Low-density calcium silicate board prepared from ardealite solid waste and preparation method of low-density calcium silicate board
By using raw materials such as phosphogypsum to prepare low-density calcium silicate boards, the problems of insufficient utilization of phosphogypsum solid waste and insufficient strength of calcium silicate boards are solved, and efficient and environmentally friendly plate production is achieved, suitable for a variety of building materials applications .
Patent Information
- Application Number
- CN202411111746.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-22
AI Technical Summary
In the prior art, the comprehensive utilization of phosphogypsum solid waste is not yet mature, resulting in waste of resources and environmental pollution, and the strength and stability of existing calcium silicate plates cannot meet the practical application requirements.
The low-density calcium silicate plate is prepared by controlling the solid content and pH value of the blanked slurry, and the water filtering on the flow slurry box is used to filter the water and rewind molding. Compacting and autoclaving processes are used to form low-density and high-strength calcium silicate plates.
It effectively improves the strength and density of calcium silicate boards, reduces production costs, realizes efficient utilization of phosphogypsum, avoids environmental pollution, and is suitable for a variety of building materials purposes.
Smart Images

Figure CN118993679A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of building materials, and particularly relates to a low-density calcium silicate board prepared by utilizing phosphogypsum solid waste and a preparation method thereof. Background Art
[0002] Calcium silicate board is a new type of green inorganic fireproof building material. Its main components are siliceous and calcium inorganic raw materials. It reacts during high temperature and high pressure steam curing to form flaky or needle-shaped tobermorite. It has the advantages of high strength, low moisture expansion rate, low thermal conductivity, good fireproof performance, and non-toxicity. Its preparation process includes powder mixing, online molding, multi-layer rewinding, static pre-curing, high temperature steam curing, shaping and sand cutting. At present, the main raw materials of domestic and foreign manufacturers are basically the same, mainly including quartz powder, cement, slaked lime, plant fiber, etc., of which siliceous and calcium raw materials account for 90% to 92%.
[0003] Phosphogypsum is an acidic solid waste produced in the production process of wet phosphoric acid. Usually, about 5 tons of phosphogypsum are produced for every ton of phosphoric acid produced. The main component is calcium sulfate dihydrate. However, since the fluoride, free phosphoric acid, heavy metals and other components contained in phosphogypsum are easy to pollute the environment, its large-scale utilization at this stage is still a difficult problem to solve. The silicon and calcium components of phosphogypsum account for more than 55-60%, and the bulk density is only 0.8-1.0g / cm 3 The comprehensive utilization of phosphogypsum can not only dispose of large amounts of solid waste and reduce the environmental harm caused by storage, but also turn waste into treasure, achieving both environmental and economic benefits in the process of increasing its added value.
[0004] At present, the utilization of phosphogypsum solid waste in China is not yet mature, and only about 15% of phosphogypsum is recycled. The main application scenarios are only in the fields of gypsum board and cement retarder, and its product strength and stability are still not guaranteed. The Chinese patent with patent number 201910419615.0 and the name of "Preparation method of anhydrous phosphogypsum-based assembled lightweight partition board" uses anhydrous phosphogypsum, semi-hydrated phosphogypsum, gypsum whiskers and other raw materials, and prepares an anhydrous phosphogypsum-based lightweight assembled partition board through processes such as adding water, mixing, and casting. However, the lightweight board prepared by this method has extremely low strength and has the problem of acid corrosion, which is difficult to meet the actual application requirements. The Chinese patent with the patent number of 201610199737.X and the name of "A phosphogypsum-based lightweight insulation board and its preparation method" prepares deacidified phosphogypsum for producing insulation gypsum board by washing, drying, grinding, calcining and other processes of phosphogypsum, but this method has the problems of high energy consumption, high water consumption, complex production process, low product strength, poor water resistance, etc. The Chinese patent application with the application number of 201811306014.0 and the name of "An environmentally friendly calcium silicate board and its preparation method" discloses a high-density calcium silicate board prepared from various industrial waste residues, in which the amount of phosphogypsum added is only about 5%, and slaked lime needs to be used for a long time of ball milling before use to achieve the purpose of acid-base neutralization. The board strength is only 6.5-6.8MPa, and there are defects such as low utilization rate, cumbersome production process and poor product strength. Summary of the invention
[0005] The primary purpose of the present invention is to overcome the shortcomings and deficiencies of the prior art and provide a method for preparing a low-density calcium silicate board using phosphogypsum solid waste.
[0006] Another object of the present invention is to provide a low-density calcium silicate board prepared by the method.
[0007] Another object of the present invention is to provide application of the low-density calcium silicate board.
[0008] The purpose of the present invention is achieved through the following technical solutions:
[0009] A method for preparing a low-density calcium silicate board using phosphogypsum solid waste comprises the following steps:
[0010] (1) Preparation of mixed slurry
[0011] Prepare the raw materials by weight: 60-70% phosphogypsum, 10-20% cement, 5-20% blast furnace slag, 5-10% quartz powder, and 5-10% reinforcing fiber; then mix the raw materials evenly, add water and stir to prepare a mixed blank slurry with a solid content of 15-20%, and control the total calcium-silicon molar ratio of the raw materials to 0.6-0.9, and control the system pH to 9-10 (the system pH is reduced from 12 to 9-10);
[0012] (2) Preparation of low-density calcium silicate board
[0013] The mixed slurry in step (1) is filtered through a slurry head box to form a thin wet material layer, which is then rewound through a forming drum to form a wet slab; the wet slab is then compacted at a pressure of 10 to 30 MPa, and then pre-cured and autoclaved to obtain the low-density calcium silicate board.
[0014] The phosphogypsum described in step (1) is primary hydrated phosphogypsum (acidic solid waste generated in the wet phosphoric acid production process), the main components of which are calcium sulfate dihydrate and silicon dioxide, the pH value is 9-11, the calcium-silicon molar ratio (the ratio of calcium element to silicon element) is 1.5-2.1, and the contents of the main components are as follows: CaSO4 63-70%, SiO2 21-26%, P2O5 0.8-1%, Al2O3 0.8-1.2%, Fe2O3 0.3-0.5%, and the moisture content is 10-11%.
[0015] The cement described in step (1) is Portland cement; preferably Portland cement 525#, with a calcium-silicon molar ratio of 5.0 to 5.3.
[0016] The blast furnace slag described in step (1) is a by-product of blast furnace ironmaking; preferably, it is basic slag with a fineness of 325 mesh, and its main components are as follows: CaO 35-38%; SiO2 30-35%; MgO 10-12%; Al2O3 15-18%; Fe2O3 <0.5%.
[0017] The quartz powder described in step (1) has a silicon dioxide content of ≥80%, a mud content of ≤1%, a whiteness of ≥65, and a particle size of 300 to 400 meshes (preferably 350 meshes).
[0018] The reinforcing fiber described in step (1) includes one or more of plant fiber, glass fiber, basalt fiber, wollastonite fiber and polyethyleneimine fiber; preferably, the reinforcing fiber is a fiber obtained by mixing plant fiber, glass fiber, basalt fiber and wollastonite fiber in a weight ratio of 1:1, or a fiber obtained by mixing plant fiber and polyethyleneimine fiber in a weight ratio of 1:1.
[0019] The plant fiber is preferably unbleached softwood pulp prepared by the kraft process, with a weight average length of 1.8 to 2.22 mm and a degree of polymerization of 1200.
[0020] The weight average length of the glass fiber is preferably 3 to 4 mm.
[0021] The weight average length of the wollastonite fibers is preferably 2 to 3 mm.
[0022] The molecular weight of the polyethyleneimine fiber is preferably 200,000, and the weight-average length of the fiber is preferably 5 to 8 mm.
[0023] The weight average length of the basalt fiber is preferably 3 to 4 mm.
[0024] The thickness of the wet slab described in step (2) can be set according to actual needs, preferably 6 mm to 12 mm; more preferably 8 mm.
[0025] The plate compaction treatment described in step (2) is preferably carried out by gradually increasing pressure, and the pressure and time gradient are: 0-10MPa, 5min; 10-20MPa, 20min; 20-30MPa, 25min (compacting time is 50min in total).
[0026] The method of pre-curing and autoclaving in step (2) is as follows: firstly, pre-curing is performed by standing at 30-50°C for 8-12 hours, and then, autoclaving is performed at 180-200°C for 18-24 hours.
[0027] The method for preparing low-density calcium silicate board using phosphogypsum solid waste further comprises, after step (2), the steps of cutting, shaping, edge grinding, sanding and drying the obtained low-density calcium silicate board, and finally obtaining a finished low-density calcium silicate board.
[0028] A low-density calcium silicate board is prepared by any of the methods described above.
[0029] The density of the low-density calcium silicate board is lower than 1000±5kg / m 3 ; preferably 800~1000kg / m 3 .
[0030] Application of the low-density calcium silicate board in building materials.
[0031] Compared with the prior art, the present invention has the following advantages and effects:
[0032] 1. The present invention aims to solve the problem that acidic solid waste phosphogypsum cannot be comprehensively utilized on a large scale and easily causes waste of resources and environmental pollution. By using it as the main raw material (accounting for no less than 60% of the weight of the board) in the alkaline preparation system of calcium silicate board, a treatment method with simple application, large dosage, high added value and no pollution is provided.
[0033] 2. The present invention has found through experiments that when the amount of phosphogypsum added is low (accounting for less than 15% of the weight of the board), the density of the produced calcium silicate board is higher (1250-1550kg / m 3, which belongs to the medium density range), and with the increase of phosphogypsum dosage, the strength gradually decreases. This is because when the dosage of phosphogypsum is small, it will act as a retarder and reduce the reactivity between silicon and calcium; when the proportion of phosphogypsum is increased to more than 60%, the strength of the board is greatly improved, and the density of the board can also be low. At this time, phosphogypsum becomes the main participating substance in the silicon-calcium reaction, rather than playing the role of a retarder. In addition, because phosphogypsum has a good pH neutralization effect and excellent silicon-calcium reaction performance, it promotes the formation of tobermorite during steaming, thereby making the prepared calcium silicate board achieve the unique properties of low density and high strength.
[0034] 3. The process for preparing low-density calcium silicate board from phosphogypsum solid waste provided by the present invention can increase the density of the board from the traditional 1250-1550 kg / m 3 Reduced to 800~1000kg / m 3 , utilizing the acidity of phosphogypsum to neutralize the excessively high alkaline environment during the preparation of calcium silicate boards, reducing the pH value of the reaction system to the optimal range (pH 9-10), thereby promoting the formation of low-density, high-strength tobermorite, and preventing the ineffective degradation of reinforcing fibers under high temperature and high alkalinity, greatly improving the strength of low-density calcium silicate.
[0035] 4. In the present invention, phosphogypsum does not require any additional treatment when used, is highly compatible with existing production lines, does not require modification, and has good product performance and low production cost.
[0036] 5. The method of the present invention can be applied to the preparation of low-density calcium silicate boards for various purposes, providing a guarantee for the utilization of solid waste and the innovation of calcium silicate boards. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 This is a photo of the appearance of phosphogypsum.
[0038] Figure 2 This is a photograph of a low-density calcium silicate board prepared using phosphogypsum solid waste in the present invention.
[0039] Figure 3 This is a microscopic morphology of a low-density calcium silicate board prepared using phosphogypsum solid waste in Example 1 of the present invention. DETAILED DESCRIPTION
[0040] The present invention is described in further detail below in conjunction with examples, but the embodiments of the present invention are not limited thereto. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art. The test methods for which specific experimental conditions are not specified in the following examples are usually in accordance with conventional experimental conditions. Unless otherwise specified, the reagents and raw materials used in the present invention can be obtained commercially. In the present invention, unless otherwise specified, all percentages (%) are weight percentages (wt%).
[0041] In the embodiment of the present invention, phosphogypsum is primary aqueous phosphogypsum ( Figure 1 ), without any additional treatment, the main components are calcium sulfate dihydrate and silicon dioxide, the pH is 9-11, the calcium-silicon molar ratio is 1.5-2.1, and the main components are shown in the following table:
[0042]
[0043]
[0044] In the embodiment of the present invention, the cement is Portland cement 525#, and the calcium-silicon molar ratio is 5.0-5.3.
[0045] In the embodiment of the present invention, blast furnace slag is a by-product of blast furnace ironmaking, preferably basic slag, and has a fineness of 325 mesh. The main components are shown in the following table:
[0046] raw material CaO(%) <![CDATA[SiO2(%)]]> MgO(%) <![CDATA[Al2O3(%)]]> <![CDATA[Fe2O3(%)]]> Blast furnace slag 35-38 30-35 10-12 15-18 <0.5
[0047] In the embodiment of the present invention, the silica content in the quartz powder is ≥80%, the mud content is ≤1%, the whiteness is ≥65, and the particle size is 350 mesh;
[0048] In an embodiment of the present invention, the reinforcing fiber comprises one or more of plant fiber, glass fiber, basalt fiber, wollastonite fiber, and polyethyleneimine fiber; wherein the plant fiber is unbleached coniferous wood pulp prepared by the sulfate process, purchased from Guangdong Yingtong Paper Co., Ltd., with a weight-average length of 1.8 to 2.22 mm, a degree of polymerization of 1200, and a model of SA3570; the glass fiber is an alkali-free glass fiber purchased from China Jushi Co., Ltd., with a weight-average length of 3 to 4 mm, and a model of D1640; the polyethyleneimine fiber is purchased from China Jushi Co., Ltd., with a molecular weight of 200,000, a fiber weight-average length of 5 to 8 mm, and a model of PEI9460; the basalt fiber is purchased from Sinoma Science & Technology Co., Ltd., with a weight-average length of 3 to 4 mm, and a model of XW7630; the wollastonite fiber is purchased from Hebei Hezhen Industrial Co., Ltd., with a weight-average length of 2 to 3 mm, and a model of GH18.
[0049] Example 1 Preparation of low-density calcium silicate board from phosphogypsum solid waste
[0050] (1) Preparation of low-density calcium silicate board using phosphogypsum solid waste as the main raw material ( Figure 2 ), the raw material composition includes the following materials by weight: 60% phosphogypsum, 20% cement, 5% blast furnace slag, 10% quartz powder, and 5% plant fiber (as reinforcing fiber);
[0051] (2) Preparation steps:
[0052] ① The raw materials described in step (1) are mixed in a batching tank, and water is added and stirred to prepare a mixed green sheet slurry with a solid content of 15%, and the total calcium-silicon molar ratio of the raw materials is controlled to be 0.6, and the system pH is 9;
[0053] ② The mixed slurry obtained in step ① was filtered through a conventional commercial open headbox (purchased from Suxinnuo Rail Technology Co., Ltd., with a width of 1300 mm, model K1300) to prepare a thin wet material layer, and then rewound through a conventional commercial forming cylinder (purchased from Zhengzhou Fangrui Zhenghe Machinery Manufacturing Co., Ltd., with a circumference of 3200 mm, model C3200) to form a wet slab with a thickness of 8 mm;
[0054] ③ The wet slab obtained in step ② was compacted for 50 minutes under the condition of gradually increasing pressure (gradually increasing pressure from 0MPa to 30MPa), and the pressure-time gradient was: 0-10MPa, 5min; 10-20MPa, 20min; 20-30MPa, 25min; then it was allowed to stand at 30℃ for 12h for pre-curing, and then autoclaved at 190℃ for 12h to obtain a density of about 1000kg / m 3 Low-density calcium silicate board;
[0055] ④ The low-density board obtained in step ③ is cut and shaped, edged, sanded and dried to obtain the final finished board required.
[0056] Example 2 Preparation of low-density calcium silicate board from phosphogypsum solid waste
[0057] (1) preparing a low-density calcium silicate board using phosphogypsum solid waste as the main raw material, the raw material composition comprising the following materials in parts by weight: 65% phosphogypsum, 10% cement, 10% blast furnace slag, 7.5% quartz powder, and 7.5% glass fiber (as reinforcing fiber);
[0058] (2) Preparation steps:
[0059] ① The raw materials described in step (1) are mixed in a batching tank, and water is added and stirred to prepare a mixed green sheet slurry with a solid content of 17%, and the total calcium-silicon molar ratio of the raw materials is controlled to be 0.7, and the system pH is 9.5;
[0060] ② The mixed slurry obtained in step ① was filtered through a conventional commercial open headbox (purchased from Suxinnuo Rail Technology Co., Ltd., with a width of 1300 mm, model K1300) to prepare a thin wet material layer, and then rewound through a conventional commercial forming cylinder (purchased from Zhengzhou Fangrui Zhenghe Machinery Manufacturing Co., Ltd., with a circumference of 3200 mm, model C3200) to form a wet slab with a thickness of 8 mm;
[0061] ③ The wet slab obtained in step ② was compacted for 50 minutes under gradually increasing pressure, and the pressure-time gradient was: 0-10MPa, 5min; 10-20MPa, 20min; 20-30MPa, 25min; then it was allowed to stand at 40℃ for 10h for pre-curing, and then autoclaved at 180℃ for 18h to obtain a density of about 900kg / m 3 Low-density calcium silicate board;
[0062] ④ The low-density board obtained in step ③ is cut and shaped, edged, sanded and dried to obtain the final finished board required.
[0063] Example 3 Preparation of low-density calcium silicate board from phosphogypsum solid waste
[0064] (1) preparing a low-density calcium silicate board using phosphogypsum solid waste as the main raw material, wherein the raw material composition includes the following materials in parts by weight: phosphogypsum 70%, cement 10%, blast furnace slag 5%, quartz powder 5%, and reinforcing fiber 10% (including 5% basalt fiber and 5% wollastonite fiber);
[0065] (2) Preparation steps:
[0066] ① The raw materials described in step (1) are mixed in a batching tank, and water is added and stirred to prepare a mixed green sheet slurry with a solid content of 20%, and the total calcium-silicon molar ratio of the raw materials is controlled to be 0.8, and the system pH is 10;
[0067] ② The mixed slurry obtained in step ① was filtered through a conventional commercial open headbox (purchased from Suxinnuo Rail Technology Co., Ltd., with a width of 1300 mm, model K1300) to prepare a thin wet material layer, and then rewound through a conventional commercial forming cylinder (purchased from Zhengzhou Fangrui Zhenghe Machinery Manufacturing Co., Ltd., with a circumference of 3200 mm, model C3200) to form a wet slab with a thickness of 8 mm;
[0068] ③ The wet slab obtained in step ② was compacted for 50 minutes under gradually increasing pressure, and the pressure-time gradient was: 0-10MPa, 5min; 10-20MPa, 20min; 20-30MPa, 25min; then it was allowed to stand at 50℃ for 8h for pre-curing, and then autoclaved at 200℃ for 24h to obtain a density of about 800kg / m 3 Low-density calcium silicate board;
[0069] ④ The low-density board obtained in step ③ is cut and shaped, edged, sanded and dried to obtain the final finished board.
[0070] Example 4 Preparation of low-density calcium silicate board from phosphogypsum solid waste
[0071] (1) preparing a low-density calcium silicate board using phosphogypsum solid waste as the main raw material, wherein the raw material composition includes the following materials in parts by weight: 60% phosphogypsum, 10% cement, 20% blast furnace slag, 5% quartz powder, and 5% reinforcing fiber (including 2.5% plant fiber and 2.5% polyethyleneimine fiber);
[0072] (2) Preparation steps:
[0073] ① The raw materials described in step (1) are mixed in a batching tank, and water is added and stirred to prepare a mixed green sheet slurry with a solid content of 19%, and the total calcium-silicon molar ratio of the raw materials is controlled to be 0.9, and the system pH is 9.6;
[0074] ② The mixed slurry obtained in step ① was filtered through a conventional commercial open headbox (purchased from Suxinnuo Rail Technology Co., Ltd., with a width of 1300 mm, model K1300) to prepare a thin wet material layer, and then rewound through a conventional commercial forming cylinder (purchased from Zhengzhou Fangrui Zhenghe Machinery Manufacturing Co., Ltd., with a circumference of 3200 mm, model C3200) to form a wet slab with a thickness of 8 mm;
[0075] ③ The wet slab obtained in step ② was compacted for 50 minutes under gradually increasing pressure, and the pressure-time gradient was: 0-10MPa, 5min; 10-20MPa, 20min; 20-30MPa, 25min; then it was allowed to stand at 50℃ for 12h for pre-curing, and then autoclaved at 200℃ for 12h to obtain a density of 850kg / m 3 Low-density calcium silicate board;
[0076] ④ The low-density board obtained in step ③ is cut and shaped, edged, sanded and dried to obtain the final finished board.
[0077] Comparative Example 1 Preparation of Medium Density Calcium Silicate Board
[0078] In this comparative example, except that the amount of phosphogypsum is 5%, the rest of the preparation process and operation are basically the same as those in the embodiment, and the specific steps are as follows:
[0079] (1) The raw material composition of the calcium silicate board includes the following materials by weight: 5% phosphogypsum, 35% cement, 35% blast furnace slag, 15% quartz powder, and 10% reinforcing fiber (including 5% plant fiber and 5% glass fiber);
[0080] (2) Preparation steps:
[0081] ① The raw materials described in step (1) are mixed in a batching tank, and water is added and stirred to prepare a mixed green sheet slurry with a solid content of 16%, and the total calcium-silicon molar ratio of the raw materials is controlled to be 0.8, and the pH of the system is 12;
[0082] ② The mixed slurry obtained in step ① was filtered through a conventional commercial open headbox (purchased from Suxinnuo Rail Technology Co., Ltd., with a width of 1300 mm, model K1300) to prepare a thin wet material layer, and then rewound through a conventional commercial forming cylinder (purchased from Zhengzhou Fangrui Zhenghe Machinery Manufacturing Co., Ltd., with a circumference of 3200 mm, model C3200) to form a wet slab with a thickness of 8 mm;
[0083] ③ The wet slab obtained in step ② was compacted for 50 minutes under gradually increasing pressure, and the pressure-time gradient was: 0-10MPa, 5min; 10-20MPa, 20min; 20-30MPa, 25min; then it was allowed to stand at 40℃ for 12h for pre-curing, and then autoclaved at 185℃ for 12h to obtain a density of 1250kg / m 3 Medium density calcium silicate board;
[0084] ④ Cut and shape the low-density board obtained in step ③, grind the edges, sand it and dry it in a sparse manner to obtain the final finished board. Figure 3 shown.
[0085] Comparative Example 2 Preparation of Medium Density Calcium Silicate Board
[0086] In this comparative example, except that the amount of phosphogypsum is 10%, the rest of the preparation process and operation are basically the same as those in the embodiment, and the specific steps are as follows:
[0087] (1) The raw material composition of the calcium silicate board includes the following materials in parts by weight: 10% phosphogypsum, 35% cement, 35% quartz powder, 10% slaked lime, and 10% reinforcing fiber (including 5% plant fiber and 5% glass fiber);
[0088] (2) Preparation steps:
[0089] ① The raw materials described in step (1) are mixed in a batching tank, and water is added and stirred to prepare a mixed green body slurry with a solid content of 16%, and the total calcium-silicon molar ratio of the raw materials is controlled to be 0.83, and the pH of the system is 11.8;
[0090] ② The mixed slurry obtained in step ① was filtered through a conventional commercial open headbox (purchased from Suxinnuo Rail Technology Co., Ltd., with a width of 1300 mm, model K1300) to prepare a thin wet material layer, and then rewound through a conventional commercial forming cylinder (purchased from Zhengzhou Fangrui Zhenghe Machinery Manufacturing Co., Ltd., with a circumference of 3200 mm, model C3200) to form a wet slab with a thickness of 8 mm;
[0091] ③ The wet slab obtained in step ② was compacted for 50 minutes under gradually increasing pressure, and the pressure-time gradient was: 0-10MPa, 5min; 10-20MPa, 20min; 20-30MPa, 25min; then it was allowed to stand at 40℃ for 12h for pre-curing, and then autoclaved at 185℃ for 12h to obtain a density of about 1250kg / m 3 Medium density calcium silicate board;
[0092] ④ The low-density board obtained in step ③ is cut and shaped, edged, sanded and dried to obtain the final finished board required.
[0093] Comparative Example 3 Preparation of Medium Density Calcium Silicate Board
[0094] In this comparative example, except that the amount of phosphogypsum is 15%, the rest of the preparation process and operation are basically the same as those in the embodiment, and the specific steps are as follows:
[0095] (1) The raw material composition of the calcium silicate board includes the following materials by weight: 15% phosphogypsum, 35% cement, 35% quartz powder, 5% slaked lime, and 10% reinforcing fiber (including 5% plant fiber and 5% glass fiber);
[0096] (2) Preparation steps:
[0097] ① The raw materials described in step (1) are mixed in a batching tank, and water is added and stirred to prepare a mixed green sheet slurry with a solid content of 16%, and the total calcium-silicon molar ratio of the raw materials is controlled to be 0.85, and the pH of the system is 11.6;
[0098] ② The mixed slurry obtained in step ① was filtered through a conventional commercial open headbox (purchased from Suxinnuo Rail Technology Co., Ltd., with a width of 1300 mm, model K1300) to prepare a thin wet material layer, and then rewound through a conventional commercial forming cylinder (purchased from Zhengzhou Fangrui Zhenghe Machinery Manufacturing Co., Ltd., with a circumference of 3200 mm, model C3200) to form a wet slab with a thickness of 8 mm;
[0099] ③ The wet slab obtained in step ② was compacted for 50 minutes under gradually increasing pressure, and the pressure-time gradient was: 0-10MPa, 5min; 10-20MPa, 20min; 20-30MPa, 25min; then it was allowed to stand at 40℃ for 12h for pre-curing, and then autoclaved at 185℃ for 12h to obtain a density of about 1250kg / m 3 Medium density calcium silicate board;
[0100] ④ The low-density board obtained in step ③ is cut and shaped, edged, sanded and dried to obtain the final finished board required.
[0101] Comparative Example 4 Preparation of Low-density Calcium Silicate Board
[0102] In this comparative example, conventional light filler diatomaceous earth is used as the main raw material to prepare low-density calcium silicate board. Except for the different raw material ratios, the rest of the preparation process and operation are basically the same as those in the embodiment.
[0103] (1) The raw material composition of the low-density calcium silicate board includes the following materials in parts by weight: 30% diatomaceous earth, 30% cement, 30% quartz powder, and 10% reinforcing fiber (including 5% plant fiber and 5% glass fiber);
[0104] (2) Preparation steps:
[0105] ① The raw materials described in step (1) are mixed in a batching tank, and water is added and stirred to prepare a mixed green sheet slurry with a solid content of 15%, and the total calcium-silicon molar ratio of the raw materials is controlled to be 0.6, and the pH of the system is 11.5;
[0106] ② The mixed slurry obtained in step ① was filtered through a conventional commercial open headbox (purchased from Suxinnuo Rail Technology Co., Ltd., with a width of 1300 mm, model K1300) to prepare a thin wet material layer, and then rewound through a conventional commercial forming cylinder (purchased from Zhengzhou Fangrui Zhenghe Machinery Manufacturing Co., Ltd., with a circumference of 3200 mm, model C3200) to form a wet slab with a thickness of 8 mm;
[0107] ③ The wet slab was compacted for 50 minutes under gradually increasing pressure, with the pressure-time gradient of: 0-10MPa, 5min; 10-20MPa, 20min; 20-30MPa, 25min; then it was allowed to stand at 30℃ for 12h for pre-curing, and then autoclaved at 180℃ for 12h to obtain a density of about 900kg / m 3 Low-density calcium silicate board;
[0108] ④ The low-density board obtained in step ③ is cut and shaped, edged, sanded and dried to obtain the final finished board required.
[0109] Comparative Example 5 Preparation of Low-density Calcium Silicate Board
[0110] In this comparative example, conventional lightweight filler hollow glass microspheres (purchased from Zhengzhou Saint-Laite Hollow Microsphere New Materials Co., Ltd., with a particle size of 40 to 50 μm, composition: 90% silicon dioxide, 5% aluminum oxide, and 5% calcium oxide) are used as the main raw material to prepare low-density calcium silicate board. Except for the different raw material ratios, the rest of the preparation process and operation are basically the same as the embodiment.
[0111] (1) The raw material composition of the low-density calcium silicate board includes the following materials by weight: 10% hollow glass beads, 32% cement, 30% quartz powder, 20% slaked lime, and 8% reinforcing fiber (including 8% plant fiber);
[0112] (2) Preparation steps:
[0113] ① The raw materials described in step (1) are mixed in a batching tank, and water is added and stirred to prepare a mixed green sheet slurry with a solid content of 20%, and the total calcium-silicon molar ratio of the raw materials is controlled to be 0.9, and the pH of the system is 12;
[0114] ② The mixed slurry obtained in step ① was filtered through a conventional commercial open headbox (purchased from Suxinnuo Rail Technology Co., Ltd., with a width of 1300 mm, model K1300) to prepare a thin wet material layer, and then rewound through a conventional commercial forming cylinder (purchased from Zhengzhou Fangrui Zhenghe Machinery Manufacturing Co., Ltd., with a circumference of 3200 mm, model C3200) to form a wet slab with a thickness of 8 mm;
[0115] ③ The wet slab obtained in step ② was compacted for 50 minutes under gradually increasing pressure, and the pressure-time gradient was: 0-10MPa, 5min; 10-20MPa, 20min; 20-30MPa, 25min; then it was allowed to stand at 50℃ for 8h for pre-curing, and then autoclaved at 200℃ for 24h to obtain a density of about 800kg / m 3 Low-density calcium silicate board;
[0116] ④ The low-density board obtained in step ③ is cut and shaped, edged, sanded and dried to obtain the final finished board required.
[0117] Effect Example
[0118] The low-density calcium silicate boards prepared in Examples 1 to 4, the medium-density calcium silicate boards prepared in Comparative Examples 1 to 3, and the conventional low-density calcium silicate boards prepared in Comparative Examples 4 to 5 were tested for flexural strength (GB / T 7019-2014), density (GB / T 7019-2014), freeze-thaw resistance (GB / T 7019-2014), water absorption (GB / T 7019-2014), non-flammability (GB / T 5465-2010), and shrinkage (JC / T 564.1-2008). The results are shown in Table 1.
[0119] Table 1 Performance test results of the plates of the embodiment and the comparative example
[0120] Test Project Flexural strength(MPa) <![CDATA[Density (kg / m 3 )]]> Freeze-thaw resistance (times) Water absorption (%) Shrinkage rate (%) Non-flammable Example 1 11.3 1003 ≥25 30.4 0.025 Level A Example 2 10.6 895 ≥25 32.5 0.021 Level A Example 3 10.2 806 ≥25 35.6 0.018 Level A Example 4 10.5 850 ≥25 33.9 0.019 Level A Comparative Example 1 8.3 1250 ≥25 28.6 0.047 Level A Comparative Example 2 7.6 1244 ≥25 28.9 0.042 Level A Comparative Example 3 6.9 1240 ≥25 29.2 0.038 Level A Comparative Example 4 8.7 907 20 36.9 0.043 Level A Comparative Example 5 7.6 802 17 35.6 0.059 Level A
[0121] Through experimental comparison, it is proved that the low-density calcium silicate board made of phosphogypsum solid waste prepared by the present invention can effectively improve the strength of the calcium silicate board, and its density can be between 800 and 1000 kg / m 3 The preparation time can be controlled. It can effectively neutralize the acidic impurities in the phosphogypsum, turning the phosphogypsum into treasure, which can not only reduce the production cost of low-density calcium silicate board, but also effectively protect the environment and make full use of resources. The above data can prove that the technology of the present invention can reduce the density of the board while improving the strength and other performance indicators of the low-density calcium silicate board.
[0122] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A method for preparing low-density calcium silicate board using phosphogypsum solid waste, characterized in that: The steps include: (1) Preparation of mixed slurry Prepare the raw materials by weight: 60-70% phosphogypsum, 10-20% cement, 5-20% blast furnace slag, 5-10% quartz powder, and 5-10% reinforcing fiber; then mix the raw materials evenly, add water and stir to prepare a mixed blank slurry with a solid content of 15-20%, and control the total calcium-silicon molar ratio of the raw materials to 0.6-0.9, and control the system pH to 9-10; (2) Preparation of low-density calcium silicate board The mixed slurry in step (1) is filtered through a headbox to form a thin wet material layer, and then rewound through a forming drum to form a wet slab; Then the wet slab is subjected to a plate compaction treatment at a pressure of 10 to 30 MPa, and then subjected to a pre-curing and autoclaving curing treatment to obtain the low-density calcium silicate board.
2. The method according to claim 1, characterized in that: The phosphogypsum described in step (1) is primary hydrated phosphogypsum, the main components of which are calcium sulfate dihydrate and silicon dioxide, the pH value is 9 to 11, and the calcium-silicon molar ratio is 1.5 to 2.1; The cement described in step (1) is Portland cement; The blast furnace slag described in step (1) is basic slag with a fineness of 325 mesh; The quartz powder described in step (1) has a silicon dioxide content of ≥80%, a mud content of ≤1%, a whiteness of ≥65, and a particle size of 300-400 meshes.
3. The method according to claim 2, characterized in that: The cement described in step (1) is Portland cement 525#, and the molar ratio of calcium to silicon is 5.0-5.
3.
4. The method according to claim 1, characterized in that: The reinforcing fibers described in step (1) include one or more of plant fibers, glass fibers, basalt fibers, wollastonite fibers and polyethyleneimine fibers.
5. The method according to claim 4, characterized in that: The reinforcing fiber described in step (1) is a fiber obtained by mixing plant fiber, glass fiber, basalt fiber and wollastonite fiber in a weight ratio of 1:1, or a fiber obtained by mixing plant fiber and polyethyleneimine fiber in a weight ratio of 1:
1.
6. The method according to claim 1, characterized in that: The plate compaction treatment in step (2) is carried out by gradually increasing the pressure, and the pressure and time gradient are: 0-10 MPa, 5 min; 10-20 MPa, 20 min; 20-30 MPa, 25 min; The method of pre-curing and autoclaving in step (2) is as follows: firstly, pre-curing is performed by standing at 30-50°C for 8-12 hours, and then, autoclaving is performed at 180-200°C for 18-24 hours.
7. The method according to claim 1, characterized in that: The thickness of the wet slab described in step (2) is 6 mm to 12 mm.
8. The method according to claim 1, characterized in that After step (2), the method further includes the steps of cutting, shaping, edge grinding, sanding and drying the obtained low-density calcium silicate board, and finally obtaining a finished low-density calcium silicate board.
9. A low-density calcium silicate board, characterized in that: It is prepared by the method according to any one of claims 1 to 8.
10. Use of the low-density calcium silicate board according to claim 9 in building materials.
Citation Information
Cited By
High-strength environment-friendly ardealite nano geopolymer aggregate and preparation method thereof
CN121135253A