Tungsten-containing material and dc discharge lamp electrode
By controlling the oxygen production amount and potassium content in the tungsten-containing material, the problem of low illuminance maintenance caused by excessive oxygen in the discharge lamp electrode is solved, and a more stable beam output and longer lamp life is achieved, which is suitable for high temperature conditions. high strength material applications.
Patent Information
- Application Number
- CN202380033063.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-15
- Filing Date
- 2023-04-11
- Publication Date
- 2024-11-19
AI Technical Summary
When used as discharge lamp electrodes, existing tungsten-containing materials have problems with low illuminance maintenance. This is mainly due to the high amount of oxygen generated under high temperature conditions that lead to the deformation and scattering of the material, which leads to blackening of the glass inside of the lamp and the light beam being reduced. In turn, shorten the life of the lamp.
The oxygen production amount between 2100°C and 2300°C and 20ppm or less is detected and controlled by the oxygen separator method, and potassium of 5ppm or less is added to the tungsten material to optimize the crystal grain size and density of the material to suppress oxygen The release and recrystallization properties of tungsten improve the stability and life of the material.
It effectively suppresses the blackening of the discharge lamp, improves the long-term maintenance ability of the light beam, extends the life of the lamp, and is suitable for high-intensity material needs under high temperature conditions, such as the furnace components of nuclear fusion furnaces.
Smart Images

Figure BDA0005074850590000081 
Figure HDA0005074850610000011
Abstract
Description
Technical Field
[0001] The present invention relates to a tungsten-containing material. This application claims priority based on Japanese patent application No. 2022-067481 filed on April 15, 2022. All the contents described in the Japanese patent application are incorporated herein by reference. Background Art
[0002] Conventionally, tungsten-containing materials are disclosed in, for example, Japanese Patent Application Laid-Open No. 2003-027111 (Patent Document 1), Japanese Patent Application Laid-Open No. 2007-169789 (Japanese Patent No. 5265867) (Patent Document 2), and Japanese Patent Application Laid-Open No. 2005-183355 (Japanese Patent No. 4167199) (Patent Document 3).
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2003-027111
[0006] Patent Document 2: Japanese Patent Application Publication No. 2007-169789
[0007] Patent Document 3: Japanese Patent Application Publication No. 2005-183355 Summary of the invention
[0008] A tungsten-containing material having an oxygen generation amount at 2100° C. to 2300° C. of more than 1 ppm and less than 20 ppm as detected by oxygen analysis based on an oxygen separator method, and containing potassium in an amount of 5 ppm to 30 ppm. BRIEF DESCRIPTION OF THE DRAWINGS
[0009] [ Figure 1 ] Figure 1 is a graph showing the relationship between the power and temperature of the oxygen separator used in the embodiment. DETAILED DESCRIPTION
[0010] [Problems to be Solved by the Present Disclosure]
[0011] Conventional tungsten-containing materials have a problem of low illuminance maintenance factor when used as discharge lamp electrodes.
[0012] Hereinafter, embodiments of the present invention will be described with reference to the drawings.
[0013] (1) Contents of this disclosure
[0014] Japanese Patent Publication No. 2007-169789 (Patent Document 2) discloses a method for manufacturing a component or semi-finished product having the following contents from a material containing a group of molybdenum, molybdenum alloy, tungsten and tungsten alloy: an average relative density greater than 98.55%; a relative core density greater than 98.3%; and a relative density greater than 100 grains / mm in a state deformed by processing and in a direction perpendicular to the direction of deformation due to processing. 2 The method comprises the following steps.
[0015] A step of preparing a powder having a particle size of 0.5 to 10 μm as measured by the Fischer method and a step of pressurizing the powder at a pressure of 100 to 500 MPa.
[0016] The process includes sintering at a temperature of (0.55 to 0.92) × the solidus temperature to make the relative density D become 90% < D < 98.5%, and performing hot isotropic pressing at a temperature of (0.40 to 0.65) × the solidus temperature and a pressure of 50 to 300 MPa without using a mold.
[0017] Through radial forging or rolling processing, the degree of forming become The forming process is carried out in a manner.
[0018] Japanese Patent Gazette No. 2003-027111 (Patent Document 1) discloses a method for manufacturing a high-melting-point metal material, wherein a casting made of at least one of Mo and W or an alloy containing at least one of Mo and W is plastically processed in a temperature range of 700°C to 1700°C in such a way that the cross-section becomes non-circular, thereby obtaining a high-melting-point metal material.
[0019] Japanese Patent Publication No. 2005-183355 (Patent Document 3) discloses a tungsten electrode characterized by containing less than 5 ppm of Si, 5 to 20 ppm of K, and 5 to 20 ppm of Al, with the remainder being substantially composed of tungsten, and having a diameter of more than 15 mm. A tungsten electrode for discharge lamps is disclosed, which has a density of 19100 kg / m 3 In the above, the area of the portion where the aspect ratio of the crystal grain size is 2 to 20 exceeds 50%.
[0020] Tungsten is one of the materials with a high melting point (melting point is about 3,400℃), and its characteristics can be effectively used for high-temperature furnace parts, filaments, discharge lamps, etc.
[0021] In particular, when used in a discharge lamp, a temperature load exceeding 2,500° C. is considered to be required, and tungsten to which potassium is added is often used as an electrode as a material capable of withstanding this load.
[0022] During use, the tip of the electrode of a discharge lamp using potassium-doped tungsten may be consumed and scattered by discharge, and impurities may be scattered / attached to the inner surface of the lamp glass, which is called blackening. In addition, the deformation of the tip may induce flickering of the light source generated by the discharge, resulting in a loss of stability required as a light source, and if the lamp is used for exposure of electronic component circuits, the life of the lamp will be shortened.
[0023] By adding potassium to tungsten, the recrystallization characteristics of the tungsten material are improved, and the growth of crystal grains at the tip of the electrode when the discharge lamp is turned on is also suppressed.
[0024] In Patent Documents 1 and 2, which are prior art, in order to improve the characteristics of the discharge lamp using the above technology, the amount of K added to tungsten is controlled, the specific gravity is increased, and the lamp life is improved by miniaturizing the recrystallized grains during use of the electrode.
[0025] In the present disclosure, it is found that the main cause of the reduction in the illuminance maintenance factor due to the blackening of the lamp is the oxygen generated in the tungsten material in a specific temperature range, and that the deformation and consumption / scattering of tungsten can be improved by reducing the amount of oxygen.
[0026] The anode of a DC discharge lamp used for semiconductor exposure and lighting uses tungsten material. However, the anode receives electrons and is heated to a high temperature. During the discharge of the lamp, the oxygen contained in the material reacts with tungsten and volatilizes / scatters in the form of a low-melting-point oxide, thereby blackening the inside of the lamp glass and causing a reduction in the light beam. The deformation also reduces the quality of the point light source required as an exposure power source, resulting in a short life.
[0027] When conventional tungsten materials are used for lamps, the scattering of tungsten and other impurities caused by oxygen components may cause the inside of the lamp glass to blacken, making it impossible to use stably.
[0028] In the present disclosure, novel production conditions are adopted to produce a tungsten-containing material in which the amount of oxygen contained in the material is controlled, preferably the amount of potassium and the crystal grain size are controlled.
[0029] The tungsten material disclosed herein can be used not only for electrodes of discharge lamps but also for furnace parts used at high temperatures such as nuclear fusion reactors, which require high-strength materials and hate the release of oxygen.
[0030] The tungsten-containing material disclosed herein has an oxygen generation amount at 2100° C. to 2300° C. of more than 1 ppm and less than 20 ppm as detected by oxygen analysis using an oxygen separator method, and contains 5 ppm to 30 ppm of potassium.
[0031] (2) Determination of oxygen release
[0032] When the amount of oxygen generated exceeds 20 ppm, the glass of the lamp may blacken during use of the lamp, shortening the life of the lamp. The amount of oxygen generated is more preferably 10 ppm or less.
[0033] The method for measuring the oxygen amount is as follows.
[0034] The weight of the material to be measured was 0.10 g to 1.00 g, and the material sampled from the center of the tungsten-containing material was used.
[0035] In the measurement, the amount of oxygen detected in a predetermined temperature range (2100°C to 2300°C) based on the oxygen separator function was evaluated as the amount of oxygen released at 2100°C to 2300°C.
[0036] The analysis conditions and parameters are as follows.
[0037] [condition]
[0038] Oxygen / nitrogen / hydrogen analyzer manufactured by LECO Japan Corporation, model: ON836
[0039] Carrier gas: Helium
[0040] Flux: Nickel particles
[0041] Crucible: Standard crucible
[0042] Analysis method: Non-dispersive infrared absorption method
[0043] [parameter]
[0044] Standardized sample: YY-001-114-00 (0.119%)
[0045] Analysis Mode: Automatic
[0046] Analysis delay: 45 seconds
[0047] Integration delay: 2 seconds
[0048] Comparator: Not used
[0049] Finish line: 2 seconds
[0050] Integration time: 500 seconds
[0051] Analysis power: It takes 400 seconds to ramp up from 100W to 6000W.
[0052] Figure 1 is a graph showing the relationship between the power and temperature of the oxygen separator used in the embodiment. Figure 1 The power value and temperature correspondence table shown is 2500℃.
[0053] (3) Method for determining composition, average grain size and density
[0054] The amount of potassium added to the tungsten material needs to be more than 5ppm and less than 30ppm. Potassium acts as a grain growth inhibitor for the electrode. When it is less than 5ppm, there is no grain growth inhibitory effect. When it exceeds 30ppm, it will affect the life of the discharge lamp. With the above potassium, the grain size of the tungsten material during recrystallization becomes less than 200μm. The measurement of the grain size is carried out on the RD plane (the plane perpendicular to the rolling direction). Specifically, a magnified photograph with a magnification of 200 times is taken at an arbitrary position near the center, and a certain length (1000μm) in the field of view is used as the numerator. The number of grain boundaries crossing the certain length is used as the denominator. The grain size in the field of view is calculated by using the intercept method (intercept method) of the grain size of the field of view by taking the value of the numerator / denominator as the grain size of the field of view. A total of 6 fields of view ( / each sample) are measured, and the average value of their grain sizes is taken as the grain size.
[0055] The method for determining the amount of potassium is as follows.
[0056] The mass of the material to be measured was 0.40 g, and the material sampled from the center of the tungsten material was used.
[0057] As sample pretreatment before measurement, acid washing was performed for 5 minutes using an acid (HNO3:HF:water = 1:1:1 (volume ratio)). Then, water washing was performed for 15 minutes. The dried sample after 15 minutes of water washing was placed in a platinum dish and 1 cm nitric acid was added. 3 , hydrofluoric acid 1cm 3 Then, add 10% by volume of lithium carbonate, heat to dissolve the oxide, and adjust the volume to 50 cm 3 The solution was used as the test sample solution.
[0058] The measuring instrument used was a flame atomic absorption spectrophotometer, model number: ContrAA300, manufactured by Analytik Jena Japan Co., Ltd. The composition was measured in accordance with JIS H1403:2001 (analysis method of tungsten materials). The atomic absorption method was used as the analysis method.
[0059] The tungsten-containing material may contain calcium, silicon, aluminum, magnesium, and potassium. The total content of these components other than tungsten is 30 ppm or more and 300 ppm or less. The determination method thereof is implemented according to JIS H1403:2001 (analysis method of tungsten material).
[0060] The density of the tungsten-containing material is measured by using the Archimedean principle to measure the mass in air and water, respectively, and to calculate the density by finding the volume from the two.
[0061] The tungsten-containing material preferably has a crystal grain size of 200 μm or less. When the crystal grain size is 200 μm or less, the illuminance maintenance factor is highest when used as a DC discharge lamp.
[0062] Preferably, the density of the tungsten-containing material is 19.1 g / cm 3 above.
[0063] Preferably, tungsten-containing materials are used for discharge lamp electrodes.
[0064] Preferably, the discharge lamp electrode is a DC discharge lamp electrode.
[0065] Example
[0066] A. Manufacturing of tungsten-containing materials (rods)
[0067] (A-1) Tungsten Sintered Body Manufacturing Process
[0068] [Preparation of raw materials]
[0069] Potassium is added to the tungsten raw material in the same way as potassium-added tungsten for general lighting, and potassium-containing tungsten powder is obtained by hydrogen reduction. The amount of potassium added is adjusted by acid washing the potassium-containing tungsten powder in an intermediate process as needed. The FSSS particle size of the potassium-containing tungsten powder based on the Fischer method is 2.2 to 2.4 μm.
[0070] [Heat treatment]
[0071] Since some oxygen still remained in the powder, the powder was further heat treated in a batch electric furnace at 700° C. for 10 hours in a hydrogen atmosphere, and then cooled to room temperature in hydrogen to obtain a tungsten powder low in oxygen and containing potassium.
[0072] The oxygen content in the conventional tungsten powder is 600 to 900 ppm, whereas the oxygen content in the low-oxygen potassium-containing tungsten powder is reduced to 150 to 250 ppm by the heat treatment.
[0073] [Pressing and sintering]
[0074] The powder was stored in a manner not to be exposed to oxygen in the atmosphere, put into a rubber mold for an isostatic press, and pressed at 180 MPa using an isostatic press to produce a compact. The compact was then shaped to produce a compact.
[0075] The formed body was primarily sintered in an argon atmosphere at 1500° C. for 10 hours using a hot isotropic press (HIP) apparatus, and the primary sintered body was sintered in a hydrogen atmosphere at 2,300° C. for 30 hours using a batch sintering furnace to obtain a tungsten sintered body (tungsten-containing material).
[0076] The size of the sintered body is 100 mm in diameter x 500 mm in length. The density after sintering is 18.3 g / cm 3 .
[0077] The content of silicon contained in the sintered body is less than 5 ppm.
[0078] As a result of various tests, the FSSS particle size is preferably 1 μm or more and 10 μm or less.
[0079] When the particle size exceeds 10 μm, the specific gravity of the sintered body decreases, and there is a possibility that the density cannot be increased to withstand plastic working. It should be noted that “maybe” means that there is a small but possible possibility, and does not mean that it will be so with a high probability.
[0080] When the particle size is less than 1 μm, the density during pressing will not increase, which may cause a decrease in specific gravity after sintering.
[0081] As long as the density of the sintered body is 17.5 g / cm 3 There is no limitation on the sintering method, but it is preferably 18.0 g / cm 3 above.
[0082] In addition to vacuum atmosphere, sintering atmosphere can also be selected from inert atmospheres such as argon and hydrogen atmosphere. As long as the density after sintering is 17.5g / cm 3 The above sintering atmospheres may be combined (for example, hydrogen atmosphere before 1,200°C, vacuum atmosphere between 1,200 and 2,000°C, etc.), and the sintering temperature and sintering time may be arbitrarily selected. It is preferred to perform the heat treatment at a sintering temperature of 2,300°C or higher.
[0083] (A-2) Processing steps
[0084] After heating the tungsten sintered body in hydrogen at 1,800°C in a heating furnace, it was forged using a die using a forging machine, and forged to a diameter of 80 mm in the first process, 70 mm in the second process, 60 mm in the third process, and 50 mm in the fourth process. At this time, heating was applied every time. This time, the material forged to 50 mm was heated at a heating furnace temperature of 1,800°C and processed by rotary swaging to a diameter of 40 to 15 mm. At this time, processing was performed while sampling at an arbitrary size.
[0085] The heating atmosphere during forging may be performed in an argon or hydrogen atmosphere in addition to a nitrogen atmosphere.
[0086] The heating temperature during forging is preferably 1,600° C. to 1,800° C. If the temperature exceeds 1,800° C., the life of the heating furnace is shortened, so that the productivity is not excellent.
[0087] The total processing rate is preferably 65% or more. However, as for the processing rate, as long as the final specific gravity exceeds 19.1, it is sufficient. If it is less than 19.1, the specific gravity may not be satisfied. In addition, the specific gravity exceeds 19.1 and is closer to the theoretical specific gravity of tungsten, the better.
[0088] Through the above steps, tungsten-containing materials (tungsten rods) of sample numbers 1 to 12 were produced.
[0089] [Table 1]
[0090]
[0091] The balance consists of tungsten.
[0092] Sample No. 13 is a sample with a low potassium content manufactured by the methods shown in (A-1) and (A-2) above. In this case, the crystal grain size becomes larger, and Sample No. 14 is a sample with a small specific gravity manufactured by the methods shown in (A-1) and (A-2) above. Sample No. 15 is a sample with a low specific gravity and slightly larger particles manufactured by the methods shown in (A-1) and (A-2) above. Sample No. 16 is a sample containing potassium manufactured by the methods shown in (A-1) (wherein [heat treatment] is not implemented) and (A-2). Sample No. 17 is a sample that does not contain potassium manufactured by the methods shown in (A-1) (wherein [heat treatment] is not implemented) and (A-2). Sample No. 18 is a sample containing a large amount of potassium manufactured by the methods shown in (A-1) (wherein [heat treatment] is not implemented) and (A-2).
[0093] B. Evaluation Results
[0094] In the life measurement of the discharge lamp, a 1kW DC discharge lamp was manufactured and evaluated for its illumination maintenance rate. For the anode of the discharge lamp, the tungsten material of sample numbers 1 to 15 manufactured in the "A. Manufacturing of tungsten rod" process was processed into a 30mm electrode for use. Tungsten containing 1% by mass of thorium was used as the cathode. In high-power discharge lamps, the life extension effect of the tungsten electrode disclosed in the present invention becomes obvious. Including the results of the lamp life, the amount of oxygen released, the potassium content, the average crystal grain size, the density and the illumination maintenance rate (lamp life) are shown in Table 1. Their measurement methods are based on "(2) Determination of oxygen release" and "(3) Composition, average crystal grain size and density measurement method".
[0095] As long as the tungsten material has the above characteristics, the same effect can be achieved with a diameter of several mm. There is no restriction on the manufacturing conditions. High temperature pressing machines (HIP, HP) can be used for sintering, and plastic processing methods are not limited to forging, rolling, extrusion, etc.
[0096] For tungsten materials, the same effect can be achieved not only by simply shaping them, but also by drilling holes or performing groove processing through mechanical processing.
[0097] In Table 1, the lamp life is represented by the illuminance maintenance rate after 750 hours of lighting. Assuming that the illuminance at the time of initial lighting is 100%, the illuminance judged to be unusable is less than 90%, 100% to 95% or more is set as A, less than 95% and 93% or more is set as B, less than 93% to 91% or more is set as C, and less than 91% is set as D.
[0098] In sample numbers 16 to 18, it was confirmed that the illumination maintenance rate decreased due to the influence of large oxygen release or coarse crystal grain size. Specifically, the oxygen release needs to be more than 1 ppm and less than 20 ppm. The oxygen release is preferably more than 4 ppm and less than 9 ppm. The potassium content needs to be more than 5 ppm and less than 30 ppm.
[0099] [Supplementary Note 1] A tungsten-containing material having an oxygen generation amount at 2100° C. to 2300° C. of more than 1 ppm and less than 20 ppm as detected by oxygen analysis using an oxygen separator method, and containing 5 ppm to 30 ppm of potassium.
[0100] [Note 2]
[0101] The tungsten-containing material according to Supplementary Note 1, wherein the crystal grain size is 200 μm or less.
[0102] [Note 3]
[0103] The tungsten-containing material according to Appendix 1 or 2, characterized in that the density is 19.1 g / cm 3 above.
[0104] [Note 4]
[0105] The tungsten-containing material according to any one of Supplementary Notes 1 to 3, which is used for a discharge lamp electrode.
[0106] [Note 5]
[0107] A DC discharge lamp electrode using the tungsten-containing material described in Supplementary Note 4.
[0108] The embodiments and examples disclosed herein are illustrative in all aspects and are not restrictive. The scope of the present invention is indicated by the claims rather than the above description, and is intended to include all modifications within the meaning and scope equivalent to the claims.
Claims
1. A tungsten-containing material, wherein the amount of oxygen generated at 2100° C. to 2300° C. as detected by oxygen analysis using an oxygen separator method exceeds 1 ppm and is 20 ppm or less, and the material contains potassium in an amount of 5 ppm to 30 ppm or less.
2. The tungsten-containing material according to claim 1, wherein: The crystal grain size is 200 μm or less.
3. The tungsten-containing material according to claim 1 or 2, characterized in that: Density: 19.1 g / cm 3 above.
4. The tungsten-containing material according to any one of claims 1 to 3, which is used for discharge lamp electrodes.