Laminated busbar thermocompression bonding process for new energy automobile
By pretreating and laser cutting of waste aluminum plates, combining hot pressing and bending and insulating paint spraying technology, the high cost and complex process of thermal pressing and combining process for stacked busbars for new energy vehicles is solved, and resource utilization is achieved Improved and optimized insulation performance.
Patent Information
- Application Number
- CN202411136973.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-22
AI Technical Summary
The existing stacked busbar hot pressing process for new energy vehicles has problems of high production costs, complex processes and poor insulation effects, especially the failure to effectively utilize waste aluminum plates, resulting in waste of resources and low production efficiency.
The waste aluminum plate is pretreated and laser cut into prefabricated busbars. The integrated busbars are formed by hot pressing and bending and spraying insulating paint, which improves resource utilization and production speed while achieving excellent insulation performance.
It reduces production costs, improves resource utilization and production speed, and improves safety and insulation performance through non-toxic, halogen-free, flame-retardant insulating paint.
Smart Images

Figure CN118989871A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of electrical equipment, and in particular relates to a thermal pressing process for a laminated busbar for a new energy vehicle. Background Art
[0002] With the development of the new energy industry, the grouping technology of lithium-ion battery packs is becoming more and more important. The current battery packs are composed of a large number of single cells connected in series or in parallel to achieve the rated output power, and the busbar can well realize the series and parallel connection of multiple groups of single cells. The busbar refers to the copper or aluminum busbar connecting the main switch in the power cabinet and the switches in each branch circuit in the power supply system, and its main function is to serve as a conductor.
[0003] There are still some problems with the existing hot pressing process for laminated busbars for new energy vehicles: generally, new aluminum plates are used as manufacturing materials, which are relatively expensive, and waste aluminum plates are discarded as production consumables, thereby reducing the recycling efficiency of waste aluminum plates and increasing production costs. In addition, traditional integrated busbars require the addition of an insulating material layer, which is complicated to manufacture and has poor insulation effect. For this reason, we propose a hot pressing process for laminated busbars for new energy vehicles. Summary of the invention
[0004] The purpose of the present invention is to provide a hot pressing process for laminated busbars for new energy vehicles to solve the problems raised in the above-mentioned background technology.
[0005] To achieve the above object, the present invention provides the following technical solution: A hot pressing process for laminated busbars for new energy vehicles, comprising the following steps:
[0006] S1. Pretreatment of waste aluminum plates: Take waste aluminum plates, soak and passivate the surfaces of the waste aluminum plates to obtain aluminum plates to be processed;
[0007] S2. Cutting and setting materials: using laser cutting equipment, cutting the aluminum plate to be processed to obtain a prefabricated busbar;
[0008] S3. Fixed-point drilling: Take multiple groups of prefabricated busbars and drill holes in multiple groups of the prefabricated busbars;
[0009] S4 grinding and polishing: grinding the drilling holes and cutting edges of the multiple groups of the prefabricated busbars after S3 processing;
[0010] S5. Hot pressing and bending: The plurality of groups of prefabricated busbars after S4 treatment are heated to 100-160°C at a specified position according to the prefabrication requirements, and hot pressing and bending treatment is performed;
[0011] S6. Spraying: Spray insulating paint on the surfaces of the plurality of groups of prefabricated busbars after S5 treatment, and dry them:
[0012] S7. Assembly: The plurality of groups of prefabricated busbars processed in S6 are connected integrally by several groups of connecting bolts to form a finished integrated busbar;
[0013] S8. Inspection: Conduct conductivity test on the finished integrated busbar, and package it after passing the test.
[0014] Preferably, the immersion treatment of the surface of the waste aluminum plate in S1 specifically comprises the following steps:
[0015] S1011. Clean the surface of the waste aluminum plate to remove impurities and grease on the surface of the aluminum plate;
[0016] S1012. The cleaned waste aluminum plate is immersed in a soaking solution at a temperature of 65-75°C for 5-8 minutes;
[0017] S1013. The waste aluminum plates processed in S1012 are washed with water and then dried after washing.
[0018] Preferably, the soaking solution in S1012 comprises the following ingredients in parts by weight: 6-10 parts of bermudagrass, 3-5 parts of sodium tripolyphosphate, 15-25 parts of ethanol, 2-4 parts of silicic acid, and 60-120 parts of clean water.
[0019] Preferably, the soaking solution preparation method in S1012 specifically includes the following steps: taking materials by weight, crushing the bermudagrass, putting it into one third of clean water by weight, adding 0.1% anthraquinone by weight of the bermudagrass and 1% sodium carbonate by weight of the bermudagrass, stirring evenly, and boiling in a water bath with the temperature controlled at 85-95°C for 20-40 minutes, then cooling to room temperature, filtering the solid residue to obtain a filtrate, mixing the obtained filtrate with sodium tripolyphosphate, ethanol, silicic acid and the remaining clean water, and stirring evenly to obtain the desired soaking solution.
[0020] Preferably, the specific steps of passivating the surface of the waste aluminum plate in S1 include:
[0021] S1021. Take the waste aluminum plate after immersion treatment and spray silver oxide powder evenly on the surface of the aluminum plate at a spraying amount of 50-65g / m2;
[0022] S1022. Use a soft cloth dipped in kerosene to wipe the waste aluminum plate sprayed with silver oxide powder, the wiping pressure is 0.30-0.45MPa, and the wiping time is 4-10min;
[0023] S1023. The waste aluminum plate treated in S1022 is passivated with a passivation treatment solution at 20-35°C for 20-35 minutes;
[0024] S1024. Rinse the waste aluminum plate after the passivation treatment with deionized water and dry it at 35-40°C.
[0025] Preferably, the passivation treatment liquid in S1023 includes treatment liquid A and treatment liquid B, the mass concentration of silane coupling agent in treatment liquid A is 1.25-1.45%, the mass concentration of mixed amine is 4.5-5.5%, the mass concentration of dimethylformamide is 1.8-3.2%, and the balance is water; the mass concentration of sodium dichromate in treatment liquid B is 10-14%, the balance is water, and the pH is adjusted to 4.5-6; when in use, first use treatment liquid A for 10-15 minutes, and then use treatment liquid B for treatment.
[0026] Preferably, the laser cutting equipment in S2 includes a laser cutting head for cutting the plate, an X-axis moving assembly for horizontal movement, a Y-axis moving assembly for vertical movement, a locking assembly for fixing the plate, and a controller for controlling the operation of the equipment and setting parameters.
[0027] Preferably, the insulating paint sprayed in S6 comprises the following raw materials in parts by weight: 35-45 parts of polyurethane resin,
[0028] 15-25 parts of water-based baking varnish resin, 12-20 parts of silicone crosslinking agent, 12-24 parts of silicon dioxide, 10-18 parts of silicon hydroxide, 12-16 parts of magnesium hydroxide, 4-10 parts of iron oxide, 4-10 parts of barium sulfate, 4-8 parts of magnesium silicate, 2-5 parts of lubricant, 2-5 parts of antioxidant, 1-3 parts of compatibilizer; the preparation method of the insulating paint sprayed in S6 is specifically: take the raw materials in parts by weight and mix them, add a defoaming agent at a speed of 200-400r / min, stir for 20-40min, and obtain the insulating paint.
[0029] Preferably, the antioxidant is antioxidant 3114; the compatibilizer is ST-7 compatibilizer; and the lubricant is paraffin.
[0030] Preferably, before spraying the insulating paint, S6 further includes adding pigments of different colors into the insulating paint, and spraying the multiple groups of prefabricated busbars separately to obtain prefabricated busbars of different colors.
[0031] Compared with the prior art, the present invention has the following beneficial effects:
[0032] (1) The present invention can recycle the waste aluminum plates by pre-treating them, and use the waste aluminum plates to make integrated busbars, thereby increasing resource utilization and reducing production costs.
[0033] (2) The present invention uses laser cutting equipment to cut waste aluminum plates into prefabricated busbars and adopts a hot pressing and bending forming process, thereby reducing labor input and workload, thereby increasing production speed.
[0034] (3) The present invention performs insulation treatment on the surface of the prefabricated busbar by spraying insulating paint on the surface of the prefabricated busbar. The process is simple, and the insulating layer formed by the sprayed insulating paint has the characteristics of being non-toxic, halogen-free, and flame-retardant. At the same time, it has excellent insulation performance, which increases safety. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 It is a flow chart of the present invention. DETAILED DESCRIPTION
[0036] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0037] Example 1
[0038] See also Figure 1 The present invention provides a technical solution: a hot pressing process for laminated busbars for new energy vehicles, comprising the following steps:
[0039] S1. Pretreatment of waste aluminum plates: Take waste aluminum plates, soak and passivate the surfaces of the waste aluminum plates to obtain aluminum plates to be processed;
[0040] S2. Cutting and setting materials: using laser cutting equipment, cutting the aluminum plate to be processed to obtain a prefabricated busbar;
[0041] S3. Fixed-point drilling: Take multiple groups of prefabricated busbars and drill holes in multiple groups of the prefabricated busbars;
[0042] S4 grinding and polishing: grinding the drilling holes and cutting edges of the multiple groups of the prefabricated busbars after S3 processing;
[0043] S5. Hot pressing and bending: The plurality of groups of prefabricated busbars after S4 treatment are heated to 100-160°C at a specified position according to the prefabrication requirements, and hot pressing and bending treatment is performed;
[0044] S6. Spraying: Spray insulating paint on the surfaces of the plurality of groups of prefabricated busbars after S5 treatment, and dry them:
[0045] S7. Assembly: The plurality of groups of prefabricated busbars processed in S6 are connected integrally by several groups of connecting bolts to form a finished integrated busbar;
[0046] S8. Inspection: Conduct conductivity test on the finished integrated busbar, and package it after passing the test.
[0047] In this embodiment, preferably, the immersion treatment of the surface of the waste aluminum plate in S1 specifically includes the following steps:
[0048] S1011. Clean the surface of the waste aluminum plate to remove impurities and grease on the surface of the aluminum plate;
[0049] S1012. The cleaned waste aluminum plate is immersed in a soaking solution at a temperature of 65°C for 5 minutes;
[0050] S1013. The waste aluminum plates processed in S1012 are washed with water and then dried after washing.
[0051] In this embodiment, preferably, the soaking solution in S1012 comprises the following ingredients in parts by weight: 6 parts of bermudagrass, 3 parts of sodium tripolyphosphate, 15 parts of ethanol, 2 parts of silicic acid, and 60 parts of clean water.
[0052] In this embodiment, preferably, the soaking solution preparation method in S1012 specifically includes the following steps: taking materials by weight, crushing the bermudagrass, putting it into one-third of clean water, adding 0.1% anthraquinone by weight of the bermudagrass and 1% sodium carbonate by weight of the bermudagrass, stirring evenly, and boiling in a water bath with the temperature controlled at 85°C for 20 minutes, then cooling to room temperature, filtering the solid residue to obtain a filtrate, mixing the obtained filtrate with sodium tripolyphosphate, ethanol, silicic acid and the remaining clean water, and stirring evenly to obtain the desired soaking solution.
[0053] In this embodiment, preferably, the specific steps of passivating the surface of the waste aluminum plate in S1 include:
[0054] S1021. Take the waste aluminum plate after immersion treatment and spray silver oxide powder evenly on the surface of the aluminum plate at a spraying amount of 50g / m2;
[0055] S1022. Use a soft cloth dipped in kerosene to wipe the waste aluminum plate sprayed with silver oxide powder, the wiping pressure is 0.30MPa, and the wiping time is 4min;
[0056] S1023. The waste aluminum plate treated in S1022 is passivated with a passivation treatment solution at 20°C for 20 minutes;
[0057] S1024. Rinse the waste aluminum plate after the passivation treatment with deionized water and dry it at 35°C.
[0058] In this embodiment, preferably, the passivation treatment liquid in S1023 includes treatment liquid A and treatment liquid B, the mass concentration of silane coupling agent in treatment liquid A is 1.25%, the mass concentration of mixed amine is 4.5%, the mass concentration of dimethylformamide is 1.8%, and the balance is water; the mass concentration of sodium dichromate in treatment liquid B is 10%, the balance is water, and the pH is adjusted to 4.5; when in use, first use treatment liquid A for 10 minutes, and then use treatment liquid B for treatment.
[0059] In this embodiment, preferably, the laser cutting equipment in S2 includes a laser cutting head for cutting the plate, an X-axis moving assembly for horizontal movement, a Y-axis moving assembly for vertical movement, a locking assembly for fixing the plate, and a controller for controlling the operation of the equipment and setting parameters.
[0060] In this embodiment, preferably, the insulating paint sprayed in S6 includes the following raw materials in parts by weight: 35 parts of polyurethane resin, 15 parts of water-based baking varnish resin, 12 parts of silicone crosslinking agent, 12 parts of silicon dioxide, 10 parts of silicon hydroxide, 12 parts of magnesium hydroxide, 4 parts of iron oxide, 4 parts of barium sulfate, 4 parts of magnesium silicate, 2 parts of lubricant, 2 parts of antioxidant, and 1 part of compatibilizer; the preparation method of the insulating paint sprayed in S6 is specifically: take the raw materials in parts by weight and mix them, add a defoaming agent at a rotation speed of 200r / min, and stir for 20 minutes to obtain the insulating paint.
[0061] In this embodiment, preferably, the antioxidant is antioxidant 3114; the compatibilizer is ST-7 compatibilizer; and the lubricant is paraffin.
[0062] In this embodiment, preferably, before spraying the insulating paint, S6 further includes adding pigments of different colors into the insulating paint, and spraying the multiple groups of prefabricated busbars separately to obtain prefabricated busbars of different colors.
[0063] Example 2
[0064] See also Figure 1 The present invention provides a technical solution: a hot pressing process for laminated busbars for new energy vehicles, comprising the following steps:
[0065] S1. Pretreatment of waste aluminum plates: Take waste aluminum plates, soak and passivate the surfaces of the waste aluminum plates to obtain aluminum plates to be processed;
[0066] S2. Cutting and setting materials: using laser cutting equipment, cutting the aluminum plate to be processed to obtain a prefabricated busbar;
[0067] S3. Fixed-point drilling: Take multiple groups of prefabricated busbars and drill holes in multiple groups of the prefabricated busbars;
[0068] S4 grinding and polishing: grinding the drilling holes and cutting edges of the multiple groups of the prefabricated busbars after S3 processing;
[0069] S5. Hot pressing and bending: The plurality of groups of prefabricated busbars after S4 treatment are heated to 100-160°C at a specified position according to the prefabrication requirements, and hot pressing and bending treatment is performed;
[0070] S6. Spraying: Spray insulating paint on the surfaces of the plurality of groups of prefabricated busbars after S5 treatment, and dry them:
[0071] S7. Assembly: The plurality of groups of prefabricated busbars processed in S6 are connected integrally by several groups of connecting bolts to form a finished integrated busbar;
[0072] S8. Inspection: Conduct conductivity test on the finished integrated busbar, and package it after passing the test.
[0073] In this embodiment, preferably, the immersion treatment of the surface of the waste aluminum plate in S1 specifically includes the following steps:
[0074] S1011. Clean the surface of the waste aluminum plate to remove impurities and grease on the surface of the aluminum plate;
[0075] S1012. The cleaned waste aluminum plate is immersed in a soaking solution at a temperature of 75°C for 8 minutes;
[0076] S1013. The waste aluminum plates processed in S1012 are washed with water and then dried after washing.
[0077] In this embodiment, preferably, the soaking solution in S1012 comprises the following ingredients in parts by weight: 10 parts of bermudagrass, 5 parts of sodium tripolyphosphate, 25 parts of ethanol, 4 parts of silicic acid, and 120 parts of clean water.
[0078] In this embodiment, preferably, the soaking solution preparation method in S1012 specifically includes the following steps: taking materials by weight, crushing the bermudagrass, putting it into one-third of clean water, adding 0.1% anthraquinone by weight of the bermudagrass and 1% sodium carbonate by weight of the bermudagrass, stirring evenly, and boiling in a water bath with the temperature controlled at 95°C for 40 minutes, then cooling to room temperature, filtering the solid residue to obtain a filtrate, mixing the obtained filtrate with sodium tripolyphosphate, ethanol, silicic acid and the remaining clean water, and stirring evenly to obtain the desired soaking solution.
[0079] In this embodiment, preferably, the specific steps of passivating the surface of the waste aluminum plate in S1 include:
[0080] S1021. Take the waste aluminum plate after immersion treatment and spray silver oxide powder evenly on the surface of the aluminum plate at a spraying amount of 65g / m2;
[0081] S1022. Use a soft cloth dipped in kerosene to wipe the waste aluminum plate sprayed with silver oxide powder, the wiping pressure is 0.45MPa, and the wiping time is 10min;
[0082] S1023. The waste aluminum plate treated in S1022 is passivated at 35°C for 35 minutes using a passivation treatment solution;
[0083] S1024. Rinse the waste aluminum plate after the passivation treatment with deionized water and dry it at 40°C.
[0084] In this embodiment, preferably, the passivation treatment liquid in S1023 includes treatment liquid A and treatment liquid B, the mass concentration of silane coupling agent in treatment liquid A is 1.45%, the mass concentration of mixed amine is 5.5%, the mass concentration of dimethylformamide is 3.2%, and the balance is water; the mass concentration of sodium dichromate in treatment liquid B is 14%, the balance is water, and the pH is adjusted to 6; when in use, first use treatment liquid A for 15 minutes, and then use treatment liquid B for treatment.
[0085] In this embodiment, preferably, the laser cutting equipment in S2 includes a laser cutting head for cutting the plate, an X-axis moving assembly for horizontal movement, a Y-axis moving assembly for vertical movement, a locking assembly for fixing the plate, and a controller for controlling the operation of the equipment and setting parameters.
[0086] In this embodiment, preferably, the insulating paint sprayed in S6 includes the following raw materials in parts by weight: 45 parts of polyurethane resin, 25 parts of water-based baking varnish resin, 20 parts of silicone crosslinking agent, 24 parts of silicon dioxide, 18 parts of silicon hydroxide, 16 parts of magnesium hydroxide, 10 parts of iron oxide, 10 parts of barium sulfate, 8 parts of magnesium silicate, 5 parts of lubricant, 5 parts of antioxidant, and 3 parts of compatibilizer; the preparation method of the insulating paint sprayed in S6 is specifically: take the raw materials in parts by weight and mix them, add a defoaming agent at a rotation speed of 400r / min, and stir for 40 minutes to obtain the insulating paint.
[0087] In this embodiment, preferably, the antioxidant is antioxidant 3114; the compatibilizer is ST-7 compatibilizer; and the lubricant is paraffin.
[0088] In this embodiment, preferably, before spraying the insulating paint, S6 further includes adding pigments of different colors into the insulating paint, and spraying the multiple groups of prefabricated busbars separately to obtain prefabricated busbars of different colors.
[0089] Example 3
[0090] See also Figure 1 The present invention provides a technical solution: a hot pressing process for laminated busbars for new energy vehicles, comprising the following steps:
[0091] S1. Pretreatment of waste aluminum plates: Take waste aluminum plates, soak and passivate the surfaces of the waste aluminum plates to obtain aluminum plates to be processed;
[0092] S2. Cutting and setting materials: using laser cutting equipment, cutting the aluminum plate to be processed to obtain a prefabricated busbar;
[0093] S3. Fixed-point drilling: Take multiple groups of prefabricated busbars and drill holes in multiple groups of the prefabricated busbars;
[0094] S4 grinding and polishing: grinding the drilling holes and cutting edges of the multiple groups of the prefabricated busbars after S3 processing;
[0095] S5. Hot pressing and bending: The plurality of groups of prefabricated busbars after S4 treatment are heated to 100-160°C at a specified position according to the prefabrication requirements, and hot pressing and bending treatment is performed;
[0096] S6. Spraying: Spray insulating paint on the surfaces of the plurality of groups of prefabricated busbars after S5 treatment, and dry them:
[0097] S7. Assembly: The plurality of groups of prefabricated busbars processed in S6 are connected integrally by several groups of connecting bolts to form a finished integrated busbar;
[0098] S8. Inspection: Conduct conductivity test on the finished integrated busbar, and package it after passing the test.
[0099] In this embodiment, preferably, the immersion treatment of the surface of the waste aluminum plate in S1 specifically includes the following steps:
[0100] S1011. Clean the surface of the waste aluminum plate to remove impurities and grease on the surface of the aluminum plate;
[0101] S1012. The cleaned waste aluminum plate is immersed in a soaking solution at a temperature of 70°C for 7 minutes;
[0102] S1013. The waste aluminum plates processed in S1012 are washed with water and then dried after washing.
[0103] In this embodiment, preferably, the soaking solution in S1012 comprises the following ingredients in parts by weight: 8 parts of bermudagrass, 4 parts of sodium tripolyphosphate, 20 parts of ethanol, 3 parts of silicic acid, and 90 parts of clean water.
[0104] In this embodiment, preferably, the soaking solution preparation method in S1012 specifically includes the following steps: taking materials by weight, crushing the bermudagrass, putting it into one-third of clean water, adding 0.1% anthraquinone by weight of the bermudagrass and 1% sodium carbonate by weight of the bermudagrass, stirring evenly, and boiling in a closed water bath with the temperature controlled at 90°C for 30 minutes, then cooling to room temperature, filtering the solid residue to obtain a filtrate, mixing the obtained filtrate with sodium tripolyphosphate, ethanol, silicic acid and the remaining clean water, and stirring evenly to obtain the desired soaking solution.
[0105] In this embodiment, preferably, the specific steps of passivating the surface of the waste aluminum plate in S1 include:
[0106] S1021. Take the waste aluminum plate after immersion treatment and spray silver oxide powder evenly on the surface of the aluminum plate at a spraying amount of 55g / m2;
[0107] S1022. Use a soft cloth dipped in kerosene to wipe the waste aluminum plate sprayed with silver oxide powder, the wiping pressure is 0.38MPa, and the wiping time is 6min;
[0108] S1023. The waste aluminum plate treated in S1022 is passivated with a passivation treatment solution at 25°C for 25 minutes;
[0109] S1024. Rinse the waste aluminum plate after the passivation treatment with deionized water and dry it at 37°C.
[0110] In this embodiment, preferably, the passivation treatment liquid in S1023 includes treatment liquid A and treatment liquid B, the mass concentration of silane coupling agent in treatment liquid A is 1.35%, the mass concentration of mixed amine is 4.8%, the mass concentration of dimethylformamide is 2.2%, and the balance is water; the mass concentration of sodium dichromate in treatment liquid B is 12%, the balance is water, and the pH is adjusted to 5; when in use, first use treatment liquid A for 12 minutes, and then use treatment liquid B for treatment.
[0111] In this embodiment, preferably, the laser cutting equipment in S2 includes a laser cutting head for cutting the plate, an X-axis moving assembly for horizontal movement, a Y-axis moving assembly for vertical movement, a locking assembly for fixing the plate, and a controller for controlling the operation of the equipment and setting parameters.
[0112] In this embodiment, preferably, the insulating paint sprayed in S6 includes the following raw materials in parts by weight: 40 parts of polyurethane resin, 18 parts of water-based baking varnish resin, 16 parts of silicone crosslinking agent, 16 parts of silicon dioxide, 14 parts of silicon hydroxide, 13 parts of magnesium hydroxide, 6 parts of iron oxide, 6 parts of barium sulfate, 6 parts of magnesium silicate, 4 parts of lubricant, 4 parts of antioxidant, and 2 parts of compatibilizer; the preparation method of the insulating paint sprayed in S6 is specifically: take the raw materials in parts by weight and mix them, add a defoaming agent at a rotation speed of 300r / min, and stir for 30 minutes to obtain the insulating paint.
[0113] In this embodiment, preferably, the antioxidant is antioxidant 3114; the compatibilizer is ST-7 compatibilizer; and the lubricant is paraffin.
[0114] In this embodiment, preferably, before spraying the insulating paint, S6 further includes adding pigments of different colors into the insulating paint, and spraying the multiple groups of prefabricated busbars separately to obtain prefabricated busbars of different colors.
[0115] Principles and advantages of the present invention:
[0116] The present invention can recycle the waste aluminum plates by pre-treating them, and use the waste aluminum plates to make integrated busbars, thereby increasing resource utilization and reducing production costs; laser cutting equipment is used to cut the waste aluminum plates into prefabricated busbars, and a hot pressing and bending forming process is adopted, thereby reducing labor input and reducing the workload of personnel, thereby increasing production speed; insulating paint is sprayed on the surface of the prefabricated busbar to insulate the surface of the prefabricated busbar, the process is simple, and the insulating layer formed by the sprayed insulating paint has the characteristics of being non-toxic, halogen-free and flame-retardant, and at the same time, it has excellent insulation performance and increased safety.
[0117] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A hot pressing process for laminated busbars for new energy vehicles. Features: The following steps are involved: S1. Pretreatment of waste aluminum plates: Take waste aluminum plates, soak and passivate the surfaces of the waste aluminum plates to obtain aluminum plates to be processed; S2. Cutting and setting materials: using laser cutting equipment, cutting the aluminum plate to be processed to obtain a prefabricated busbar; S3. Fixed-point drilling: Take multiple groups of prefabricated busbars and drill holes in multiple groups of the prefabricated busbars; S4 grinding and polishing: grinding the drilling holes and cutting edges of the multiple groups of the prefabricated busbars after S3 processing; S5. Hot pressing and bending: The plurality of groups of prefabricated busbars after S4 treatment are heated to 100-160°C at a specified position according to the prefabrication requirements, and hot pressing and bending treatment is performed; S6. Spraying: Spray insulating paint on the surfaces of the plurality of groups of prefabricated busbars after S5 treatment, and dry them: S7. Assembly: The plurality of groups of prefabricated busbars processed in S6 are connected integrally by several groups of connecting bolts to form a finished integrated busbar; S8. Inspection: Conduct conductivity test on the finished integrated busbar, and package it after passing the test.
2. According to claim 1, a hot pressing process for laminated busbars for new energy vehicles, Features: The immersion treatment of the surface of the waste aluminum plate in S1 specifically includes the following steps: S1011. Clean the surface of the waste aluminum plate to remove impurities and grease on the surface of the aluminum plate; S1012. The cleaned waste aluminum plate is immersed in a soaking solution at a temperature of 65-75°C for 5-8 minutes; S1013. The waste aluminum plates processed in S1012 are washed with water and then dried after washing.
3. According to claim 2, a hot pressing process for laminated busbars for new energy vehicles, Features: The soaking solution in S1012 includes the following components in parts by weight: 6-10 parts of bermudagrass, 3-5 parts of sodium tripolyphosphate, 15-25 parts of ethanol, 2-4 parts of silicic acid, and 60-120 parts of clean water.
4. According to claim 3, a hot pressing process for laminated busbars for new energy vehicles, Features: The soaking solution preparation method in S1012 specifically includes the following steps: taking materials by weight, crushing bermudagrass, putting it into one-third of clean water, adding 0.1% anthraquinone by weight of bermudagrass and 1% sodium carbonate by weight of bermudagrass, stirring evenly, and then boiling in a water bath with the temperature controlled at 85-95°C for 20-40 minutes, then cooling to room temperature, filtering the solid residue to obtain a filtrate, mixing the obtained filtrate with sodium tripolyphosphate, ethanol, silicic acid and the remaining clean water, and stirring evenly to obtain the desired soaking solution.
5. According to claim 4, a hot pressing process for laminated busbars for new energy vehicles, Features: The specific steps of passivating the surface of the waste aluminum plate in S1 include: S1021. Take the waste aluminum plate after immersion treatment and spray silver oxide powder evenly on the surface of the aluminum plate at a spraying amount of 50-65g / m2; S1022. Use a soft cloth dipped in kerosene to wipe the waste aluminum plate sprayed with silver oxide powder, the wiping pressure is 0.30-0.45MPa, and the wiping time is 4-10min; S1023. The waste aluminum plate treated in S1022 is passivated with a passivation treatment solution at 20-35°C for 20-35 minutes; S1024. Rinse the waste aluminum plate after the passivation treatment with deionized water and dry it at 35-40°C.
6. A hot pressing process for laminated busbars for new energy vehicles according to claim 5, Features: The passivation treatment liquid in S1023 includes treatment liquid A and treatment liquid B. The mass concentration of silane coupling agent in treatment liquid A is 1.25-1.45%, the mass concentration of mixed amine is 4.5-5.5%, the mass concentration of dimethylformamide is 1.8-3.2%, and the balance is water; the mass concentration of sodium dichromate in treatment liquid B is 10-14%, the balance is water, and the pH is adjusted to 4.5-6; when in use, first use treatment liquid A for 10-15 minutes, and then use treatment liquid B for treatment.
7. According to claim 1, a hot pressing process for laminated busbars for new energy vehicles, Features: The laser cutting equipment in S2 includes a laser cutting head for cutting a plate, an X-axis moving assembly for horizontal movement, a Y-axis moving assembly for vertical movement, a locking assembly for fixing the plate, and a controller for controlling equipment operation and parameter setting.
8. According to claim 1, a hot pressing process for laminated busbars for new energy vehicles, Features: The insulating paint sprayed in S6 comprises the following raw materials in parts by weight: 35-45 parts of polyurethane resin, 15-25 parts of water-based baking varnish resin, 12-20 parts of silicone crosslinking agent, 12-24 parts of silicon dioxide, 10-18 parts of silicon hydroxide, 12-16 parts of magnesium hydroxide, 4-10 parts of iron oxide, 4-10 parts of barium sulfate, 4-8 parts of magnesium silicate, 2-5 parts of lubricant, 2-5 parts of antioxidant, 1-3 parts of compatibilizer; the preparation method of the insulating paint sprayed in S6 is specifically: take the raw materials in parts by weight and mix them, add a defoaming agent at a speed of 200-400r / min, stir for 20-40min, and obtain the insulating paint.
9. A hot pressing process for laminated busbars for new energy vehicles according to claim 8, Features: The antioxidant is antioxidant 3114; the compatibilizer is ST-7 compatibilizer; and the lubricant is paraffin.
10. A hot pressing process for laminated busbars for new energy vehicles according to claim 9, Features: Before spraying the insulating paint, the step S6 further includes adding pigments of different colors into the insulating paint, spraying the multiple groups of prefabricated busbars separately to obtain prefabricated busbars of different colors.
Citation Information
Patent Citations
High-efficiency insulating paint
CN105349012A
Surface treatment technology of aluminum plate
CN105349976A
Processing technology of new energy automobile busbar
CN105907132A
Surface treatment process for aluminum plate
CN105951150A
Laminated busbar thermocompression bonding process for new energy automobile
CN114300198A