Film formed by waste thermoplastic elastomer and laminate thereof

CN118984858APending Publication Date: 2024-11-19FOSHAN KING WONDER HI TECH CO LTD +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202180098349.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2021-06-23
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Waste thermoplastic elastomers have poor biodegradability, existing recycling and treatment methods are poor, leading to environmental pollution, and there is a lack of effective low-cost utilization technology.

Method used

Use waste thermoplastic elastomers to prepare films and laminates for fitting clothing fabrics, shoe fabrics, luggage fabrics, etc., and improve their utilization rate through appropriate formulas and molding processes, including the use of waste thermoplastic elastomers and viscosity regulators and slip agents to form suitable microstructure and functional films.

Benefits of technology

Efficient utilization of waste thermoplastic elastomers is achieved to prepare moisture-permeable, soft and wash-resistant films and laminates suitable for a variety of purposes, reducing the cost of toughened high-impact polystyrene and providing an environmentally friendly solution plan.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118984858A_ABST
    Figure CN118984858A_ABST
Patent Text Reader

Abstract

The invention discloses a film prepared from a waste thermoplastic elastomer and a laminate thereof. The composition for forming the film comprises 0.5%-99.8% of the waste thermoplastic elastomer, 0.01%-3% of a viscosity modifier, 0.01%-10% of a slipping agent for preventing the prepared film from being bonded when the prepared film is rolled, and 0%-99% of a fresh thermoplastic elastomer, wherein the thermoplastic elastomer is a polyester elastomer, a nylon elastomer, a biologically sourced nylon elastomer and / or a biologically sourced polyester elastomer and a graft thereof; the viscosity modifier is a reactive viscosity modifier and / or a non-reactive viscosity modifier; the slipping agent is fatty acid and esters thereof, fatty acid amide, metallic soap, hydrocarbon, an organosilicon compound, stearic acid, butyl stearate and / or ethylene bis stearamide. The thermal sewing position has the advantages of being good in wind resistance, breathable, capable of blocking virus liquid, smooth in appearance, free of wrinkles, soft in hand feeling and the like. The prepared film has good moisture permeability, washing performance, tensile strength and required hand feeling softness.
Need to check novelty before this filing date? Find Prior Art

Description

Film formed from waste thermoplastic elastomer and laminate thereof Technical Field

[0001] The present invention relates to the recycling of waste plastics, especially waste thermoplastic elastomers; more specifically, the present invention relates to a film formed from waste thermoplastic elastomers and a laminate thereof. Background Art

[0002] Thermoplastic elastomers (TPEs) are plastic at high temperatures, allowing them to be remolded and reshaped, while remaining elastic at room temperature. Due to their excellent mechanical properties, processing capabilities, and weather resistance, TPEs have been extensively developed, with new varieties constantly emerging. They have largely replaced traditional rubber and plastic materials and are widely used in wire and cable, sealants, diaphragm products, the footwear industry, the automotive industry, the machinery industry, and various industrial molded products. Based on the type of their primary component, TPEs can be broadly divided into seven categories: polyamide thermoplastic elastomers, copolymer thermoplastic elastomers, polyolefin thermoplastic elastomers, styrene thermoplastic elastomers, urethane thermoplastic elastomers, thermoplastic vulcanizates, and other thermoplastic elastomers.

[0003] While plastic products bring convenience to people's lives, waste plastics also pose a significant environmental burden. Thermoplastic elastomers, however, have a serious drawback: poor biodegradability and resistance to degradation after burial. Neither landfill nor incineration has proven to be a viable disposal option. Cost-effective recycling would be a better option.

[0004] Among existing technologies, only Chinese patent CN201310666587.5 discloses a method for utilizing waste thermoplastic elastomers. The method comprises the following steps: uniformly mixing 80-95 parts of waste polystyrene, 5-15 parts of waste thermoplastic elastomer, 0.1-0.3 parts of a heat stabilizer, 0.1-0.4 parts of an antioxidant, 0.1-0.3 parts of a UV absorber, 1-3 parts of a reinforcing filler, and 0.1-0.3 parts of white oil by weight; melt-kneading the mixture at 170-210°C; extruding strands through an extruder; cooling the mixture; and pelletizing the resulting high-impact polystyrene pellets. This invention provides a suitable method for utilizing waste thermoplastic elastomers and a novel approach for reducing the cost of toughening high-impact polystyrene.

[0005] Therefore, it is necessary to provide a technical solution for making more use of waste thermoplastic elastomers. For example, the application of waste thermoplastic elastomers in clothing products and the replacement of non-reusable parts in clothing products are one of the main problems that need to be solved in the existing technology.

[0006] Summary of the Invention

[0007] The purpose of the present invention is to provide a film and a laminate thereof prepared using waste thermoplastic elastomer. The obtained film can be used for laminating clothing fabrics, laminating shoe fabrics, laminating luggage fabrics, laminating glove fabrics, laminating hat fabrics, instruments and food packaging, etc.

[0008] In order to achieve the above-mentioned object of the invention, on the one hand, the present invention provides a film prepared from waste thermoplastic elastomer, wherein the thickness of the film is 3 μm to 1000 μm; and the film comprises, in percentage by weight (the same below):

[0009] 0.5%-99.8% of waste thermoplastic elastomer;

[0010] 0.01%-3% viscosity regulator;

[0011] 0.01% to 10% of a slip agent to prevent the film from sticking when it is rolled up; and

[0012] 0%-99% fresh thermoplastic elastomer;

[0013] The thermoplastic elastomer is one or more selected from the group consisting of polyester elastomer, nylon elastomer, bio-derived nylon elastomer and bio-derived polyester elastomer;

[0014] The viscosity modifier is a reactive viscosity modifier and / or a non-reactive viscosity modifier. The non-reactive viscosity modifier is selected from at least one of the following substances: paraffin wax, microcrystalline wax, polyethylene wax, oxidized polyethylene wax, polypropylene wax, sasol wax, hyperbranched polymer, APAO, ethylene bisstearamide, EVA, urea, hydroxylamine hydrochloride, hydroxylamine sulfate and cyclohexanol. The reactive viscosity modifier is an epoxy compound or a low molecular weight, multifunctional ester, alcohol or amine compound containing hydroxyl or amino groups.

[0015] The lubricant is selected from at least one member selected from the group consisting of fatty acids and their esters, fatty acid amides, metal soaps, hydrocarbons, organic silicon compounds, stearic acid, butyl stearate, and ethylene bisstearamide.

[0016] In the present invention, the waste thermoplastic elastomer used is scraps and / or offcuttings.

[0017] In the present invention, the lubricant used is to prevent adhesion during the film preparation process, especially during the film winding process. Therefore, the lubricant is different from the lubricant used in the plastic processing process.

[0018] In typical film-making processes, three types of lubricants are commonly used: oleamide, erucamide, and silica (inorganic powder). However, organic lubricants such as oleamide and erucamide are not suitable for the films of the present invention. This is primarily due to the accumulation of large amounts of precipitates on the film surface, resulting in severe blooming, which affects the film's printability, heat sealability, and color, and also hinders the subsequent lamination process. Inorganic powders, on the other hand, are an anti-blocking agent, which can affect the intended use and subsequent lamination of the films of the present invention. Therefore, one of the prerequisites for selecting a lubricant in the present invention is that it does not interfere with subsequent lamination.

[0019] Preferably, the slip agent of the present invention is fatty acid and its esters.

[0020] Similarly, in order to prevent the printability, heat sealability, and color of the prepared film from being affected, and also to prevent the subsequent lamination process from being affected, the viscosity modifier in the present invention is preferably a reactive viscosity modifier. For example, the reactive viscosity modifier can be one or more alcohol chain extenders selected from the following group: 1,4-butanediol (BDO), 1,6-hexanediol, glycerol, trimethylolpropane, diethylene glycol (DEG), triethylene glycol, neopentyl glycol (NPG), sorbitol, and diethylaminoethanol (DEAE).

[0021] Alternatively, the reactive viscosity modifier is one or more amine and ester chain extenders selected from the following group: MOCA, liquid MOCA modified with formaldehyde, ethylenediamine (DA), N,N-dihydroxy(diisopropyl)aniline (HPA), hydroquinone-bis(β-hydroxyethyl) ether (HQEE), difunctional acid derivatives, isocyanates, acid anhydrides, epoxides, glycidyl esters, and their multifunctional derivatives.

[0022] More preferably, the viscosity modifiers are epoxy compounds, glycidyl esters, and their multifunctional derivatives, as they are structurally similar to and compatible with thermoplastic elastomers, and do not degrade the moisture permeability and elastic recovery of thermoplastic elastomer films. More importantly, they may even improve the properties. More preferred are epoxy compounds, glycidyl esters, and their multifunctional derivatives with fewer functional groups, as they do not cause sudden polymerization; for example, they may contain 2-4 functional groups, particularly 3 functional groups.

[0023] In one embodiment of the present invention, the prepared film comprises:

[0024] 2.5%-99.8% of waste thermoplastic elastomers;

[0025] 0.01%-2% viscosity regulator;

[0026] 0.01%-10% of a lubricant that does not affect the fit; and

[0027] 0% - 90% fresh thermoplastic elastomer.

[0028] In order to improve the utilization rate of waste thermoplastic elastomer, in another specific embodiment of the present invention, the prepared film comprises:

[0029] 80%-99.8% of waste thermoplastic elastomers;

[0030] 0.01%-2% viscosity regulator;

[0031] 0.01% - 10% of lubricant that does not affect the fit and

[0032] 0% - 10% fresh thermoplastic elastomer.

[0033] Generally, the film of the present invention may also include some processing aids, such as antioxidants, UV agents, etc.

[0034] The film of the present invention can be made into a film of any other color. In this case, 0.1-45% of color powder needs to be added to the film formula.

[0035] In addition, functional additives such as flame retardants, aerogels, infrared powders, graphene, calcium carbonate, titanium dioxide, phase change materials, and other inorganic and organic functional powders can be added to the film formulation in a ratio of 0-70%. However, a prerequisite is that they must not affect subsequent lamination. Therefore, the specific selection and dosage require special attention.

[0036] In the present invention, the forming method of the film (which can also be called a sheet if it is thicker) is: hot melt molding extrusion with an extruder: casting, film blowing, spinneret, extrusion to form vacuum hole molding, calendering, biaxial stretching, uniaxial stretching; later mechanical punching: laser, chemical corrosion, needle punching, flower roller pressing, ultrasonic punching, etc.

[0037] The microstructure of the film prepared by the present invention may be porous or may not have pores in the strict sense, with only molecular gaps existing. Please refer to Figures 1-6.

[0038] The film (also referred to as a sheet when thick) prepared by the present invention can be washed 3-100 times, preferably 3-50 times, according to ISO6330. Its moisture permeability is typically 100-180,000 according to JIS L 1099B1, and its hydrostatic pressure is typically above 10,000 mm H2O according to JIS L 1092. It has a soft hand feel (an elastic modulus value within 300 MPa is acceptable, according to ASTM D882), a uniform appearance, and no obvious glue spots. The film is suitable for various occasions and uses, particularly clothing, such as clothing, shoes, gloves, hats, luggage, surface lamination or packaging of special devices requiring moisture permeability (such as electronic products and electronic devices), and surface lamination or packaging of foods requiring moisture permeability.

[0039] More specifically, the use of the film prepared by the present invention is one of the following:

[0040] (1) Used for laminating clothing fabrics, wherein the thickness of the film can be 5μm-50μm;

[0041] (2) For laminating shoe fabrics, wherein the thickness of the film or sheet can be 10-500 μm;

[0042] (3) Used for laminating fabrics for gloves and hats, wherein the thickness of the film can be 8-80 μm;

[0043] (4) Used for laminating luggage fabrics, wherein the thickness of the film or sheet can be 50-1000 μm;

[0044] (5) Used for surface lamination or packaging of devices requiring moisture permeability, wherein the thickness of the film or sheet can be 15-1000 μm;

[0045] (6) Used for surface lamination or packaging of food requiring moisture permeability, wherein the thickness of the film or sheet can be 15-1000 μm.

[0046] In addition, the films or sheets prepared by the present invention can undergo various surface treatments, including various functional treatment coatings or discontinuous coatings, particularly printing, functional printing (suitable for UV-curable inks, screen printing, heat transfer printing, O-LED printing, roller printing, computer printing, etc., and can be any pattern), hydrophobic treatment, hydrophilic treatment, UV or IR blocking treatment, color treatment, graphene coating, aerogel layer, phase change cooling, heat sensitivity, temperature sensitivity, pressure sensitivity, and other inorganic or organic functional coatings; surface chemical burnout treatment; and surface activation treatments such as corona, plasma, and oxidation. The thickness of the surface treatment layer is preferably at least 0.5 μm.

[0047] On the other hand, in order to achieve the purpose of the present invention, the present invention also provides a laminate comprising waste thermoplastic elastomer, the laminate comprising:

[0048] At least one layer formed of nonwoven fabric and / or woven fabric, the grammage of which layer is 7-1000 gsm; and

[0049] At least one layer formed of a composition containing waste thermoplastic elastomer, the thickness of the layer being 5-1000 μm;

[0050] Wherein, the composition containing waste thermoplastic elastomer comprises:

[0051] 0.5%-99.8% of waste thermoplastic elastomer;

[0052] 0.01%-3% viscosity regulator;

[0053] 0.01% to 10% of a slip agent to prevent the film from sticking when rolled up; and

[0054] 0%-99% fresh thermoplastic elastomer;

[0055] Among them, the thermoplastic elastomer is one or more selected from the following group: polyester elastomer, nylon elastomer, bio-derived nylon elastomer and bio-derived polyester elastomer; the viscosity modifier is a reactive viscosity modifier and / or a non-reactive viscosity modifier, and the non-reactive viscosity modifier is one or more selected from the following group: paraffin wax, microcrystalline wax, polyethylene wax, oxidized polyethylene wax, polypropylene wax, sasol wax, hyperbranched polymer, APAO, ethylene bisstearamide, EVA, urea, hydroxylamine hydrochloride, hydroxylamine sulfate and cyclohexanol; the reactive viscosity modifier is an epoxy compound, or a low molecular weight multifunctional ester, alcohol or amine compound containing hydroxyl or amino groups; the lubricant is one or more selected from the following group: fatty acids and their esters, fatty acid amides, metal soaps, hydrocarbons, organosilicon compounds, stearic acid, butyl stearate and ethylene bisstearamide.

[0056] Preferably, the laminate of the present invention further includes an adhesive layer between the layer formed of nonwoven fabric and / or textile fabric and the layer formed of the composition containing waste thermoplastic elastomer. The adhesive layer is formed of a hot melt adhesive, solvent adhesive, or water-based adhesive, and has a grammage of 3-80 gsm. For example, the film or sheet prepared by the present invention can be laminated with nonwoven and textile fabrics to form a laminate, or can be directly coated or laminated with a hot melt adhesive layer. Alternatively, after lamination with nonwoven fabric or textile fabric, a hot melt adhesive layer can be laminated to the film or fabric surface. The latter two are preferably used for pre-coating, more preferably for seam location waterstops and for subsequent lamination with other laminates, ultimately achieving full remeltability of the entire product. The hot melt adhesive layer can be continuous or discontinuous.

[0057] The film or sheet used in the laminate of the present invention can be made entirely from waste thermoplastic elastomer (excluding viscosity modifiers, lubricants, and possible functional additives), with no or minimal fresh thermoplastic elastomer. The film or sheet can have a thickness of 5-1000 μm, preferably 5-50 μm for clothing, 10-500 μm for shoes, 50-1000 μm for bags, and 8-500 μm for adhesive strips.

[0058] The laminate of the present invention can be a three-layer composite structure (the adhesive layer is regarded as one layer, the same below), that is, a layer of textile fabric is glued to a layer of film or sheet, or a five-layer composite structure, that is, two layers of textile fabric are glued to a layer of recycled film and sheet in the middle; or a composite structure with more layers.

[0059] In the laminate of the present invention, the fabric structure of the selected textile fabric can be fabric material (bonded to fleece, tricot backers, knits (mesh and jersey, single and double knit), wovens (ripstop and plainweave, twill, single and double-weaves)), foam, air layer, non-woven fabric, cotton (multi-layer interface, natural cotton, Thinsulate, etc.); the material components of the fabric are mainly PP, PE, PET, PLA, PBAT, PVA, nylon, polypropylene, ultra-high density polyethylene, polyethylene, polypropylene, polyvinyl chloride, polystyrene, polymethyl methacrylate, polyester, polyoxymethylene, polyamide, polyphenylene ether, polyurethane, polysulfone, rubber, polyetheretherketone (PEEK), PPS, polyimide (PI), polyetherimide (PAI) and other chemical fiber resins, alone or in mixtures, or recycled alone or in mixtures, and can also be natural fabrics.

[0060] When laminating (or compounding), the moisture permeability must be above 100g / m²*24h and the number of washes must be at least three times. The adhesive can be hot melt adhesive, solvent adhesive, or water-based adhesive, such as polyurethane, polyester, APEO, or nylon. The adhesive can be applied in any discontinuous pattern, such as dots, grids, sprays, or patterns. Methods that do not require adhesive can also be used, such as burn-in lamination, sprinkling lamination, and regular hot lamination.

[0061] Lamination method: Glue can be pre-applied on the film (sheet) or fabric, and then the fabric and film (sheet) are laminated by heating; or they can be laminated while applying glue; or the surface of the fabric or film (sheet) can be activated to have a bonding effect by burning and pasting, and then laminated.

[0062] The laminate of the present invention can be formulated to have suitable washing performance, moisture permeability, softness to the touch, etc. according to the occasion.

[0063] The present invention will be further described below with reference to the accompanying drawings and specific embodiments. However, these specific embodiments are merely illustrations of certain specific embodiments of the present invention and are not intended to limit the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0064] FIG1 is a scanning electron microscope diagram of a thin film structure without pores in a strict physical sense;

[0065] FIG2 is a scanning electron microscope diagram of a nanowire mesh interlaced structure formed by electrospinning;

[0066] FIG3 is a scanning electron microscope schematic diagram of a thin film structure formed by solution pores;

[0067] FIG4 is a scanning electron microscope diagram of a film structure formed by physical stretching;

[0068] FIG5 is a schematic diagram of a scanning electron microscope of a structure formed by a direct-laid nonwoven method;

[0069] FIG6 is a scanning electron microscope diagram of a thin film structure obtained by a regular physical-mechanical pore forming method;

[0070] FIG7 is a graph showing elastic modulus test. DETAILED DESCRIPTION

[0071] In the following specific embodiments, the test methods for water vapor permeability, hydrostatic pressure, elastic modulus, elongation at break, etc. are as follows:

[0072] (1) Hydrostatic pressure test:

[0073] A) Testing standard: AATCC127;

[0074] B) Sampling Standard: Take at least three 200mm x 200mm samples diagonally, avoiding folding and contamination of the test area. Before testing, condition the samples at (21±2)°C and (65±2)% humidity for at least 4 hours. The front and back of the fabric must be distinguished.

[0075] C) Test Method: At (21±2)°C, wipe off any water on the clamping device. Clamp the conditioned sample so that the front of the sample is in contact with the water surface. Select the test program, increase the pressure at a rate of 60 mbar / min, and record the water pressure when the third water droplet appears. The three water drops should be located in different locations and not within 3mm of the clamp edge.

[0076] (2) Moisture permeability: JIS L1099B1 method potassium acetate method:

[0077] Equipment: Constant temperature box: 30±2℃, water tank temperature in the constant temperature box: about 23℃; balance with an inner diameter of 56mm and a moisture permeable cup of 75mm height;

[0078] Auxiliary membrane: PTFE membrane with a pore size of 80% and a thickness of 25um. The auxiliary membrane is used to seal the mouth of the moisture-permeable cup containing the moisture absorbent;

[0079] Desiccant: Add 100ml of deionized water to every 300g of potassium acetate and let it sit for a day and night to form crystals;

[0080] Sampling: approximately 20cm x 20cm;

[0081] Test steps:

[0082] Fix the sample to the support frame with a rubber band, then place it in the constant temperature water tank of the constant temperature box to a depth of about 10mm and leave it there for 15 minutes. Put 2 / 3 of the moisture absorbent (about 23℃) in the moisture permeable cup, fix the mouth of the moisture permeable cup with an auxiliary film and a rubber band, place the assembled moisture permeable cup on a balance and weigh it a1. After weighing, place the moisture permeable cup upside down on the fixed test sample. After 15 minutes, take out the moisture permeable cup and place it on a balance and weigh it a2 to calculate the moisture permeability.

[0083] (3) Elastic modulus: ASTM D882:

[0084] Equipment: Tensile testing machine with stable moving speed; Thickness gauge accurate to 0.0025mm; Film sample cutting machine: Cut samples must not have visible gaps or jagged edges;

[0085] Sampling: Cut according to the required test direction, with a sample width of 15mm and a length of 300mm (if the cut sample has obvious notches or jagged edges, it should be discarded and re-cut). Prepare at least 5 samples in each direction, and then place the cut samples at 23±1℃ and relative humidity of 50±5% for no less than 40 hours;

[0086] Test steps:

[0087] According to the agreed load cell, the clamp spacing is 250mm, the tensile speed is 25mm / min, the tensile machine is set, and the force value is reset to zero;

[0088] Measure the thickness and width of the sample and input them into the tensile testing machine software. Clamp the sample and try to make the initial force value 0. Click Start. When the inflection point of the maximum slope appears in the graph (as shown in Figure 7), stop the test, read out and record the result (Mpa).

[0089] (4) Elongation at break: ASTM D882:

[0090] Equipment: Tensile testing machine with a stable moving speed; thickness gauge accurate to 0.0025mm; film sample cutting machine: the cut samples must not have visible notches or serrations. Sampling: Cut according to the required test direction, the sample width is 15mm and the length is not less than 150mm (if the cut sample has obvious notches or serrations, it should be recut). Prepare at least 5 samples in each direction, and then place the cut samples at 23±1℃ and relative humidity 50±5% for not less than 40 hours.

[0091] Test steps:

[0092] According to the agreed load cell, the clamp spacing is 50mm, the tensile speed is 500mm / min, the tensile machine is set, and the force value is reset to zero;

[0093] Clamp the specimen and try to make the initial force value 0. Click Start and test until the specimen breaks. Read and record the elongation % at break (if the specimen slips or breaks at a defect during the test, the result will be invalid).

[0094] Preparation of thin films:

[0095] The melt of the above formulation can flow out through the gap at the front end of the die to form a film. After leaving the die, the melt passes through a short gap and reaches the low-temperature casting roll surface, where it is rapidly cooled and shaped. The melt of the above formulation can also be blown out through high-pressure air from a rotating die to form a tubular film. After leaving the die, the melt passes through a short gap and reaches the low-temperature casting roll surface, where it is rapidly cooled and shaped. The above formulation can also be melt-extruded into a forming process (vacuum hole forming), and after heating and softening the flat plastic hard sheet, it is vacuum-adsorbed on the mold surface and cooled to form.

[0096] Alternatively, the above formulation may be plasticized to a temperature close to the viscosity flow temperature and passed through the gap between a series of horizontal rollers rotating in opposite directions, so that the material is subjected to extrusion and extension to form a thin sheet product with a certain thickness, width and smooth surface. Alternatively, the above film or cast sheet may be subjected to longitudinal and transverse biaxial or uniaxial stretching at a temperature below the melting point of the film material and above the glass transition temperature, and then appropriately cooled or heat-set or subjected to special processing (such as corona treatment, coating, etc.) under tension.

[0097] Regarding advanced hole formation, the above-mentioned formula film can be mechanically punched, using a mechanical shaft to drive a high-strength drill needle to drill holes in the material with a cutting force generated by high rotation. Laser drilling can also be used, using a high-power density laser beam to irradiate the processed material, causing it to quickly heat to the vaporization temperature and evaporate to form holes. Chemical etching can also be used, which refers to removing the protective film of the area to be etched after exposure and development. During etching, the area is exposed to a chemical solution to achieve a dissolving and corroding effect, forming a concave and convex or hollow shape. The holes can also be pierced by a needle-like object. This needle-like object can be in the form of a roller or a template, and the needle can be hot or cold. Roll forming can also be used, using a rotating roller with a smooth surface or a certain shape to press the raw material to produce a product of a certain shape. Ultrasonic drilling can also be used, and the output signal is sent to a transducer composed of piezoelectric ceramics, which converts ultrasonic electrical energy into mechanical vibration energy. The vibration head repeatedly vibrates in the presence of abrasive powder (usually diamond grit) and water, causing the processed part to be ground through and the appropriate small hole to be punched.

[0098] Preparation of laminates:

[0099] The film prepared by the above-mentioned film preparation method according to the formula of this patent is compounded with various fabric structures and fabric components of the above-mentioned claim 9, which can be a two-layer structure, a sandwich three-layer structure, or a structure with more than three layers; the compounding method adopted can be liquid glue rolling or spraying, hot melt glue after melting and then rolling or spraying, hot melt glue net, grid, film can also be compounded after melting by roller pressing, and can also be bonded by burning and pasting to finally form a laminate of the patented product.

[0100] Example 1: Effect of film thickness

[0101] Following the above film preparation process, a series of films were prepared to investigate the effects of film thickness on moisture permeability, hydrostatic pressure, and the number of washes (hydrostatic pressure after a certain number of washes). The results are shown in Table 1. The prepared films did not contain fresh thermoplastic elastomer.

[0102] Table 1 The influence of thickness on the performance of typical products

[0103]

[0104] The data in Table 1 show that the thinner the film thickness, the higher the moisture permeability; the thicker the film thickness, the higher the hydrostatic pressure, and the smaller the effect of the number of water washings on the hydrostatic pressure.

[0105] Therefore, when considering the use of the film of the present invention, the influence of thickness must be considered and an appropriate thickness must be selected.

[0106] Example 2: Effect of viscosity modifier content

[0107] Following the above film preparation process, a series of films were prepared to investigate the effects of viscosity modifier dosage on moisture permeability, hydrostatic pressure, number of washes (hydrostatic pressure after washes), and hand feel (as measured by elastic modulus). The results are shown in Table 2. The prepared films did not contain fresh thermoplastic elastomer and had a film thickness of 15 μm.

[0108] Table 2 Effect of viscosity regulator on product performance

[0109]

[0110] The data in Table 2 shows that for typical waste thermoplastic elastomers, without the addition of a viscosity modifier or with too low a concentration, only a liquid substance is produced during film formation, failing to form a film or a stable film. Of course, if the waste thermoplastic elastomer itself contains a viscosity modifier, the situation is different.

[0111] Example 3: Effect of the proportion of waste thermoplastic elastomer

[0112] Following the above film preparation process, a series of films were prepared to investigate the effects of different proportions of waste thermoplastic elastomer on moisture permeability, hydrostatic pressure, number of washes (hydrostatic pressure after a certain number of washes), and hand feel (characterized by elastic modulus). The results are shown in Table 3. The prepared films had a thickness of 15 μm.

[0113] Table 3 Effect of different ratios of waste thermoplastic elastomers on product performance

[0114]

[0115] From the data in Table 3, it can be found that, except for the viscosity regulator and the lubricant, even if all waste thermoplastic elastomers are used and the amount of fresh thermoplastic elastomer is zero, a film with excellent water vapor permeability, hydrostatic pressure and hand feel can still be produced.

[0116] Example 4: Effects of different materials

[0117] Following the above film preparation process, a series of films were prepared to investigate the effects of different materials (polyester elastomer, nylon elastomer, and bio-based elastomer) on moisture permeability, hydrostatic pressure, number of washes (hydrostatic pressure after a certain number of washes), and hand feel (characterized by elastic modulus). The results are shown in Table 4. The prepared films did not contain fresh thermoplastic elastomer and had a thickness of 15 μm.

[0118] Table 4 The influence of different materials on product performance

[0119]

[0120] From the data in Table 4, it can be found that films with excellent moisture permeability, hydrostatic pressure and hand feel can be produced by using different materials such as polyester elastomer, nylon elastomer, bio-based elastomer, or their mixtures. The reason may be that the melting points of these materials are similar.

[0121] Example 5: Effect of film structure

[0122] Following the above film preparation process, a series of films were prepared to investigate the effects of the porous and non-porous films on moisture permeability, hydrostatic pressure, number of washes (hydrostatic pressure after a certain number of washes), and hand feel (characterized by elastic modulus). The results are shown in Table 5. The prepared films did not contain fresh thermoplastic elastomer and had a film thickness of 15 μm.

[0123] Table 5 The influence of hole, no hole and different hole types on product performance

[0124]

[0125] From the data in Table 5, it can be found that the moisture permeability of various films with different structures is not much different, but the strength, number of washing times and elastic modulus are somewhat different; overall, the non-porous film has the best performance, and the film structure with solution pores, the film structure with physical stretching pores, and the film structure with regular physical and mechanical pore formation methods also perform well.

[0126] Example 6

[0127] Experiments No. 142-147 conducted by the applicant are formulations with a waste thermoplastic elastomer ratio of 75%, Experiments No. 148-153 are formulations with a waste thermoplastic elastomer ratio of 50%, Experiments No. 154-159 are formulations with a waste thermoplastic elastomer ratio of 25%, and Experiments No. 160-164 are formulations with a waste thermoplastic elastomer ratio of 10%. They were prepared using the process methods of Figures 2 to 6 respectively, and the resulting products have performance close to that of the products in Table 5.

Claims

1. A film prepared from waste thermoplastic elastomer, the thickness of the film being 3 μm - 1000 μm, wherein, the film comprises: 0.5% - 99.8% of waste thermoplastic elastomer; 0.01% - 3% of viscosity regulator; 0.01% - 10% of slip agent to prevent the film from sticking during winding; and 0% - 99% of fresh thermoplastic elastomer; wherein, the thermoplastic elastomer is one or more selected from the following group: polyester elastomer, nylon elastomer, nylon elastomer of biological origin, and polyester elastomer of biological origin; the viscosity regulator is a reactive viscosity regulator and / or a non-reactive viscosity regulator, and the non-reactive viscosity regulator is one or more selected from the following group of substances: paraffin wax, microcrystalline wax, polyethylene wax, oxidized polyethylene wax, polypropylene wax, Sasol wax, hyperbranched polymer, APAO, ethylene bisstearamide, EVA, urea, hydroxylamine hydrochloride, hydroxylamine sulfate, and cyclohexanol; the reactive viscosity regulator is an epoxy compound, or a low molecular weight polyfunctional ester or alcohol or amine compound containing a hydroxyl group or an amino group; the slip agent is one or more selected from the following group: fatty acids and their esters, fatty acid amides, metal soaps, hydrocarbons, silicone compounds, stearic acid, butyl stearate, and ethylene bisstearamide.

2. The film according to claim 1, wherein, the film comprises: 2.5% - 99.8% of waste thermoplastic elastomer; 0.01% - 2% of viscosity regulator; 0.01% - 10% of slip agent that does not affect adhesion; and 0% - 90% of fresh thermoplastic elastomer.

3. The film according to claim 1, wherein, the waste thermoplastic elastomer is scrap and / or head and tail materials.

4. The film according to claim 1, wherein, the reactive viscosity regulator is one or more alcohol chain extenders selected from the following group: 1,4-butanediol (BDO), 1,6-hexanediol, glycerol, trimethylolpropane, diethylene glycol (DEG), triethylene glycol, neopentyl glycol (NPG), sorbitol, and diethylaminoethanol (DEAE).

5. The film according to claim 1, wherein, the reactive viscosity regulator is one or more amine and ester chain extenders selected from the following group: MOCA, liquid MOCA prepared by formaldehyde modification, ethylenediamine (DA), N,N-dihydroxy(diisopropyl)aniline (HPA), hydroquinone-bis(β-hydroxyethyl)ether (HQEE), bifunctional acid derivatives, isocyanates, acid anhydrides, epoxy compounds, and glycidyl esters and their polyfunctional derivatives.

6. The film according to claim 1, wherein, the reactive viscosity regulator is an epoxy compound.

7. The film according to claim 1, wherein, the film further comprises 0.1 - 45% of color powder.

8. The film according to any one of claims 1 - 7, wherein, the uses of the film are as follows: (1) For laminating clothing fabrics, wherein the thickness of the film is 5 μm - 50 μm; (2) For laminating shoe fabrics, wherein the thickness of the film is 10 - 500 μm; (3) For laminating glove and hat fabrics, wherein the thickness of the film is 8 - 80 μm; (4) For laminating luggage fabrics, wherein the thickness of the film is 50 - 1000 μm; (5) For surface lamination or packaging of devices requiring moisture permeability, wherein the thickness of the film is 15 - 1000 μm; (6) For surface lamination or packaging of foods requiring moisture permeability, wherein the thickness of the film is 15 - 1000 μm.

9. A laminate comprising waste thermoplastic elastomer, the laminate comprising: At least one layer formed of non-woven fabric and / or textile fabric, the grammage of the layer being 7 - 1000 gsm; And At least one layer formed of a composition containing waste thermoplastic elastomer, the thickness of the layer being 5 - 1000 μm; Wherein the composition containing waste thermoplastic elastomer comprises: 0.5% - 99.8% of waste thermoplastic elastomer; 0.01% - 3% of viscosity regulator; 0.01% - 10% of slip agent to prevent adhesion during winding of the produced film; and 0% - 99% of fresh thermoplastic elastomer; Wherein the thermoplastic elastomer is one or more selected from the following group: polyester elastomer, nylon elastomer, nylon elastomer of biological origin, and polyester elastomer of biological origin; The viscosity regulator is a reactive viscosity regulator and / or a non-reactive viscosity regulator, and the non-reactive viscosity regulator is one or more selected from the following group of substances: paraffin wax, microcrystalline wax, polyethylene wax, oxidized polyethylene wax, polypropylene wax, Sasol wax, hyperbranched polymer, APAO, ethylene bisstearamide, EVA, urea, hydroxylamine hydrochloride, hydroxylamine sulfate, and cyclohexanol; the reactive viscosity regulator is an epoxy compound, or a low molecular weight polyfunctional ester or alcohol or amine compound containing a hydroxyl group or an amino group; The slip agent is one or more selected from the following group: fatty acids and their esters, fatty acid amides, metal soaps, hydrocarbons, silicone compounds, stearic acid, butyl stearate, and ethylene bisstearamide.

10. The laminate according to claim 9, wherein, Between the layer formed of non-woven fabric and / or textile fabric and the layer formed of the composition containing waste thermoplastic elastomer, the laminate further comprises an adhesive layer formed of hot melt adhesive, solvent adhesive or water-based adhesive, and the grammage of the adhesive layer is 3 - 80 gsm.

Citation Information

Patent Citations

  • Film prepared from waste thermoplastic elastomer and laminate thereof

    CN113105738A