Preparation method of TC18 titanium alloy forge piece

Through electrode composition uniformity control, VAR smelting and multi-step forging processes, combined with overall heat treatment and commutation piercing, the problem of low material uniformity and efficiency in the preparation of TC18 titanium alloy forgings is solved, and high performance, high efficiency and low energy are achieved consuming production.

CN118989216APending Publication Date: 2024-11-22SHAANXI HANGYU NONFERROUS METAL PROCESSING CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411098936.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

During the preparation of TC18 titanium alloy forgings, there are problems such as difficult to ensure material structure uniformity and performance stability, high energy consumption and low efficiency, and it is difficult to meet the needs of modern industry for efficient, environmentally friendly and high-quality production.

Method used

Through electrode composition uniformity control and three VAR smelting, combined with billet forging, intermediate forging and finished product forging processes, the overall heat treatment is carried out, and the reversing pier pulling process is applied, and the forging process is optimized to improve material composition uniformity and tissue density, and reduce the Energy consumption.

Benefits of technology

The composition uniformity and mechanical properties of TC18 titanium alloy forgings have been significantly improved, the production cycle has been shortened, the production efficiency has been improved, and the production goals of high performance, high efficiency, low energy consumption and environmental protection have been achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118989216A_ABST
    Figure CN118989216A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of forge piece preparation, in particular to a TC18 titanium alloy forge piece preparation method which comprises the steps that a TC18 titanium alloy raw material is subjected to electrode component uniformity control and cast ingot smelting, and a TC18 titanium alloy cast ingot is obtained; the TC18 titanium alloy cast ingot is subjected to cogging forging, intermediate forging and finished product forging, and a semi-finished forge piece is obtained; and the semi-finished forge piece is subjected to overall heat treatment, and the TC18 titanium alloy forge piece is obtained. According to the method, the key problems in the TC18 titanium alloy forge piece preparation process are successfully solved, the production goals of high performance, high efficiency, low energy consumption and environmental protection are achieved, and the method has important application value and social benefits.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of forging preparation, and in particular to a method for preparing a TC18 titanium alloy forging. Background Art

[0002] The nominal composition of TC18 titanium alloy is Ti-5Al-5Mo-4.5V-1Cr-1Fe. This composition design makes the alloy perform well in mechanical properties. In the annealed state, the strength limit of TC18 titanium alloy can reach 1080MPa, and after strengthening heat treatment, its strength can exceed 1200MPa or even higher. In addition, the alloy also maintains good elongation, cross-sectional shrinkage and impact toughness, providing a solid material foundation for the manufacture of high-load-bearing structural parts.

[0003] Given the excellent performance of TC18 titanium alloy, it has been widely used in many fields. First, in the field of aerospace, TC18 titanium alloy is widely used to manufacture various high-load-bearing structural parts, such as aircraft landing gear, engine parts, etc. These parts need to withstand huge loads and complex stress environments, and the high strength and toughness of TC18 titanium alloy just meet these requirements.

[0004] However, despite the many advantages of TC18 titanium alloy, its preparation process is relatively complex and faces many challenges. Traditional preparation methods often fail to ensure the uniformity of the material's structure and the stability of its performance, resulting in uneven quality of the finished products. In addition, traditional methods also have problems such as high energy consumption and low efficiency, which makes it difficult to meet the needs of modern industry for efficient, environmentally friendly, and high-quality production. Summary of the invention

[0005] In view of this, the present invention proposes a preparation method of TC18 titanium alloy forgings, which is mainly to solve the problem of how to reduce energy consumption, improve production efficiency and meet the demand of modern industry for high-quality forgings while ensuring material properties.

[0006] The present invention provides a method for preparing a TC18 titanium alloy forging, the method comprising:

[0007] The TC18 titanium alloy raw material is subjected to electrode composition uniformity control and ingot melting to obtain a TC18 titanium alloy ingot;

[0008] The TC18 titanium alloy ingot is subjected to blank forging, intermediate forging and finished forging to obtain a semi-finished forging;

[0009] The semi-finished forging is subjected to overall heat treatment to obtain a TC18 titanium alloy forging.

[0010] In some embodiments of the present application, when the TC18 titanium alloy raw material is subjected to electrode composition uniformity control and ingot smelting to obtain a TC18 titanium alloy ingot, the process includes:

[0011] The TC18 titanium alloy raw material is subjected to electrode welding by vacuum argon-filled plasma arc welding. The electrode specification during electrode welding is φ500 mm, and the weight of a single electrode is 120 kg.

[0012] In some embodiments of the present application, after electrode welding is performed on the TC18 titanium alloy raw material by vacuum argon plasma arc welding, the method further includes:

[0013] The TC18 titanium alloy raw material after electrode welding is melted into ingots through three VAR melting methods.

[0014] In some embodiments of the present application, in the three-stage VAR smelting method, the current intensity during the first smelting is 12KA, the current intensity during the second smelting is 16KA, and the current intensity during the third smelting is 20KA.

[0015] In some embodiments of the present application, the pressure in the stable stage of the last smelting in the three-VAR smelting method is no more than 5 Pa, and the riser depth is no more than 60 mm.

[0016] In some embodiments of the present application, the specification of the TC18 titanium alloy ingot is Φ620mm.

[0017] In some embodiments of the present application, when the TC18 titanium alloy ingot is subjected to blank forging, intermediate forging and finished product forging to obtain a semi-finished forging, the process includes:

[0018] The deformation amount of the blank forging fire is 50% to 75%;

[0019] The deformation amount of the intermediate forging fire is 45% to 60%;

[0020] In the forging of the finished product, the forging times below the phase transformation point of the finished product are not less than twice.

[0021] In some embodiments of the present application, when the TC18 titanium alloy ingot is subjected to blank forging, intermediate forging and finished forging to obtain a semi-finished forging, the process further includes:

[0022] The heating temperature of the blank forging is 1150°C to 1200°C, and the final forging temperature is not less than 850°C;

[0023] The heating temperature of the intermediate forging is Tβ-50°C to Tβ+100°C, and the final forging temperature is not less than 800°C;

[0024] The heating temperature for forging the finished product is Tβ-40°C to 60°C, and the final forging temperature is not less than 800°C.

[0025] In some embodiments of the present application, when the semi-finished forging is subjected to overall heat treatment to obtain a TC18 titanium alloy forging, the process includes:

[0026] performing solution heat treatment and aging heat treatment on the semi-finished forging in sequence;

[0027] Among them, the temperature during the solution heat treatment is 830-850°C, the holding time is 2h, and the cooling method is furnace cooling; the temperature during the aging heat treatment is 610-630°C, the holding time is 6h, and the cooling method is air cooling.

[0028] In some embodiments of the present application, when the TC18 titanium alloy ingot is subjected to blanking forging, intermediate forging and finished forging to obtain a semi-finished forging, the process further includes:

[0029] Carry out reversing pier pulling for no less than 10 times.

[0030] Compared with the prior art, the present invention has the following beneficial effects: the present invention significantly improves the composition uniformity and organizational density of TC18 titanium alloy ingots through strict electrode composition uniformity control and three-time VAR smelting method. This not only helps to reduce defects and impurities inside the material, but also further enhances the mechanical properties of the alloy, such as strength, elongation and impact toughness, thereby ensuring the high quality of the forgings. At the same time, by optimizing the forging process, including multi-fire deformation of blank forging, intermediate forging and finished product forging, as well as reasonable heating temperature and final forging temperature control, the forgings can shorten the production cycle while maintaining high performance and improve production efficiency. In addition, the application of the reversing upsetting process also further improves the plasticity and processing properties of the material, which is beneficial to subsequent processing and forming. Compared with the traditional preparation method, the present invention effectively reduces energy consumption through refined smelting and forging process control. In particular, the VAR smelting method is carried out in a vacuum and argon-filled environment, which reduces the generation of oxidation and other harmful gases, and is beneficial to environmental protection and sustainable development. In summary, the present invention successfully solves the key problems in the preparation process of TC18 titanium alloy forgings through an innovative preparation method, achieves the production goals of high performance, high efficiency, low energy consumption and environmental protection, and has important application value and social benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Various other advantages and benefits will become apparent to those of ordinary skill in the art by reading the detailed description of the preferred embodiments below. The accompanying drawings are only used for the purpose of illustrating the preferred embodiments and are not to be considered as limiting the present invention. In the accompanying drawings:

[0032] Figure 1A flow chart of a method for preparing a TC18 titanium alloy forging provided in an embodiment of the present invention. DETAILED DESCRIPTION

[0033] Exemplary embodiments of the present disclosure will be described in more detail below with reference to the accompanying drawings. Although exemplary embodiments of the present disclosure are shown in the accompanying drawings, it should be understood that the present disclosure can be implemented in various forms and should not be limited by the embodiments described herein. On the contrary, these embodiments are provided in order to enable a more thorough understanding of the present disclosure and to fully convey the scope of the present disclosure to those skilled in the art. It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments can be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in conjunction with the implementation regulations.

[0034] See also Figure 1 As shown, this embodiment provides a method for preparing a TC18 titanium alloy forging, the method comprising:

[0035] S101: Controlling the electrode composition uniformity and ingot melting of the TC18 titanium alloy raw material to obtain a TC18 titanium alloy ingot;

[0036] S102: subjecting the TC18 titanium alloy ingot to blank forging, intermediate forging and finished forging to obtain a semi-finished forging;

[0037] S103: performing overall heat treatment on the semi-finished forging to obtain a TC18 titanium alloy forging.

[0038] Specifically, this embodiment uses a high-grade grade 1 small-particle titanium sponge to ensure uniform mixing with the intermediate alloy and good purity. TC18 titanium alloy not only contains a large amount of alloy elements, but also has a large deviation between the melting point and density of each alloy element and the matrix Ti. In order to ensure the uniformity of the ingot composition, an intermediate alloy with a melting point and density close to the matrix Ti is selected as an additive to reduce the deviation from the matrix Ti and ensure the uniformity of the composition. Sponge titanium is selected to remove foreign matter and oxidized, nitrided, etc. sponge titanium to ensure the purity of sponge titanium. An electronic scale or electronic balance is used to accurately weigh sponge titanium and alloy additives to ensure the accuracy of the ingredients. All raw materials are mechanically mixed and then pressed to obtain TC18 titanium alloy raw materials. The mixing time is strictly controlled to ensure the uniformity of the raw material distribution.

[0039] It is understandable that in this embodiment, the composition uniformity of the TC18 titanium alloy raw material is ensured by strict electrode composition uniformity control and ingot melting step (S101), which lays a good foundation for the subsequent forging process. This helps to reduce defects inside the material, such as segregation, inclusions, etc., thereby improving the mechanical properties and corrosion resistance of the forging. The three-step forging process (S102) of blank forging, intermediate forging and finished product forging can gradually refine the grains, improve the organizational structure of the material, and eliminate the residual stress generated during the forging process, thereby improving the dimensional accuracy and surface quality of the forging. In addition, this multi-step forging process also helps to improve the density and uniformity of the material, and further enhance the overall performance of the forging. The introduction of the overall heat treatment step (S103) aims to further adjust and optimize the organizational structure of the forging, eliminate forging stress, and improve the plasticity and toughness of the forging through reasonable heating, heat preservation and cooling processes. At the same time, the overall heat treatment can also improve the dimensional stability and fatigue resistance of the forging, ensuring that the final TC18 titanium alloy forging can meet the use requirements under various complex working conditions. The preparation method in this embodiment has clear steps, is easy to control, and the steps are closely connected, which is conducive to realizing automation and large-scale production. This can not only improve production efficiency and reduce production costs, but also ensure the stability and consistency of product quality. The preparation method of TC18 titanium alloy forgings provided in this embodiment shows significant advantages in terms of material properties, forging process, finished product quality and production efficiency, and has broad application prospects and promotion value.

[0040] In some embodiments of the present application, when the TC18 titanium alloy raw material is subjected to electrode composition uniformity control and ingot smelting to obtain a TC18 titanium alloy ingot, the process includes:

[0041] The TC18 titanium alloy raw material is subjected to electrode welding by vacuum argon-filled plasma arc welding. The electrode specification during electrode welding is φ500 mm, and the weight of a single electrode is 120 kg.

[0042] It can be understood that in this embodiment, by adopting the vacuum argon plasma arc welding method, the intrusion of oxygen and other impurities during the welding process is effectively avoided, thereby significantly improving the quality of electrode welding. This welding method ensures the strength and sealing of the welded joint, laying a solid foundation for the subsequent ingot smelting. The selection of the electrode specification of φ500mm and the weight design of a single electrode of 120 kg is based on in-depth consideration of the material properties and smelting process requirements of TC18 titanium alloy. Electrodes of this specification and weight are not only easy to operate, but also can maintain a stable current and temperature distribution during the smelting process, which helps to obtain a titanium alloy ingot with a more uniform composition. By strictly controlling the electrode composition uniformity of the TC18 titanium alloy raw material and adopting advanced process measures during the smelting process, the final titanium alloy ingot is more uniform in composition. This uniformity not only improves the mechanical properties and corrosion resistance of the ingot, but also reduces defects and scrap rates in subsequent processing. The optimized electrode welding and ingot smelting process make the entire production process smoother and more efficient. This can not only shorten the production cycle and reduce production costs, but also quickly respond to market demand and enhance the competitiveness of enterprises. In the production process of TC18 titanium alloy ingots, this embodiment achieves a significant improvement in the uniformity of ingot composition by optimizing electrode welding and ingot melting processes, and brings about a series of beneficial effects such as improved production efficiency, reduced production costs, and promotion of technological innovation.

[0043] In some embodiments of the present application, after electrode welding is performed on the TC18 titanium alloy raw material by vacuum argon plasma arc welding, the method further includes:

[0044] The TC18 titanium alloy raw material after electrode welding is melted into ingots through three VAR melting methods.

[0045] In some embodiments of the present application, in the three-stage VAR smelting method, the current intensity during the first smelting is 12KA, the current intensity during the second smelting is 16KA, and the current intensity during the third smelting is 20KA.

[0046] In some embodiments of the present application, the pressure in the stable stage of the last smelting in the three-VAR smelting method is no more than 5 Pa, and the riser depth is no more than 60 mm.

[0047] It is understandable that in this embodiment, after the TC18 titanium alloy raw material is electrode welded by vacuum argon plasma arc welding, the ingot is further melted by three VAR (Vacuum Arc Remelting) melting methods, which brings significant beneficial effects. VAR melting is carried out under a vacuum environment, which effectively avoids the reaction of the material with impurities such as oxygen and nitrogen in the air during the melting process, thereby improving the purity of the TC18 titanium alloy. With the increase of the number of melting times, the impurity content is further reduced, and the overall quality of the material is improved. By gradually increasing the current intensity during melting (from 12KA to 16KA and then to 20KA), not only the melting efficiency is improved, but also the convection and mixing in the melt are promoted, which helps to refine the grain structure. The refined grain structure can improve the mechanical properties and fatigue resistance of the material. During the VAR melting process, the molten metal is stirred under the action of electromagnetic force, which helps to eliminate defects such as component segregation and bubbles in the melt, thereby improving the uniformity of the material. This improvement in uniformity is of great significance for improving the overall performance of the material and extending its service life. The last melting stabilization stage maintains a pressure of no more than 5Pa, which helps to further reduce the gas content in the melt, especially the content of harmful gases such as hydrogen and oxygen. Low gas content can reduce defects such as pores and cracks in the material during subsequent processing and use, and improve the density and reliability of the material. Controlling the riser depth within a range of no more than 60mm helps to reduce the waste of ingots and improve the utilization rate of materials. At the same time, a reasonable riser design also helps to ensure the quality and performance of the ingot. The vacuum argon plasma arc welding in this embodiment combined with the three VAR melting methods can significantly improve the purity of the TC18 titanium alloy raw material, refine the grain structure, improve the uniformity of the material, reduce the gas content, and control the riser depth to improve the utilization rate of materials, thereby comprehensively improving the performance and quality of the TC18 titanium alloy.

[0048] In some embodiments of the present application, the specification of the TC18 titanium alloy ingot is Φ620mm.

[0049] It is understandable that the specification of Φ620mm in this embodiment makes the TC18 titanium alloy ingot more standardized and unified in size, which is conducive to achieving higher efficiency and precision in subsequent processing, manufacturing and application processes. Standardized ingot size can reduce process adjustments and equipment replacements caused by size differences, thereby reducing production costs and time costs. Secondly, the specification of Φ620mm also meets the requirements of titanium alloy ingot size in certain specific fields. For example, in high-end manufacturing industries such as aerospace and shipbuilding, there are strict requirements for material size, and this specification of TC18 titanium alloy ingot just meets the needs of these fields, providing strong support for its application in high-end manufacturing. In addition, the specification of Φ620mm also helps to improve the mechanical and physical properties of TC18 titanium alloy ingots. By optimizing the size and shape of the ingot, the internal organizational structure can be made more uniform and dense, thereby improving its mechanical properties such as tensile strength, yield strength, and fatigue strength. At the same time, it also helps to improve its physical properties such as thermal conductivity and electrical conductivity, thereby meeting a wider range of application needs.

[0050] In some embodiments of the present application, when the TC18 titanium alloy ingot is subjected to blank forging, intermediate forging and finished product forging to obtain a semi-finished forging, the process includes:

[0051] The deformation amount of the blank forging fire is 50% to 75%;

[0052] The deformation amount of the intermediate forging fire is 45% to 60%;

[0053] In the forging of the finished product, the forging times below the phase transformation point of the finished product are not less than twice.

[0054] In some embodiments of the present application, when the TC18 titanium alloy ingot is subjected to blank forging, intermediate forging and finished forging to obtain a semi-finished forging, the process further includes:

[0055] The heating temperature of the blank forging is 1150°C to 1200°C, and the final forging temperature is not less than 850°C;

[0056] The heating temperature of the intermediate forging is Tβ-50°C to Tβ+100°C, and the final forging temperature is not less than 800°C;

[0057] The heating temperature for forging the finished product is Tβ-40°C to 60°C, and the final forging temperature is not less than 800°C.

[0058] Specifically, Tβ refers to the β phase transition point temperature of titanium alloy. For TC18 titanium alloy, this temperature is usually around 880℃. This is the temperature point at which the titanium alloy transforms from α phase or α+β phase to complete β phase. At Tβ temperature, the crystal structure of the material changes, and the temperature control requirements during forging are very strict to ensure the performance and quality of the final material.

[0059] It can be understood that in this embodiment, the performance and quality of the final semi-finished forgings are significantly improved by finely controlling the forging process of the TC18 titanium alloy ingot. Specifically, by controlling the deformation of each fire in the blank forging, intermediate forging and finished forging stages, especially by performing no less than two fires below the phase transition point in the finished forging, it is helpful to refine the grains and reduce internal defects such as holes and inclusions, thereby optimizing the organizational structure of the material. This optimized organizational structure can significantly improve the mechanical properties of the material, such as strength, toughness and fatigue life. Precise forging temperature control (such as the heating temperature of the blank forging is 1150℃~1200℃, and the final forging temperature is not less than 850℃; the heating temperature of the intermediate forging is Tβ-50℃~Tβ+100℃, and the final forging temperature is not less than 800℃; the heating temperature of the finished product forging is Tβ-40℃~60℃, and the final forging temperature is not less than 800℃) ensures that the material is in the best hot working state during the forging process, reduces the problems of overburning and cracking caused by too high or too low temperature, and improves the utilization rate of the material. The TC18 titanium alloy ingot forging process described in this embodiment shows significant beneficial effects in improving material properties, improving material utilization, enhancing process stability and repeatability, reducing costs and improving efficiency.

[0060] In some embodiments of the present application, when the semi-finished forging is subjected to overall heat treatment to obtain a TC18 titanium alloy forging, the process includes:

[0061] performing solution heat treatment and aging heat treatment on the semi-finished forging in sequence;

[0062] Among them, the temperature during the solution heat treatment is 830-850°C, the holding time is 2h, and the cooling method is furnace cooling; the temperature during the aging heat treatment is 610-630°C, the holding time is 6h, and the cooling method is air cooling.

[0063] It can be understood that the specific process steps and parameter settings adopted in this embodiment when the semi-finished forgings are subjected to overall heat treatment to obtain TC18 titanium alloy forgings have brought significant beneficial effects. First, in the solution heat treatment stage, the temperature is set between 830 and 850 ° C, and the holding time is maintained for 2 hours, followed by furnace cooling. The main purpose of this step is to fully dissolve the alloying elements in the forging into the matrix phase to form a uniform solid solution, while eliminating some of the internal stresses and structural defects generated during the forging process. Through precise temperature control and holding time, the dissolution effect of the alloying elements can be ensured, and the uniformity and performance stability of the forgings can be improved. Next, in the aging heat treatment stage, the temperature is set between 610 and 630 ° C, the holding time is up to 6 hours, and then air cooling is adopted. The main purpose of the aging heat treatment is to precipitate the alloying elements dissolved in the matrix phase in the solution treatment at a certain speed and manner at low temperature to form a fine dispersed phase. These dispersed phases can significantly enhance the strength and toughness of the forgings while maintaining good plasticity and creep resistance. Through appropriate aging temperature and holding time, the distribution and morphology of the precipitated phase can be optimized, thereby further improving the comprehensive performance of the forging. The overall heat treatment process in this embodiment achieves fine regulation of the structure and performance of TC18 titanium alloy forgings by accurately controlling the temperature, holding time and cooling method of solid solution and aging heat treatment. This process can not only significantly improve the strength and toughness of the forgings, but also maintain good plasticity and creep resistance, meeting the needs of high-end aviation, aerospace and other fields for high-performance titanium alloy forgings. In addition, the process also has the advantages of simple operation, easy control, and low cost, and has high application value and promotion prospects.

[0064] In some embodiments of the present application, when the TC18 titanium alloy ingot is subjected to blanking forging, intermediate forging and finished forging to obtain a semi-finished forging, the process further includes:

[0065] Carry out reversing pier pulling for no less than 10 times.

[0066] It is understandable that in this embodiment, by introducing a reversing upsetting process of no less than 10 fires, the TC18 titanium alloy ingot is subjected to blank forging, intermediate forging and finished product forging to achieve the purpose of preparing semi-finished forgings, and the reversing upsetting process can effectively refine the grain structure of the titanium alloy material. During multiple heating and forging processes, the grains of the titanium alloy will undergo repeated crushing and recrystallization, thereby significantly reducing the grain size, which helps to improve the strength and toughness of the material. Through multiple reversing upsetting, the internal structure of the titanium alloy will be more evenly distributed. This includes the uniform distribution of alloying elements and the homogenization of phase structure, which helps to improve the comprehensive properties of the material, such as fatigue resistance, corrosion resistance, etc. During the forging process, internal defects such as shrinkage cavities and looseness that may exist in the ingot will be gradually compacted and eliminated. The reversing upsetting process can further enhance this effect through repeated forging of multiple fires, ensuring that the semi-finished forgings finally obtained have higher density and fewer internal defects. Due to grain refinement and homogenization of the structure, the material is easier to cut, drill or shape in the subsequent mechanical processing process, thereby improving production efficiency and reducing processing costs. The semi-finished forgings finally obtained will have significant improvements in strength, toughness, fatigue resistance, etc. The improvement of these properties makes the forgings have a wider application prospect in high-end manufacturing fields such as aerospace, petrochemicals, etc. In summary, the reversing upsetting process in the embodiment of the present application is of great significance to the forging process of TC18 titanium alloy ingots, and can significantly improve the quality and performance of the final product.

[0067] Those skilled in the art will appreciate that the embodiments of the present application may be provided as methods, systems or computer program products. Therefore, the present application may adopt the form of a complete hardware embodiment, a complete software embodiment or an embodiment in combination with software and hardware. Moreover, the present application may adopt the form of a computer program product implemented on one or more computer-usable storage media (including but not limited to disk storage, CD-ROM, optical storage, etc.) that contain computer-usable program code.

[0068] The present application is described with reference to flowcharts and / or block diagrams of methods, devices (systems) and computer program products according to embodiments of the present application. It should be understood that each process and / or box in the flowchart and / or block diagram, as well as the combination of processes and / or boxes in the flowchart and / or block diagram, can be implemented by computer program instructions. These computer program instructions can be provided to a processor of a general-purpose computer, a special-purpose computer, an embedded processor or other programmable data processing device to generate a machine, so that the instructions executed by the processor of the computer or other programmable data processing device generate instructions for implementing the processes in the flowchart and / or block diagram. Figure 1 A process or multiple processes and / or boxes Figure 1 A device that provides the functions specified in a block or multiple blocks.

[0069] These computer program instructions may also be stored in a computer-readable memory capable of directing a computer or other programmable data processing device to operate in a specific manner, so that the instructions stored in the computer-readable memory produce an article of manufacture comprising an instruction device, which implements the process Figure 1 A process or multiple processes and / or boxes Figure 1 A function specified in one or more boxes.

[0070] These computer program instructions can also be loaded onto a computer or other programmable data processing device so that a series of operating steps are executed on the computer or other programmable device to produce a computer-implemented process, thereby providing instructions for implementing the process. Figure 1 A process or multiple processes and / or boxes Figure 1 The steps for the functions specified in one or more boxes.

[0071] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the specific implementation methods of the present invention can still be modified or replaced by equivalents. Any modification or equivalent replacement that does not depart from the spirit and scope of the present invention should be covered within the scope of protection of the claims of the present invention.

Claims

1. A method for preparing a TC18 titanium alloy forging, characterized in that: The steps include: The TC18 titanium alloy raw material is subjected to electrode composition uniformity control and ingot melting to obtain a TC18 titanium alloy ingot; The TC18 titanium alloy ingot is subjected to blank forging, intermediate forging and finished forging to obtain a semi-finished forging; The semi-finished forging is subjected to overall heat treatment to obtain a TC18 titanium alloy forging.

2. The method for preparing a TC18 titanium alloy forging according to claim 1, characterized in that: When the TC18 titanium alloy raw material is subjected to electrode composition uniformity control and ingot melting to obtain the TC18 titanium alloy ingot, the process includes: The TC18 titanium alloy raw material is subjected to electrode welding by vacuum argon-filled plasma arc welding. The electrode specification during electrode welding is φ500 mm, and the weight of a single electrode is 120 kg.

3. The method for preparing a TC18 titanium alloy forging according to claim 2, characterized in that: After the TC18 titanium alloy raw material is subjected to electrode welding by vacuum argon-filled plasma arc welding, the method further comprises: The TC18 titanium alloy raw material after electrode welding is melted into ingots through three VAR melting methods.

4. The method for preparing a TC18 titanium alloy forging according to claim 3, characterized in that: In the three-stage VAR smelting method, the current intensity during the first smelting is 12KA, the current intensity during the second smelting is 16KA, and the current intensity during the third smelting is 20KA.

5. The method for preparing a TC18 titanium alloy forging according to claim 4, characterized in that: The pressure in the stable stage of the last smelting in the three-stage VAR smelting method is not greater than 5Pa, and the riser depth is not greater than 60mm.

6. The method for preparing a TC18 titanium alloy forging according to claim 5, characterized in that: The specification of the TC18 titanium alloy ingot is Φ620mm.

7. The method for preparing a TC18 titanium alloy forging according to claim 6, characterized in that: The TC18 titanium alloy ingot is subjected to blank forging, intermediate forging and finished product forging to obtain a semi-finished forging, comprising: The deformation amount of the blank forging fire is 50% to 75%; The deformation amount of the intermediate forging fire is 45% to 60%; In the forging of the finished product, the forging times below the phase transformation point of the finished product are not less than twice.

8. The method for preparing a TC18 titanium alloy forging according to claim 7, characterized in that: When the TC18 titanium alloy ingot is subjected to blank forging, intermediate forging and finished product forging to obtain a semi-finished forging, the method further comprises: The heating temperature of the blank forging is 1150°C to 1200°C, and the final forging temperature is not less than 850°C; The heating temperature of the intermediate forging is Tβ-50°C to Tβ+100°C, and the final forging temperature is not less than 800°C; The heating temperature for forging the finished product is Tβ-40°C to 60°C, and the final forging temperature is not less than 800°C.

9. The method for preparing a TC18 titanium alloy forging according to claim 8, characterized in that: The semi-finished forging is subjected to overall heat treatment to obtain a TC18 titanium alloy forging, comprising: performing solution heat treatment and aging heat treatment on the semi-finished forging in sequence; Among them, the temperature during the solution heat treatment is 830-850°C, the holding time is 2h, and the cooling method is furnace cooling; the temperature during the aging heat treatment is 610-630°C, the holding time is 6h, and the cooling method is air cooling.

10. The method for preparing a TC18 titanium alloy forging according to claim 9, characterized in that: When the TC18 titanium alloy ingot is subjected to blanking forging, intermediate forging and finished product forging to obtain a semi-finished forging, the method further comprises: Carry out reversing pier pulling for no less than 10 times.

Citation Information

Patent Citations

  • Preparation method for titanium alloy TC18 through vacuum smelting

    CN102644006A

  • High-thermal-conductivity rigid direct-cooling VAR smelting method

    CN114231770A

  • Efficient preparation method of titanium alloy forged material

    CN115069952A

  • Manufacturing method of ultra-thin and ultra-wide TC18 titanium alloy structural member

    CN117286354A

  • Smelting and forging method for titanium alloy with low component range

    CN117551904A