] In some embodiments, the sphericity Sp of the lithium supplement meets the following conditions: 0.5≤Sp≤0.9;

[0066] More preferably, the sphericity Sp of the lithium supplement is in the range of one or any two of 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.76, 0.77, 0.78, 0.79, 0.8, 0.85, and 0.9.

[0067] The sphericity of the lithium supplement is related to its dispersion and bonding strength when distributed in the electrode, and extends to the overall contact area after the positive electrode contacts the electrolyte. Therefore, it is related to the electrochemical reaction and cycle stability of the secondary battery. When the sphericity of the lithium supplement is within the above range, the particles of the lithium supplement in the positive electrode have high dispersion and strong bonding ability, and the degree of lithium supplementation is high and it is not easy to fall off.

[0068] In some embodiments, the sphericity Sp of the lithium supplement is obtained by dynamic image particle analyzer analysis, and the specific method is: Winner100 is used to identify and analyze the positive electrode material at a magnification of 100 to 500, and the sphericity of the lithium supplement is calculated and counted by software, and the number of lithium supplement particles is analyzed to be ≥500.

[0069] In some embodiments, the particle dispersion N of the lithium supplement agent satisfies: 10≤N≤20;

[0070] More preferably, the particle dispersion N of the lithium supplement is in the range of one or any two of 10, 11, 12, 13, 14, 15, 16, 18, and 20.

[0071] In some embodiments, the particle dispersion N of the lithium supplement is calculated as follows:

[0072] N=(D v99 -D v10 ) / D v50 ;

[0073] The Dv 10 μm is the particle size corresponding to when the cumulative particle size distribution of the lithium supplement reaches 10% based on the volume standard;

[0074] The Dv 50 μm is the particle size corresponding to when the cumulative particle size distribution number of the lithium supplement reaches 50% based on the volume standard.

[0075] In some embodiments, the Dv of the lithium supplement is 99 μm satisfies: 6μm≤Dv 99 μm≤20μm;

[0076] Further preferably, the Dv of the lithium supplement is 99 μm is a range value of one or any two of 6 μm, 8 μm, 10 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 18 μm, and 20 μm.

[0077] Particle dispersion of lithium supplement and its particle size Dv 99 It directly affects the specific surface area of ​​the positive electrode plate prepared by it. The lithium supplement agent with small particles and large dispersion can provide a larger reaction contact area for the plate and a greater density, which is also helpful for compensating lithium release of the lithium supplement agent. Larger and more concentrated lithium supplement agents can ensure the structural stability of the lithium supplement agent and the bonding strength of the electrode material. When the particle dispersion and particle size of the lithium supplement agent are within the above range, the secondary battery has ideal cycle stability and lithium supplement activity.

[0078] In some embodiments, the secondary battery further comprises a negative electrode sheet, wherein the negative electrode sheet comprises a current collector and a negative electrode membrane;

[0079] The secondary battery satisfies: 0.1≤(H1-H2) / H2≤0.4;

[0080] The H1 μm is the thickness of the positive electrode membrane, and H2 μm is the thickness of the negative electrode membrane.

[0081] More preferably, the H1μm is a range value of one or any two of 30μm, 40μm, 50μm, 80μm, 100μm, 120μm, 150μm, 180μm, 200μm, 220μm, 230μm, and 250μm.

[0082] Further preferably, the H2μm is a range value of one or any two of 20μm, 30μm, 50μm, 80μm, 100μm, 120μm, 150μm, 180μm, 200μm, 205μm, and 210μm.

[0083] In the secondary battery described in the present application, based on the design of the lithium replenisher in the positive electrode plate, a suitable thickness correspondence between the positive electrode plate and its corresponding negative electrode film layer is constructed, which can make the lithium deintercalation and lithium replenishment in the secondary battery more sufficient and complete, and effectively inhibit the battery gas production and lithium plating of the plate.

[0084] In some embodiments, the positive electrode material is further provided with a coating layer, the coating layer includes at least one of a carbon element, a metal oxide, and a solid electrolyte, and the positive electrode sheet satisfies: 1.2≤C×Sp / Dv 99 ≤11.5;

[0085] Wherein, C nm is the thickness of the coating layer.

[0086] Further preferably, the thickness C nm of the coating layer is within the range of one or any two of 25 nm, 30 nm, 50 nm, 60 nm, 70 nm, 80 nm, 100 nm, 120 nm, 150 nm, 180 nm, and 200 nm.

[0087] The positive electrode material serves as the main body of lithium deintercalation and lithium replenishment. After the coating layer is set, its conductivity and stability can be effectively improved. The coating layer and its thickness are related to the bonding strength of the lithium replenisher on the positive electrode plate and the lithium replenishment efficiency. When the relationship between the coating layer thickness of the positive electrode material and the sphericity and particle size of the lithium replenisher is within the above range, the coating layer has a low impact on the lithium replenisher, the lithium replenisher can fully release and compensate for the active lithium, and can also maintain a larger electrode contact area.

[0088] In some implementation places, the thickness C nm of the coating layer is tested by ultra-thin sectioning / TEM scanning analysis of the positive electrode film of the positive electrode plate.

[0089] The test method is:

[0090] (1) First, the cathode material with a coating layer needs to be made into ultra-thin slices with a thickness of 50 to 300 nm, and a TEM sample is made through processes such as embedding, curing, cutting, and slicing;

[0091] (3) Place the sample on the TEM sample holder and enter the TEM test;

[0092] (3) Open the test data in the TEM software, select the boundary between the bottom layer and the coating layer, measure the thickness of the coating layer, and select at least 10 positions for measurement to ensure the accuracy of the measurement results;

[0093] (4) Record and calculate the average results of all measurements to obtain the value C nm of the coating layer.

[0094] In some embodiments, the secondary battery further includes an electrolyte, the electrolyte including a first additive and a second additive;

[0095] The first additive includes at least one of vinylene carbonate and vinyl ethylene carbonate;

[0096] The second additive includes at least one of LiFSI, LiODFB, LiPO2F2, LiBF4, and LiBOB.

[0097] The present application is further described below with specific examples, which are not to be construed as limiting the scope of protection claimed in the present application:

[0098] Example 1

[0099] A secondary battery comprises a positive electrode sheet, a negative electrode sheet and an electrolyte.

[0100] The method for preparing the positive electrode sheet comprises the following steps:

[0101] The positive electrode material is lithium iron phosphate (Dv' 10 、Dv' 50 、Dv' 99 0.2μm, 1.2μm, 8μm respectively), lithium supplement Li5FeO5 (Dv 99 14 μm), conductive carbon black, and binder PVDF are mixed in N-methylpyrrolidone in a mass ratio of 96.5:0.5:0.7:2.3 to prepare a slurry, which is then coated on a 14 μm carbon-coated aluminum foil, and then the electrode is dried, rolled, slit and cut to obtain a positive electrode sheet;

[0102] The method for preparing the negative electrode sheet comprises the following steps:

[0103] Graphite, conductive carbon black (SP), CMC and SBR were mixed evenly in a mass ratio of 96.5:0.5:1.1:2.1, and then the mixture was added into water and continued to be fully mixed to prepare negative electrode slurry, and the slurry was coated on both sides of 6μm copper foil. The obtained electrode sheet was dried, rolled, slit and cut to obtain a negative electrode sheet.

[0104] The positive electrode sheet and the negative electrode sheet are assembled into a secondary battery in a glove box with a PP separator and an electrolyte, and the secondary battery is prepared through shaping, baking, packaging, liquid injection, formation, and capacity division processes;

[0105] The preparation method of the electrolyte is: vinylene carbonate, ethyl methyl carbonate and propyl propionate are mixed in a mass ratio of 1:1:1, and then an appropriate amount of lithium hexafluorophosphate and an additive are added, wherein the additive is obtained by mixing vinylene carbonate and LiFSI in a mass ratio of 1:1, and the additive accounts for 2wt% of the electrolyte.

[0106] Embodiments 2 to 27

[0107] The secondary batteries provided in Examples 2 to 27 are substantially the same as those in Example 1, except that the parameters shown in Table 1 are changed.

[0108] Among them, the coating layer of the positive electrode material of Examples 23 to 26 is carbon-coated; and in each embodiment: the thickness H1 and H2 of the positive electrode membrane and the negative electrode membrane can be changed by adjusting the coating amount of the positive electrode slurry and the negative electrode slurry; the content n of the lithium supplement agent can be changed by adjusting the amount of the lithium supplement agent added in the positive electrode slurry; the sphericity Sp, particle dispersion N and D of the lithium supplement agent v99 It can be adjusted by jet ball milling and screening the lithium supplement; the non-Faraday capacitance Cdl of the positive electrode diaphragm can be adjusted by adjusting the content ratio of the positive electrode material in the positive electrode sheet, the particle size distribution of the positive electrode material, the compaction density of the positive electrode material powder, and the porosity and compaction density of the positive electrode sheet, and the positive electrode formula (such as the conductive agent content); when the positive electrode material in the positive electrode diaphragm is provided with a coating layer, the thickness C of the coating layer can be changed by adjusting the proportion of added carbon.

[0109] Comparative Examples 1 to 4

[0110] A secondary battery, which is different from Example 1 only in that the parameters shown in Table 1 are changed.

[0111] The parameters of each embodiment and comparative example are shown in Table 1.

[0112] Where X = 10 × Cdl × Sp × N / Dv 99;Y=(H1-H2) / H2;Z=C×Sp / Dv 99 , n is the mass content of lithium supplement in the positive electrode membrane.

[0113] Table 1

[0114]

[0115]

[0116] The secondary batteries prepared in the above embodiments and comparative examples were tested for performance respectively, and the specific methods are as follows:

[0117] (1) The secondary battery obtained in each embodiment and comparative example recorded the nominal discharge capacity C0, then cycled 8000 times at 25°C at a rate of 0.5C / 0.5C at an operating voltage of 2.5-3.65V, recorded the discharge capacity C after the cycle, and calculated the capacity retention rate by the following formula:

[0118] Capacity retention rate (%) = C / C0 × 100%;

[0119] (2) At 25° C., the secondary batteries obtained in each embodiment and comparative example were subjected to three charge-discharge cycles at a rate of 0.5C and 2.5 to 3.65V, and then the rate was increased to 1C and subjected to 10 charge-discharge cycles. The secondary batteries were then disassembled to observe the lithium deposition at the interface of the negative electrode plate. The secondary batteries were classified into four levels according to the degree of lithium deposition: no lithium deposition, slight lithium deposition, moderate lithium deposition, and severe lithium deposition, wherein no lithium deposition means that the lithium deposition area is less than 2%, slight lithium deposition means 2% to 10%, moderate lithium deposition means 10% to 30%, and severe lithium deposition means more than 30%;

[0120] (3) At 25°C, the secondary batteries obtained in each embodiment and comparative example were subjected to three charge-discharge cycles at a rate of 0.5C and 2.5-3.65V, and then the rate was increased to 3C and subjected to 10 charge-discharge cycles. The secondary batteries were then disassembled to observe the lithium deposition at the interface of the negative electrode plate. The secondary batteries were divided into four levels according to the degree of lithium deposition: no lithium deposition, slight lithium deposition, moderate lithium deposition and severe lithium deposition, wherein no lithium deposition means that the lithium deposition area is less than 2%, slight lithium deposition means 2%-10%, moderate lithium deposition means 10%-30%, and severe lithium deposition means more than 30%.

[0121] The test results are shown in Table 2.

[0122] Table 2

[0123]

[0124]

[0125]

[0126] From Table 2 we can see that:

[0127] When the secondary battery meets: 1.8≤10×Cdl×Sp×N / Dv 99 When ≤22, the secondary battery has ideal electrochemical properties, the capacity retention rate after 8000 cycles can reach more than 80%, and the secondary battery has high stability and safety. No lithium plating occurs after ten cycles of high-rate testing.

[0128] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that the technical solutions described in the above embodiments may still be modified, or some or all of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A secondary battery, characterized in that: It includes a positive electrode sheet, the positive electrode sheet includes a current collector and a positive electrode membrane, and the positive electrode membrane contains a positive electrode material and a lithium supplement; The positive electrode sheet satisfies: 1.8≤10×Cdl×Sp×N / Dv 99 ≤22; Wherein, the Cdl nF is the non-Faraday capacitance of the positive electrode plate; The Sp is the sphericity of the lithium supplement; N is the particle dispersion of the lithium supplement; Dv 99 μm is the particle size corresponding to when the cumulative particle size distribution number of the lithium supplement reaches 99% based on the volume standard.

2. The secondary battery according to claim 1, characterized in that: The positive electrode material includes at least one of lithium iron phosphate, lithium manganese phosphate, lithium manganese iron phosphate, lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, and nickel cobalt manganese oxide; And / or, the lithium supplement includes at least one of Li5FeO5, Li6CoO4, Li2NiO2, Li2MnO3, Li2MoO3, Li2DHBN, and Li2C2O4.

3. The secondary battery according to claim 1, characterized in that: The secondary battery satisfies at least one of the following conditions: (1) 0.6nF ≤ Cdl nF ≤ 1.8nF; (2) 0.5 ≤ Sp ≤ 0.9; (3)10≤N≤20; (4)6μm≤Dv 99 μm≤20μm。 4. The secondary battery according to claim 1, wherein: The positive electrode material satisfies at least one of the following conditions: (1)0.1μm≤Dv' 10 μm≤0.5μm; (2)0.6μm≤Dv' 50 μm≤1.5μm; (3)1μm≤Dv' 99 μm≤10μm; The Dv' 10 μm is the particle size corresponding to 10% of the cumulative particle size distribution of the positive electrode material based on the volume standard; The Dv' 50 μm is the particle size corresponding to 50% of the cumulative particle size distribution of the positive electrode material based on the volume standard; The Dv' 99 μm is the particle size corresponding to 99% of the cumulative particle size distribution of the positive electrode material based on the volume standard.

5. The secondary battery according to claim 1, characterized in that: The mass content of the lithium supplement agent in the positive electrode membrane is 0.3-5wt%.

6. The secondary battery according to claim 1, characterized in that: The secondary battery further comprises a negative electrode sheet, wherein the negative electrode sheet comprises a current collector and a negative electrode membrane; The secondary battery satisfies: 0.1≤(H1-H2) / H2≤0.4; The H1 μm is the thickness of the positive electrode membrane, and H2 μm is the thickness of the negative electrode membrane.

7. The secondary battery according to claim 1, characterized in that: The positive electrode material is also provided with a coating layer, and the coating layer includes at least one of carbon element, metal oxide, and solid electrolyte.

8. The secondary battery according to claim 7, characterized in that: The positive electrode sheet satisfies: 1.2≤C×Sp / Dv 99 ≤11.5; wherein C nm is the thickness of the coating layer.

9. The secondary battery according to claim 8, characterized in that: 25nm≤C nm≤200nm.

10. An electrical device, characterized in that: The invention comprises the secondary battery as claimed in claims 1 to 9, wherein the secondary battery is used as a power supply for the electrical device.

Citation Information

Patent Citations

  • Nonaqueous lithium power storage element

    CN108475588A

  • Lithium supplement agent for lithium ion battery as well as preparation method and application of lithium supplement agent

    CN114989059A

  • Lithium iron phosphate composite material containing lithium supplement agent, preparation method and application of lithium iron phosphate composite material and battery containing lithium iron phosphate composite material

    CN115353085A

  • Positive electrode lithium supplement agent, positive electrode lithium supplement pole piece prepared from positive electrode lithium supplement agent and lithium ion battery prepared from positive electrode lithium supplement agent

    CN115764010A

  • Secondary battery and battery pack

    CN117276538A