Polyethylene plastic hydrogenolysis catalyst and preparation method thereof

CN118988345APending Publication Date: 2024-11-22NORTHWESTERN POLYTECHNICAL UNIV

Patent Information

Application Number
CN202411287503.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

然而塑料较强的化学惰性使其难以在自然环境条件下得到有效降解,目前常用的机械回收和热能回收等方式存在一定的不足,发展塑料制品的高价值回收方式十分必要

Benefits of technology

(1)本发明的RuxNiy/SiO2催化剂的初湿浸渍-还原制备法所采用的原料均为直接购买的商业产品且无需额外处理,制备方法简单可控,成本较低,稳定性强,可重复利用,具有较好的应用前景;

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118988345A_ABST
    Figure CN118988345A_ABST
Patent Text Reader

Abstract

The invention discloses a RuxNiy / SiO2 catalyst for hydrogenolysis of polyethylene plastic into liquid fuel and a preparation method of the RuxNiy / SiO2 catalyst. The preparation method comprises the following steps: dissolving soluble ruthenium salt and nickel salt in a hydrochloric acid solution, carrying out ultrasonic treatment to completely dissolve precursor salt, dropwise adding the precursor solution to a silicon dioxide carrier, stirring, carrying out vacuum drying, and reducing by using hydrogen argon to obtain the RuxNiy / SiO2 catalyst. The RuxNiy / SiO2 catalyst prepared by the invention has excellent polyethylene plastic hydrogenolysis performance, 100% complete conversion of polyethylene can be realized under mild conditions, and the highest C5-C40 yield can reach 96.8%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a polyethylene plastic hydrogenolysis catalyst, belonging to the technical field of heterogeneous catalysis. Background Art

[0002] With the improvement of people's living standards, plastic products are widely used in daily life due to their advantages such as light weight and easy processing. However, the strong chemical inertness of plastic makes it difficult to be effectively degraded in the natural environment. The commonly used mechanical recycling and thermal energy recycling methods have certain shortcomings. It is necessary to develop high-value recycling methods for plastic products.

[0003] The key to achieving high-value conversion of polyethylene plastics lies in the development of catalysts with high selectivity, high activity and high stability. At present, the most widely used catalysts in the field of polyethylene plastic hydrogenolysis are single metal Ru-based catalysts such as Ru / C, Ru / FAU, etc. Due to the characteristics of Ru metal, a large number of terminal CC bonds will break on the catalyst surface, resulting in a large amount of low-value gaseous products (mainly methane), which is not conducive to the high-value recovery of polyethylene plastic products. Summary of the invention

[0004] The purpose of the present invention is to improve the selectivity of Ru-based catalysts for high-value liquid products of polyethylene plastic hydrogenolysis reaction, and to provide a novel bimetallic alloy Ru-based catalyst for hydrogenolysis of polyethylene plastic into liquid fuel. x Ni y / SiO2 catalyst and preparation method thereof.

[0005] The implementation process of the present invention is as follows: A catalyst for hydrogenolysis of polyethylene plastic into liquid fuel, the catalyst composition is: Ru x Ni y / SiO2, wherein SiO2 is a carrier, the molar ratio of Ru and Ni is x:y (1-20): (1-10), x and y are positive integers or decimals, Ru x Ni y The loading amount is 1~10 wt%.

[0006] Preferably, the molar ratio of Ru to Ni is 1-10:1-5, such as Ru1Ni5, Ru1Ni3, Ru7Ni1, etc.

[0007] The preparation method of the above catalyst comprises the following steps: (1) Dissolving soluble ruthenium salt and nickel salt in 0.001-1M hydrochloric acid, adding silica support for impregnation, wherein the molar ratio of ruthenium salt to nickel salt is (1-20): (1-10), and the loading amount of ruthenium and nickel is 1-10 wt%; (2) removing the hydrochloric acid solution to obtain a solid product; (3) The product obtained in step (2) is reduced in a 5-20 vol% H2 / Ar hydrogen-argon mixture at 400-700°C to obtain Ru x Ni y / SiO2 catalyst.

[0008] In the above preparation method, in step (1), the soluble ruthenium salt is selected from ammonium chlororuthenate, ruthenium trichloride, hexaammineruthenium chloride or ruthenium nitrosyl nitrate, and the soluble nickel salt is selected from nickel nitrate or nickel chloride.

[0009] In the above preparation method, in step (1), the molar ratio of Ru to Ni is 1-10:1-5.

[0010] The application of the catalyst prepared by the above method in the hydrogenolysis of polyethylene plastics comprises the following reaction steps: (1) adding a catalytic amount of a catalyst and polyethylene in a reactor, wherein the polyethylene is selected from one of high-density polyethylene, low-density polyethylene and linear low-density polyethylene, and introducing 1-4 MPa hydrogen; (2) Heating to 200-300°C for full hydrogenolysis reaction; (3) Collect the liquid products and use gas chromatograph to perform quantitative analysis on the liquid products. The polyethylene conversion rate is 100% and the C5-C40 product yield is 73-97%.

[0011] The present invention is a novel bimetallic alloy Ru prepared by incipient wetness impregnation-reduction method x Ni y / SiO2 catalyst has a simple process flow and strong operability. The ruthenium salt and the nickel salt are dissolved in a hydrochloric acid solution, and the two metals are fully dissolved by ultrasonic treatment. The two metals are added dropwise on a silica carrier and stirred. The preparation is completed after drying and reduction treatment.

[0012] When preparing the catalyst, a second metal element is introduced to alloy with Ru, and the electronic structure and adsorption-desorption equilibrium of the active metal Ru are regulated, so that the selectivity of the product can be regulated. In recent years, the application research of transition metal Ni in the field of polyethylene plastic hydrogenolysis has gradually increased. Therefore, Ni is introduced as an alloying element of Ru in the present invention to achieve the selectivity regulation of Ru-based catalysts.

[0013] Compared with the prior art, the present invention has the following advantages and beneficial effects: (1) Ru of the present invention x Ni y The raw materials used in the incipient wetness impregnation-reduction preparation method of SiO2 catalyst are all directly purchased commercial products and do not require additional treatment. The preparation method is simple and controllable, with low cost, strong stability, and can be reused, and has good application prospects; (2) The present invention improves the selectivity of the reaction of hydrogenolysis of polyethylene plastic to produce liquid fuel by adjusting the input Ru / Ni atomic ratio. The catalyst has the best comprehensive performance when the Ru / Ni atomic ratio is 3 / 1. (3) Ru prepared by the present invention x Ni y / SiO2 catalyst has excellent performance in hydrogenolysis of polyethylene plastics and can achieve 100% complete conversion of polyethylene under mild conditions (250°C, 1~4 MPa H2), with a C5-C40 yield as high as 96.8%. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 It is the transmission electron microscope image of Ru3Ni1 / SiO2 catalyst; Figure 2 For Ru x Ni y / X-ray diffraction spectrum of SiO2 catalyst; Figure 3 This is the distribution of liquid products of Ru3Ni1 / SiO2 catalyst for degradation of high-density polyethylene. The amount of high-density polyethylene is 1 g, the amount of catalyst is 50 mg, the H2 pressure is 1 MPa, the reaction temperature is 250℃, and the reaction time is 12 h. Figure 4 This is the distribution of liquid products of Ru3Ni1 / SiO2 catalyst degradation of high-density polyethylene. The amount of high-density polyethylene is 1 g, the amount of catalyst is 50 mg, the H2 pressure is 3 MPa, the reaction temperature is 250℃, and the reaction time is 12 h. Figure 5 This is the distribution of liquid products of high-density polyethylene degradation by Ru3Ni1 / SiO2 catalyst. The amount of high-density polyethylene is 1 g, the amount of catalyst is 50 mg, the H2 pressure is 4 MPa, the reaction temperature is 250℃, and the reaction time is 12 h. Figure 6 This is the distribution of liquid products of high-density polyethylene degradation by Ru9Ni1 / SiO2 catalyst. The amount of high-density polyethylene is 1 g, the amount of catalyst is 50 mg, the H2 pressure is 3 MPa, the reaction temperature is 250℃, and the reaction time is 6 h. DETAILED DESCRIPTION

[0015] The present invention is further described in detail below in conjunction with the examples and drawings. In the description of the present invention, it should be noted that any embodiment described as "exemplary" herein is not necessarily to be interpreted as being superior or better than other embodiments. The reagents used in the examples can be purchased conventionally from the market unless otherwise specified. Example 1

[0016] In this embodiment, silicon dioxide is used as a catalyst carrier, ammonium chlororuthenate (IV) and nickel nitrate hexahydrate (II) are catalyst metal precursors, wherein the atomic ratio of Ru and Ni is 3 / 1, and the two metals account for 5% of the total mass of the catalyst. The concentration of the hydrochloric acid solution is 0.03 M. The specific steps of catalyst preparation are as follows: (1) Weigh 76.32 mg of ammonium chlororuthenate (IV) and 21.15 mg of nickel (II) nitrate hexahydrate and dissolve them in 1200 μl of hydrochloric acid solution (0.03 M), and perform ultrasonic treatment to fully dissolve them to obtain a precursor solution; (2) Immerse the precursor solution in step (1) in 500 mg of silica and stir thoroughly; (3) transferring the product obtained in step (2) to a vacuum drying oven and drying at 80° C. for 12 h, and grinding to obtain a product powder; (4) heating the product obtained in step (3) to 550°C in a 5 vol% H2 / Ar hydrogen-argon mixture at a rate of 5°C / min and maintaining the temperature for 3 h to obtain a Ru3Ni1 / SiO2 catalyst; (5) Add 50 mg of Ru3Ni1 / SiO2 catalyst and 1 g of high-density polyethylene into the reactor, and introduce 1 MPa of hydrogen; (6) Heating to 250°C for 12 h to allow for full hydrogenolysis reaction; (7) After the reaction is completed, the reactor is cooled to room temperature, the headspace gas in the reactor is slowly discharged, and the liquid product is dissolved with dichloromethane, and a gas chromatograph is used for qualitative and quantitative analysis. The solid residue is obtained after filtration. The conversion rate of high-density polyethylene is 100%, and the yield of C5-C40 liquid products is 90.2%. Figure 3 This is the carbon number distribution diagram of the liquid product.

[0017] The TEM image of the prepared Ru3Ni1 / SiO2 catalyst is shown in Figure 1 As shown in the figure, the prepared catalyst surface is successfully loaded with metal nanoparticles. The element surface scanning results show that Ru and Ni elements are gathered in the same position to form an alloy structure. Figure 2 Figure 2 is the XRD diffraction pattern of different Ru / Ni atomic ratios (the loading amount is kept at 5%). As the amount of Ni added increases, the diffraction peak of Ru obviously shifts to a high angle, which confirms the formation of the Ru-Ni alloy structure.

[0018] The present invention x Ni y / Test method for hydrogenolysis of polyethylene plastic into liquid fuel using SiO2 catalyst: Use HP-1 chromatographic column and FID detector to analyze the liquid product. The specific test method is as follows: Liquid product test method: Chromatographic column: HP-1, 30 m×320 μm×0.25 μm Detector: FID Starting temperature: 35°C Heating rate: 25℃ / min End temperature: 320℃, hold for 13.8 min Gas flow rate: 1.1 ml / min Split ratio: 20 Inlet temperature: 300°C Detector temperature: 300°C The liquid product was quantitatively and qualitatively analyzed according to the external standard method, that is, the peak time and peak area of ​​the FID signal measured with the C7-C40 standard substance (1 mg / ml) were compared to obtain the concentration C of the liquid product and the mass m=C×V of the product. Example 2

[0019] In this embodiment, the Ru3Ni1 / SiO2 catalyst of Example 1 was used. Similarly, when the H2 pressure was 3 MPa, the conversion rate of high-density polyethylene was 100%, and the yield of C5-C40 liquid products was 82.2%. Figure 4 Table 1 shows that the Ru3Ni1 / SiO2 catalyst has excellent degradation effect on different types of polyethylene plastics, among which the yield of liquid product of degraded linear low-density polyethylene is the highest, reaching 88.3%.

[0020] Example 3

[0021] In this example, the same Ru3Ni1 / SiO2 catalyst as in Example 1 was used. Similarly, when the H2 pressure was 4 MPa, the conversion rate of high-density polyethylene was 100%, and the yield of C5-C40 liquid products was 96.9%. Figure 5 is the carbon number distribution diagram of the liquid product. Table 2 shows that Ru3Ni1 / SiO2 catalyst can achieve complete degradation of high-density polyethylene under different pressure conditions. Under low pressure (1MPa) conditions, the yield of Ru3Ni1 / SiO2 catalyst catalytic conversion of high-density polyethylene into liquid fuel is as high as 90.2%.

[0022] Example 4

[0023] In this embodiment, silicon dioxide is used as a catalyst carrier, ammonium chlororuthenate (IV) is a soluble ruthenium salt precursor, the prepared catalyst has the same ruthenium loading (4.2%) as in Example 1, and the concentration of the hydrochloric acid solution is 0.03 M.

[0024] The mass of ammonium chlororuthenate (IV) weighed during the catalyst preparation process was 76.32 mg. Similarly, the Ru / SiO2 catalyst was prepared by the same method. After 12 hours of reaction, high-density polyethylene could be 100% degraded, and the yield of liquid product was only 10.0%.

[0025] In this example, silicon dioxide is used as a catalyst carrier, nickel (II) nitrate hexahydrate is used as a soluble nickel salt precursor, and the prepared catalyst has the same nickel loading (0.8%) as that in Example 1. The concentration of the hydrochloric acid solution is 0.03M.

[0026] The mass of hydrated nickel (II) nitrate weighed during the catalyst preparation process was 21.15 mg. Similarly, Ni / SiO2 catalyst was prepared by the same method. After 12 h of reaction, the degradation rate of high-density polyethylene was only 2.1%. Table 3 shows the comparison of the degradation results of high-density polyethylene by Ru / SiO2 catalyst, Ni / SiO2 catalyst and bimetallic Ru3Ni1 / SiO2 catalyst. The single metal Ni / SiO2 catalyst does not have the ability to degrade polyethylene under the same reaction conditions. The conversion rate of high-density polyethylene by single metal Ru / SiO2 and bimetallic Ru3Ni1 / SiO2 catalysts was 100%, but the yield of high-value liquid products by Ru3Ni1 / SiO2 catalyst was significantly higher than that of Ru / SiO2, which confirmed that the addition of Ni has a significant gain effect on improving the Ru-based catalyst in catalyzing the high-value conversion of polyethylene into liquid fuels.

[0027] Example 6

[0028] In this embodiment, silicon dioxide is used as a catalyst carrier, ammonium chlororuthenate (IV) and nickel nitrate hexahydrate (II) are catalyst metal precursors, wherein the atomic ratio of Ru and Ni is 9 / 1, accounting for 5% of the total mass of the catalyst. The concentration of the hydrochloric acid solution is 0.03 M.

[0029] The mass of ammonium chlororuthenate (IV) weighed during the catalyst preparation process was 85.57 mg, and the mass of nickel (II) nitrate hexahydrate weighed was 7.9 mg. Similarly, the Ru9Ni1 / SiO2 catalyst was prepared by the same method.

[0030] (1) Add 50 mg of Ru9Ni1 / SiO2 catalyst and 1 g of high-density polyethylene into the reactor and introduce 3 MPa of hydrogen; (2) Heating to 250°C for 6 h to allow for full hydrogenolysis reaction; (3) After the reaction is completed, the reactor is cooled to room temperature, the headspace gas in the reactor is slowly discharged, and the liquid product is dissolved with dichloromethane, and a gas chromatograph is used for qualitative and quantitative analysis. The solid residue is obtained after filtration. The conversion rate of high-density polyethylene is 100%, and the yield of C5-C40 liquid products is 76.7%. Figure 6 Table 4 shows the carbon number distribution of the liquid product. x Ni y Comparison of the degradation results of high-density polyethylene by Ru / SiO2 at 3 MPa x Ni y The loading amount of Ru is 5 wt%. x Ni y The yield of converting high-density polyethylene into liquid fuel by using Ru1Ni1 / SiO2 catalyst gradually increased, reaching a maximum of 93.3%. At the same time, the catalysts with high nickel content, Ru1Ni1 / SiO2 and Ru1Ni3 / SiO2, required 100 mg of catalyst and 18 or 36 hours of reaction to completely convert high-density polyethylene.

[0031]

[0032] Obviously, the above-mentioned implementation cases of the present invention are merely examples for clearly explaining the present invention, and are not intended to limit the implementation methods of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is impossible to list all the implementation methods here. Any obvious changes or modifications derived from the technical solution of the present invention are still within the scope of protection of the present invention.

Claims

1. A catalyst for hydrogenolysis of polyethylene plastic into liquid fuel, characterized in that The catalyst composition is: Ru x Ni y / SiO2, wherein SiO2 is a carrier, the molar ratio of Ru and Ni is x:y (1-20): (1-10), x and y are positive integers or decimals, Ru x Ni y The loading amount is 1~10 wt%.

2. The catalyst according to claim 1, characterized in that: The molar ratio of Ru and Ni is (1~10):(1~5).

3. The catalyst according to claim 2, characterized in that: The molar ratio of Ru to Ni is 1:

3.

4. The method for preparing the catalyst according to claim 1, characterized in that The following steps are involved: (1) Dissolving soluble ruthenium salt and nickel salt in 0.001-1M hydrochloric acid, adding silica support for impregnation, wherein the molar ratio of ruthenium salt to nickel salt is (1-20): (1-10), and the loading amount of ruthenium and nickel is 1-10 wt%; (2) removing the hydrochloric acid solution to obtain a solid product; (3) The product obtained in step (2) is reduced in a 5-20 vol% H2 / Ar hydrogen-argon mixture at 400-700°C to obtain Ru x Ni y / SiO2 catalyst.

5. The preparation method according to claim 4, characterized in that: The soluble ruthenium salt is selected from ammonium chlororuthenate, ruthenium trichloride, hexaammineruthenium chloride or ruthenium nitrosyl nitrate, and the soluble nickel salt is selected from nickel nitrate or nickel chloride.

6. The preparation method according to claim 4, characterized in that: The molar ratio of Ru and Ni is (1~10):(1~5).

7. Use of the catalyst according to claim 1 in the hydrogenolysis of polyethylene plastics.

8. The use according to claim 7, characterized in that The reaction steps are as follows: (1) adding a catalytic amount of a catalyst and polyethylene in a reactor, wherein the polyethylene is selected from one of high-density polyethylene, low-density polyethylene and linear low-density polyethylene, and introducing 1-4 MPa hydrogen; (2) Heating to 200-300°C for full hydrogenolysis reaction; (3) Collect the liquid products and use gas chromatograph to perform quantitative analysis on the liquid products. The polyethylene conversion rate is 100% and the C5-C40 product yield is 73-97%.

Citation Information

Patent Citations

  • Metal catalyst and preparation method as well as application thereof in cyclohexane preparation by selective hydrogenation of benzene

    CN104941637A

  • Ru-based degradable polyethylene catalyst and preparation method and application thereof

    CN114768800A

  • Supported RuM nano-alloy catalyst and preparation method thereof

    CN118162158A

  • Endolysins LysPALS22 of Jumbo bacteriophage PALS2 from Staphylococcus aureus

    KR1020210143685A

Cited By

  • FeRu / CeO2 catalyst as well as preparation method and application thereof

    CN119771445A