Tooth filling material and preparation method thereof

Through the combination of resin matrix, filler, photoinitiation system and prepolymerized resin powder, the problem of insufficient polishing, color and heat conduction performance of tooth filler materials is solved, and high-performance tooth filler materials are realized, reducing shrinkage rate and improving mechanics Strength and anti-carious ability, suitable for early treatment of dental erosion in adolescents.

CN118986749AInactive Publication Date: 2024-11-22JUMENG (WUXI) MEDICAL TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411060608.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing tooth filling materials have poor polishing performance, color and heat-preventing properties when used, and have a large shrinkage rate when curing, resulting in difficulty in gaps and disinfection, which cannot effectively solve the early treatment needs of teenage dental erosion.

Method used

Prepolymerized resin powder is prepared by polymerization of bisphenol A glycidyl methacrylate and free radical initiator using a combination of resin matrix, filler, photoinitiation system and prepolymerized resin powder, combining nanosilica particles, quartz powder and For porcelain powder, silane coupling agent and photoinitiator are used to reduce shrinkage and improve density and mechanical properties.

Benefits of technology

It realizes excellent polishing performance and color of tooth filling materials to simulate natural teeth, reduces shrinkage, improves mechanical strength and anti-carious ability, and improves the overall performance of tooth filling materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118986749A_ABST
    Figure CN118986749A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of tooth filling materials, in particular to a tooth filling material and a preparation method thereof.The tooth filling material comprises a resin matrix, filler, a photo-initiation system, a coupling agent and prepolymerized resin powder, and the prepolymerized resin powder is formed by polymerizing bisphenol A glycidyl dimethacrylate and a free radical initiator; the particle size of the prepolymerized resin powder is 0.5 mu m, and the prepolymerized resin powder comprises the following components in percentage by mass: 16% of a resin matrix, 60% of a filler, 0.17% of a photo-initiation system, 0.23% of a coupling agent and 23.6% of prepolymerized resin powder.The tooth filling material has excellent polishing performance, can simulate the color of natural teeth to a certain extent, improves the aesthetic property, reduces the shrinkage rate, and can be used for preparing the tooth filling material. The nano silicon dioxide particles, the quartz powder and the porcelain powder are added, so that the mechanical strength and the wear resistance of the tooth filling material are improved, and the nano fluorine-containing resin is added, so that the caries resistance of tooth hard tissues can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a filling material and a preparation method thereof, in particular to a tooth filling material and a preparation method thereof, belonging to the technical field of tooth filling materials. Background Art

[0002] The incidence of dental erosion in adolescents is increasing year by year. Dental erosion is caused by the action of acidic substances on the tooth surface. Although dental erosion is a multifactorial disease, studies have shown that dental erosion in adolescents is closely related to the frequent drinking of carbonated beverages. Further development of dental erosion can lead to pulp inflammation and local inflammation in the jaw, and even lead to tooth loss and extraction, and loss of chewing function. As the disease progresses, patients not only suffer more physiological pain, but also increase the difficulty and cost of treatment in the middle and late stages of the disease. At present, the early treatment of dental erosion is mainly based on demineralized enamel re-enhancement and enamel defect repair technology. The materials currently used for enamel defect repair are mainly resin-based repair materials and ceramic repair materials. Among them, resin-based repair materials and repair technologies are widely used in clinical enamel defect repair due to their easy operation, superior physical and chemical properties, and flexible color selection.

[0003] Common tooth filling materials can fill tooth cavities with resin-based restorative materials. However, the polishing performance, color, and heat conduction resistance of composite resin tooth filling materials are not very high. In addition, the large shrinkage rate during curing can easily lead to gaps, and it is difficult to disinfect.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] The object of the present invention is to provide a tooth filling material and a preparation method thereof in order to solve the above problems, which has high polishing performance, color and anti-heat conduction performance, and a small shrinkage rate during curing.

[0006] The present invention achieves the above-mentioned purpose through the following technical scheme. A tooth filling material comprises a resin matrix, a filler, a photoinitiator system, a coupling agent and a prepolymerized resin powder. The prepolymerized resin powder is polymerized by bisphenol A dimethacrylate glycidyl ester and a free radical initiator. The prepolymerized resin powder has a particle size of 0.5 μm and comprises the following components by mass fraction: 16% of the resin matrix, 60% of the filler, 0.17% of the photoinitiator system, 0.23% of the coupling agent, and 23.6% of the prepolymerized resin powder. When used, the mass fraction of each component is the mass fraction in the tooth filling material. The resin matrix has good biosafety and physical and mechanical properties. The coupling agent is used to connect the organic matrix and the inorganic filler. The filler is used to improve the density, tensile strength, hardness and toughness of the tooth filling material. The photoinitiator system is used to initiate a free radical polymerization reaction. The prepolymerized resin powder is used to reduce the shrinkage rate of the tooth filling material. The free radical initiator is used to initiate a free radical polymerization reaction. The bisphenol A dimethacrylate glycidyl ester is a composite resin monomer.

[0007] Furthermore, in order to better prepare the prepolymerized resin powder, the prepolymerized resin powder is prepared by a solid method using bisphenol A diglycidyl methacrylate and a free radical initiator, wherein the free radical initiator is diacyl peroxide, and the amount of the free radical initiator is 0.3% of the mass of the bisphenol A diglycidyl methacrylate.

[0008] Furthermore, in order to better prepare the resin matrix, the resin matrix includes bisphenol A dimethacrylate glycidyl ester, nano fluorine-containing resin and active diluent. By mass percentage, the content of bisphenol A dimethacrylate glycidyl ester is 10%, the content of the nano fluorine-containing resin is 5.9%, and the content of the active diluent is 0.1%. The nano fluorine-containing resin is used to release fluoride ions and reduce secondary caries at the edge of the filling body. The active diluent is used to reduce the viscosity of the reaction system and can also maintain the performance of the prepared resin matrix.

[0009] Furthermore, in order to improve the performance of the tooth filling material, the filler is composed of nano-silica particles, quartz powder and porcelain powder. The particle sizes of the nano-silica particles are 15nm, 55nm and 95nm. In terms of mass percentage, the mass fraction of the nano-silica particles with a particle size of 15nm is 2.5%, the mass fraction of the nano-silica powder particles with a particle size of 55nm is 5%, and the mass fraction of the nano-silica particles with a particle size of 95nm is 2.5%. The quartz powder is quartz powder with a particle size of 0.5μm, and the mass fraction of the quartz powder with a particle size of 0.5μm is 25%. The porcelain powder is quartz powder with a particle size of 0.5μm, and the mass fraction of the porcelain powder with a particle size of 0.5μm is 25%.

[0010] Furthermore, in order to initiate a free radical polymerization reaction, the photoinitiator system includes a photoinitiator and a promoter, wherein the photoinitiator is camphorquinone, and the promoter is ethyl dimethylaminobenzoate. In terms of mass percentage, the mass fraction of the photoinitiator is 0.05%, and the mass fraction of the promoter is 0.12%. The camphorquinone is used to polymerize the resin matrix.

[0011] Furthermore, in order to improve the polymerization of the resin matrix and the filler and facilitate filling, the coupling agent is a silane coupling agent, the tooth restoration material is a viscous colloid, and the silane coupling agent is used to reduce the viscosity of the synthetic resin melt, improve the dispersion of the filler, and improve the processing performance.

[0012] A method for preparing a tooth filling material comprises the following steps:

[0013] S1. First, the bisphenol A dimethacrylate glycidyl ester and the free radical initiator are prepared by a solid method to obtain the prepolymerized resin powder;

[0014] S2. Then the bisphenol A diglycidyl methacrylate, the nano-fluorine-containing resin and the reactive diluent are uniformly mixed to obtain the resin matrix;

[0015] S3. Then the resin matrix and the photoinitiator system are stirred and mixed to obtain a mixture A;

[0016] S4. Add the filler to the mixture A, and then add the coupling agent and stir to obtain a mixture B;

[0017] S5. Add the prepolymerized resin powder to the mixture B, stir and mix to obtain a tooth restoration material.

[0018] Furthermore, in order to prepare the pre-polymerized resin powder with uniform particles and better exert the polymerization effect of the photoinitiator and the promoter, the bisphenol A dimethyl methacrylate is first mixed with the diacyl peroxide, back-stirred for 6 hours, and then heated to 65°C for polymerization for 6 hours. The polymerized product is then cyclically crushed, dried and sieved to obtain the pre-polymerized resin powder. The resin matrix, the photoinitiator and the promoter are stirred and mixed at a speed of 8 r / min for 30 minutes.

[0019] Furthermore, in order to better exert the effect of the filler, the nano-silica particles are first added to the above-mentioned mixture A and stirred and mixed at a stirring speed of 6 r / min and a stirring time of 15 min, and then the quartz powder and the porcelain powder are added and stirred and mixed at a stirring speed of 7 r / min and a stirring time of 15 min to obtain a mixture B, in which the quartz powder and the porcelain powder are added at the same time.

[0020] Furthermore, in order to optimize the mechanical properties of the tooth filling material, the steps of mixing the mixture B with the prepolymerized resin powder are as follows: adding the prepolymerized resin powder to the mixture B and stirring to mix, the stirring speed is 15 r / min, the stirring time is 45 min, and then continuing to stir under vacuum conditions, the stirring speed is 7 r / min, the stirring time is 15 min, and then moving to continue stirring under normal pressure, the stirring speed is 12 r / min, the stirring time is 45 min, and then moving to reverse stirring under vacuum conditions, the stirring speed is 6 r / min, the stirring time is 8 min, and the tooth filling and repair material is obtained after stirring.

[0021] The technical effects and advantages of the present invention are as follows: 1. The tooth filling material has excellent polishing performance, can simulate the color of natural teeth to a certain extent, improve aesthetics, and reduce shrinkage.

[0022] 2. By adding nano-silica particles, quartz powder and porcelain powder, the mechanical strength and wear resistance of tooth filling materials are improved.

[0023] 3. By adding nano-fluorine-containing resin, the caries resistance of the hard tissue of the teeth can be improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 The following is a table of the composition of the raw materials of the present invention;

[0025] Figure 2 is a performance test table of the present invention;

[0026] Figure 3 is a flow chart of the preparation method of the present invention; DETAILED DESCRIPTION

[0027] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] See also Figure 1-Figure 3 As shown, a tooth filling material includes a resin matrix, a filler, a photoinitiator system, a coupling agent and a prepolymerized resin powder. The prepolymerized resin powder is polymerized by bisphenol A dimethyl methacrylate and a free radical initiator. The prepolymerized resin powder has a particle size of 0.5 μm and includes the following components by mass fraction: 16% of the resin matrix, 60% of the filler, 0.17% of the photoinitiator system, 0.23% of the coupling agent, and 23.6% of the prepolymerized resin powder. The tooth restoration material is a viscous colloid, and the coupling agent is a silane coupling agent. When in use, the resin matrix, filler, photoinitiator system, coupling agent and prepolymerized resin powder are commercially available, and the amount of each component is added according to the mass fraction of the component in the tooth restoration material.

[0029] The prepolymerized resin powder is prepared by a solid method using bisphenol A diglycidyl methacrylate and a free radical initiator. The free radical initiator is diacyl peroxide, and the amount of the free radical initiator is 0.3% of the mass of bisphenol A diglycidyl methacrylate. When used, a corresponding amount of diacyl peroxide and bisphenol A diglycidyl methacrylate are mixed and stirred, and then the temperature is raised for polymerization.

[0030] The resin matrix includes bisphenol A dimethacrylate glycidyl ester, nano fluorine-containing resin and active diluent. Calculated by mass percentage, the content of bisphenol A dimethacrylate glycidyl ester is 10%, the content of nano fluorine-containing resin is 5.9%, and the content of active diluent is 0.1%. When in use, the corresponding mass of bisphenol A dimethacrylate glycidyl ester and nano fluorine-containing resin are first stirred and mixed at a stirring speed of 5r / min for 5 minutes, and then the active diluent is added thereto, and then stirred for 30 minutes at the same stirring speed.

[0031] The filler is composed of nano silicon dioxide particles, quartz powder and porcelain powder. The particle sizes of the nano silicon dioxide particles are 15nm, 55nm and 95nm. In terms of mass percentage, the mass fraction of the nano silicon dioxide particles with a particle size of 15nm is 2.5%, the mass fraction of the nano silicon dioxide powder particles with a particle size of 55nm is 5%, the mass fraction of the nano silicon dioxide particles with a particle size of 95nm is 2.5%, the quartz powder is quartz powder with a particle size of 0.5μm, the mass fraction of the quartz powder with a particle size of 0.5μm is 25%, and the porcelain powder is quartz powder with a particle size of 0.5μm. The mass fraction of quartz powder with a particle size of 0.5μm and porcelain powder with a particle size of 0.5μm is 25%. When in use, first stir and mix the nano-silicon dioxide particles with a particle size of 15nm, the nano-silicon dioxide powder particles with a particle size of 55nm and the nano-silicon dioxide particles with a particle size of 95nm at a stirring speed of 8r / min and a stirring time of 20min. Then, add the corresponding doses of quartz powder and porcelain powder and stir and mix them at a stirring speed of 4r / min and a stirring time of 30min to obtain the filler.

[0032] The photoinitiator system includes a photoinitiator and an accelerator. The photoinitiator is camphorquinone and the accelerator is ethyl dimethylaminobenzoate. In terms of mass percentage, the mass fraction of the photoinitiator is 0.05% and the mass fraction of the accelerator is 0.12%. When in use, camphorquinone and ethyl dimethylaminobenzoate are mixed in corresponding proportions to obtain the photoinitiator system.

[0033] A method for preparing a tooth filling material comprises the following steps:

[0034] S1. First, bisphenol A dimethacrylate glycidyl ester is mixed with diacyl peroxide, and stirred for 6 hours, and then moved into an oven for polymerization, and the temperature is raised to 65° C. for polymerization, and the polymerization time is 6 hours. After the polymerization is completed, the finished product is removed and poured into a pulverizer for cyclic pulverization. After the pulverization is completed, it is ground, and then dried by a hot air blower. After drying, it is filtered through a sieve, and the pre-polymerized resin powder that does not meet the requirements is sieved out to obtain a pre-polymerized resin powder with uniform particles. The pre-polymerized resin powder that does not meet the requirements is pulverized and ground again;

[0035] S2. Then bisphenol A diglycidyl methacrylate, nano-fluorine-containing resin and reactive diluent were placed in a blender and uniformly mixed to obtain a resin matrix;

[0036] S3. The resin matrix and the photoinitiator system are then placed in another mixer and stirred and mixed. The resin matrix and the photoinitiator and the accelerator are stirred and mixed at a speed of 8r / min for 30min to obtain a mixture A;

[0037] S4. First, the mixture A was placed in a blender, and then a filler was added thereto and stirred and mixed at a stirring speed of 6 r / min for 15 min, and then a coupling agent was added and stirred and mixed at a stirring speed of 7 r / min for 15 min to obtain a mixture B;

[0038] S5. Then add prepolymer resin powder into mixture B and stir to mix, with a stirring speed of 15r / min and a stirring time of 45min. Then exhaust the air in the mixer through an exhaust fan to make the stirring environment under vacuum conditions. Continue stirring at a stirring speed of 7r / min and a stirring time of 15min. Then move to normal pressure and continue stirring at a stirring speed of 12r / min and a stirring time of 45min. Then put it under vacuum conditions and stir in the reverse direction at a stirring speed of 6r / min and a stirring time of 8min. After stirring, the tooth filling and repair material is obtained.

[0039] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.

[0040] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A tooth filling material, comprising a resin matrix, a filler, a photoinitiator system, a coupling agent and a prepolymerized resin powder, characterized in that: The prepolymerized resin powder is polymerized from bisphenol A dimethylglycidyl methacrylate and a free radical initiator. The prepolymerized resin powder has a particle size of 0.5 μm and comprises the following components by mass fraction: 16% of the resin matrix, 60% of the filler, 0.17% of the photoinitiator system, 0.23% of the coupling agent, and 23.6% of the prepolymerized resin powder.

2. The tooth filling material according to claim 1, characterized in that: The prepolymerized resin powder is prepared by solid method from bisphenol A diglycidyl methacrylate and a free radical initiator, wherein the free radical initiator is diacyl peroxide, and the amount of the free radical initiator is 0.3% of the mass of the bisphenol A diglycidyl methacrylate.

3. The tooth filling material according to claim 1, characterized in that: The resin matrix comprises bisphenol A dimethacrylate glycidyl ester, nanometer fluorine-containing resin and active diluent. Calculated by mass percentage, the content of bisphenol A dimethacrylate glycidyl ester is 10%, the content of nanometer fluorine-containing resin is 5.9%, and the content of active diluent is 0.1%.

4. The tooth filling material according to claim 1, characterized in that: The filler consists of nano silicon dioxide particles, quartz powder and porcelain powder. The particle sizes of the nano silicon dioxide particles are 15nm, 55nm and 95nm. In terms of mass percentage, the mass fraction of the nano silicon dioxide particles with a particle size of 15nm is 2.5%, the mass fraction of the nano silicon dioxide powder particles with a particle size of 55nm is 5%, and the mass fraction of the nano silicon dioxide particles with a particle size of 95nm is 2.5%. The quartz powder is quartz powder with a particle size of 0.5μm, and the mass fraction of the quartz powder with a particle size of 0.5μm is 25%. The porcelain powder is quartz powder with a particle size of 0.5μm, and the mass fraction of the porcelain powder with a particle size of 0.5μm is 25%.

5. The tooth filling material according to claim 1, characterized in that: The photoinitiator system comprises a photoinitiator and an accelerator. The photoinitiator is camphorquinone, and the accelerator is ethyl dimethylaminobenzoate. In terms of mass percentage, the mass fraction of the photoinitiator is 0.05%, and the mass fraction of the accelerator is 0.12%.

6. The tooth filling material according to claim 1, characterized in that: The coupling agent is a silane coupling agent, and the tooth repair material is a viscous colloid.

7. A method for preparing a tooth filling material, for preparing the tooth filling material according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1. First, the bisphenol A dimethacrylate glycidyl ester and the free radical initiator are prepared by a solid method to obtain the prepolymerized resin powder; S2. Then the bisphenol A diglycidyl methacrylate, the nano-fluorine-containing resin and the reactive diluent are uniformly mixed to obtain the resin matrix; S3. Then the resin matrix and the photoinitiator system are stirred and mixed to obtain a mixture A; S4. Add the filler to the mixture A, and then add the coupling agent and stir to obtain a mixture B; S5. Add the prepolymerized resin powder to the mixture B, stir and mix to obtain a tooth restoration material.

8. The method for preparing a tooth filling material according to claim 7, characterized in that: First, the bisphenol A dimethyl acrylate glycidyl ester and the diacyl peroxide are mixed, back-stirred for 6 hours, and then the temperature is raised to 65° C. for polymerization for 6 hours. The polymerized product is then cyclically crushed, dried and sieved to obtain the prepolymerized resin powder. The resin matrix, the photoinitiator and the accelerator are stirred and mixed at a speed of 8 r / min for 30 minutes.

9. The method for preparing a tooth filling material according to claim 7, characterized in that: The steps of mixing the mixture A with the filler are as follows: first, add the nano-silicon dioxide particles to the mixture A and stir and mix them at a stirring speed of 6 r / min and a stirring time of 15 min, then add the quartz powder and the porcelain powder and stir and mix them at a stirring speed of 7 r / min and a stirring time of 15 min to obtain a mixture B.

10. The method for preparing a tooth filling material according to claim 7, characterized in that: The steps of mixing the mixture B with the prepolymerized resin powder are as follows: adding the prepolymerized resin powder into the mixture B and stirring to mix, the stirring speed is 15 r / min, the stirring time is 45 min, and then continuing to stir under vacuum conditions, the stirring speed is 7 r / min, the stirring time is 15 min, and then transferring to normal pressure to continue stirring, the stirring speed is 12 r / min, the stirring time is 45 min, and then transferring to vacuum conditions to reversely stir, the stirring speed is 6 r / min, the stirring time is 8 min, and the tooth filling and repair material is obtained after the stirring is completed.