Transparent substrate with antireflection film, and image display device

By forming a diffusion layer on the transparent substrate and an anti-reflection film that meets the specific diffuse light value, the color deviation problem in large μ-LED displays is solved, and the color change control is achieved, which improves the taste and beauty of the display.

CN118984954AInactive Publication Date: 2024-11-19AGC INC
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202380032985.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-08
Filing Date
2023-04-05
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In large μ-LED displays, the existing transparent substrate with anti-reflection film has obvious color deviation due to the change in the color tone of diffuse reflected light, which affects the taste and beauty of the display.

Method used

By forming a diffusion layer and an anti-reflection film on one main surface of the transparent substrate, and satisfying the a* and b* value ranges of diffuse reflected light at a specific angle, ensuring that the tone changes are not easy to detect, and at the same time, the dielectric layer with a laminated structure is constructed. The anti-reflection film is used to suppress the tone changes of diffusely reflected light.

Benefits of technology

It realizes a transparent substrate with anti-reflective film that is not easy to detect when tiling, improves the taste and beauty of the display, and is suitable for image display devices such as large μ-LED displays.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118984954A_ABST
    Figure CN118984954A_ABST
Patent Text Reader

Abstract

The present invention relates to a transparent substrate with an antireflection film, which is provided with a transparent substrate having two main surfaces, and a diffusion layer and an antireflection film that are provided on one main surface of the transparent substrate in this order from the transparent substrate side, when the reflection of the other main surface of the transparent substrate is removed and the light source is incident on the one main surface side at an incident angle of 45 degrees, a * and b * of diffuse reflection light at angles of 15 degrees, 25 degrees, and 45 degrees with respect to specular reflection light satisfy the following formulae (1)-(3). (1)-8 < = a * < = 1 (2)-2 < = b * < = 6 (3) b * < =-1 * a *-1
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a transparent substrate with an antireflection film and an image display device having the same. Background Art

[0002] In recent years, for aesthetic reasons, a method has been adopted in which a transparent substrate such as a cover glass is provided in front of an image display device such as a liquid crystal display (LCD). Furthermore, in order to prevent external light from being reflected into the transparent substrate, a transparent substrate having an antireflection film (hereinafter also referred to as a transparent substrate with an antireflection film) is known. For example, Patent Document 1 discloses a transparent substrate with an antireflection film that has light absorption and insulating properties.

[0003] Furthermore, to prevent reflection of external light, it is also known to provide a diffusion layer on a transparent substrate. This diffusion layer diffuses incident light, thereby suppressing reflection. However, when used in an image display device, a transparent substrate with a diffusion layer can sometimes cause the image to appear whitish when the display is off due to the diffused light. Therefore, by further providing an anti-reflection film as described above on the diffusion layer, it is possible to suppress reflection of incident light and thus reduce the whitish appearance. This can effectively suppress reflection while enhancing the black texture of the image when the display is off.

[0004] However, μ-LED displays, which use μ-LED elements as light sources, have recently attracted attention as image display devices. Large μ-LED displays are manufactured by arranging and connecting (tiling) approximately 200 small A5-sized (148mm x 210mm) LED panels without gaps.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2018-115105 Summary of the Invention

[0008] As disclosed in Patent Document 1, the anti-reflection film utilizes optical interference, so the optical path length sometimes changes depending on the incident angle and the exit angle of the light, causing the reflected color (hue) to change in various ways. In particular, when the anti-reflection film is provided on the diffusion layer, light is easily diffusely reflected by the diffusion layer, so the change in hue caused by the angle tends to become more obvious. Moreover, in the case of manufacturing large μ-LED displays, when multiple LED panels are tiled, if the diffuse reflection color (hue of the diffusely reflected light) of each panel is different, there is a risk that the appearance will become a variety of colors, especially when the display is turned off, and the quality will be greatly reduced.

[0009] Therefore, an object of the present invention is to provide a transparent substrate with an antireflection film in which color deviation is hardly noticeable even when tiling is performed, and an image display device including the same.

[0010] The present inventors have found through experiments that the diffuse reflection light at various angles when light is incident on a transparent substrate with an anti-reflection film at a predetermined angle is * and b * The present invention has been completed by satisfying the prescribed requirements and providing a transparent substrate with an antireflection film in which color deviation is hardly noticeable when tiling.

[0011] That is, the present invention relates to the following 1 to 13.

[0012] 1. A transparent substrate with an anti-reflection film, comprising: a transparent substrate having two main surfaces; and a diffusion layer and an anti-reflection film provided on one main surface of the transparent substrate in this order from the transparent substrate side;

[0013] When the reflection from the other main surface of the transparent substrate is removed and the light source is incident on the one main surface at an incident angle of 45°, the a value of the diffuse reflected light at angles of 15°, 25° and 45° relative to the specular reflected light under a D65 light source is * and b * The following formulas (1) to (3) are satisfied.

[0014] (1)-8≤a * ≤1

[0015] (2)-2≤b * ≤6

[0016] (3)b * ≤-1×a * -1

[0017] 2. The transparent substrate with an antireflection film according to 1 above, wherein the haze value is 30% or more.

[0018] 3. The transparent substrate with an anti-reflection film according to 1 or 2 above, wherein the L of the diffusely reflected light at 15° is * is 15 to 35, and the L of the diffuse reflected light at 25° * 5 to 20.

[0019] 4. The transparent substrate with an antireflection film according to 1 or 2 above, wherein the light transmittance (Y) is 20 to 90%.

[0020] 5. The transparent substrate with an anti-reflection film according to 1 or 2 above, wherein the sheet resistance of the anti-reflection film is 10 4 Ω / □ or more.

[0021] 6. The transparent substrate with an anti-reflection film according to 1 or 2 above, wherein the transmission color b under D65 light source is * Below 5.

[0022] 7. A transparent substrate with an anti-reflection film according to 1 or 2 above, wherein the anti-reflection film has a stacked structure comprising at least two dielectric layers having different refractive indices, at least one of the dielectric layers being mainly composed of an oxide of Si, and at least one other layer of the layers of the stacked structure being mainly composed of a mixed oxide, wherein the mixed oxide is a mixed oxide of at least one oxide selected from Group A consisting of Mo and W and at least one oxide selected from Group B consisting of Si, Nb, Ti, Zr, Ta, Al, Sn, and In, and the content of the elements of Group B contained in the mixed oxide is 65% by mass or less relative to the total of the elements of Group A contained in the mixed oxide and the elements of Group B contained in the mixed oxide.

[0023] 8. The transparent substrate with an antireflection film according to 1 or 2 above, further comprising an antifouling film on the antireflection film.

[0024] 9. The transparent substrate with an antireflection film according to 1 or 2 above, wherein the transparent substrate comprises glass.

[0025] 10. The transparent substrate with an antireflection film according to 1 or 2 above, wherein the transparent substrate comprises at least one resin selected from the group consisting of polyethylene terephthalate, polycarbonate, acrylic, silicone, and triacetyl cellulose.

[0026] 11. The transparent substrate with an antireflection film according to 1 or 2 above, wherein the transparent substrate is a laminate of glass and at least one resin selected from the group consisting of polyethylene terephthalate, polycarbonate, acrylic, silicone, and triacetyl cellulose.

[0027] 12. The transparent substrate with an antireflection film according to 11 above, wherein the glass is chemically strengthened.

[0028] 13. An image display device comprising the transparent substrate with an antireflection film according to 1 or 2 above.

[0029] According to one embodiment of the present invention, a transparent substrate with an anti-reflection film and an image display device including the same can be provided, wherein color deviation is not noticeable even when the substrate is tiled. Since color deviation is not noticeable even when the substrate is tiled, the quality and aesthetics of the transparent substrate with an anti-reflection film and the image display device including the same can be improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1This is a cross-sectional view schematically showing a configuration example of a transparent substrate with an antireflection film according to one embodiment of the present invention.

[0031] Figure 2 is an example of diffuse reflection light at each angle * and b * Schematic diagram of the determination method.

[0032] Figure 3 is a representing the diffuse reflection light at each angle in each example * and b * Graph of the measurement results. DETAILED DESCRIPTION

[0033] The present invention will be described in detail below, but the present invention is not limited to the following embodiments and can be arbitrarily deformed and implemented without departing from the scope of the present invention. In addition, the " to " indicating a numerical range is used to include the numerical value recorded before and after it as the meaning of the lower limit and upper limit.

[0034] It should be noted that, in this specification, the presence of another layer, film, etc. on the principal surface of a substrate such as a transparent substrate, on a layer such as a diffusion layer, or on a film such as an antireflection film is not limited to a configuration in which the other layer, film, etc. is disposed in contact with the principal surface, layer, or film; any configuration in which the layer, film, etc. is disposed above the principal surface, layer, or film is sufficient. For example, the presence of a diffusion layer on the principal surface of a transparent substrate may mean that the diffusion layer is disposed in contact with the principal surface of the transparent substrate, or another arbitrary layer, film, etc. may be disposed between the transparent substrate and the diffusion layer.

[0035] A transparent substrate with an antireflection film according to one embodiment of the present invention comprises: a transparent substrate having two main surfaces; and a diffusion layer and an antireflection film provided on one main surface of the transparent substrate in this order from the transparent substrate side; when the reflection from the other main surface of the transparent substrate is removed and a light source is incident on the one main surface side at an incident angle of 45°, the diffuse reflection light at angles of 15°, 25°, and 45° relative to the specular reflection light under a D65 light source is a * and b * The following formulas (1) to (3) are satisfied.

[0036] (1)-8≤a * ≤1

[0037] (2)-2≤b * ≤6

[0038] (3)b * ≤-1×a * -1

[0039] (Transparent substrate with anti-reflection film)

[0040] Figure 1This is a cross-sectional view schematically showing a configuration example of a transparent substrate with an antireflection film according to one embodiment of the present invention. Figure 1 The illustrated transparent substrate 1 with an antireflection film includes a transparent substrate 10 , a diffusion layer 31 , and an antireflection film 30 . Figure 1 In the embodiment, a diffusion layer 31 is formed on one main surface of a transparent substrate 10, and an antireflection film 30 is formed on the diffusion layer 31. The antireflection film is, for example, a multilayer film having a laminated structure in which at least two dielectric layers having different refractive indices are laminated. Figure 1 In the embodiment, the anti-reflection film 30 is a multilayer film formed by stacking a first dielectric layer 32 and a second dielectric layer 34. Figure 1 In the embodiment, a diffusion layer 31 is further formed on the transparent substrate 10 . However, as described later, a diffusion layer may be formed on the surface of the transparent substrate itself by performing a surface treatment on the transparent substrate.

[0041] A transparent substrate with an antireflection film according to one embodiment of the present invention comprises a diffusion layer and an antireflection film on one principal surface of the transparent substrate in this order from the transparent substrate side. This provides a transparent substrate with an antireflection film having an excellent blackened texture, suppressing reflection of external light and whitening caused by diffusely reflected light.

[0042] In the transparent substrate with an antireflection film according to one embodiment of the present invention, when the reflection from the other main surface of the transparent substrate is eliminated and a light source is incident on one main surface at an incident angle of 45°, the a of the diffusely reflected light at angles of 15°, 25°, and 45° relative to the specularly reflected light under a D65 light source is * and b * The following formulas (1) to (3) are satisfied.

[0043] (1)-8≤a * ≤1

[0044] (2)-2≤b * ≤6

[0045] (3)b * ≤-1×a * -1

[0046] In this specification, the "diffuse reflected light at each angle of 15°, 25°, and 45°" obtained by the above method may be referred to as "diffuse reflected light at each angle". In addition, when it is referred to as "diffuse reflected light at 15°", it means the diffuse reflected light at 15° among the "diffuse reflected light at each angle", and the same applies to the case where the angle is different. In addition, unless otherwise specified, a * 、b * and L * Refers to a under D65 light source * 、b * and L* .

[0047] Figure 2 is an example of diffuse reflection light at each angle * and b * Schematic diagram of the determination method. Figure 2 In the transparent substrate 1 with an anti-reflection film shown in FIG. 1 , the transparent substrate 10 includes one main surface 11 and another main surface 12. A diffusion layer 31 and an anti-reflection film 30 are formed on the one main surface 11. Figure 2 In the exemplified measurement method, the transparent substrate 1 with an anti-reflection film removes the reflection of the other main surface by sticking a black tape 20 on the other main surface 12. Light is incident from a light source 50 to one main surface 11 side of the transparent substrate 1 with an anti-reflection film at an incident angle of 45°. As the incident light source, a light source that emits light in the entire visible light region is used. As the light source, a white light source such as a high color rendering white LED is appropriately used. Taking the mirror reflection light 61 of the incident light 60 as the reference (0°), the diffuse reflection lights 72, 73 and 74 are diffuse reflection lights of 15°, 25° and 45° respectively. It should be noted that here, the mirror reflection light 61 is set to 0°, the direction in which the angle of the side where the incident light 60 is located increases is set to the + direction, and the direction in which the angle of the side opposite to the incident light 60 increases is set to the - direction. For the diffuse reflection light at each of these angles, the reflectivity of the visible light wavelength is measured, and the L under the D65 light source is calculated. * 、a * and b * This measurement can be performed using, for example, CM-M6 manufactured by Konica Minolta. As a method for removing the reflection of the other main surface, Figure 2 As an example, a method of laminating black tape to the other main surface can be cited. As an example of black tape for removing reflection from the other main surface, "Kutsukirimiel" manufactured by Tomogawa Paper Co., Ltd. can be cited. The black tape used has a low diffuse reflectance and has little effect on the diffuse reflectance measurement of the surface having the anti-reflection film on the transparent substrate.

[0048] The inventors conducted in-depth research and found through experiments that the diffuse reflection of light at various angles is * and b * By satisfying the above formulas (1) to (3), a transparent substrate with an anti-reflection film in which color deviation is not easily noticeable when tiling can be obtained, thereby completing the present invention. * and b * Different from each other means that the color tone changes depending on the angle at which the transparent substrate with the anti-reflection film is observed. In this way, the color tone changes depending on the observation angle, which usually causes the color deviation to be noticeable when the substrate is tiled. However, the present invention has found that when the a of the diffusely reflected light at each angle is * and b *When the above equations (1) to (3) are satisfied, the change in color tone when the angle is changed is not easily noticeable. The reason is presumably as follows. That is, when the a of the diffusely reflected light at each angle is * and b * When the above formulas (1) to (3) are satisfied, the hue changes from colorless to green depending on the viewing angle. * and b * The difference is not easy to feel due to the angle, and the color deviation is not easy to detect. * and b * By limiting the range of possible variations, the magnitude of the color change due to angle becomes smaller, and thus, it is thought that color deviation becomes less noticeable. Furthermore, by satisfying the above equations (1) to (3), the color difference between adjacent transparent substrates with anti-reflection coatings on both sides when tiled is limited, and it is also expected that the joints between multiple substrates will be less noticeable.

[0049] a of diffuse reflected light at various angles * -8≤a * ≤1. From the perspective of improving the black feeling when the display is turned off, a * On the other hand, from the viewpoint of maintaining the reflected color in the range of colorless to green, a * It is 1 or less, preferably 0.8 or less, and more preferably 0.6 or less.

[0050] b of diffuse reflected light at various angles * -2≤b * ≤6. From the perspective of maintaining the reflected color in the range of colorless to green, b * On the other hand, from the perspective of improving the black feeling when the display is turned off, b * It is 6 or less, preferably 5 or less, and more preferably 4 or less.

[0051] a of diffuse reflected light at various angles * and b * Satisfy b * ≤-1×a * 1. This keeps the reflected color from colorless to green, so it is preferable. * and b * Preferably satisfy b * ≤-1×a * -1.2, preferably satisfying b * ≤-1×a * -1.5.

[0052] Among the diffuse reflection lights at various angles, the diffuse reflection lights at angles close to the specular reflection lights of the incident light, for example, the diffuse reflection lights at angles of 15° and 25°, have a higher brightness (L) than the diffuse reflection lights at angles of 45°. * Moreover, the color of the diffuse reflected light with high brightness is more likely to be felt more strongly than the color of the diffuse reflected light without such brightness. From this point of view, the a of the diffuse reflected light at 15° and 25° is preferably * and b * A value close to zero or a smaller value of L* is achieved. This appropriately controls the color tone of light at an angle that is more strongly perceived in diffusely reflected light, thereby making color deviation less noticeable.

[0053] L under D65 light source with 15° diffuse reflection * It is preferably 15 to 35, more preferably 20 to 30. The L value of the diffuse reflected light under the D65 light source at 15° is * It is preferably 15 or more, more preferably 20 or more. In addition, the L value of the diffuse reflected light at 15° under the D65 light source is * It is preferably 35 or less, more preferably 30 or less. The L value of the diffusely reflected light at 15° is * In this range, the transparent substrate with an antireflection film has appropriate light diffusing properties (anti-glare properties) or low reflectivity, and can appropriately suppress reflection of external light.

[0054] L under D65 light source with 25° diffuse reflection * It is preferably 5 to 20, more preferably 7 to 15. L under D65 light source of diffuse reflected light at 25° * It is preferably 5 or more, more preferably 7 or more. L under D65 light source of 25° diffuse reflected light * It is preferably 20 or less, more preferably 15 or less. The L of the diffusely reflected light at 25° is * In this range, the transparent substrate with an antireflection film has appropriate light diffusing properties (anti-glare properties) or low reflectivity, and can appropriately suppress reflection of external light.

[0055] In addition, it is preferred that the L of the diffuse reflected light at 15° * is 15 to 35, and the L of the diffuse reflected light at 25° * 5 to 20. As a result, the transparent substrate with the anti-reflection film has more appropriate light diffusion (anti-glare) or low reflectivity, and can appropriately suppress the reflection of external light. * By with a * and b * The same method can be used to measure and calculate using, for example, CM-M6 manufactured by Konica Minolta Inc.

[0056] In the transparent substrate with an antireflection film according to one embodiment of the present invention, the haze value is preferably 30% or greater, more preferably 40% or greater, and even more preferably 50% or greater, from the perspective of adequately preventing reflection. From the perspective of improving image clarity when used in an image display device, the haze value is preferably, for example, 90% or less. The haze value may range from 30% to 90%.

[0057] A transparent substrate with an anti-reflection film having a relatively high haze value as described above is suitable for use in large μ-LED displays. The reason for this is that, first, when the display is large, it is more likely to cause reflections of lighting and external light, so it is required to more appropriately prevent reflections. Furthermore, secondly, in large μ-LED displays, the pixel pitch is relatively large, so even if the haze value is relatively high, it is easy to become a high-definition display. However, in a transparent substrate with an anti-reflection film having such a high haze value, the diffuse reflection component becomes more, so the change in color tone caused by the angle of the diffusely reflected light tends to become particularly significant. In contrast, according to the present invention, even in the case of a high haze value, color deviation during tiling can be appropriately suppressed.

[0058] It should be noted that in applications such as LCD displays, for example, a transparent substrate with an antireflection film having a haze value of about 0 to 30% is suitably used. Depending on the application, etc., the haze value may be, for example, 30% or less, or even lower, as long as it is within the range that can achieve the effects of the present invention.

[0059] The haze value can be adjusted by, for example, the surface shape of the diffusion layer. The haze value is measured using a haze meter (HZ-V3 manufactured by Suga Test Instruments Co., Ltd.) or the like in accordance with JIS K 7136:2000.

[0060] (Light transmittance: Y)

[0061] The light transmittance (Y) of the transparent substrate with an anti-reflection film of this embodiment is preferably 20 to 90%. If the light transmittance (Y) is within the above range, it has appropriate light absorption capacity, so when used as a cover glass of an image display device, it is possible to suppress light reflection. As a result, the contrast of the bright area of ​​the image display device is improved. The above light transmittance (Y) is more preferably 50 to 90%, and further preferably 60 to 90%. That is, the light transmittance (Y) is preferably 20% or more, more preferably 50% or more, and further preferably 60% or more. The light transmittance (Y) is preferably 90% or less.

[0062] In addition, the light transmittance (Y) can be measured by the method specified in JIS Z 8701 (1999) as described in Examples below.

[0063] In the transparent substrate with an anti-reflection film of this embodiment, in order to make the light transmittance (Y) 20 to 90%, it is preferred to mainly use a mixed oxide of at least one oxide selected from Group A consisting of Mo and W and at least one oxide selected from Group B consisting of Si, Nb, Ti, Zr, Ta, Al, Sn and In as the first dielectric layer of the anti-reflection film and adjust the oxidation amount of the film.

[0064] The light transmittance (Y) in the transparent substrate with anti-reflection film of this embodiment can be adjusted by controlling the irradiation time, irradiation output, distance from the substrate, and oxidizing gas amount of the oxidation source when forming the first dielectric layer as the high refractive index layer in the above-mentioned anti-reflection film.

[0065] (Sheet resistance)

[0066] In the transparent substrate with an anti-reflection film of this embodiment, the sheet resistance of the anti-reflection film is preferably 10 4 Ω / □ or more. Since the sheet resistance of the anti-reflection film is within the above range and the anti-reflection film is insulating, when used as a cover glass for an image display device, even when a touch panel is applied, the capacitance change caused by finger contact required for a capacitive touch sensor can be maintained, allowing the touch panel to function. The sheet resistance is more preferably 10 6 Ω / □ or more, more preferably 10 8 Ω / □ or more.

[0067] In addition, the sheet resistance can be measured by the method specified in JIS K 6911 (2006) as described in Examples below.

[0068] In the transparent substrate with an anti-reflection film of this embodiment, in order to make the sheet resistance of the anti-reflection film 10 4 Ω / □ or more, for example, by adjusting the metal content in the anti-reflection film.

[0069] (b in the transmitted color under D65 light source * value)

[0070] In the transparent substrate with an anti-reflection film of this embodiment, the b in the transmission color under the D65 light source is * The value is preferably 5 or less. * If the value is within the above range, the transmitted light will not have a yellowish tint, so it is suitable for use as a cover glass for image display devices. * The value is more preferably 3 or less, and further preferably 2 or less. * The lower limit of the value is preferably -6 or more, more preferably -4 or more. * The value is within the above range, because the transmitted light becomes colorless and does not block the transmitted light, so it is preferred.* The value can be -6 to 5.

[0071] It should be noted that the b in the transmitted color under D65 light source * The value can be measured by the method specified in JIS Z 8729 (2004).

[0072] (Transparent substrate)

[0073] The refractive index of the transparent substrate having two main surfaces in this embodiment (hereinafter referred to as the transparent substrate) is preferably 1.4 to 1.7. If the refractive index of the transparent substrate is within this range, reflection from the bonding surface can be sufficiently suppressed during optical bonding of displays, touch panels, etc. The refractive index is more preferably 1.45 or greater, and even more preferably 1.47 or greater. Furthermore, it is more preferably 1.65 or less, and even more preferably 1.6 or less.

[0074] The transparent substrate preferably comprises at least one of glass and resin. More preferably, the transparent substrate comprises both glass and resin. By comprising glass in the transparent substrate, the strength, flatness, and durability of the transparent substrate with the anti-reflection film can be made excellent. In addition, by laminating the laminate formed by the resin substrate and the anti-glare layer described later to the glass substrate, a diffusion layer can be easily formed. In the transparent substrate with the anti-reflection film formed with the diffusion layer by this method, the transparent substrate comprises both glass and resin.

[0075] When the transparent substrate comprises glass, the type of glass is not particularly limited, and glasses having various compositions can be used. The glass preferably contains sodium and preferably has a composition that is moldable and can be strengthened by chemical strengthening treatment. Specific examples of such glass include aluminosilicate glass, soda-lime glass, borosilicate glass, lead glass, alkali-barium glass, and aluminoborosilicate glass.

[0076] In addition, in this specification, when a transparent substrate is made of glass, the transparent substrate is also referred to as a glass substrate.

[0077] The thickness of the glass substrate is not particularly limited. For efficient chemical strengthening during chemical strengthening, the thickness is preferably 5 mm or less, more preferably 3 mm or less, and even more preferably 1.5 mm or less. Alternatively, the thickness may be, for example, 0.2 mm or greater. The thickness of the glass substrate can range from 0.2 mm to 5 mm.

[0078] The glass substrate is preferably chemically strengthened glass. This improves the strength of the transparent substrate with the anti-reflection film. It should be noted that when the glass substrate is subjected to the anti-glare treatment described below, chemical strengthening is preferably performed after the anti-glare treatment and before the anti-reflection film (multilayer film) is formed.

[0079] When the transparent substrate includes a resin, the type of resin is not particularly limited, and resins with various compositions can be used. Among them, the above-mentioned resin is preferably a thermoplastic resin or a thermosetting resin, for example, polyvinyl chloride resin, polyethylene resin, polypropylene resin, polystyrene resin, polyvinyl acetate resin, polyester resin, polyurethane resin, cellulose resin, acrylic resin, AS (acrylonitrile-styrene) resin, ABS (acrylonitrile-butadiene-styrene) resin, fluorine resin, thermoplastic elastomer, polyamide resin, polyimide resin, polyacetal resin, polycarbonate resin, modified polyphenylene ether resin, polyethylene terephthalate resin, polybutylene terephthalate resin, polylactic acid resin, cyclic polyolefin resin, polyphenylene sulfide resin, etc. Among them, preferred cellulose resin, triacetyl cellulose resin, polycarbonate resin, polyethylene terephthalate resin, etc. can be mentioned. These resins can be used alone or in combination of two or more.

[0080] In terms of excellent visible light transparency and easy availability, the resin particularly preferably includes at least one resin selected from the group consisting of polyethylene terephthalate, polycarbonate, acrylic acid, silicone, and triacetyl cellulose.

[0081] In addition, in this specification, when a transparent substrate contains a resin, the transparent substrate is also referred to as a resin substrate.

[0082] The resin substrate is preferably in the form of a film. When the resin substrate is in the form of a film, that is, a resin film, its thickness is not particularly limited, but is preferably 20 to 300 μm, more preferably 30 to 130 μm.

[0083] The transparent substrate may be a composite substrate composed of a glass substrate and a resin substrate laminated together. More specifically, the transparent substrate may be a glass substrate provided with the resin substrate.

[0084] (Diffusion layer)

[0085] The diffusion layer in this embodiment is provided on one main surface of the transparent substrate. The diffusion layer is a layer that diffuses specularly reflected light to reduce glare and reflection, and an anti-glare layer is an example of a hard coat layer that has been given a specularly reflected light diffusion function (anti-glare properties).

[0086] The anti-glare layer has a concavo-convex shape on one side, utilizing external or internal scattering to increase the haze value and impart anti-glare properties. The anti-glare layer is formed from an anti-glare layer composition, which is formed by dispersing a particulate substance that at least inherently has anti-glare properties in a solution containing a polymer resin as a binder. The anti-glare layer can be formed by applying the anti-glare layer composition to one main surface of a transparent substrate, for example.

[0087] Examples of the above-mentioned particulate substances having anti-glare properties include inorganic fine particles such as silica, clay, talc, calcium carbonate, calcium sulfate, barium sulfate, aluminum silicate, titanium oxide, synthetic zeolite, alumina, and montmorillonite, and organic fine particles containing styrene resins, polyurethane resins, benzoguanamine resins, silicone resins, acrylic resins, and melamine resins.

[0088] In addition, as the polymer resin of the binder of the above-mentioned hard coat layer or the above-mentioned anti-glare layer, for example, a polymer resin containing polyester resin, acrylic resin, acrylic urethane resin, polyester acrylate resin, polyurethane acrylate resin, epoxy acrylate resin, urethane resin, etc. can be used.

[0089] In this method, the diffusion layer can be formed directly on a transparent substrate, or a laminate composed of a resin substrate and an anti-glare layer can be prepared in advance and attached to a glass substrate, etc., thereby obtaining a structure in which the diffusion layer is provided on a composite substrate of a glass substrate and a resin substrate. The diffusion layer is preferably formed on a film-like resin substrate in this laminate. This method facilitates and facilitates the formation of the diffusion layer.

[0090] Specific examples of the laminate consisting of a resin matrix and an anti-glare layer include anti-glare PET films and anti-glare TAC films. Examples of the anti-glare PET film include BHC-III and EHC-30a manufactured by Higashiyama Film Co., Ltd. and products manufactured by Reiko Co., Ltd. In addition, examples of the anti-glare TAC film include anti-glare TAC film (manufactured by TOPPAN TOMOEGAWAOPTICAL FILMS, trade name VZ50) and anti-glare TAC film (manufactured by TOPPAN TOMOEGAWA OPTICAL FILMS, trade name VH66H).

[0091] Alternatively, the diffusion layer may be formed on the surface of the transparent substrate itself by subjecting the transparent substrate to a surface treatment.

[0092] For example, when a glass substrate is used, a method of forming desired irregularities by surface treatment on the main surface of the glass can be used.

[0093] Specifically, a method of chemically treating the main surface of the glass substrate includes, for example, frosting. The frosting may be performed by immersing the glass substrate as a treatment object in a mixed solution of hydrogen fluoride and ammonium fluoride to chemically treat the immersed surface.

[0094] In addition, in addition to chemical treatment methods such as frosting, physical treatment methods such as so-called sandblasting, in which crystalline silica powder, silicon carbide powder, etc. are blown onto the surface of the glass substrate with pressurized air, or rubbing a brush with crystalline silica powder, silicon carbide powder, etc. wetted with water, can also be used.

[0095] A transparent substrate with an anti-reflection film having such a diffusion layer has a surface irregularity due to the irregularities of the diffusion layer. The Sa (arithmetic mean surface roughness) of the transparent substrate with an anti-reflection film is preferably 0.05 to 0.6 μm, more preferably 0.05 to 0.55 μm. This Sa range is preferred because it easily suppresses reflections of reflected images. Sa is specified in ISO 25178 and can be measured, for example, using a KEYENCE VK-X3000 laser microscope.

[0096] For a transparent substrate with an antireflection film, the developed area ratio Sdr (hereinafter also referred to as "Sdr") calculated from the surface area obtained by measurement using a laser microscope VK-X3000 manufactured by KEYENCE is preferably 0.001 to 0.4, and more preferably 0.0025 to 0.2. When the Sdr is within this range, reflection of the reflected image is easily suppressed, which is preferred.

[0097] Sdr is defined in ISO 25178 and is expressed by the following formula.

[0098] Development area ratio Sdr = {(AB) / B}

[0099] A: Surface area (developed area) reflecting actual concavity and convexity in the measurement area

[0100] B: The area of ​​the flat surface without unevenness in the measurement area

[0101] The Sdq (root mean square slope) of the transparent substrate with an antireflection film is preferably 0.03 to 0.50, more preferably 0.07 to 0.49. This range of Sdq is preferred because it helps suppress reflections of reflected images. Sdq is specified in ISO 25178 and can be measured, for example, using a KEYENCE laser microscope VK-X3000.

[0102] The Spc (average of the principal curvatures of the surface peaks) of the transparent substrate with an antireflection film is preferably 150 to 6000 (1 / mm). This Spc range is preferred because it is easier to suppress reflections of reflected images. Spc is specified in ISO 25178 and can be measured, for example, using a KEYENCE laser microscope VK-X3000.

[0103] In addition, the above-mentioned Sa, Sdr, Sdq, and Spc are values ​​measured on the main surface of the transparent substrate with an antireflection film on the side provided with the diffusion layer and the antireflection film.

[0104] (Barrier layer)

[0105] In the case where the transparent substrate includes a resin substrate, such as when a diffusion layer is formed by laminating a laminate composed of a resin substrate and an anti-glare layer to a glass substrate, it is preferable to have a barrier layer between the diffusion layer and the anti-reflection film. By providing the barrier layer between the transparent resin substrate and the anti-reflection film, it is preferable because it has the advantages of being able to suppress the influence of moisture and oxygen that attempt to penetrate the anti-reflection film from the resin substrate, and the optical properties are less likely to change. Examples of the barrier layer include metal nitride films, metal oxide films, and more specifically SiN films. x Film, SiO x However, from the viewpoint of more effectively suppressing the change of optical characteristics, SiN x To prevent moisture and other substances from penetrating the anti-reflection film, the barrier layer preferably has a thickness of 2 nm or greater, more preferably 4 nm or greater, and particularly preferably 8 nm or greater. On the other hand, to prevent an increase in the reflectivity of the transparent substrate with the anti-reflection film, the thickness is preferably 50 nm or less. The barrier layer can be formed using known film-forming methods such as sputtering, vacuum evaporation, and coating.

[0106] (Anti-reflective film)

[0107] The antireflection film in this embodiment has a function of suppressing reflection of light, and has a laminated structure in which at least two dielectric layers having mutually different refractive indices are laminated, for example.

[0108] Figure 1 The anti-reflection film (multilayer film) 30 shown is a laminated structure formed by laminating two layers of a first dielectric layer 32 and a second dielectric layer 34 having different refractive indices. By laminating the first dielectric layer 32 and the second dielectric layer 34 having different refractive indices, the reflection of light is suppressed. For example, Figure 1 The first dielectric layer 32 is a high refractive index layer, and the second dielectric layer 34 is a low refractive index layer.

[0109] The antireflection film has a laminated structure comprising at least two dielectric layers having different refractive indices. At least one of the dielectric layers is primarily composed of a Si oxide, and at least one other layer in the laminated structure is primarily composed of a mixed oxide comprising at least one oxide selected from Group A consisting of Mo and W and at least one oxide selected from Group B consisting of Si, Nb, Ti, Zr, Ta, Al, Sn, and In. The content of the elements of Group B in the mixed oxide is preferably 65% ​​by mass or less relative to the total of the elements of Group A and Group B contained in the mixed oxide. Furthermore, the layer primarily composed of Si oxide may contain at least one oxide selected from Nb, Ti, Zr, Ta, Al, Sn, W, Mo, and In, within a range that does not affect reflectivity. The above-described antireflection film structure provides an insulating antireflection film having uniform light absorption in the visible light range. Since the anti-reflection film has light absorption capability, for example, in a structure in which the anti-reflection film is formed on the diffusion layer, light reflected by the surface of the diffusion layer (i.e., closer to the transparent substrate than the anti-reflection film) can be absorbed to a certain extent. As a result, the whitening caused by diffuse reflection in the diffusion layer can be more effectively suppressed, and thus the black texture when the screen is turned off when used in an image display device can be further improved. In addition, since the anti-reflection film is insulating, the transparent substrate with the anti-reflection film can also be preferably used for applications such as touch panels. In addition, by setting the content of the dielectric layer to an appropriate range, even in harsh environments such as high temperature environments such as 80°C and 95°C, high temperature and high humidity environments such as temperature and humidity of 65°C 95% and 85°C 85%, environments irradiated with strong UV light, and environments exposed to rain, an anti-reflection film with little change in optical properties and appearance can be obtained.

[0110] Figure 1 In the illustrated antireflection film (multilayer film) 30, the first dielectric layer 32 (high refractive index layer) is preferably primarily composed of a mixed oxide comprising at least one oxide selected from Group A consisting of Mo and W and at least one oxide selected from Group B consisting of Si, Nb, Ti, Zr, Ta, Al, Sn, and In. Furthermore, the content of the elements of Group B in the mixed oxide (hereinafter referred to as the Group B content) relative to the total of the elements of Group A and Group B contained in the mixed oxide is preferably 65% ​​by mass or less. Here, "primarily" refers to the component with the highest content (by mass) in the first dielectric layer 32, for example, containing 70% by mass or more of the component.

[0111] If the content of group B in the first dielectric layer (ABO) 32 composed of a mixed oxide of at least one oxide selected from group A consisting of Mo and W and at least one oxide selected from group B consisting of Si, Nb, Ti, Zr, Ta, Al, Sn and In is less than 65 mass%, the yellowing of the transmitted light can be suppressed.

[0112] The at least one oxide selected from Group A is preferably Mo or Mo and W, and the at least one oxide selected from Group B is preferably Nb. That is, the first dielectric layer is preferably a mixed oxide of Mo and Nb or a mixed oxide of Mo, W, and Nb, and more preferably a mixed oxide of Mo, W, and Nb.

[0113] As described later, the second dielectric layer can be, for example, an oxygen-deficient silicon oxide layer. Conventionally, oxygen-deficient silicon oxide layers have a yellowish tint in visible light. However, if the first dielectric layer is a mixed oxide of Mo and Nb or a mixed oxide of Mo, W, and Nb, the yellowing of the silicon oxide layer can be suppressed, and thus it is preferred. Furthermore, to improve reliability, the silicon oxide layer can contain at least one oxide selected from Nb, Ti, Zr, Ta, Al, Sn, W, Mo, and In, and each oxide can also be oxygen-deficient. Furthermore, when forming the second dielectric layer on a diffusion layer having a high haze, i.e., a large surface unevenness, as described above, high oxidation stability is required during film formation. If the first dielectric layer is a mixed oxide of Mo, W, and Nb, excellent oxidation stability during film formation is likely to be achieved, which is more preferred.

[0114] From the viewpoint of transmittance with the transparent substrate, the refractive index of the first dielectric layer 32 at a wavelength of 550 nm is preferably 1.8 to 2.3.

[0115] The extinction coefficient of the first dielectric layer 32 is preferably 0.005 to 3, more preferably 0.04 to 0.38. An extinction coefficient of 0.005 or greater allows for achieving the desired absorptivity with an appropriate number of layers. Furthermore, an extinction coefficient of 3 or less facilitates achieving a balance between reflective tone and transmittance.

[0116] The second dielectric layer 34 (low refractive index layer) is preferably mainly composed of Si oxide (SiO x Here, "mainly" refers to the component with the largest content (by mass) in the second dielectric layer 34, for example, it contains 70% by mass or more of the component. The second dielectric layer 34 (low refractive index layer) is mainly composed of Si oxide (SiO x ) structure, becomes low refractive index, and the reflectivity reduction effect becomes high, so it is preferred. It should be noted that SiO xCompletely oxidized silicon oxide (SiO2) may also be used, but oxygen-deficient silicon oxide is preferred from the perspective of improving optical reliability and scratch resistance. Furthermore, to improve reliability, the silicon oxide layer may contain at least one oxide selected from the group consisting of Nb, Ti, Zr, Ta, Al, Sn, W, Mo, and In, and each oxide may also be oxygen-deficient.

[0117] Figure 1 The anti-reflection film (multilayer film) 30 shown is a stacked structure of two layers in total formed by stacking a first dielectric layer 32 and a second dielectric layer 34, but the anti-reflection film (multilayer film) in this embodiment is not limited to this, and can also be a stacked structure formed by stacking more than three dielectric layers with different refractive indices. In this case, it is not necessary for all dielectric layers to have different refractive indices. That is, the stacked structure can be a stacked structure formed by stacking more than two dielectric layers in a manner where the refractive indices of adjacent layers are different, and the number of stacked layers can also be more than three layers. For example, in the case of a three-layer stacked structure, it can be a three-layer stacked structure of a low refractive index layer, a high refractive index layer, and a low refractive index layer, or a three-layer stacked structure of a high refractive index layer, a low refractive index layer, and a high refractive index layer. In the former case, the two low refractive index layers can have the same refractive index as each other, and in the latter case, the two high refractive index layers can have the same refractive index as each other. In the case of a four-layer stacked structure, it can be a four-layer stacked structure of a low refractive index layer, a high refractive index layer, a low refractive index layer, and a high refractive index layer, or a four-layer stacked structure of a high refractive index layer, a low refractive index layer, a high refractive index layer, and a low refractive index layer. In this case, at least one of the low refractive index layers and the high refractive index layers that are respectively present in two layers can have the same refractive index.

[0118] In the case of a laminated structure in which three or more layers having different refractive indices are laminated, the laminated structure may include the first dielectric layer (ABO) 32 and the second dielectric layer (SiO x ) 34. In this case, the first dielectric layer (ABO) 32 and the second dielectric layer (SiO x )34, including a three-layer stacked structure of a low refractive index layer, a high refractive index layer, and a low refractive index layer, or a three-layer stacked structure of a high refractive index layer, a low refractive index layer, and a high refractive index layer, or a four-layer stacked structure of a low refractive index layer, a high refractive index layer, a low refractive index layer, and a high refractive index layer, or a four-layer stacked structure of a high refractive index layer, a low refractive index layer, a high refractive index layer, and a low refractive index layer.

[0119] Among them, the outermost layer is preferably the second dielectric layer (SiO x )34. In order to obtain low reflectivity, if the outermost layer is the second dielectric layer (SiO x), it can be made relatively easily. In addition, the reflectivity may sometimes increase slightly, but in order to improve reliability, the second dielectric layer may further contain at least one oxide selected from Nb, Ti, Zr, Ta, Al, Sn, W, Mo and In. In order to suppress the increase in reflectivity, the content of metals other than Si, excluding oxygen, is preferably 30 at% or less, more preferably 20 at% or less, and further preferably 15 at% or less. In addition, when the anti-fouling film described later is formed on the anti-reflection film 30, from the viewpoint of bonding related to the durability of the anti-fouling film, the anti-fouling film is preferably formed on the second dielectric layer (SiO x )superior.

[0120] The first dielectric layer (ABO) 32 is preferably amorphous. If it is amorphous, it can be produced at a relatively low temperature, and when the transparent substrate is made of resin, the resin is not damaged by heat, and thus it can be suitably used.

[0121] It should be noted that as a light-absorbing and insulating transparent film, a half-tone mask used in the field of semiconductor manufacturing is known. As a half-tone mask, Mo-SiO containing a small amount of Mo can be used. x Oxygen-deficient films such as PDMS films are also known. Furthermore, narrow-bandgap films used in semiconductor manufacturing are known as light-absorbing and insulating translucent films. However, these films have a high absorption capacity for short-wavelength visible light, resulting in a yellowish tint in the transmitted light. Therefore, they are not suitable for cover glasses of image display devices.

[0122] In a preferred embodiment of the present invention, the first dielectric layer 32 having increased Mo and W contents and the SiO x The second dielectric layer 34 having the structure of the above can provide a transparent substrate with an antireflection film having light absorbing ability, insulating properties, and excellent adhesion and strength.

[0123] The anti-reflection film 30 in this embodiment can be formed on the main surface of the transparent substrate using a known film-forming method such as sputtering, vacuum deposition, or coating. Specifically, the dielectric layers constituting the anti-reflection film 30 are formed on the main surface of the diffusion layer 31 using a known film-forming method such as sputtering, vacuum deposition, or coating in the order in which they are stacked.

[0124] Examples of the sputtering method include magnetron sputtering, pulse sputtering, AC sputtering, and digital sputtering.

[0125] For example, magnetron sputtering is a method in which a magnetic field is generated by setting a magnet on the back side of a dielectric material serving as a matrix, and gas ion atoms collide with the surface of the dielectric material and escape to form a film with a thickness of several nanometers by sputtering. This method can form a continuous film of a dielectric oxide or nitride serving as the dielectric material.

[0126] For example, digital sputtering differs from conventional magnetron sputtering in that it first forms an extremely thin metal film by sputtering, followed by oxidation by irradiation with oxygen plasma, oxygen ions, or oxygen radicals. This process is repeated in the same chamber to form a thin film of metal oxide. In this case, the film-forming molecules are metal when attached to the substrate, so it is speculated that the film is more ductile than when the film is attached to a metal oxide. Therefore, it is believed that the rearrangement of the film-forming molecules occurs easily even at the same energy, resulting in a dense and smooth film.

[0127] It should be noted that the above is an example of a preferred structure of the anti-reflection film, but the structure of the anti-reflection film is not limited to this. For example, when it is desired to maintain high brightness of a display, it is sometimes appropriate to use an anti-reflection film that does not have light absorption ability or has a high transmittance and a light transmittance of 90% or more as a transparent substrate with an anti-reflection film. Even in such a transparent substrate with an anti-reflection film including a high transmittance anti-reflection film, if the a of the diffusely reflected light at each angle is * and b * Within the above range, the effect of suppressing color deviation during tiling can be obtained. As a composition of a highly transmissive anti-reflection film, for example, a low refractive index layer is the same as the second dielectric layer 34, and a high refractive index layer is a layer that does not have light absorption capability or has high transmissivity. As an example of a high refractive index layer in this case, for example, a layer mainly composed of Ti oxide (TiO x ) layer, Nb oxide (NbO x ) layer, a layer composed of Ta oxide (TaO x ) is preferably composed mainly of Ti oxide (TiO x In this case, each layer forming the antireflection film can also be formed using a known film-forming method such as sputtering, vacuum evaporation, and coating.

[0128] When a highly transmissive antireflection film is provided, the light transmittance (Y) of the transparent substrate with the antireflection film may be, for example, 90 to 96%, and preferably 93 to 96%.

[0129] (Anti-fouling film)

[0130] From the perspective of protecting the outermost surface of the antireflection film, the transparent substrate with an antireflection film of this embodiment may further include an antifouling film (also referred to as an "anti-fingerprint (AFP) film") on the antireflection film. The antifouling film may be composed of, for example, a fluorinated organosilicon compound. Any fluorinated organosilicon compound can be used as long as it can impart antifouling, water repellency, and oil repellency. Examples include fluorinated organosilicon compounds having one or more groups selected from polyfluoropolyether groups, polyfluoroalkylene groups, and polyfluoroalkyl groups. A polyfluoropolyether group refers to a divalent group having a structure in which a polyfluoroalkylene group and an etheric oxygen atom are alternately bonded.

[0131] In addition, as commercially available fluorine-containing silicone compounds having one or more groups selected from a polyfluoropolyether group, a polyfluoroalkylene group and a polyfluoroalkyl group, KP-801 (trade name, manufactured by Shin-Etsu Chemical Co., Ltd.), KY178 (trade name, manufactured by Shin-Etsu Chemical Co., Ltd.), KY-130 (trade name, manufactured by Shin-Etsu Chemical Co., Ltd.), KY-185 (trade name, manufactured by Shin-Etsu Chemical Co., Ltd.), OPTOOL (registered trademark) DSX and OPTOOL AES (both trade names, manufactured by Daikin Industries, Ltd.) and the like can be preferably used.

[0132] When the transparent substrate with an antireflection film in this embodiment includes an antifouling film, the antifouling film is disposed on the antireflection film. When the antireflection films are disposed on both principal surfaces of the transparent substrate, the antifouling film can be formed on the antireflection films on both sides, or alternatively, the antifouling film can be laminated on only one principal surface. This is because the antifouling film can be disposed in any location where it is likely to come into contact with hands, etc., and the selection can be made based on the intended use, etc.

[0133] (Method for Manufacturing Transparent Substrate with Antireflection Film)

[0134] The method for producing the transparent substrate with an anti-reflection film of this embodiment is not particularly limited, and can be produced by, for example, sequentially forming a diffusion layer and an anti-reflection film on a transparent substrate. Furthermore, as required, a barrier layer, an antifouling film, and the like can also be further formed.

[0135] The method of forming each layer is as described above, but in order to make the diffuse reflection light at each angle * and b *In order to satisfy the above-mentioned formulas (1) to (3), it is preferred to appropriately adjust the film composition of the anti-reflection film, the light transmittance (Y) of the transparent substrate with the anti-reflection film, and other values. In addition, in the case of a transparent substrate with an anti-reflection film having a high transmittance, it is difficult to optimize using the transmittance, so it is preferred to more strictly adjust the film thickness of each layer of the anti-reflection film. As a specific adjustment method, it is preferred to make the mirror reflectivity of green light with a wavelength of 500nm to 550nm higher than that of blue light with a wavelength of 450nm to 500nm and red light with a wavelength of 600nm to 650nm at multiple light incident angles. In this way, the mirror reflection color can be maintained from black (colorless) to green at multiple light incident angles, and as a result, there is a tendency that the diffuse reflection color at multiple incident angles can also be maintained from colorless to green. The angular dependence of the mirror reflection color can be easily predicted by using thin film simulation software. In addition, not only satisfying (1) to (3), but also adjusting the film thickness of each layer to reduce the b caused by the diffuse reflection angle is not the only way. * The change in is also beneficial in reducing the deviation of the reflected color.

[0136] For example, when the high refractive index layer is a mixed oxide layer of Mo, W, and Nb and the low refractive index layer is a SiOx layer, by satisfying the following, diffuse reflection light at various angles can be easily obtained. * and b * The tendency of the transparent substrate with an antireflection film to satisfy the above-mentioned formulas (1) to (3).

[0137] For example, the total thickness of the antireflection film is preferably 200 nm to 250 nm, more preferably 210 nm to 245 nm. This can suppress the angular dependence of the diffuse reflection color, that is, the increase in the change in the color tone of the diffuse reflection light caused by the angle, and tends to easily satisfy equations (1) to (3).

[0138] The number of layers of the antireflection film is preferably 4 to 8, more preferably 4 to 6. This can ensure mass productivity while suppressing an increase in the angular dependence of the diffuse reflection color, and tends to easily satisfy equations (1) to (3).

[0139] Furthermore, the thickness of the first, high-refractive-index layer is the most important of the various layer thicknesses, preferably ranging from 1 to 25 nm, and more preferably from 2 to 15 nm. This can suppress the angular dependence of diffuse reflection color, i.e., the increase in the change in the color tone of diffuse reflection light due to angle, and tends to more easily satisfy equations (1) to (3).

[0140] (use)

[0141] The transparent substrate with an anti-reflection film of this embodiment can be suitably used as a cover glass for an image display device, particularly a cover glass for a display such as a large μ-LED display, which is a display obtained by tiling multiple displays (such as LED panels). Alternatively, the transparent substrate with an anti-reflection film of this embodiment can also be suitably used in situations where the haze required for the transparent substrate with an anti-reflection film is high and the change in color tone caused by the angle tends to become more significant. In addition to this, the transparent substrate with an anti-reflection film of this embodiment can also be suitably used as a cover glass for various image display devices such as liquid crystal displays, organic EL displays, and electronic paper displays.

[0142] (Image Display Device)

[0143] An image display device according to one embodiment of the present invention includes the transparent substrate with the anti-reflection film. Examples of image display devices include a small display (e.g., an LED panel) that is used in a tiled manner and includes the transparent substrate with the anti-reflection film, and a large display, preferably a large μ-LED display, that is tiled. Furthermore, examples include a transparent substrate with the anti-reflection film provided on various displays, such as liquid crystal displays, organic EL displays, and electronic paper displays.

[0144] Example

[0145] The present invention is described in detail below with reference to the following examples, but the present invention is not limited thereto. Examples 1 and 2 are comparative examples, and Examples 3 and 4 are examples.

[0146] (evaluate)

[0147] The following evaluations were performed on the transparent substrate with an antireflection film of each example.

[0148] (a of diffuse reflected light at each angle * b * L * )

[0149] Black tape (Kukiri Miel, manufactured by Tomogawa Paper Co., Ltd.) was applied to the main surface (the other main surface) of the transparent substrate with an anti-reflection film that did not have a diffusion layer and an anti-reflection film. This eliminated reflection from the other main surface, and a light source was incident at an angle of 45° on the main surface (one main surface) with a diffusion layer and an anti-reflection film. The reflectance of the diffusely reflected light at angles of 15°, 25°, and 45° relative to the specularly reflected light was measured for visible light wavelengths, and a was calculated under a D65 light source. * 、b * and L * (Diffuse reflection color) The measurement was performed using CM-M6 manufactured by Konica Minolta Inc.

[0150] (Haze)

[0151] The haze value (transmission haze) of the produced transparent substrate with an antireflection film was measured in accordance with JIS K 7136:2000 using a haze meter (HZ-V3 manufactured by Suga Test Instruments Co., Ltd.).

[0152] (Light transmittance: Y)

[0153] In the produced transparent substrate with an anti-reflection film, the light transmittance (Y) of the outermost surface of the anti-reflection film was measured using the method specified in JIS Z 8701 (1999). It should be noted that in this specification, the light transmittance (Y) of the outermost surface of the anti-reflection film is referred to as the light transmittance (Y) of the transparent substrate with an anti-reflection film. Specifically, with black tape attached to the other of the two main surfaces of the transparent substrate, the one not on the anti-reflection film side, to eliminate back reflection, the spectral transmittance was measured using a spectrophotometer (manufactured by Shimadzu Corporation, trade name: SolidSpec-3700), and the light transmittance (stimulus value Y specified in JIS Z 8701 (1999)) was calculated.

[0154] (Transmittance color of transparent substrate with anti-reflection film under D65 light source (b * value))

[0155] The color index (b) specified in JIS Z 8729 (2004) was determined from the transmission spectrum obtained by measuring the above spectral transmittance. * The light source used is D65.

[0156] (Color deviation evaluation)

[0157] For each example, 16 transparent substrates with anti-reflection films made under the same conditions were prepared for testing. For example, in the case of Example 1, 16 transparent substrates with anti-reflection films were prepared under the conditions of Example 1 and by slightly changing the film thickness of each layer under the conditions of Example 1. Black tape (made by Tomogawa Paper Co., Ltd., Kutsukirimi El) was attached to the main surface (the other main surface) without the diffusion layer and the anti-reflection film, and then arranged (tiled) in a vertical and horizontal order of 4 and 4 without gaps. For the transparent substrates with anti-reflection films after tiling, the color deviation was visually evaluated according to the following criteria. The same test was performed for the other examples. The evaluation results are shown in Table 1.

[0158] Good: When white LED illumination was reflected onto the principal surface (one principal surface) of the transparent substrate with an anti-reflection film, which had a diffusion layer and an anti-reflection film, and observed from various angles ranging from 0° to 45°, with the illumination position relative to the transparent substrate set to 0°, the white illumination reflected onto the transparent substrate with an anti-reflection film appeared to be only achromatic to green, indicating minimal color difference between the substrates. Furthermore, when viewed from the front, the transparent substrate with an anti-reflection film had a strong black appearance, demonstrating very good quality as a display surface material.

[0159] When white LED illumination is reflected onto the principal surface (one principal surface) of a transparent substrate with an anti-reflection coating, which has a diffusion layer and an anti-reflection coating, and observed from various angles ranging from 0° to 45° (with the illumination position relative to the transparent substrate being 0°), the white illumination reflected onto the transparent substrate with an anti-reflection coating appears to be achromatic to green, resulting in inconspicuous color differences between the substrates. Furthermore, when viewed from the front, the black color of the transparent substrate with an anti-reflection coating is slightly weaker, with a white-green tint appearing, but the resulting surface material provides good quality for a display.

[0160] Not allowed: When white LED lighting is reflected onto the main surface (one main surface) of a transparent substrate with an anti-reflection film on the side having a diffusion layer and an anti-reflection film, and when the position of the lighting relative to the transparent substrate with the anti-reflection film is set to 0° and observed from various angles within the range of 0° to 45°, the white lighting reflected on the transparent substrate with the anti-reflection film may appear as achromatic, red, blue, green, etc., resulting in significant color differences between the substrates.

[0161] (Example 1)

[0162] A transparent substrate with an antireflection film was prepared by sequentially forming a diffusion layer and an antireflection film on one main surface of a transparent substrate by the following method.

[0163] (Formation of Diffusion Layer)

[0164] An anti-glare PET film (manufactured by Reiko Co., Ltd., Sa: 0.259 μm, Sdr: 0.0620, Sdq: 0.361, Spc: 1703 (1 / mm), haze: 60%) was laminated to one main surface of a chemically strengthened glass substrate (Dragon Trail: a registered trademark, manufactured by AGC Corporation) measuring 50 mm in length by 50 mm in width by 1.1 mm in thickness using an acrylic adhesive (transparent adhesive). This laminate (resin film + anti-glare layer) was then provided on the transparent substrate. The values ​​of Sa, Sdr, Sdq, and Spc are measured without an anti-reflection film formed on the diffusion layer. However, the values ​​of Sa, Sdr, Sdq, and Spc of the anti-reflection film-coated transparent substrate after the anti-reflection film was formed vary little from the above values ​​and are considered to be within the above-described preferred range.

[0165] (Film formation of barrier layer)

[0166] Next, a SiN layer was formed as a barrier layer on the diffusion layer to a thickness shown in Table 1. For example, in Example 1, the barrier layer had a thickness of 15 nm.

[0167] The barrier layer is formed by repeatedly performing the following operations at high speed to form a silicon nitride film, and a silicon nitride (SiN) film with a predetermined film thickness is formed. x ) layer: using digital sputtering method and using silicon target, while maintaining the pressure of argon gas at 0.2Pa, at a frequency of 100kHz and a power density of 10.0W / cm 2 Pulse sputtering was performed with an inversion pulse width of 3 μsec to form a thin silicon film, which was then nitrided with nitrogen gas. The nitrogen flow rate during nitridation was 800 sccm, and the input power of the nitridation source was 600 W.

[0168] (Formation of Anti-Reflection Film)

[0169] Next, an antireflection film having the film structure shown in Table 1 was formed by alternately forming NMWO layers (high refractive index layers) and SiO layers (low refractive index layers) on the barrier layer. It should be noted that the NMWO layer refers to a mixed oxide layer of Nb, Mo, and W. For example, the film structure of the antireflection film of Example 1 in Table 1 is a four-layer antireflection film formed by forming a 4nm NMWO layer on the barrier layer, followed by a 33nm SiO layer, then a 110nm NMWO layer, and finally an 81nm SiO layer. The film formation methods for the SiO layer and the NMWO layer are as follows.

[0170] (NMWO layer formation)

[0171] The oxide film is formed by repeatedly performing the following operation at high speed, thereby forming an NMWO layer of a predetermined thickness: using a target prepared by mixing niobium, molybdenum, and tungsten in a weight ratio of 45:30:25 and sintering, the film is formed by digital sputtering at a frequency of 100 kHz and a power density of 10.0 W / cm while maintaining the pressure of argon gas at 0.2 Pa. 2 Pulse sputtering was performed under conditions of a 3μsec inversion pulse width to form a very thin metal film, which was then oxidized with oxygen. The NMWO layer formed using this method was analyzed by depth-direction composition analysis using X-ray photoelectron spectroscopy (XPS) using argon ion sputtering. The results showed that, excluding oxygen, the content of Nb was 51.9 at%, Mo was 33.5 at%, W was 14.6 at%, and the content of group B elements was 45% by weight.

[0172] (SiO layer formation)

[0173] The silicon oxide film is formed by repeatedly performing the following operations at high speed, and a silicon oxide [silicon dioxide (SiO x )] layer: using a digital sputtering method and a silicon target, while maintaining the pressure at 0.2 Pa with argon gas, at a frequency of 100 kHz and a power density of 10.0 W / cm 2 Pulse sputtering was performed with an inversion pulse width of 3 μsec to form a thin silicon film, which was then oxidized with oxygen. The oxygen flow rate during oxidation was 500 sccm, and the input power of the oxidation source was 1000 W.

[0174] (Forming of antifouling film)

[0175] KY-185 (trade name, manufactured by Shin-Etsu Chemical Co., Ltd.), a fluorinated organosilicon compound, was placed in a metal crucible (evaporation source) and heated to evaporate at 230-350°C. The resulting particles were allowed to evaporate and diffuse into a vacuum chamber containing a substrate, adhering to the substrate surface. A 4 nm thick antifouling film was formed while monitoring the deposition rate using a crystal oscillator.

[0176] (Example 2)

[0177] A transparent substrate with an antireflection film was obtained in the same manner as in Example 1 except that the film composition of the antireflection film was changed as shown in Table 1 to form an antireflection film consisting of 6 layers.

[0178] (Example 3)

[0179] A transparent substrate with an antireflection film was obtained in the same manner as in Example 1 except that the film compositions of the antireflection film and the barrier layer were changed as shown in Table 1 and the film forming method of the NMWO layer was changed as follows to form an antireflection film consisting of 6 layers.

[0180] (NMWO layer formation)

[0181] The oxide film is formed by repeatedly performing the following operation at high speed, thereby forming an NMWO layer of a predetermined thickness: using a target prepared by mixing and sintering niobium, molybdenum, and tungsten in a weight ratio of 24:30:46 by digital sputtering, while maintaining the pressure of argon gas at 0.2 Pa, at a frequency of 100 kHz and a power density of 10.0 W / cm 2 Pulse sputtering was performed under conditions of a 3μsec inversion pulse width to form a very thin metal film, which was then oxidized with oxygen. The NMWO layer formed using this method was analyzed by depth-direction composition analysis using X-ray photoelectron spectroscopy (XPS) using argon ion sputtering. The results showed that, excluding oxygen, the content of Nb was 31.5 at%, Mo was 38.1 at%, W was 30.5 at%, and the content of group B elements was 24% by weight.

[0182] (Example 4)

[0183] A transparent substrate with an antireflection film was obtained in the same manner as in Example 1, except that the film composition of the antireflection film was changed as shown in Table 1, and the high refractive index layer was a TiO layer, forming an antireflection film consisting of six layers. The TiO layer was formed as follows.

[0184] (Film Formation of TiO Layer)

[0185] The oxide film is formed by repeatedly performing the following operations at high speed, thereby forming a film of titanium oxide [titanium dioxide (TiO x )] layer: digital sputtering method using titanium target, while maintaining the pressure of argon gas at 0.2Pa, at a frequency of 100kHz and a power density of 10.0W / cm 2 Pulse sputtering was performed with an inversion pulse width of 3 μsec to form a metal film of minute thickness, which was then oxidized with oxygen. The oxygen flow rate during oxidation was 1000 sccm, and the input power of the oxidation source was 1000 W.

[0186] The results of the above evaluations of the transparent substrates with antireflection films obtained in each example are shown in Table 1. * and b * Shown in Figure 3 . Figure 3In the figure, (a) to (d) are the diffuse reflection light at each angle of Examples 1 to 4, respectively. * and b * In each figure, if the curve is within the area indicated by the dotted line, it means a * and b * All equations (1) to (3) are satisfied.

[0187]

[0188] The results in Table 1 confirm that in Examples 3 and 4 as embodiments, the a values ​​of the diffuse reflected light are measured. * and b * By satisfying all of the equations (1) to (3), it is possible to suppress color deviation during tiling.

[0189] As described above, this specification discloses the following matters.

[0190] 1. A transparent substrate with an anti-reflection film, comprising: a transparent substrate having two main surfaces; and a diffusion layer and an anti-reflection film provided on one main surface of the transparent substrate in this order from the transparent substrate side;

[0191] When the reflection from the other main surface of the transparent substrate is removed and the light source is incident on the one main surface at an incident angle of 45°, the a value of the diffuse reflected light at angles of 15°, 25° and 45° relative to the specular reflected light under a D65 light source is * and b * The following formulas (1) to (3) are satisfied.

[0192] (1)-8≤a * ≤1

[0193] (2)-2≤b * ≤6

[0194] (3)b * ≤-1×a * -1

[0195] 2. The transparent substrate with an antireflection film according to 1 above, wherein the haze value is 30% or more.

[0196] 3. The transparent substrate with an anti-reflection film according to 1 or 2 above, wherein the L of the diffusely reflected light at 15° is * is 15 to 35, and the L of the diffuse reflected light at 25° * 5 to 20.

[0197] 4. The transparent substrate with an antireflection film according to any one of 1 to 3 above, wherein the light transmittance (Y) is 20 to 90%.

[0198] 5. The transparent substrate with an anti-reflection film according to any one of 1 to 4 above, wherein the sheet resistance of the anti-reflection film is 10 4 Ω / □ or more.

[0199] 6. The transparent substrate with an antireflection film according to any one of 1 to 5 above, wherein the transmission color b under D65 light source is * Below 5.

[0200] 7. A transparent substrate with an anti-reflection film according to any one of 1 to 6 above, wherein the anti-reflection film has a stacked structure formed by stacking at least two dielectric layers having different refractive indices, at least one of the dielectric layers is mainly composed of an oxide of Si, and at least one other layer of the layers of the stacked structure is mainly composed of a mixed oxide, the mixed oxide being a mixed oxide of at least one oxide selected from Group A consisting of Mo and W and at least one oxide selected from Group B consisting of Si, Nb, Ti, Zr, Ta, Al, Sn, and In, and the content of the elements of Group B contained in the mixed oxide is 65% by mass or less relative to the total of the elements of Group A contained in the mixed oxide and the elements of Group B contained in the mixed oxide.

[0201] 8. The transparent substrate with an antireflection film according to any one of 1 to 7 above, further comprising an antifouling film on the antireflection film.

[0202] 9. The transparent substrate with an antireflection film according to any one of 1 to 8 above, wherein the transparent substrate comprises glass.

[0203] 10. The transparent substrate with an antireflection film according to any one of 1 to 9 above, wherein the transparent substrate comprises at least one resin selected from the group consisting of polyethylene terephthalate, polycarbonate, acrylic, silicone, and triacetyl cellulose.

[0204] 11. The transparent substrate with an antireflection film according to any one of 1 to 10 above, wherein the transparent substrate is a laminate of glass and at least one resin selected from the group consisting of polyethylene terephthalate, polycarbonate, acrylic, silicone, and triacetyl cellulose.

[0205] 12. The transparent substrate with an antireflection film according to 9 or 11 above, wherein the glass is chemically strengthened.

[0206] 13. An image display device comprising the transparent substrate with an antireflection film according to any one of 1 to 12 above.

[0207] The present invention has been described in detail and with reference to specific embodiments, but it will be apparent to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the present invention. This application is based on Japanese patent application (Japanese Patent Application No. 2022-064751) filed on April 8, 2022, the contents of which are incorporated herein by reference.

[0208] Explanation of symbols

[0209] 1Transparent substrate with anti-reflection film

[0210] 10 Transparent substrate

[0211] 11 A main surface

[0212] 12 Another main face

[0213] 20 black tape

[0214] 30 anti-reflective film

[0215] 31 diffusion layer

[0216] 32 first dielectric layer

[0217] 34 second dielectric layer

[0218] 50 light sources

[0219] 60 incident light

[0220] 61 Specular Reflection Light

[0221] 72, 73, 74 diffuse light

Claims

1. A transparent substrate with an anti-reflection film, comprising: a transparent substrate having two main surfaces, and a diffusion layer and an anti-reflection film provided on one main surface of the transparent substrate in order from the transparent substrate side, When the reflection from the other main surface of the transparent substrate is removed and the light source is incident on the one main surface at an incident angle of 45°, the a value of the diffuse reflected light at angles of 15°, 25° and 45° relative to the specular reflected light under the D65 light source is * and b * Satisfying the following equations (1) to (3), (1)-8≤a * ≤1 (2)-2≤b * ≤6 (3)b * ≤-1×a * -1。 2. The transparent substrate with an anti-reflection film according to claim 1, in, The haze value is 30% or more.

3. The transparent substrate with an anti-reflection film according to claim 1 or 2, in, The 15° diffuse reflected light L * is 15 to 35, and the L of the diffuse reflected light at 25° * 5 to 20.

4. The transparent substrate with an anti-reflection film according to claim 1 or 2, in, The light transmittance Y is 20 to 90%.

5. The transparent substrate with an anti-reflection film according to claim 1 or 2, in, The sheet resistance of the anti-reflection film is 10 4 Ω / □ or more.

6. The transparent substrate with an anti-reflection film according to claim 1 or 2, in, b of the transmitted color under D65 light source * Is 5 or less.

7. The transparent substrate with an anti-reflection film according to claim 1 or 2, in, The antireflection film has a stacked structure in which at least two dielectric layers having different refractive indices are stacked, at least one of the dielectric layers is mainly composed of Si oxide, and at least one other layer of the layers of the stacked structure is mainly composed of a mixed oxide, which is a mixed oxide of at least one oxide selected from the group A consisting of Mo and W and at least one oxide selected from the group B consisting of Si, Nb, Ti, Zr, Ta, Al, Sn and In, and the content of the elements of the group B contained in the mixed oxide is 65% by mass or less relative to the total of the elements of the group A contained in the mixed oxide and the elements of the group B contained in the mixed oxide.

8. The transparent substrate with an anti-reflection film according to claim 1 or 2, in, An antifouling film is further provided on the antireflection film.

9. The transparent substrate with an anti-reflection film according to claim 1 or 2, in, The transparent substrate comprises glass.

10. The transparent substrate with an anti-reflection film according to claim 1 or 2, in, The transparent substrate includes at least one resin selected from the group consisting of polyethylene terephthalate, polycarbonate, acrylic, silicone, and triacetyl cellulose.

11. The transparent substrate with an antireflection film according to claim 1 or 2, in, The transparent substrate is a laminate of glass and at least one resin selected from the group consisting of polyethylene terephthalate, polycarbonate, acrylic acid, silicone and triacetyl cellulose.

12. The transparent substrate with an anti-reflection film according to claim 11, in, The glass is chemically strengthened. 13 . An image display device comprising the transparent substrate with an antireflection film according to claim 1 or 2 .

Citation Information

Patent Citations

  • Transparent substrate with antireflection film

    JP2018115105A