1000MPa-grade-strength TC4ELI wire material for dental central screw and preparation method of 1000MPa-grade-strength TC4ELI wire material
By adding intermediate alloys to TC4ELI titanium alloy and using multiple melting, forging, rolling, thermal drawing, double heat treatment and electric straightening processes, the composition deviation and insufficient performance of TC4ELI wire for dental central screws was solved. It achieves high strength, high plasticity and excellent straightness, meeting the special wire index of dental central screws.
Patent Information
- Application Number
- CN202411192011.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-06
AI Technical Summary
In the prior art, TC4ELI titanium alloy wire material for dental central screws has problems such as large composition deviation, high strength but low plasticity, insufficient elongation, and inability to meet dental processing requirements.
By adding an intermediate alloy to the metal titanium, three times of smelting, forging, rolling, hot drawing and double heat treatment were performed, combined with the electric straightening process, the composition was prepared with high uniformity, tensile strength between 1000-1100MPa, elongation, TC4ELI silk material with a rate greater than 20%.
The comprehensive performance improvement of TC4ELI wire for dental central screws has been achieved, with high composition uniformity, short production cycle, reduced cost and optimized straightness, meeting the index requirements of special wire for dental central screws.
Smart Images

Figure CN119082525A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of medical titanium alloy material processing, and in particular to a 1000MPa-grade strength TC4ELI wire for dental central screws and a preparation method thereof. Background Art
[0002] Medical titanium alloys have been widely used in artificial joints (such as hip, ankle, elbow, finger, shoulder joints, etc.), bone trauma products (intramedullary nails, bone plates, screws, etc.), spinal fixation systems, and orthodontic products (brackets, implants, and correction archwires) with their excellent biocompatibility, corrosion resistance, and comprehensive mechanical properties. Ti-6Al-4V (TC4 alloy) is a typical medical titanium alloy currently used in clinical practice. On the basis of TC4 alloy, TC4ELI titanium alloy reduces the content of interstitial elements C, N, O and impurity element Fe, and its strength is lower than that of TC4. It has good plasticity, toughness, and high damage tolerance.
[0003] Imported brands account for more than 90% of the oral implant market in my country, and domestic brands account for about 10%. Artificial dental implants are an important field in the oral medical industry, with broad development prospects and market potential. With the development of my country's economy and society and the improvement of people's living standards, people's demand and awareness of oral health will continue to increase. Especially with the acceleration of the aging process, there will be more and more people with missing teeth, and the demand for artificial implants will become more and more vigorous.
[0004] Dental implants consist of a crown, abutment, and implant from top to bottom, where the abutment and implant are connected by a screw (central screw), such as Figure 1 .
[0005] The dental abutment is an important part of the dental implant restoration process, and can be understood as a bridge connecting the implant and the restoration. The connection between the implant abutment and the implant is internal or external, and is retained by the central screw. The central screw is a key component in dental implant restoration, with a large market demand and good development prospects. Therefore, researching and developing a method for preparing TC4ELI titanium alloy wire for dental central screws to achieve domestic substitution has great social and economic significance.
[0006] However, the existing technology has the problem of large deviations in components between different batches, resulting in large deviations in indicators between batches and high discreteness; the strength index is higher than 1100MPa, the elongation is lower than 17%, the strength is high and the plasticity is low, which does not meet the medium strength and high plasticity index requirements for central screws; the straightness of 0.3-0.5mm / m cannot meet the needs of longitudinal cutting equipment for dental processing. Summary of the invention
[0007] In order to solve the above problems, the purpose of the present invention is to provide a method for preparing 1000MPa grade strength TC4ELI wire for dental central screws with high composition uniformity, tensile strength between 1000-1100MPa, and elongation greater than 20%.
[0008] In order to achieve the above object, the present invention provides the following technical solutions:
[0009] A method for preparing 1000MPa-grade strength TC4ELI wire for dental central screws comprises the following steps:
[0010] (1) adding an intermediate alloy to metallic titanium according to a designed composition ratio to obtain an alloy mixture;
[0011] (2) pressing the alloy mixture into electrodes and performing smelting three times to obtain finished ingots;
[0012] (3) forging and rolling the finished ingot to obtain a rod blank;
[0013] (4) hot drawing and cutting the rod blank to obtain a hot drawn blank;
[0014] (5) performing a double heat treatment on the hot drawn blank; the double heat treatment method comprises first performing full annealing and air cooling to room temperature, and then performing stress relief annealing and air cooling to room temperature;
[0015] (6) After double heat treatment, electrical straightening is performed, and then polishing is performed to obtain the 1000 MPa strength TC4ELI wire for the dental central screw;
[0016] Preferably, the metallic titanium in step (1) is sponge titanium; and the intermediate alloy is aluminum-vanadium alloy and titanium-iron alloy.
[0017] Preferably, the alloy mixture in step (1) comprises the following elements in weight percentage:
[0018] Aluminum (Al): 5.9%-6.2%, vanadium (V): 3.9%-4.2%, iron (Fe): 0.15%-0.20%, carbon (C): ≤0.05%, nitrogen (N): ≤0.02%, oxygen (O): ≤0.13%, hydrogen (H): ≤0.005%, and titanium (Ti) is the balance.
[0019] Preferably, the smelting in step (2) is carried out in a vacuum consumable smelting furnace; the smelting current is 18-21 kA, the smelting voltage is 30-34 V, the smelting vacuum degree is <1.33 Pa, and the hot capping time accounts for 1 / 4 to 1 / 3 of the smelting time.
[0020] Preferably, the forging in step (3) is to heat the finished ingot to 1100-1150°C in the β phase region, with a total deformation of 70%-90%; the rolling is to heat the ingot to 900-980°C, with a total deformation greater than 90%; and the rolling is performed twice.
[0021] Preferably, the specific method of the hot drawing in step (4) is: stopping the hot drawing when the rod blank is hot drawn to a diameter that is 15% to 20% larger than the size of the final product.
[0022] Preferably, the temperature of the complete annealing in step (5) is 680-720° C., and the holding time is 60-120 min.
[0023] Preferably, the stress relief annealing in step (5) is performed at a temperature of 480-520° C. and a holding time of 30-60 min.
[0024] Preferably, the current of the electrical straightening in step (6) is 180-200A, the insulation time is 8-12s, the counterweight is 12-15kg, and the straightness meets 0.2mm / m.
[0025] Another object of the present invention is to provide a 1000MPa grade strength TC4ELI wire for dental central screws prepared by the above method.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] The present invention further controls the composition range on the basis of the chemical composition of the existing medical titanium alloy Ti-6Al-4V, and after strict VAR smelting parameter setting, double heat treatment technology and straightening technology, the prepared TC4ELI titanium alloy wire for dental central screws has excellent comprehensive performance compared with conventional medical wires. The smelting process adopted by the present invention can make the TC4ELI wire composition highly uniform, and the double heat treatment + electrical straightening process is adopted, which has a short production cycle, significant cost reduction, excellent comprehensive performance, high straightness, high product comprehensive performance consistency, low range, and meets the index requirements of special wire for dental central screws. The wire produced by the method of the present invention has a tensile strength of 1000-1100MPa, an elongation greater than 20%, a cross-sectional shrinkage greater than 40%, a maximum torque greater than 45N·m, and a straightness of no more than 0.2mm / m. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is a diagram of the structure of a dental implant;
[0029] Figure 2 This is the microstructure diagram of TC4ELI wire in Example 1. DETAILED DESCRIPTION
[0030] The present invention provides a method for preparing 1000MPa-grade strength TC4ELI wire for dental central screws, the steps of which are as follows:
[0031] (1) adding an intermediate alloy to metallic titanium according to a designed composition ratio to obtain an alloy mixture;
[0032] (2) pressing the alloy mixture into electrodes and performing smelting three times to obtain finished ingots;
[0033] (3) forging and rolling the finished ingot to obtain a rod blank;
[0034] (4) hot drawing and cutting the rod blank to obtain a hot drawn blank;
[0035] (5) performing a double heat treatment on the hot drawn blank; the double heat treatment method comprises first performing full annealing and air cooling to room temperature, and then performing stress relief annealing and air cooling to room temperature;
[0036] (6) After double heat treatment, electrical straightening is performed, and then polishing is performed to obtain the 1000 MPa strength TC4ELI wire for the dental central screw;
[0037] In a specific embodiment of the present invention, the metallic titanium in step (1) is sponge titanium; and the intermediate alloy is an aluminum-vanadium alloy and a titanium-iron alloy.
[0038] In a specific embodiment of the present invention, the alloy mixture in step (1) comprises the following elements in weight percentage:
[0039] Aluminum (Al): 5.9%-6.2%, vanadium (V): 3.9%-4.2%, iron (Fe): 0.15%-0.20%, carbon (C): ≤0.05%, nitrogen (N): ≤0.02%, oxygen (O): ≤0.13%, hydrogen (H): ≤0.005%, and titanium (Ti) is the balance.
[0040] In a specific embodiment of the present invention, the smelting in step (2) is carried out in a vacuum consumable smelting furnace; the smelting current is 18-21 kA, the smelting voltage is 30-34 V, the smelting vacuum degree is <1.33 Pa, and the hot capping time is not less than 120 min.
[0041] In a specific embodiment of the present invention, the forging in step (3) is to heat the finished ingot to 1100-1150°C in the β phase region, with a total deformation of 70%-90%; the rolling is to heat the ingot to 900-980°C, with a total deformation greater than 90%; and the rolling is performed twice.
[0042] In a specific embodiment of the present invention, the specific method of the hot drawing in step (4) is: the hot drawing of the rod blank is stopped when the diameter is 15% to 20% of the size of the final product.
[0043] In a specific embodiment of the present invention, the temperature of the complete annealing in step (5) is 680-720° C., and the holding time is 60-120 min.
[0044] In a specific embodiment of the present invention, the stress relief annealing in step (5) is performed at a temperature of 480-520° C. and a holding time of 30-60 min.
[0045] In a specific embodiment of the present invention, the current of the electrical straightening in step (6) is 180-200A, the insulation time is 8-12s, the counterweight is 12-15kg, and the straightness meets 0.2mm / m.
[0046] The present invention will be further described below in conjunction with the embodiments.
[0047] Example 1
[0048] A method for preparing 1000MPa grade strength TC4ELI wire for dental central screws, the steps are as follows:
[0049] (1) Add aluminum-vanadium alloy and titanium-iron alloy to "grade 1" titanium sponge according to the following composition ratio design to obtain an alloy mixture:
[0050] Aluminum (Al): 6.2%, vanadium (V): 4.1%, iron (Fe): 0.16%, oxygen (O): 0.11%, and titanium (Ti) as the balance;
[0051] (2) pressing the alloy mixture into an electrode, and performing three smelting in a vacuum consumable smelting furnace to obtain a finished ingot; wherein the smelting current is 19 kA, the smelting voltage is 31 V, the smelting vacuum is 0.72-0.85 Pa, the starting weight of the hot sealing is 250 kg, and the hot sealing time is 150 min;
[0052] (3) After the finished ingot is ultrasonically inspected, the bottom and top of the cap are sawed off for forging; the forging method is to heat the ingot to 1120° C. in the β phase region in an electric furnace and forge it to The billet has a deformation of 85%;
[0053] After the surface defects of the billet are repaired, it is heated to 980℃ in a resistance furnace and rolled to Deformation 90%, reheating 920℃ and rolling to bar billet The deformation amount is 95%, and the rod blank is obtained;
[0054] (4) The rod blank is hot drawn to and cut the material to obtain hot drawn billet;
[0055] (5) performing a double heat treatment on the hot drawn blank; the double heat treatment method comprises first performing a complete annealing on the hot drawn blank at a temperature of 700° C. for 60 minutes, and air cooling to room temperature; then performing a stress relief annealing at a temperature of 500° C. for 40 minutes, and air cooling to room temperature;
[0056] (6) After double heat treatment, electrical straightening is performed with a current of 190A, a holding time of 10s, a counterweight of 12kg, and a straightness of no more than 0.2mm / m; then polishing is performed. The dental central screw uses 1000MPa strength TC4ELI wire. The chemical composition of the ingot was tested. The ingot composition conforms to the GB / T3620.1-2016 standard and the composition is uniform. The results are shown in Table 1. The microstructure of the TC4ELI wire in Example 1 is as follows Figure 2 .
[0057] Embodiments 2 to 4
[0058] The 1000 MPa strength TC4ELI wire for dental central screws was prepared according to the composition ratio and method of Example 1. The chemical composition of the ingot was tested, and the ingot composition met the GB / T3620.1-2016 standard and was uniform in composition. The results are shown in Table 1.
[0059] Table 1 Measured values of chemical composition of examples
[0060]
[0061] The mechanical properties of the titanium alloy wires prepared in Examples 1 to 4 were measured according to the method described in GB / T 228.1-2010. The results are shown in Table 2.
[0062] Table 2 Room temperature mechanical properties of examples
[0063]
[0064]
[0065] The maximum torque of the dental central screws prepared in Examples 1 to 4 was tested using an electronic torsion testing machine. Each group of samples was tested 5 times and the average value was calculated. The results are shown in Table 3.
[0066] Table 3 Maximum torque test of embodiment
[0067] Serial number Maximum torque / N·m Average value / N·m Example 1 48 / 50 / 50 / 49 / 49 49.2 Example 2 50 / 52 / 50 / 53 / 52 51.4 Example 3 55 / 55 / 53 / 54 / 53 54 Example 4 51 / 54 / 55 / 52 / 55 53.4
[0068] The straightness of the wire was tested with a feeler gauge on the straightness testing platform. Each group of samples was measured 5 times and the average value was calculated. The results are as follows.
[0069] Table 4 Straightness test of embodiment
[0070] Serial number Straightness mm / m Average value mm / m Example 1 0.15 / 0.14 / 0.16 / 0.18 / 0.16 0.158 Example 2 0.16 / 0.14 / 0.15 / 0.18 / 0.16 0.158 Example 3 0.15 / 0.14 / 0.14 / 0.16 / 0.14 0.146 Example 4 0.15 / 0.14 / 0.15 / 0.17 / 0.16 0.154
[0071] Comparative Example 1
[0072] A TC4ELI wire production and preparation method, the specific steps are as follows:
[0073] (1) Raw material selection: "Grade 1" sponge titanium is used as the raw material, aluminum-vanadium alloy and titanium-iron alloy are used as additive alloys, and the design values are as follows: aluminum (Al): 6.2%, vanadium (V): 4.1%, iron (Fe): 0.16%, oxygen (O): 0.11%, and titanium (Ti) as the balance;
[0074] (2) Ingot smelting: The raw materials prepared in step (1) are mixed and pressed into electrodes, and smelted three times in a vacuum consumable arc furnace, with a smelting current of 22 kA, a smelting voltage of 28 V, a smelting vacuum of 1.0 to 1.3 Pa, a heat capping starting weight of 200 kg, and a heat capping time of 105 min;
[0075] (3) Forging: After ultrasonic testing, the ingot is sawn to cut the bottom and mouth of the cap for forging; the ingot is heated to 1100° C. in the β phase region in an electric furnace, and forged to a square billet of 150 mm with a deformation of 85%;
[0076] (4) Rolling: After the surface defects of the billet are repaired, it is heated to 980℃ in a resistance furnace and rolled to Deformation 90%, reheating 920℃ and rolling to bar billet Deformation 95%;
[0077] (4) Hot drawing: The rolled bar is hot drawn to Get Pansi;
[0078] (5) Heat treatment: The finished coiled wire is subjected to annealing heat treatment at 700°C for 70 min and then air-cooled to room temperature;
[0079] (6) Cold straightening and cutting: the straightened material is cut into fixed length, with a straightness of 0.3-0.5 mm / m;
[0080] (7) Rough polishing: to
[0081] (8) Vacuum stress relief annealing: temperature 550°C, holding time 180 min, cooling to below 90°C, vacuum degree 6.0×10 -3 Pa.
[0082] (9) Fine polishing to finished product
[0083] The chemical composition of the ingot was tested and the results are shown in Table 5.
[0084] Comparative Examples 2 to 4
[0085] TC4ELI wire was prepared according to the method of Comparative Example 1. The chemical composition of the ingot was tested, and the results are shown in Table 5.
[0086] Table 5 Comparative Examples Chemical Composition Measured Values
[0087]
[0088] The mechanical properties of the titanium alloy wire prepared in the “Comparative Example” were measured according to the method described in GB / T 228.1-2010. The results are shown in Table 6.
[0089] Table 6 Room temperature mechanical properties of comparative examples
[0090]
[0091]
[0092] The maximum torque test of the dental central screw was carried out using an electronic torsion testing machine. The results are shown in Table 7.
[0093] Table 7 Comparative maximum torque test
[0094] Serial number Maximum torque / N·m Average value / N·m Comparative Example 1 34 / 32 / 33 / 34 / 32 33.0 Comparative Example 2 30 / 31 / 30 / 31 / 30 30.4 Comparative Example 3 32 / 31 / 30 / 32 / 31 31.2 Comparative Example 4 28 / 29 / 30 / 28 / 29 28.8
[0095] The straightness of the wire was tested with a feeler gauge on the straightness testing platform. The results are shown in Table 8.
[0096] Table 8 Comparative straightness test
[0097] Serial number Straightness mm / m Average value mm / m Comparative Example 1 0.35 / 0.36 / 0.37 / 0.36 / 0.37 0.362 Comparative Example 2 0.34 / 0.36 / 0.38 / 0.36 / 0.35 0.370 Comparative Example 3 0.42 / 0.40 / 0.38 / 0.41 / 0.40 0.402 Comparative Example 4 0.40 / 0.38 / 0.39 / 0.40 / 0.40 0.394
[0098] By comparison, it can be seen that different TC4ELI wires are obtained by using different VAR furnace smelting parameters in Comparative Examples 1 to 4 and Examples 1 to 4. From the perspective of chemical composition, the upper and lower parts of the comparative examples have large differences and poor composition uniformity, especially the deviation of the volatile element aluminum (Al) is 0.22%, and the deviation of the incremental element oxygen (O) is 0.011%. However, the chemical composition of the wire of the embodiment has a small dispersion of metal elements in the upper and lower parts, and the incremental control of impurity elements is excellent, which lays a good foundation for the performance consistency of subsequent dental central screw wires.
[0099] By comparison, it is found that the present invention adopts a dual heat treatment system of full annealing heat treatment + stress relief heat treatment, replacing the conventional atmospheric heat treatment + rough polishing + vacuum stress relief heat treatment process, which greatly reduces production costs, improves production efficiency, and solves the problem of inconsistent performance between batches. The straightness index of the "Implementation Example" using the electric straightening process is further controlled to 0.16mm / m, meeting the requirements of the dental material center-type CNC lathe. The comprehensive index of the TC4ELI wire for the central screw prepared in the "Implementation Example" is better than that of the "Comparative Example", and the average maximum torque is increased by more than 60%. The product has high consistency in comprehensive performance and low range, meeting the index requirements of special wire for dental central screws: strength 1000MPa~1100MPa, elongation index greater than 20%, and maximum torque greater than 35N·m.
[0100] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing 1000MPa grade strength TC4ELI wire for dental central screws, It is characterized in that The following steps are involved: (1) adding an intermediate alloy to metallic titanium according to a designed composition ratio to obtain an alloy mixture; (2) pressing the alloy mixture into electrodes and performing smelting three times to obtain finished ingots; (3) forging and rolling the finished ingot to obtain a rod blank; (4) hot drawing and cutting the rod blank to obtain a hot drawn blank; (5) performing a double heat treatment on the hot drawn blank; the double heat treatment method comprises first performing full annealing and air cooling to room temperature, and then performing stress relief annealing and air cooling to room temperature; (6) After the double heat treatment, electrical straightening is performed, and then polishing is performed to obtain the 1000 MPa strength TC4ELI wire for the dental central screw.
2. The method for preparing the 1000MPa grade strength TC4ELI wire for dental central screw according to claim 1, It is characterized in that The metallic titanium in step (1) is sponge titanium; and the intermediate alloy is aluminum-vanadium alloy and titanium-iron alloy.
3. The method for preparing the 1000MPa grade strength TC4ELI wire for dental central screw according to claim 1, It is characterized in that The alloy mixture of step (1) comprises the following elements in weight percentage: Aluminum: 5.9%-6.2%, vanadium: 3.9%-4.2%, iron: 0.15%-0.20%, carbon: ≤0.05%, nitrogen: ≤0.02%, oxygen: ≤0.13%, hydrogen: ≤0.005%, and titanium is the balance.
4. The method for preparing the 1000MPa grade strength TC4ELI wire for dental central screw according to claim 1, It is characterized in that The smelting in step (2) is carried out in a vacuum consumable smelting furnace; the smelting current is 18-21 kA, the smelting voltage is 30-34 V, the smelting vacuum degree is less than 1.33 Pa, and the hot sealing time is not less than 120 min.
5. The method for preparing the 1000MPa grade strength TC4ELI wire for dental central screw according to claim 1, It is characterized in that In step (3), the forging is to heat the finished ingot to 1100-1150° C. in the β phase region, with a total deformation of 70%-90%; the rolling is to heat the ingot to 900-980° C. with a total deformation greater than 90%; and the rolling is performed twice.
6. The method for preparing the 1000MPa grade strength TC4ELI wire for dental central screw according to claim 1, It is characterized in that The specific method of the hot drawing in step (4) is: the hot drawing of the rod blank is stopped when the diameter is 15% to 20% larger than the size of the final product.
7. The method for preparing the 1000MPa grade strength TC4ELI wire for dental central screw according to claim 1, It is characterized in that The temperature of the complete annealing in step (5) is 680-720° C., and the holding time is 60-120 min.
8. The method for preparing the 1000MPa grade strength TC4ELI wire for dental central screw according to claim 1, It is characterized in that The stress relief annealing temperature in step (5) is 480-520° C., and the holding time is 30-60 min.
9. The method for preparing the 1000MPa grade strength TC4ELI wire for dental central screw according to claim 1, It is characterized in that The current of the electrical straightening in step (6) is 180-200A, the insulation time is 8-12s, the counterweight is 12-15kg, and the straightness meets 0.2mm / m.
10. A 1000MPa strength TC4ELI wire for dental central screws, It is characterized in that Prepared according to the preparation method according to any one of claims 1 to 9.