A cellulose inorganic composite film, a high temperature resistant battery separator and its preparation method and application
The cellulose inorganic composite film prepared by bacterial cellulose and composite powder solves the problems of polyolefin separators being prone to fracture and poor thermal stability at high temperatures, and achieves the improvement of high temperature resistance and electrochemical performance of lithium-ion batteries, which are suitable for high efficiency , safe lithium-ion battery separator.
Patent Information
- Application Number
- CN202111405836.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-24
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2041-11-24
AI Technical Summary
Existing polyolefin separators are prone to fracture at high temperatures, and have poor thermal stability and rate performance, which affects the cycle life and safety performance of lithium-ion batteries.
Cellulose inorganic composite membrane made of bacterial cellulose and composite powder is used as the battery separator. The composite powder includes organic polymer compounds and inorganic substances, and is prepared by ultrasonic dispersion and suction filtration membrane forming technology, with high mechanical strength and acid and alkali resistance. Corrosion performance.
It improves the high temperature resistance of lithium-ion batteries, adjustable membrane thickness, high ion conductivity, excellent electrochemical performance, extends the cycle life and safety performance of the battery and reduces production costs.
Smart Images

Figure BDA0003372192500000071 
Figure BDA0003372192500000072 
Figure HDA0003372192510000011
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium ion battery manufacturing, and specifically relates to a cellulose inorganic composite membrane, a lithium ion battery separator, and a preparation method and application thereof. Background Art
[0002] With the vigorous development of electric vehicles and energy storage industries, the research and development of lithium-ion batteries with large capacity, long life, high safety and fast charging has attracted widespread attention. Lithium-ion batteries have the characteristics of high energy density, long cycle life and no memory effect; they are also safe, environmentally friendly, reliable and can be charged and discharged quickly, so they have become a hot spot in technical research in recent years.
[0003] The battery separator is an important component of lithium-ion batteries. It not only provides an ion transmission channel for liquid batteries, but also prevents direct contact between the cathode and the anode, preventing the positive and negative electrodes of the battery from short-circuiting. At present, polyolefin separators have become the main separators due to their considerable mechanical strength, electrochemical stability and appropriate separator thickness. At present, commercial polyolefin separators are mainly polypropylene (PP), polyethylene (PE) and their combined films. However, separators such as polypropylene (PP) and polyethylene (PE) based on polymer polyolefins have several problems, such as poor battery rate performance and thermal stability of the separator, which affect the cycle life and safety performance of the battery. In the production process, this type of polyolefin battery separator is prone to breakage during the winding process and is prone to shrinkage when subjected to high temperatures. Therefore, the baking temperature before battery injection cannot be too high. Once it is too high, the separator will shrink severely, causing the battery to short-circuit, affecting the safety performance of the battery.
[0004] In recent years, the scientific community has been trying to develop a battery separator that can overcome the lower thermal stability and poor rate performance of commercial separators. Therefore, providing a high temperature resistant battery separator is a technical problem that needs to be solved urgently in this field. Summary of the invention
[0005] The purpose of the present invention is to provide a method for preparing a cellulose inorganic composite membrane.
[0006] Another object of the present invention is to provide a cellulose inorganic composite membrane prepared by the above preparation method.
[0007] Another object of the present invention is to provide the use of the above-mentioned cellulose inorganic composite film as a high temperature resistant battery separator.
[0008] Another object of the present invention is to provide a lithium ion battery, wherein the battery separator of the lithium ion battery is made of the above-mentioned cellulose inorganic composite film.
[0009] To achieve the above objectives, on the one hand, the present invention provides a cellulose-inorganic composite membrane, the components of which include bacterial cellulose and composite powder; the composite powder includes an organic polymer compound and an inorganic substance;
[0010] The mass ratio of bacterial cellulose to composite powder is 5-50:25-200;
[0011] The mass ratio of the organic polymer compound to the inorganic substance is 10-300:100-300.
[0012] Optionally, the mass ratio of bacterial cellulose to composite powder is 15:50, 15:100, 15:150, 25:50, 25:100, 25:150, 25:200, 35:50, 35:100, 35:150, 45:100, 45:150, 45:200, and any value between the above two points.
[0013] Optionally, the mass ratio of the organic polymer compound to the inorganic substance is 50:100, 50:150, 50:200, 50:250, 100:150, 100:250, 150:150, 150:200, 150:250, 200:100, 200:150, 200:250, 250:100, 250:150, 250:200, 250:300, and any value between the above two points.
[0014] Optionally, the organic polymer compound is selected from at least one of sodium alginate, carboxymethyl cellulose and polyacrylic acid;
[0015] The inorganic substance is selected from at least one of diatomaceous earth, zeolite, kaolin and montmorillonite.
[0016] Optionally, the thickness of the cellulose inorganic composite membrane is 20 to 90 μm, the porosity is 13% to 91%, and the liquid absorption rate is 0.17 to 0.36 g / cm 3 , heat-resistant temperature is above 400℃.
[0017] On the other hand, the present application provides a method for preparing the above-mentioned cellulose inorganic composite membrane, wherein a suspension containing bacterial cellulose and composite powder is formed into a membrane to obtain the cellulose inorganic composite membrane.
[0018] Optionally, in the suspension, the mass ratio of the bacterial cellulose to the composite powder is 5-50:25-200.
[0019] Optionally, the composite powder and bacterial cellulose are dispersed in anhydrous ethanol and ultrasonically treated for 30 to 50 minutes to obtain a uniformly dispersed suspension solution, which is then filtered to form a membrane.
[0020] The membrane formed by suction filtration is a self-supporting membrane, and the prepared cellulose inorganic composite membrane is filled with inorganic particles.
[0021] Optionally, the preparation method of the composite powder includes: mixing raw materials containing organic polymer compounds and inorganic substances with water, stirring, filtering, drying, and grinding to obtain the composite powder.
[0022] Optionally, the concentration of the organic polymer compound is 0.25 to 1 g / L; the concentration of the inorganic substance is 0.5 to 1.5 g / L.
[0023] Optionally, the inorganic material is vacuum dried at 100-120° C. for 10-12 hours before mixing;
[0024] The stirring time is 10 to 12 hours;
[0025] The drying is performed by vacuum drying at 100-120° C. for 10-12 hours.
[0026] Optionally, the bacterial cellulose needs to be pre-treated, and the pre-treatment includes grinding, crushing, and freeze-drying the cleaned bacterial cellulose.
[0027] Optionally, the cleaning of the bacterial cellulose comprises the following steps:
[0028] (a) stirring bacterial cellulose in a mixed solution of deionized water and ethanol for 24 hours as one treatment, and repeating it three times;
[0029] (b) stirring the bacterial cellulose obtained in step (a) in an alkaline solution in an oil bath at 50 to 60° C. for 6 to 8 hours, and then washing with deionized water until neutral;
[0030] (c) stirring the bacterial cellulose obtained in step (b) in a mixed solution of deionized water and ethanol for 24 hours, repeating the treatment three times;
[0031] The volume ratio of deionized water to ethanol is 1:1.
[0032] Optionally, the alkaline solution is selected from one of 0.1 mol / L sodium hydroxide or potassium hydroxide solutions.
[0033] On the other hand, the present application provides an application of the above-mentioned cellulose inorganic composite membrane and the cellulose inorganic composite membrane prepared by the above-mentioned preparation method as a battery separator, and the battery separator has good high temperature resistance.
[0034] Among them, "high temperature resistant" means that the battery separator can still maintain its original safety performance under high temperature conditions.
[0035] On the other hand, the present application provides a lithium-ion battery, wherein the battery separator of the lithium-ion battery is prepared from the above-mentioned cellulose inorganic composite membrane or the cellulose inorganic composite membrane obtained by the above-mentioned preparation method.
[0036] The beneficial effects of the present invention include:
[0037] The high temperature resistant battery separator provided by the present invention is composed of organic polymer fibers, organic polymers and inorganic materials, and has strong mechanical strength and good acid and alkali corrosion resistance. The thickness of the separator is adjustable (20-90 μm) without affecting the normal performance of the battery; the separator can be bent arbitrarily, and is particularly suitable for wearable batteries.
[0038] The high temperature resistant battery separator provided by the present invention not only has the function of isolating the positive and negative electrodes, but also has a guiding effect on lithium ions. It has high ion conductivity and good wettability to organic electrolytes, ensuring the orderly transmission of liquids, so that the composite separator has both excellent physical properties and electrochemical properties, thereby improving the battery rate performance and long-term shelf performance.
[0039] The high temperature resistant battery diaphragm obtained by the present invention has a simple preparation method, a pollution-free process, low commercialization cost, and flexible operation, and is particularly suitable for low-cost large-scale energy storage lithium-ion battery systems; the diaphragm has high porosity and liquid absorption rate, which is more conducive to the infiltration of electrolytes and ion migration; the diaphragm has excellent thermal stability, which greatly improves the safety performance of lithium-ion batteries; after the diaphragm is applied to lithium-ion batteries, it exhibits better long cycle performance and rate cycle performance, and is a very potential diaphragm for lithium-ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 This is a scanning electron microscope image of the high temperature resistant battery separator in Example 4 of the present invention.
[0041] Figure 2 This is a TGA curve diagram of the high temperature resistant battery separator in Example 4 of the present invention.
[0042] Figure 3 This is a DTG curve diagram of the high temperature resistant battery separator in Example 4 of the present invention.
[0043] Figure 4 This is a digital photo of the high temperature resistant battery separator in Example 4 of the present invention after being treated at 800°C.
[0044] Figure 5 This is the cyclic voltammetry curve of the lithium iron phosphate lithium ion battery separator in Example 8 of the present invention.
[0045] Figure 6 This is the long cycle performance curve of the lithium iron phosphate lithium ion battery separator in Example 8 of the present invention.
[0046] Figure 7This is the rate performance curve of the lithium iron phosphate lithium ion battery separator in Example 8 of the present invention.
[0047] Figure 8 This is the cyclic voltammetric performance curve of the lithium iron phosphate lithium ion battery separator in Comparative Example 1.
[0048] Fig. 9 This is the long cycle performance curve of the lithium iron phosphate lithium-ion battery separator in Comparative Example 1.
[0049] Fig.10 This is the rate performance curve of the lithium iron phosphate lithium-ion battery separator in Comparative Example 1.
[0050] Fig.11 This is a scanning electron microscope image of the cross section of the high temperature resistant battery separator in Example 4 of the present invention. DETAILED DESCRIPTION
[0051] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0052] Example 1
[0053] This embodiment provides a method for preparing a filling powder material for a high temperature resistant battery separator, wherein the preparation method comprises the following steps:
[0054] Weigh 1 g of sodium alginate and add it to 100 mL of deionized water, stirring to dissolve until a clear solution is obtained;
[0055] Weigh 2 g of diatomaceous earth, dry it in vacuum at 120°C for 12 hours, and then cool it down naturally;
[0056] Add dried diatomaceous earth to the sodium alginate solution, stir for 12 hours, and filter;
[0057] The powder was dried at 120° C. in a vacuum oven for 12 hours and then ground to obtain a filling powder material for a high temperature resistant battery separator.
[0058] Example 2
[0059] This embodiment provides a method for preparing a filling powder material for a high temperature resistant battery separator, wherein the preparation method comprises the following steps:
[0060] Weigh 2 g of sodium alginate and add it to 100 mL of deionized water, stirring to dissolve until a clear solution is obtained;
[0061] Weigh 2 g of diatomaceous earth, dry it in vacuum at 120°C for 12 hours, and then cool it down naturally;
[0062] Add dried diatomaceous earth to the sodium alginate solution, stir for 12 hours, and filter;
[0063] The powder was dried at 120° C. in a vacuum oven for 12 hours and then ground to obtain a filling powder material for a high temperature resistant battery separator.
[0064] Example 3
[0065] This embodiment provides a method for preparing bacterial cellulose fibers for high temperature resistant battery separators, wherein the preparation method comprises the following steps:
[0066] The bacterial cellulose taken out of the refrigerator was cut into pieces, and washed in 400 mL of a mixed solution of water and ethanol in a volume ratio of 1:1. The solution was stirred for 24 hours, and the mixed solution was changed every 8 hours for 3 times.
[0067] The washed bacterial cellulose was placed in a 500 mL round-bottom flask containing 300 mL of 1 mol / L sodium hydroxide solution, purified in an oil bath at 60°C for 6 hours, and then washed with a mixed solution of water and ethanol in a volume ratio of 1:1 until neutral.
[0068] The neutral bacterial cellulose was further placed in 400 mL of a mixed solution of water and ethanol in a volume ratio of 1:1 for washing, stirred for 24 hours, and the mixed solution was changed every 8 hours for 3 times.
[0069] The bacterial cellulose was crushed with an analytical grinder until no obvious lumps were visible, and then freeze-dried to obtain bacterial cellulose fibers.
[0070] Example 4
[0071] This embodiment provides a method for preparing a high temperature resistant battery separator, wherein the preparation method comprises the following steps:
[0072] 100 mg of the filling powder material of the high temperature resistant battery separator prepared in Example 1 and 25 mg of the bacterial cellulose fiber prepared in Example 3 were dispersed in 50 mL of anhydrous ethanol, and ultrasonically dispersed for 30 minutes to obtain a uniformly dispersed suspension. 12 mL of the above suspension was taken, filtered to form a membrane, and vacuum dried at 120°C for 12 hours to obtain the high temperature resistant battery separator of the present invention, which was recorded as separator 1# and had a thickness of 79 μm.
[0073] Figure 1 This is a scanning electron microscope image of the diaphragm 1# prepared in Example 4. It can be seen that the structure of the diaphragm has many pores and is suitable for storing electrolyte.
[0074] Figure 2 , Figure 3These are the TGA and DTG test data of diaphragm 1# prepared in Example 4. The thermal stability temperature of the diaphragm is as high as over 800°C, and it has very good thermal safety performance.
[0075] Figure 4 This is a digital photo of the diaphragm 1# prepared in Example 4 after high temperature treatment at 800°C. After being kept at 800°C for 3 minutes, it still maintains its original complete shape and has toughness.
[0076] Example 5
[0077] 150 mg of the filling powder material of the high temperature resistant battery separator prepared in Example 1 and 25 mg of the bacterial cellulose fiber prepared in Example 3 were dispersed in 50 mL of anhydrous ethanol, and ultrasonically dispersed for 30 minutes to obtain a uniformly dispersed suspension. 12 mL of the above suspension was taken, filtered to form a membrane, and vacuum dried at 120°C for 12 hours to obtain the high temperature resistant battery separator of the present invention, which was recorded as separator 2# and had a thickness of 94 μm.
[0078] Example 6
[0079] 100 mg of the filling powder material of the high temperature resistant battery separator prepared in Example 1 and 35 mg of the bacterial cellulose fiber prepared in Example 3 were dispersed in 50 mL of anhydrous ethanol, and ultrasonically dispersed for 30 minutes to obtain a uniformly dispersed suspension. 12 mL of the above suspension was taken, filtered to form a membrane, and vacuum dried at 120°C for 12 hours to obtain the high temperature resistant battery separator of the present invention, which was recorded as separator 3# and had a thickness of 86 μm.
[0080] Example 7
[0081] 100 mg of the filling powder material of the high temperature resistant battery separator prepared in Example 2 and 25 mg of the bacterial cellulose fiber prepared in Example 3 were dispersed in 50 mL of anhydrous ethanol, and ultrasonically dispersed for 30 minutes to obtain a uniformly dispersed suspension. 12 mL of the above suspension was taken, filtered to form a membrane, and vacuum dried at 120°C for 12 hours to obtain the high temperature resistant battery separator of the present invention, which was recorded as separator 4# and had a thickness of 79 μm.
[0082] Test Case
[0083] The porosity and liquid absorption rate were tested by the differential weight method. Specifically, the initial mass W0 of the diaphragm was weighed and recorded, then immersed in a solvent (n-butanol) for 1 hour, and then the mass W1 of the diaphragm after absorbing the solvent was weighed. The porosity and liquid absorption rate were calculated using the following formula.
[0084] The formula for calculating porosity is:
[0085]
[0086] Calculate the liquid absorption rate formula:
[0087]
[0088] Where ρ is the density of n-butanol, g / cm 3 ;
[0089] V is the volume of the diaphragm, cm 3 ;
[0090] W0 is the initial mass of the diaphragm, mg;
[0091] W1 is the mass of the diaphragm after being fully absorbed by the solvent, mg.
[0092] Table 1 shows the porosity and liquid absorption test data of the high temperature resistant battery separators prepared in Examples 4 to 7 of the present invention and Celgard 2400PP. By comparison, it can be seen that the porosity and liquid absorption of the high temperature resistant battery separators prepared in the present invention are higher than those of Celgard 2400PP.
[0093] The Celgard 2400PP is a polypropylene diaphragm purchased from Celgard Company.
[0094] Table 1.
[0095] Serial number Test items Porosity (%) <![CDATA[Liquid absorption rate (g / cm 3 )]]> 1 Diaphragm 1# 25.80881058 0.312427383 2 Diaphragm 2# 24.74796238 0.281622853 3 Diaphragm 3# 34.15117244 0.368571641 4 Diaphragm 4# 38.50399658 0.330766192 5 Celgard 2400PP 24.74796238 0.281622853
[0096] Example 8
[0097] This application example provides a lithium iron phosphate lithium-ion battery, which uses the high temperature resistant battery separator provided in Example 4 as a separator. The assembly of the battery includes the following specific steps:
[0098] 1) 0.4 g of lithium iron phosphate, 0.05 g of conductive carbon black and 0.05 g of polyvinylidene fluoride (PVDF) binder were weighed in a mass ratio of 8:1:1, nitrogen-methylpyrrolidone (NMP) was used as a dispersant (1.05 g), and the mixture was uniformly mixed by magnetic stirring to obtain a slurry;
[0099] 2) coating the above slurry on an aluminum foil with a thickness of 200 μm, placing it in a 60° C. oven to dry for 2 h, and then placing it in a 120° C. vacuum oven to dry for 12 h to obtain a lithium iron phosphate electrode;
[0100] 3) Use one of the above-mentioned electrode plates as the positive electrode of the battery, a 200μm commercial lithium plate as the negative electrode of the battery, cut the high temperature resistant battery separator prepared in Example 4 into 19mm round pieces as the battery separator, use commercial 3011R electrolyte as the electrolyte, and assemble a button-type lithium iron phosphate lithium-ion battery.
[0101] The electrochemical performance of the obtained lithium iron phosphate lithium-ion battery was tested. The test process used a Solatronanalytical 1400CellTest System electrochemical workstation to test the cyclic voltammetry curve. The voltage test range was 2.5 to 3.8 V and the scan rate was 0.1 mV / s.
[0102] The obtained lithium iron phosphate lithium-ion battery was subjected to a battery charge and discharge long cycle performance test. The test process adopted a LAND battery test system to test the battery charge and discharge long cycle curve. The voltage test range was 2.5 to 3.8 V, and the charge and discharge current density was 5C.
[0103] The obtained lithium iron phosphate lithium-ion battery was subjected to a battery charge and discharge rate performance test. The test process adopted a LAND battery test system to test the battery charge and discharge rate cycle curve. The voltage test range was 2.5 to 3.8 V, and the charge and discharge current density was 0.1, 0.5, 1, 2, and 5 C.
[0104] Figure 5 This is the cyclic voltammetric performance curve of the lithium iron phosphate lithium ion battery separator of Example 8. The CV curve with substantially symmetrical redox peaks indicates that the material has good performance and small polarization.
[0105] Figure 6 This is the long cycle performance test of the lithium iron phosphate lithium-ion battery diaphragm of Example 8. At a current density of 5C, the specific capacity of the lithium-ion battery described in the present invention reaches 123.9mAh / g. After 100 cycles, the lithium-ion battery still has a capacity retention rate of 98.45%, indicating that the long cycle performance of the diaphragm described in the present invention is good.
[0106] Figure 7 This is the rate cycle test of the lithium iron phosphate lithium ion battery separator of Example 8. At a current density of 0.1C, the specific capacity of the lithium ion battery of the present invention reaches a specific capacity of 148.1mAh / g. After multiple rate charge and discharge, the current returns to the initial size, and the specific capacity of the battery is still 139.7mAh / g, and the capacity retention rate is 94.33%. It shows that the battery assembled with the separator prepared by the method of the present invention has excellent rate charge and discharge performance.
[0107] Comparative Example 1
[0108] This application example provides a lithium iron phosphate lithium-ion battery. The battery uses a Celgard 2400PP diaphragm as a diaphragm and is assembled using the same preparation steps and parameters as Example 8.
[0109] Figure 8 This is the cyclic voltammetric performance curve of the lithium iron phosphate lithium-ion battery of comparative example 1.
[0110] Fig. 9 Comparative Example 1 Long cycle performance test of lithium iron phosphate lithium-ion battery. In the lithium iron phosphate battery, at a current density of 5C, the specific capacity of the lithium-ion battery reaches 123.2mAh / g. After 100 cycles, the battery capacity drops significantly, the capacity retention rate is only 94.07%, and the cycle life is short.
[0111] Fig.10 This is a rate cycle test of the lithium iron phosphate lithium-ion battery in Example 1. In the lithium iron phosphate battery, at a current density of 0.1C, the specific capacity of the lithium-ion battery reaches 146.4mAh / g. After multiple rate charge and discharge, the current returns to the initial size, and the specific capacity of the battery decreases significantly, with a specific capacity of 136.3mAh / g, and the capacity retention rate is only 93.1%, and the rate performance is poor.
[0112] Matters not covered in the present invention are known technologies. The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a cellulose inorganic composite membrane, characterized in that: Forming a suspension containing bacterial cellulose and composite powder into a film to obtain the cellulose inorganic composite film; The preparation method of the composite powder comprises: mixing raw materials containing organic polymer compounds and inorganic substances with water, stirring, filtering, drying and grinding to obtain the composite powder; The components of the cellulose-inorganic composite membrane include bacterial cellulose and composite powder; the composite powder includes organic polymer compounds and inorganic substances; The mass ratio of the bacterial cellulose to the composite powder is 5-50:25-200; The mass ratio of the organic polymer compound to the inorganic substance is 10-300:100-300; The organic polymer compound is selected from at least one of sodium alginate, carboxymethyl cellulose and polyacrylic acid; The inorganic substance is selected from at least one of diatomaceous earth, zeolite, kaolin and montmorillonite; The thickness of the cellulose inorganic composite membrane is 20 to 90 μm, the porosity is 13% to 91%, and the liquid absorption rate is 0.17 to 0.36 g / cm 3 , heat resistance temperature is greater than 400℃.
2. The preparation method according to claim 1, characterized in that: In the suspension, the mass ratio of the bacterial cellulose to the composite powder is 5-50:25-200.
3. The preparation method according to claim 1, characterized in that: The concentration of the organic polymer compound is 0.25-1 g / L, and the concentration of the inorganic substance is 0.5-1.5 g / L.
4. The preparation method according to claim 1, characterized in that: The inorganic substances are vacuum dried at 100-120° C. for 10-12 hours before mixing; The stirring time is 10 to 12 hours; The drying is performed by vacuum drying at 100-120° C. for 10-12 hours.
5. The preparation method according to claim 1, characterized in that: The bacterial cellulose needs to be pre-treated, and the pre-treatment includes grinding, crushing and freeze-drying the cleaned bacterial cellulose.
6. The preparation method according to claim 5, characterized in that: The cleaning comprises the following steps: (a) stirring bacterial cellulose in a mixed solution of deionized water and ethanol for 24 hours as one treatment, and repeating it three times; (b) stirring the bacterial cellulose obtained in step (a) in an alkaline solution in an oil bath at 50 to 60° C. for 6 to 8 hours, and then washing with deionized water until neutral; (c) stirring the bacterial cellulose obtained in step (b) in a mixed solution of deionized water and ethanol for 24 hours, repeating the treatment three times; The volume ratio of the deionized water to the ethanol is 1:
1.
7. The preparation method according to claim 6, characterized in that: The alkaline solution is selected from one of 0.1 mol / L sodium hydroxide or potassium hydroxide solutions.
8. Use of the cellulose inorganic composite membrane prepared by the preparation method according to any one of claims 1 to 7 as a battery separator.
9. A lithium ion battery, characterized in that: The battery separator of the lithium-ion battery is prepared from the cellulose inorganic composite membrane obtained by the preparation method according to any one of claims 1 to 7.