Catalyst for preparing ethylene by degrading polyethylene as well as preparation method and application of catalyst
Through the use of PdxInyWO3/CeO2 catalyst, the problem of high temperature and high pressure and uncontrollable selectivity during polyethylene pyrolysis is solved, and the high selectivity conversion of polyethylene to ethylene under low temperature conditions is achieved. It is suitable for a variety of polyethylene plastics. Sex reached 81%.
Patent Information
- Application Number
- CN202411287511.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-09-13
AI Technical Summary
The prior art requires high temperature and high pressure conditions during the pyrolysis of polyethylene, and the product selectivity is uncontrollable, making it difficult to achieve efficient and highly selective ethylene recovery.
Using PdxInyWO3/CeO2 catalyst, the temperature of polyethylene converted to ethylene is reduced through the synergistic action of palladium, indium and cerium oxide, and the selectivity is improved. The catalyst is made from cerium oxide as a support, and palladium and indium are uniformly dispersed on the support surface, and are calcined and reduced. Processing and preparation to achieve high selective conversion below 250°C.
Polyethylene is highly selectively converted into ethylene at lower temperatures, and the catalyst activity is stable. It is suitable for a variety of polyethylene plastics with a selectivity of 81%. It is widely used in low-density and high-density polyethylene with different molecular weights.
Smart Images

Figure CN118988306A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a preparation method and application of a catalyst for preparing ethylene by degrading polyethylene, belonging to the technical field of waste plastics treatment. Background Art
[0002] Chemical recycling of plastic waste is a process of converting it into intermediate chemicals such as oil and gas through a series of chemical reactions. Chemical recycling of waste plastics is a very promising way. Studies have shown that the potential energy obtained from recycling global waste plastics is equivalent to the value of 3.5 billion barrels of oil, and the recycled carbon resources can reduce carbon emissions by 30%. Therefore, the conversion of waste polyolefins into high-value products is of great significance to solving global climate and energy problems.
[0003] The carbon chain of polyolefins is randomly broken during pyrolysis, the products are complex and the reaction temperature required is high. In 2018, Laura used plasma technology to recover 22-25% of ethylene from high-density polyethylene (HDPE) waste plastics, which is 55 times higher than the ethylene obtained from HDPE waste by traditional pyrolysis methods (Green Chemistry, 2018, 20(8): 1813-1823). In 2002, Mastral studied the temperature and retention time of fluidized bed reactors to convert HDPE into ethylene and found that the highest ethylene yield of 41.9% was obtained under the conditions of 780°C and a retention time of 1.34 s (Journal of Analytical and Applied Pyrolysis, 2002, 63(2002): 1-15). In 2014, Kannan et al. used flash pyrolysis technology to depolymerize low-density polyethylene (LDPE) into monomer ethylene at 950-1000°C, with an ethylene selectivity of 48% (Energy & Fuels, 2014, 28(5): 3363-3366). The use of catalysts can reduce the reaction temperature of polyethylene pyrolysis to ethylene. In 2012, Donaj used TiCl4 / MgCl2 catalyst to degrade polyethylene and polypropylene mixed plastics at 500°C to obtain 22.3% ethylene and 22.1% propylene. The addition of TiCl4 / MgCl2 catalyst significantly increased the yield of gaseous olefins, especially propylene, which was higher than the olefin yield obtained by the pyrolysis process alone (Chemical Engineering Journal, 2012, 207(2): 27-34). Since the Gibbs free energy of the depolymerization of polyolefins to monomers is high, the chemical depolymerization of polyolefins tends to produce byproducts with low Gibbs free energy, so only a small amount of monomer selectivity is achieved.
[0004] Obviously, the depolymerization of polyolefin plastics requires harsh conditions such as high temperature and high pressure, and the product selectivity is uncontrollable. The use of catalysts to crack polyolefin plastics shows great advantages in lowering the reaction temperature and improving product selectivity. Therefore, the development of heterogeneous catalyst systems with higher application prospects to achieve efficient and highly selective recovery of polyolefin plastics is a key scientific issue that needs to be solved in this field. Summary of the invention
[0005] In order to overcome the shortcomings of the prior art, the purpose of the present invention is to provide a method for preparing a catalyst for catalyzing the degradation of polyethylene to produce ethylene. The catalyst uses cerium oxide as a carrier and metal palladium, indium and tungsten oxide as active metals. The highly dispersed active metals on the carrier play a key role in the catalytic conversion of polyethylene and can catalyze the conversion of polyethylene into ethylene at a relatively low temperature.
[0006] To solve the above technical problems, the implementation process of the present invention is as follows: A catalyst for preparing ethylene by degrading polyethylene, the catalyst comprising: Pd x In y WO3 / CeO2, wherein CeO2 is a carrier, and the mass of WO3 is 1-40% of the mass of cerium oxide; preferably, the mass of WO3 is 1-20% of the mass of cerium oxide; more preferably, the mass of WO3 is 1-10% of the mass of cerium oxide; Pd x In y The loading amount is 0.2-20 wt%, x and y are positive integers or decimals, and the molar ratio of Pd to In is 1-50:1-50; preferably, the molar ratio of Pd to In is 1-20:1-20; more preferably, the molar ratio of Pd to In is 1-10:1-10.
[0007] A Pd catalyst for the degradation of polyethylene to produce ethylene x In y The preparation method of WO3 / CeO2 comprises the following steps: (1) loading a soluble palladium salt onto a cerium oxide support; (2) loading soluble indium salt and tungsten salt onto the carrier obtained in step (1); (3) calcining the product obtained in step (2) at 250-600° C. in an air atmosphere; (4) The product obtained in step (3) is reduced in a 5-50 vol% H2 / Ar hydrogen-argon mixture at 400-800°C to obtain a ternary Pd x In y WO3 / CeO2 catalyst.
[0008] Preferably, in step (1), the soluble palladium salt is selected from palladium acetylacetonate, ammonium tetrachloropalladate, palladium acetate, palladium nitrate, palladium sulfate, diammonium dichloride palladium or tetraaminopalladium nitrate, and the carrier is selected from cerium oxide, aluminum oxide, zeolite or silicon oxide.
[0009] Preferably, in step (2), the soluble indium salt is selected from indium nitrate, indium chloride, indium iodide, indium fluoride, indium sulfate, indium acetate or indium phosphate, and the soluble tungsten salt is selected from ammonium metatungstate, ammonium paratungstate, phosphotungstic acid or tungsten pentachloride.
[0010] Preferably, in steps (1) and (2), the palladium loading is 0.1-10 wt %, the indium loading is 0.1-10 wt %, and the mass of WO3 is 1-10% of the mass of cerium oxide.
[0011] Preferably, in steps (1) and (2), the molar ratio of palladium to indium is 1-10:1-10, and the catalyst is expressed as Pd x In y WO3 / CeO 2, Such as: Pd1In9WO3 / CeO2, Pd9In1WO3 / CeO2, Pd1In3WO3 / CeO2, Pd3In1WO3 / CeO2, etc.
[0012] Preferably, the parameters for calcining the sample in step (3) are as follows: heating rate 0.8-20°C / min, calcination temperature 250-600°C, and holding time 1-6 h.
[0013] Preferably, the parameters of the reduction process in step (4) are as follows: heating rate 1-20°C / min, reducing gas 5-10 vol% hydrogen-argon mixture, gas flow rate 10-200 sccm, reduction temperature 400-800°C, and holding time 1-6 h. In order to solve the above technical problems, the second object of the present invention is to provide an application scheme for catalyzing the degradation of polyethylene to produce ethylene.
[0014] The catalytic conversion reaction of polyethylene plastic is carried out in an intermittent high-temperature and high-pressure reactor. The specific steps and conditions are as follows: (1) Adding a catalytic amount of a catalyst and polyethylene into a reactor, wherein the polyethylene is selected from one or more of low-density polyethylene, linear low-density polyethylene, and high-density polyethylene, and introducing nitrogen protection; (2) Heating to 200-350°C for full reaction; (3) Collect the gaseous products and use a gas chromatograph to perform quantitative analysis on the gaseous products. The polyethylene conversion rate is 25-58%, and the ethylene selectivity is 0-81%.
[0015] Through the above scheme, the catalyst for catalyzing the degradation of polyethylene to produce ethylene is prepared by the present invention. The catalyst uses Pd, In, and WO3 as active metals and cerium oxide as a carrier, and the active metals are highly dispersed in the carrier. The catalyst achieves carbon chain dehydrogenation through the synergistic effect of palladium and indium, and achieves carbon-carbon bond cleavage through WO3, and can convert polyethylene into ethylene with high selectivity under low temperature and solvent-free conditions.
[0016] Compared with the prior art, the present invention has the following advantages and beneficial effects: (1) The raw materials used in the present invention are all directly purchased commercial products and do not require additional processing. The preparation method is simple and controllable, has strong stability, can be reused, and has good application prospects; (2) The active metals of the catalyst are evenly dispersed on the surface of the carrier, providing more effective active sites; (3) Compared with the reported systems, this system can convert polyethylene to ethylene at a lower temperature (250°C) with a selectivity of up to 81%; (4) This system can be applied to a variety of polyethylene plastics, including one or more of low-density polyethylene, linear low-density polyethylene, and high-density polyethylene with different molecular weights, covering a wide range of degradable plastics. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 This is the spherical aberration electron microscope image of Pd1In3WO3 / CeO2 catalyst; Figure 2 This is the spherical aberration electron microscope image of Pd1In1WO3 / CeO2 catalyst; Figure 3 This is the spherical aberration electron microscope image of Pd1In5WO3 / CeO2 catalyst; Figure 4 This is the spherical aberration electron microscope image of Pd1In7WO3 / CeO2 catalyst; Figure 5 This is the spherical aberration electron microscope image of Pd3In1WO3 / CeO2 catalyst; Figure 6 This is the spherical aberration electron microscope image of Pd7In1WO3 / CeO2 catalyst; Figure 7 Pd x In y X-ray diffraction spectrum of WO3 / CeO2 catalyst; Figure 8 This is the peak spectrum of gas products of polyethylene degradation by Pd1In3WO3 / CeO2 catalyst on gas chromatography. DETAILED DESCRIPTION
[0018] The present invention will be described clearly and completely below in conjunction with the embodiments and drawings. Obviously, the embodiments described are only a part of the embodiments of the present invention, rather than all the embodiments. The reagents or instruments used without indicating the manufacturer are all conventional reagent products that can be obtained commercially. Example
[0019] In this embodiment, cerium oxide is used as a carrier, palladium acetylacetonate, indium nitrate, and ammonium metatungstate are used as metal precursors, wherein the mass of cerium oxide is 1000 mg, the mass of WO3 in the prepared catalyst is 10% of the mass of cerium oxide, the molar ratio of Pd to In is 1:3, the palladium loading is 0.8 wt%, and the indium loading is 2.8 wt%. The specific steps for preparing the Pd1In3WO3 / CeO2 catalyst are as follows: (1) Weigh 28.18 mg of di(acetylacetonate)palladium and 1000 mg of cerium oxide, dissolve the di(acetylacetonate)palladium in 800 μl of chloroform, load the palladium precursor on the cerium oxide using the incipient wetness impregnation method, and dry the impregnated product in a vacuum drying oven; (2) Grind the solid product in step (1) and transfer it to a beaker and add deionized water. Weigh 106.91 mg of ammonium metatungstate and 81.40 mg of indium nitrate and transfer them to the beaker and stir. (3) removing water from the solid-liquid mixture in step (2) using a rotary evaporator at a speed of 125 rpm and a vacuum degree of 100 mbar at 60°C; (4) The product of step (3) was calcined in a muffle furnace at 300°C for 2 h.
[0020] (5) The calcined product of step (4) was reduced using a 5 vol% hydrogen-argon mixture at 500°C for 2 h.
[0021] The spherical aberration electron microscope image of the prepared Pd1In3WO3 / CeO2 catalyst is shown in Figure 1 As shown, it can be seen that the catalyst obtained by impregnation-calcination-reduction is spherical, the diameter of the carrier cerium oxide is about 25 nm, and metal particles with a diameter of about 2 nm are evenly distributed on the surface of the cerium oxide carrier. Figure 7 Only the characteristic peaks of cerium oxide were observed in the XRD diffraction pattern, excluding the presence of bulk metal, indicating that the metal dispersion was good. Example
[0022] Similar to Example 1, cerium oxide was used as a carrier, palladium acetylacetonate, indium nitrate, and ammonium metatungstate were used as metal precursors, wherein the mass of cerium oxide was 1000 mg, and the mass of WO3 in the catalyst was 10% of the mass of cerium oxide. The difference was that the molar ratio of Pd and In was changed to 1:1, the palladium loading was 1.7 wt%, and the indium loading was 1.9 wt%. The spherical aberration electron microscope of the Pd1In1WO3 / CeO2 catalyst obtained under the same preparation conditions as Example 1 is as follows Figure 2 As shown, the active metal is in the form of particles with a diameter of approximately 5 nm. Figure 7 No relevant peaks of palladium, indium and tungsten oxide were observed in the XRD diffraction pattern, indicating that no bulk metal was generated and the metal dispersion was good. Example
[0023] Similar to Example 1, cerium oxide was used as a carrier, palladium acetylacetonate, indium nitrate, and ammonium metatungstate were used as metal precursors, wherein the mass of cerium oxide was 1000 mg, and the mass of WO3 in the catalyst was 10% of the mass of cerium oxide. The difference was that the molar ratio of Pd and In was changed to 1:5, the palladium loading was 0.6 wt%, and the indium loading was 3.1 wt%. The spherical aberration electron microscope of the Pd1In5WO3 / CeO2 catalyst obtained under the same preparation conditions as Example 1 is as follows Figure 3 As shown, the size of the supported cerium oxide is about 15 nm, and no obvious metal particles are observed. Figure 7 No relevant peaks of palladium, indium and tungsten oxide were observed in the XRD diffraction pattern, indicating that no bulk metal was generated. Example
[0024] Similar to Example 1, cerium oxide was used as a carrier, palladium acetylacetonate, indium nitrate, and ammonium metatungstate were used as metal precursors, wherein the mass of cerium oxide was 1000 mg, and the mass of WO3 in the catalyst was 10% of the mass of cerium oxide. The difference was that the molar ratio of Pd and In was changed to 1:7, the palladium loading was 0.42 wt%, and the indium loading was 3.2 wt%. The spherical aberration electron microscope of the Pd1In7WO3 / CeO2 catalyst obtained under the same preparation conditions as Example 1 is as follows Figure 4 As shown, the size of the carrier cerium oxide is about 20 nm, and a layer of active metal is dispersed on the surface of the carrier. Figure 7 No relevant peaks of palladium, indium and tungsten were observed in the XRD diffraction pattern, indicating that no bulk metal was generated. Example
[0025] Similar to Example 1, cerium oxide was used as a carrier, palladium acetylacetonate, indium nitrate, and ammonium metatungstate were used as metal precursors, wherein the mass of cerium oxide was 1000 mg, and the mass of WO3 in the catalyst was 10% of the mass of cerium oxide. The difference was that the molar ratio of Pd and In was changed to 3:1, the palladium loading was 2.7 wt%, and the indium loading was 1 wt%. The spherical aberration electron microscope of the Pd3In1WO3 / CeO2 catalyst obtained under the same preparation conditions as Example 1 is as follows Figure 5 As shown, the size of the supported cerium oxide is about 10 nm, and active metal particles with a diameter of about 2 nm can be observed on the surface of cerium oxide. Figure 7 No relevant peaks of palladium, indium and tungsten oxide were observed in the XRD diffraction pattern, indicating that no bulk metal was generated. Example
[0026] Similar to Example 1, cerium oxide was used as a carrier, palladium acetylacetonate, indium nitrate, and ammonium metatungstate were used as metal precursors, wherein the mass of cerium oxide was 1000 mg, and the mass of WO3 in the catalyst was 10% of the mass of cerium oxide. The difference was that the molar ratio of Pd to In was 7:1, the palladium loading was 3.6 wt%, and the indium loading was 0.5 wt%. The spherical aberration electron microscope of the Pd7In1WO3 / CeO2 catalyst obtained under the same preparation conditions as Example 1 is as follows Figure 6 As shown, the size of the cerium oxide carrier is about 15 nm. Metal particles with a diameter of about 2 nm are dispersed on the surface of the carrier. Figure 7 No peaks related to active metals were observed in the XRD diffraction pattern, indicating that no bulk metal was generated, further demonstrating that this preparation method can be used to prepare a series of catalysts with highly dispersed active metals. Example
[0027] A method for catalyzing the degradation of polyolefin plastics to prepare ethylene comprises the following steps: adding 100 mg of low-density polyethylene and 200 mg of Pd1In3WO3 / CeO2 catalyst into a reactor, and filling with 4 MPa of nitrogen. Adjusting the reaction time to 12 h and the reaction temperature to 250°C. Collecting gaseous products after the reaction is completed. Using gas chromatography to quantitatively analyze the gaseous products. Figure 8 This is the peak spectrum of the gas phase produced in the catalytic conversion of polyethylene on the gas chromatography; it can be seen from the figure that the retention time of ethylene on the gas chromatography is 9.3 min, and the ethylene selectivity is as high as 81%. Example
[0028] Similar to Example 7, except that Pd1In1WO3 / CeO2 catalyst, Pd1In5WO3 / CeO2 catalyst, Pd1In7WO3 / CeO2 catalyst, Pd3In1WO3 / CeO2 catalyst and Pd7In1WO3 / CeO2 catalyst were used respectively to catalyze the polyethylene reaction.
[0029]
[0030] As can be seen from Table 1, the results of catalytic conversion of polyethylene under different ratios of palladium and indium are that the Pd1In3WO3 / CeO2 catalyst has the highest polyethylene conversion rate (58%) and the highest ethylene product selectivity (81%).
[0031] Example 9 Similar to Example 1, the difference is that alumina, silica and zeolite (SBA-15) are used as carriers respectively, the carrier mass is 1000 mg, the mass of WO3 in the catalyst is 10% of the mass of cerium oxide, the molar ratio of Pd and In is 1:3, the palladium loading is 0.8 wt%, and the indium loading is 2.8 wt%. Table 2 shows the results of polyethylene conversion catalyzed by different carriers. When cerium oxide is used as a carrier, the polyethylene conversion rate is the highest, and polyethylene will be converted into ethylene to the maximum extent; when alumina is used as a carrier, the polyethylene conversion rate is lower than that of the catalyst with cerium oxide as a carrier, and there is a very small amount of ethylene in the degradation product, and the main product is ≥C4 product; when the carrier is SiO2, the catalyst activity is the lowest; when the carrier is SBA-15, the polyethylene conversion rate is equivalent to that of the catalyst with cerium oxide as a carrier, but the degradation product is mainly ≥C4 product. Experiments have shown that alkaline carriers are more conducive to the depolymerization of polyethylene to produce ethylene.
[0032]
[0033] Obviously, the above embodiments of the present invention are only examples for clearly explaining the present invention, and are not intended to limit the implementation methods of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is impossible to list all the implementation methods here. All obvious changes or modifications derived from the technical solution of the present invention are still within the scope of protection of the present invention.
Claims
1. A catalyst for preparing ethylene by degradation of polyethylene, characterized in that The catalyst composition is: Pd x In y WO3 / CeO2, where CeO2 is the carrier and the mass of WO3 is 1-40% of the mass of cerium oxide; Pd x In y The loading amount is 0.2~20 wt%, x and y are positive integers or decimals, and the molar ratio of Pd to In is 1~50:1~50.
2. The polyethylene degradation catalyst for preparing ethylene according to claim 1, characterized in that: The mass of WO3 is 1-20% of the mass of cerium oxide, and the molar ratio of Pd to In is 1-20:1-20.
3. The polyethylene degradation catalyst for preparing ethylene according to claim 2, characterized in that: The mass of WO3 is 1-10% of the mass of cerium oxide, and the molar ratio of Pd to In is 1-10:1-10.
4. A catalyst Pd for the degradation of polyethylene to produce ethylene x In y The preparation method of WO3 / CeO2 comprises the following steps: (1) loading a soluble palladium salt onto a cerium oxide support; (2) Loading soluble indium salt and tungsten salt onto the carrier obtained in step (1), Pd x In y The loading amount is 0.2~20 wt%, x and y are positive integers or decimals, and the molar ratio of Pd to In is 1~50:1~50; (3) calcining the product obtained in step (2) at 250-600° C. in an air atmosphere; (4) The product obtained in step (3) is reduced in a 5-50 vol% H2 / Ar hydrogen-argon mixture at 400-800°C to obtain a ternary Pd x In y WO3 / CeO2 catalyst.
5. The preparation method according to claim 4, characterized in that: In step (1), the soluble palladium salt is selected from palladium acetylacetonate, ammonium tetrachloropalladate, palladium acetate, palladium nitrate, palladium sulfate, diammonium dichloride palladium or tetraaminopalladium nitrate, and the carrier is selected from cerium oxide, aluminum oxide, zeolite or silicon oxide.
6. The preparation method according to claim 4, characterized in that: In step (2), the soluble indium salt is selected from indium nitrate, indium chloride, indium iodide, indium fluoride, indium sulfate, indium acetate or indium phosphate, and the soluble tungsten salt is selected from ammonium metatungstate, ammonium paratungstate, phosphotungstic acid or tungsten pentachloride.
7. The preparation method according to claim 4, characterized in that: In steps (1) and (2), the molar ratio of palladium to indium is 1-10:1-10.
8. The preparation method according to claim 4, characterized in that: The sample calcination parameters in step (3) are: heating rate 0.8~20°C / min; the parameters of the reduction process in step (4) are: heating rate 1~20°C / min, reducing gas 5~10 vol% hydrogen-argon mixture.
9. Use of the catalyst according to claim 1 in the production of ethylene by degradation of polyethylene.
10. The use according to claim 9, characterized in that The steps and conditions of polyethylene degradation reaction are: (1) Adding a catalytic amount of a catalyst and polyethylene into a reactor, wherein the polyethylene is selected from one or more of low-density polyethylene, linear low-density polyethylene, and high-density polyethylene, and introducing nitrogen protection; (2) Heating to 200-350°C for full reaction; (3) Collect the gaseous products and use a gas chromatograph to perform quantitative analysis on the gaseous products. The polyethylene conversion rate is 25-58%, and the ethylene selectivity is 0-81%.
Citation Information
Patent Citations
Difunctional coupling catalyst for hydrocracking of waste plastics and preparation method of difunctional coupling catalyst
CN114471597A
Method for preparing light oil from retired polyolefin through low-temperature catalytic hydrogenolysis of two-dimensional nanosheets
CN115725318A
Simple and rapid Ru / WO3 degradation polyethylene catalyst and preparation method and application thereof