Carboxyl-terminated polylactic acid as well as preparation method and application thereof

Through the reaction of cyclic acid anhydride and end-hydroxy polylactic acid, combined with appropriate catalysts and reaction conditions, the problem of difficult control of the molecular weight and acid value of traditional end-carboxylic polylactic acid is solved, and the light color end-carboxylic polylactic acid is achieved, which broadens its application range , especially in the field of biodegradable protective coatings.

CN118994552APending Publication Date: 2024-11-22ANHUI BBCA FERMENTATION TECH ENG RES
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411141400.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In the traditional end-carboxylic polylactic acid synthesis method, the molecular weight and acid value are difficult to accurately control, the color is dark, the equipment requirements are high, and the operation is cumbersome, which limits the application range of the material.

Method used

The cyclic anhydride and terminal hydroxyl polylactic acid are used to mix reactions in the presence of a catalyst to generate terminal carboxy polylactic acid. By controlling the reaction temperature and time, the controllability of molecular weight and acid value is ensured, and by selecting appropriate catalysts and reaction conditions, Reduce color deviation.

Benefits of technology

It achieves precise control of the molecular weight and acid value of end-carboxylic polylactic acid, with a light color (white or light yellow), and is suitable for degradable protective coatings, replacing traditional petroleum-based materials, reducing white pollution and carbon emissions, and protecting the environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994552A_ABST
    Figure CN118994552A_ABST
Patent Text Reader

Abstract

The invention provides carboxyl-terminated polylactic acid as well as a preparation method and application thereof. The structure of the carboxyl-terminated polylactic acid is shown as a formula I or a formula II. The carboxyl-terminated polylactic acid prepared by the preparation method disclosed by the invention is controllable in molecular weight and relatively light in color and luster, can replace a traditional petroleum-based material to be applied to the aspect of degradable protective paint, and can effectively reduce white pollution and carbon emission and protect the environment. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of chemical industry, and specifically relates to carboxyl-terminated polylactic acid and a preparation method and application thereof. Background Art

[0002] Polylactic acid is a green functional polymer material with excellent biocompatibility and biodegradability, which is polymerized from small molecule lactic acid generated by microbial fermentation of biomass raw materials (corn starch, wheat starch, sweet potato starch, natural fiber). It can be completely degraded into water and carbon dioxide. Compared with petroleum-based general-purpose plastics, it is more in line with the concept of circular economy and sustainable development. Not only is the product easy to degrade and will not cause environmental pollution, but it can also fundamentally solve the problem of rising costs caused by the depletion of oil resources and environmental governance. At present, traditional polylactic acid materials on the market are hard and brittle, and have poor impact resistance, which limits the application range of polylactic acid materials. Therefore, it is urgent to develop a new type of polylactic acid material (carboxyl-terminated polylactic acid) to broaden the application range of polylactic acid.

[0003] At present, the traditional method for synthesizing carboxyl-terminated polylactic acid is mainly: using lactic acid as raw material, gradually heating under vacuum conditions to generate prepolymers, then gradually heating to high temperature under high vacuum conditions to continue polycondensation reaction, and finally adding organic acid or acid anhydride as end group modifier to synthesize carboxyl-terminated polylactic acid. In this method, the molecular weight of carboxyl-terminated polylactic acid mainly depends on the degree of reaction of lactic acid under high vacuum and gradient heating conditions for dehydration polycondensation. When the prepolymer is generated in the early stage, the dehydration amount is large and easy to collect, so the degree of polymerization can be roughly judged. When the molecular weight continues to increase in the later stage, the water output is small and the deviation is large, making it difficult to accurately control the degree of polymerization; in addition, high temperature and long-term reaction often lead to the synthesized carboxyl-terminated polylactic acid with a darker color, which cannot meet specific use requirements; and the equipment requirements are high (such as high vacuum, dehydration device), the operation is cumbersome, the synthesized carboxyl-terminated polylactic acid is only linear, and the molecular weight and acid value are also unstable. Therefore, it is urgent to develop a new method for synthesizing carboxyl-terminated polylactic acid. Summary of the invention

[0004] In order to solve one of the above technical problems existing in the prior art, the present invention provides a carboxyl-terminated polylactic acid and a preparation method and application thereof. The carboxyl-terminated polylactic acid of the present invention has light color, controllable molecular weight and acid value.

[0005] The first aspect of the present invention provides a carboxyl-terminated polylactic acid, the general structural formula of which is shown in the following formula I or formula II:

[0006]

[0007]

[0008] In Formula I, R 1 is selected from substituted or unsubstituted C2 ~ 8 Alkylene, substituted or unsubstituted C 2 ~ 3 Alkylene-OC 2 ~ 3 Alkylene, the substitution is selected from C 1 ~ 3 The alkyl group;

[0009] In Formula II, R 1 Selected from Where R 1a , R 1b , R 1c are each independently selected from substituted or unsubstituted C 1 ~ 6 Alkylene, R 1d Selected from hydrogen or C 1 ~ 6 Alkyl, R 1a , R 1b and R 1c When the substituent is contained, the substituent is independently selected from C 1 ~ 3 alkyl;

[0010] In Formula I and Formula II, R 2 are each independently selected from substituted or unsubstituted phenylene, substituted or unsubstituted C 2 ~ 4 Alkenylene, substituted or unsubstituted C 2 ~ 4 The alkylene group, the substituents used in the substitution are each independently selected from C 1 ~ 6 Alkyl, carboxyl, C 2 ~ 10 a, b, c are each independently selected from any integer in the range of 4-138.

[0011] According to some embodiments of the present invention, in Formula I, the sum of a and b is selected from any integer of 12-278.

[0012] According to some embodiments of the present invention, in Formula II, the sum of a, b, and c is selected from any integer of 12-278.

[0013] According to some embodiments of the present invention, R 2 The substituents used in the substitution are each independently selected from C 1 To C 3 Alkyl, carboxyl, C 6 ~ 10 The alkenyl group.

[0014] According to some embodiments of the present invention, R 2 The substituents used in the substitution are independently selected from methyl, carboxyl and decenyl.

[0015] According to some embodiments of the present invention, in Formula I, R 1 Selected from 1,2-ethylene, 1,3-propylene, 1,4-butylene, 1,5-pentylene, 1,6-hexylene, -CH 2 -CH(CH 3 )-、-CH 2 CH 2 -O-CH 2 CH 2 -、-CH 2 -CH 2 -CH(CH 3 )-CH 2 -CH 2 -or-CH 2 -C(CH 3 ) 2 -CH 2 -.

[0016] According to some embodiments of the present invention, in Formula II, R 1 Selected from Where R 1a , R 1b , R 1c Each independently selected from C 1 ~ 3 Alkylene, R 1d Selected from hydrogen or C 1 ~ 4 alkyl.

[0017] According to some embodiments of the present invention, in Formula II, R 1 Selected from Where R 1d Selected from hydrogen or C 1 ~ 4 alkyl.

[0018] According to some embodiments of the present invention, in Formula II, R 1 Selected from

[0019] According to some embodiments of the present invention, in Formula I and Formula II, the R 2 Each independently selected from the following groups which are unsubstituted or substituted by one or more substituents selected from carboxyl, methyl, propenyl, hexenyl, octenyl and decenyl: phenylene, vinylene, ethylene, propylene.

[0020] According to some embodiments of the present invention, in Formula I and Formula II, the R2 The group selected from phenylene, carboxyl-substituted phenylene, -CH=CH-, 1,2-ethylene, 1,3-propylene, methyl-substituted 1,2-ethylene, and decenyl-substituted 1,2-ethylene.

[0021] According to some embodiments of the present invention, the number average molecular weight of the carboxyl-terminated polylactic acid is 1000-20000, for example, 1000, 1215, 1500, 1700, 2300, 5630, 8610, 10200, 11600, 13621, 16253, 19310, 19500, or 20000.

[0022] According to some embodiments of the present invention, the number average molecular weight of the carboxyl-terminated polylactic acid is 1500-19500.

[0023] According to some embodiments of the present invention, the acid value of the terminal carboxyl polylactic acid is 5.6-168.3 mgKOH / g, for example, 5.6 mgKOH / g, 8.0 mgKOH / g, 8.3 mgKOH / g, 10.2 mgKOH / g, 36.3 mgKOH / g, 56.8 mgKOH / g, 87.2 mgKOH / g, 100.0 mgKOH / g, 113.6 mgKOH / g, 129.1 mgKOH / g, 141.3 mgKOH / g, 159.3 mgKOH / g, and 168.3 mgKOH / g.

[0024] According to some embodiments of the present invention, the acid value of the carboxyl-terminated polylactic acid is 8.0-100.0 mgKOH / g.

[0025] The second aspect of the present invention provides a method for preparing the carboxyl-terminated polylactic acid described in the first aspect, comprising the following steps: in the presence of a first catalyst, mixing a cyclic acid anhydride with a hydroxyl-terminated polylactic acid to generate the carboxyl-terminated polylactic acid, wherein the hydroxyl-terminated polylactic acid has a structure shown in the following formula I-1 or formula II-1:

[0026]

[0027] Among them, in formula (I-1), R 1 The definitions of a, b are the same as those in Formula I; in Formula (II-1), R 1 , a, b and c are as defined in Formula II.

[0028] According to some embodiments of the present invention, the general structural formula of the cyclic anhydride is as follows:

[0029]

[0030] Where R 2The definition of is the same as above in this article.

[0031] According to some embodiments of the present invention, in the cyclic anhydride, R 2 is selected from substituted or unsubstituted phenylene, -CH=CH-, substituted or unsubstituted C 2 ~ 4 The alkylene group, the substituents used in the substitution are each independently selected from C 1 ~ 6 Alkyl, carboxyl, C 2 ~ 10 The alkenyl group.

[0032] According to some embodiments of the present invention, R 2 The substituents used in the substitution are each independently selected from C 1 ~ 3 Alkyl, carboxyl, C 6 ~ 10 The alkenyl group.

[0033] According to some embodiments of the present invention, R 2 The substituents used in the substitution are independently selected from methyl, carboxyl and decenyl.

[0034] According to some embodiments of the present invention, in the cyclic anhydride, R 2 One or more selected from the group consisting of phenylene, carboxyl-substituted phenylene, -CH=CH-, 1,2-ethylene, 1,3-propylene, methyl-substituted 1,2-ethylene, and decenyl-substituted 1,2-ethylene.

[0035] According to some embodiments of the present invention, the cyclic acid anhydride is selected from one or more of phthalic anhydride, trimellitic anhydride, maleic anhydride, glutaric anhydride, succinic anhydride, methylsuccinic anhydride, and decenylsuccinic anhydride.

[0036] According to some embodiments of the present invention, the first catalyst is selected from zinc catalysts and / or tin catalysts. In some embodiments, the zinc catalyst is selected from zinc oxide and zinc chloride. In some embodiments, the tin catalyst is selected from one or more of stannous chloride, stannous octoate and dibutyltin dilaurate. In some embodiments, the added mass of the first catalyst is 0.005%-0.1% of the total mass of the terminal hydroxyl polylactic acid and the cyclic anhydride, for example 0.005%, 0.009%, 0.01%, 0.03%, 0.06%, 0.09%, 0.1%.

[0037] According to some embodiments of the preparation method of the present invention, the molar ratio of the cyclic anhydride to the hydroxyl group of the hydroxy-terminated polylactic acid is (1.0-1.2):1, for example, 1:1, 1.1:1, 1.2:1.

[0038] According to some embodiments of the preparation method of the present invention, the temperature of the mixing reaction is 130-180°C, for example, 130°C, 140°C, 155°C, 160°C, 175°C, 180°C.

[0039] According to some embodiments of the preparation method of the present invention, the temperature of the mixing reaction is 140-170°C.

[0040] According to some embodiments of the preparation method of the present invention, the mixing reaction time is 3-15 hours, for example, 3 hours, 5 hours, 8 hours, 10 hours, 12 hours, and 15 hours.

[0041] According to some embodiments of the preparation method of the present invention, the mixing reaction time is 5-8 hours.

[0042] According to some embodiments of the preparation method of the present invention, the hydroxy-terminated polylactic acid is synthesized by a method comprising the following steps: in the presence of a second catalyst, lactide and a polyol are polymerized to generate the hydroxy-terminated polylactic acid.

[0043] According to some embodiments of the preparation method of the present invention, the lactide is selected from one or more of L-lactide, D-lactide, and Meso-lactide.

[0044] According to some embodiments of the preparation method of the present invention, the polyol is selected from one or more of ethylene glycol, diethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, glycerol, 1,4-butanediol, neopentyl glycol, 1,5-pentanediol, 1,6-hexanediol, trimethylolpropane, and 3-methyl-1,5-pentanediol.

[0045] According to some embodiments of the preparation method of the present invention, the second catalyst is selected from a zinc catalyst and / or a tin catalyst. In some embodiments, the zinc catalyst is selected from zinc oxide and zinc chloride. In some embodiments, the tin catalyst is selected from one or more of stannous chloride, stannous octoate and dibutyltin dilaurate.

[0046] According to some embodiments of the preparation method of the present invention, the second catalyst is the same as the first catalyst used in the mixed reaction of the cyclic anhydride and the hydroxy-terminated polylactic acid.

[0047] According to some embodiments of the preparation method of the present invention, the second catalyst is different from the first catalyst used in the mixed reaction of the cyclic anhydride and the hydroxy-terminated polylactic acid.

[0048] According to some embodiments of the preparation method of the present invention, the mass ratio of the polyol to the lactide is 1:(5-350), preferably 1:(5-300). In some embodiments, the mass ratio of the polyol to the lactide is 1:(6-321).

[0049] According to some embodiments of the preparation method of the present invention, the added amount of the second catalyst is 0.005%-0.1% of the total mass of lactide and polyol, preferably 0.01%-0.1%.

[0050] According to some embodiments of the preparation method of the present invention, the temperature of the polymerization reaction is 130-180°C.

[0051] According to some embodiments of the preparation method of the present invention, the temperature of the polymerization reaction is 140-170°C.

[0052] According to some embodiments of the preparation method of the present invention, the polymerization reaction time is 3-15 hours.

[0053] According to some embodiments of the preparation method of the present invention, the polymerization reaction time is 5-8 hours.

[0054] According to some embodiments of the preparation method of the present invention, the polymerization reaction is carried out in an inert atmosphere such as nitrogen.

[0055] According to some embodiments of the preparation method of the present invention, the polymerization reaction is a melt polymerization reaction.

[0056] According to some embodiments of the preparation method of the present invention, the preparation method of the carboxyl-terminated polylactic acid comprises the following steps:

[0057] (1) in the presence of the second catalyst, polymerizing lactide and a polyol to obtain a reaction solution containing the hydroxy-terminated polylactic acid;

[0058] (2) mixing the cyclic acid anhydride with the reaction solution containing the hydroxyl-terminated polylactic acid obtained in step (1) to generate the carboxyl-terminated polylactic acid.

[0059] The third aspect of the present invention provides an application of the carboxyl-terminated polylactic acid described in the first aspect of the present invention or the carboxyl-terminated polylactic acid prepared by the preparation method described in the second aspect of the present invention in a degradable protective coating.

[0060] According to some embodiments of the application of the present invention, the degradable protective coating is a degradable protective coating for a metal shell or a degradable protective coating for a plastic shell.

[0061] The beneficial effects of the present invention are as follows: the present invention firstly polymerizes lactide and polyol under the action of a catalyst to generate terminal hydroxyl polylactic acid, and then reacts the terminal hydroxyl polylactic acid with a cyclic acid anhydride to obtain terminal carboxyl polylactic acid. The obtained terminal carboxyl polylactic acid has a controllable molecular weight and a lighter color (white or light yellow). It can replace traditional petroleum-based materials and be applied to degradable protective coatings, and can effectively reduce white pollution and carbon emissions, thereby protecting the environment. BRIEF DESCRIPTION OF THE DRAWINGS

[0062] Figure 1 These are photos of carboxyl-terminated polylactic acid prepared in Example 3 and Comparative Example 2 of the present application. DETAILED DESCRIPTION

[0063] In order to make the purpose, technical scheme and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments and drawings. The specific embodiments described herein are only used to explain the present invention and are not intended to constitute any limitation to the present invention. In addition, in the following description, the description of known structures and technologies is omitted to avoid unnecessary confusion of the concepts of the present disclosure. Such structures and technologies are also described in many publications.

[0064] The general reaction formula for preparing carboxyl-terminated polylactic acid in the embodiment of the present invention is:

[0065]

[0066] or,

[0067]

[0068] Where R 1 , R 2 , a, b and c are as defined above in this article.

[0069] The method for detecting the molecular weight of the carboxyl-terminated polylactic acid in the embodiment of the present invention is: weigh 5-10 mg of the carboxyl-terminated polylactic acid, add 0.5-0.6 mL of deuterated chloroform to dissolve it, and measure and calculate the molecular weight by hydrogen nuclear magnetic resonance spectrum.

[0070] The acid value of the carboxyl-terminated polylactic acid in the embodiment of the present invention is detected according to the determination of acid value in polyester polyols HGT2708-1995; specifically, 0.05-3.00 g of carboxyl-terminated polylactic acid is weighed in a conical flask, 20-30 ml of a toluene-ethanol mixture (the volume ratio of toluene to ethanol is 2:1) is added, the conical flask is shaken to completely dissolve the sample, 10 drops of phenolphthalein indicator solution are added, and potassium hydroxide ethanol standard titration solution is used to titrate until the solution is slightly red and does not fade for 30 seconds, and the acid value is calculated.

[0071] The hydroxyl value of the carboxyl-terminated polylactic acid in the embodiment of the present invention is detected according to the determination of hydroxyl value in polyester polyols in HG / T 2709-1995; specifically, 0.05-8.00 g of carboxyl-terminated polylactic acid is weighed into a conical flask, 25 mL of acetic anhydride pyridine solution is added, refluxed in an oil bath at 115° C. for 1 hour, 10 mL of water is added and refluxed for 10 minutes, 15 mL of n-butanol is taken to rinse the condenser and the wall of the conical flask, 10 drops of phenolphthalein indicator are added, and potassium hydroxide ethanol standard solution is used to titrate until the solution is slightly red and does not fade for 30 seconds, and the hydroxyl value is calculated.

[0072] Example 1

[0073] Preliminarily heat and evacuate the 2L reaction bottle to remove the air and moisture in the bottle, and then fill it with nitrogen for standby use. Keep the nitrogen in the bottle slightly positive pressure and add 80.50g of trimethylolpropane and 519.50g of L-lactide, turn on heating and stirring to melt the trimethylolpropane and L-lactide and mix them evenly, and use vacuum equipment to evacuate and replace with nitrogen three times, weigh 0.06g of zinc oxide and add it to the reaction bottle in a nitrogen environment, and maintain the reaction temperature at 140℃ for 8h to obtain a reaction solution containing terminal hydroxyl polylactic acid (the theoretical value of the synthesized terminal hydroxyl polylactic acid calculated based on the feed amount is About 600g, sampling will be taken 2-3 times to determine the end point during the reaction, and the sampling amount is 10g-20g each time, so that the content of terminal hydroxyl polylactic acid in the reaction liquid is about 540g), and then 399.01g of decenyl succinic anhydride is weighed and added to the above reaction bottle under nitrogen environment, stirred evenly and the reaction temperature is maintained at 140℃ for 8h to obtain terminal carboxyl polylactic acid, which is a light yellow solid after cooling, with a number average molecular weight of 1712 and an acid value of 98.25mgKOH / g. Hydroxyl value: not detected (indicating that the terminal hydroxyl polylactic acid and the decenyl succinic anhydride have been completely reacted to convert into terminal carboxyl polylactic acid).

[0074] Example 2

[0075] Preliminarily heat and evacuate the 2L reaction bottle to remove the air and moisture in the bottle, and then fill it with nitrogen for standby use. Keep the nitrogen in the bottle slightly positive pressure and add 17.73g of 1,6-hexanediol and 582.27g of L-lactide, turn on heating and stirring to melt 1,6-hexanediol and L-lactide and mix them evenly, and use vacuum equipment to evacuate and replace with nitrogen three times, weigh 0.12g of zinc chloride and add it to the reaction bottle in a nitrogen environment, and maintain the reaction temperature at 145℃ for 7h to obtain a reaction solution containing terminal hydroxyl polylactic acid (calculated according to the amount of feed). The theoretical value is about 600g. During the reaction, samples will be taken 2-3 times to determine the end point. The sampling amount is 10g-20g each time, so that the content of terminal hydroxyl polylactic acid in the reaction liquid is about 540g). Then 31.07g of glutaric anhydride is weighed and added to the above reaction bottle under nitrogen environment. Stir evenly and maintain the reaction temperature at 145℃ for 7h to obtain carboxyl-terminated polylactic acid. After cooling, it is a white solid with a number average molecular weight of 4234 and an acid value of 26.82mgKOH / g. Hydroxyl value: not detected (indicating that the terminal hydroxyl polylactic acid and glutaric anhydride have been completely reacted to convert into carboxyl-terminated polylactic acid).

[0076] Example 3

[0077] Preliminarily heat and evacuate the 2L reaction bottle to remove the air and moisture in the bottle, and then fill it with nitrogen for standby use. Keep the nitrogen in the bottle slightly positive pressure and add 9.13g of 1,3-propylene glycol and 590.87g of L-lactide. Turn on heating and stirring to melt and mix 1,3-propylene glycol and L-lactide evenly. At the same time, use vacuum equipment to evacuate and replace with nitrogen three times. Weigh 0.12g of stannous chloride and add it to the reaction bottle in a nitrogen environment. Maintain the reaction temperature at 150℃ and react for 7h to obtain a reaction solution containing terminal hydroxyl polylactic acid (calculated according to the amount of feed). The theoretical value is about 600g. During the reaction, samples will be taken 2-3 times to determine the end point. The sampling amount is 10g-20g each time, so that the content of terminal hydroxyl polylactic acid in the reaction liquid is about 540g). Then 21.65g of maleic anhydride is weighed and added to the above reaction bottle under nitrogen environment. Stir evenly and maintain the reaction temperature at 150℃ for 7h to obtain terminal carboxyl polylactic acid. After cooling, it is a white solid with a number average molecular weight of 5024 and an acid value of 22.64mgKOH / g. Hydroxyl value: not detected (indicating that the terminal hydroxyl polylactic acid and maleic anhydride have completely reacted to convert into terminal carboxyl polylactic acid).

[0078] Example 4

[0079] Preliminarily heat and evacuate the 2L reaction bottle to remove the air and moisture in the bottle, and then fill it with nitrogen for standby use. Keep the nitrogen in the bottle slightly positive pressure and add 9.01g of 1,4-butanediol and 590.99g of D-lactide, turn on heating and stirring to melt 1,4-butanediol and D-lactide and mix them evenly, and use vacuum equipment to evacuate and replace with nitrogen three times, weigh 0.30g of stannous chloride and add it to the reaction bottle in a nitrogen environment, and maintain the reaction temperature at 150℃ for 6h to obtain a reaction solution containing terminal hydroxyl polylactic acid (the theoretical amount of the synthesized terminal hydroxyl polylactic acid is calculated based on the feed amount). The theoretical value is about 600g. During the reaction, samples will be taken 2-3 times to determine the end point. The sampling amount is 10g-20g each time. In this way, the content of terminal hydroxyl polylactic acid in the reaction liquid is about 540g). Then 21.09g of methylsuccinic anhydride is weighed and added to the above reaction bottle under nitrogen environment. Stir evenly and maintain the reaction temperature at 150℃ for 6h to obtain terminal carboxyl polylactic acid. After cooling, it is a light yellow solid with a number average molecular weight of 5934 and an acid value of 19.34mgKOH / g. Hydroxyl value: not detected (indicating that the terminal hydroxyl polylactic acid and methylsuccinic anhydride have been completely reacted to convert into terminal carboxyl polylactic acid).

[0080] Example 5

[0081] Preliminarily heat and evacuate the 2L reaction bottle to remove the air and moisture in the bottle, and then fill it with nitrogen for standby use. Keep the nitrogen in the bottle slightly positive pressure and add 9.10g of diethylene glycol and 590.90g of D-lactide, turn on heating and stirring to melt and mix diethylene glycol and D-lactide evenly, and use vacuum equipment to evacuate and replace with nitrogen three times at the same time, weigh 0.30g of stannous octoate and add it to the reaction bottle in a nitrogen environment, and maintain the reaction temperature at 150℃ for 6h to obtain a reaction solution containing terminal hydroxyl polylactic acid (the theoretical value of the synthesized terminal hydroxyl polylactic acid calculated based on the feed amount is about The reaction mixture is 600g, and samples are taken 2-3 times to determine the end point during the reaction. The sampling amount is 10g-20g each time, so that the content of terminal hydroxyl polylactic acid in the reaction liquid is about 540g). Then 15.52g of succinic anhydride is weighed and added to the above reaction bottle under nitrogen environment. Stir evenly and maintain the reaction temperature at 150℃ for 6h to obtain terminal carboxyl polylactic acid. After cooling, it is a white solid with a number average molecular weight of 6786 and an acid value of 16.56mgKOH / g. Hydroxyl value: not detected (indicating that the terminal hydroxyl polylactic acid and succinic anhydride have completely reacted to convert into terminal carboxyl polylactic acid).

[0082] Example 6

[0083] The 2L reaction bottle was preliminarily heated and evacuated to remove the air and moisture in the bottle, and then filled with nitrogen for standby use. Keeping the nitrogen in the bottle slightly positive pressure, 6.25g of neopentyl glycol and 593.75g of L-lactide were added, and the heating and stirring were turned on to melt the neopentyl glycol and L-lactide and mix them evenly. At the same time, a vacuum device was used to evacuate and replace the nitrogen three times. 0.42g of stannous octoate was weighed and added to the reaction bottle under nitrogen environment, and the reaction temperature was maintained at 160°C for 5h to obtain a reaction solution containing terminal hydroxyl polylactic acid (the theoretical value of the synthesized terminal hydroxyl polylactic acid calculated based on the feed amount is about The reaction mixture is 600g, and samples are taken 2-3 times to determine the end point during the reaction. The sampling amount is 10g-20g each time, so that the content of terminal hydroxyl polylactic acid in the reaction liquid is about 540g). Then 16.36g of phthalic anhydride is weighed and added to the above reaction bottle under nitrogen environment. Stir evenly and maintain the reaction temperature at 160℃ for 5h to obtain terminal carboxyl polylactic acid. After cooling, it is a light yellow solid with a number average molecular weight of 9760 and an acid value of 11.75mgKOH / g. Hydroxyl value: not detected (indicating that the terminal hydroxyl polylactic acid and phthalic anhydride have completely reacted to convert into terminal carboxyl polylactic acid).

[0084] Example 7

[0085] Preliminarily heat and evacuate the 2L reaction bottle to remove the air and moisture in the bottle, and then fill it with nitrogen for standby use. Keep the nitrogen in the bottle slightly positive pressure and add 3.04g of 1,2-propylene glycol and 596.96g of mixed lactide (L-lactide: 477.57g, Meso-lactide: 119.39g), turn on heating and stirring to melt and mix 1,2-propylene glycol and mixed lactide evenly, and use vacuum equipment to evacuate and replace with nitrogen three times, weigh 0.42g of dibutyltin dilaurate and add it to the reaction bottle in a nitrogen environment, and maintain the reaction temperature at 170℃ for 5h to obtain a reaction solution containing terminal hydroxyl polylactic acid (according to the input The theoretical value of the synthesized hydroxy-terminated polylactic acid is about 600g. During the reaction, samples will be taken 2-3 times to determine the end point, and the sampling amount is 10g-20g each time, so that the content of hydroxy-terminated polylactic acid in the reaction solution is about 540g). Then 13.89g of 1,2,4-trimethic anhydride is weighed and added to the above reaction bottle under nitrogen environment, stirred evenly and the reaction temperature is maintained at 170℃ for 5h to obtain carboxyl-terminated polylactic acid, which is a light yellow solid after cooling, with a number average molecular weight of 14428 and an acid value of 16.12mgKOH / g. Hydroxyl value: not detected (indicating that the hydroxy-terminated polylactic acid and 1,2,4-trimethic anhydride have been completely reacted to convert into carboxyl-terminated polylactic acid).

[0086] Example 8

[0087] Preliminarily heat and evacuate the 2L reaction bottle to remove the air and moisture in the bottle, and then fill it with nitrogen for standby use. Keep the nitrogen in the bottle slightly positive pressure and add 1.86g of ethylene glycol and 598.13g of mixed lactide (D-lactide: 418.70g, Meso-lactide: 179.43g), turn on heating and stirring to melt the ethylene glycol and mixed lactide and mix them evenly, and use vacuum equipment to evacuate and replace with nitrogen three times at the same time, weigh 0.60g of stannous octoate and add it to the reaction bottle in a nitrogen environment, and maintain the reaction temperature at 170℃ for 5h to obtain a reaction solution containing terminal hydroxyl polylactic acid (the theoretical value of the synthesized terminal hydroxyl polylactic acid calculated based on the feed amount is about The reaction mixture is 600g, and samples are taken 2-3 times to determine the end point during the reaction. The sampling amount is 10g-20g each time, so that the content of terminal hydroxyl polylactic acid in the reaction solution is about 540g). Then weigh 10.20g of mixed anhydride (1,2,4-trimethylbenzene anhydride: 5.34g, phthalic anhydride: 4.12g) and add it to the above reaction bottle under nitrogen environment. Stir evenly and maintain the reaction temperature at 170℃ for 5h to obtain terminal carboxyl polylactic acid. After cooling, it is a light yellow solid with a number average molecular weight of 19122 and an acid value of 8.56mgKOH / g. Hydroxyl value: not detected (indicating that the terminal hydroxyl polylactic acid and the mixed anhydride (1,2,4-trimethylbenzene anhydride and phthalic anhydride) have been completely reacted to convert into terminal carboxyl polylactic acid).

[0088] Comparative Example 1

[0089] Preliminarily heat and evacuate the 2L reaction bottle to remove the air and moisture in the bottle, and then fill it with nitrogen for standby use. Keep the nitrogen in the bottle slightly positive pressure and add 80.50g of trimethylolpropane and 519.50g of L-lactide, turn on heating and stirring to melt the trimethylolpropane and L-lactide and mix them evenly, and use vacuum equipment to evacuate and replace with nitrogen three times, weigh 0.06g of zinc oxide and add it to the reaction bottle in a nitrogen environment, and maintain the reaction temperature at 140℃ for 8h to obtain a reaction solution containing terminal hydroxyl polylactic acid (the theoretical value of the synthesized terminal hydroxyl polylactic acid calculated based on the feed amount is about 600g During the reaction, samples will be taken 2-3 times to determine the endpoint, and the sampling amount is 10g-20g each time, so that the content of terminal hydroxyl polylactic acid in the reaction liquid is about 540g). Then 170.66g of acetic anhydride is weighed and added to the above reaction bottle under nitrogen environment. Stir evenly and maintain the reaction temperature at 140℃ for 8h. Use vacuum equipment to evacuate and replace with nitrogen three times to obtain end-capped polylactic acid, which is a light yellow solid after cooling. The number average molecular weight is 1124 and the acid value is 0.12mgKOH / g.

[0090] In Comparative Example 1, a linear acid anhydride and terminal hydroxyl polylactic acid are reacted, and the prepared polylactic acid terminal has no carboxyl functional group and cannot react with epoxy resin, and the obtained polylactic acid is a blocked terminal polylactic acid.

[0091] Comparative Example 2

[0092] To a 2L reaction bottle, 600g of L-lactic acid was added, and dehydration prepolymerization was carried out at 100°C, 110°C, 120°C, 130°C, and 140°C for 2h (a total of 8h) under a vacuum degree of 4-5kpa, and nitrogen was charged to maintain a slight positive pressure of nitrogen in the reaction bottle. 0.60g of stannous chloride was added, and the condensation reaction was carried out at 150°C, 160°C, 170°C, and 180°C for 3h (a total of 12h) under a vacuum degree of <500pa, and nitrogen was charged to maintain a slight positive pressure of nitrogen in the reaction bottle. Maleic anhydride: 69.88g was added and reacted at 170°C for 5h under a nitrogen environment to obtain terminal carboxyl polylactic acid, which was a brown-yellow solid after cooling, with a number average molecular weight of 5324 and an acid value of 21.67mgKOH / g.

[0093] Comparative Example 3

[0094] To a 2L reaction flask, add 600g of D-lactic acid, and under a vacuum degree of 4-5kpa, dehydrate and prepolymerize at 100°C, 110°C, 120°C, 130°C, and 140°C for 2h (a total of 8h), respectively. Nitrogen was charged into the reaction flask to maintain a slight positive pressure of nitrogen. 0.60g of stannous chloride was added, and under a vacuum degree of <500pa, condensation reaction was carried out at 150°C, 160°C, 170°C, and 180°C for 3h (a total of 12h), nitrogen was charged into the reaction flask to maintain a slight positive pressure of nitrogen. 122.35g of phthalic anhydride was added, and the reaction was carried out at 170°C for 5h under a nitrogen environment to obtain carboxyl-terminated polylactic acid, which was a brown-yellow solid after cooling. The number average molecular weight was 2462, and the acid value was 46.05mgKOH / g.

[0095] Figure 1 The following are photos of carboxyl-terminated polylactic acid prepared in Example 3 and Comparative Example 2, wherein the left photo is the carboxyl-terminated polylactic acid prepared in Example 3, and the right photo is the carboxyl-terminated polylactic acid prepared in Comparative Example 2. Figure 1 It can be seen that the carboxyl-terminated polylactic acid prepared by the method of the present invention is lighter in color (white or light yellow) than the carboxyl-terminated polylactic acid prepared by the traditional method.

[0096] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A carboxyl-terminated polylactic acid, the structure of which is shown in the following formula I or formula II: In Formula I, R 1 is selected from substituted or unsubstituted C 2 ~ 8 Alkylene, substituted or unsubstituted C 2 ~ 3 Alkylene-OC 2 ~ 3 Alkylene, when R 1 When containing a substituent, the substituent is selected from C 1 ~ 3 alkyl; In Formula II, R 1 Selected from Where R 1a , R 1b , R 1c are each independently selected from substituted or unsubstituted C 1 ~ 6 Alkylene, R 1d Selected from hydrogen or C 1 ~ 6 Alkyl, R 1a , R 1b and R 1c When the substituent is contained, the substituent is independently selected from C 1 ~ 3 alkyl; In Formula I and Formula II, R 2 are each independently selected from substituted or unsubstituted phenylene, substituted or unsubstituted C 2 ~ 4 Alkenylene, substituted or unsubstituted C 2 ~ 4 Alkylene, when R 2 When containing substituents, the substituents are each independently selected from C 1 ~ 6 Alkyl, carboxyl, C 2 ~ 10 Preferably, the substituents are each independently selected from C 1 ~ 3 Alkyl, carboxyl, C 6 ~ 10 The alkenyl group; a, b, and c are each independently selected from any integer between 4 and 138.

2. The carboxyl-terminated polylactic acid according to claim 1, It is characterized in that In Formula I, R 1 Selected from 1,2-ethylene, 1,3-propylene, 1,4-butylene, 1,5-pentylene, 1,6-hexylene, -CH 2 -CH(CH 3 )-、-CH 2 CH 2 -O-CH 2 CH 2 -、-CH 2 -CH 2 -CH(CH 3 )-CH 2 -CH 2 -or-CH 2 -C(CH 3 ) 2 -CH 2 -; In Formula II, R 1 Selected from In Formula I and Formula II, the R 2 Each independently selected from the following groups which are unsubstituted or substituted by one or more substituents selected from carboxyl, methyl, propenyl, hexenyl, octenyl and decenyl: phenylene, vinylene, ethylene, propylene; Preferably, R 2 Each is independently selected from phenylene, carboxyl-substituted phenylene, -CH=CH-, 1,2-ethylene, 1,3-propylene, methyl-substituted 1,2-ethylene, and decenyl-substituted 1,2-ethylene.

3. The carboxyl-terminated polylactic acid according to claim 1 or 2, It is characterized in that In formula I, the sum of a and b is selected from any integer of 12-278; and / or, in formula II, the sum of a, b, c is selected from any integer of 12-278; and / or, the number average molecular weight of the carboxyl-terminated polylactic acid is 1000-20000, preferably 1500-19500; and / or, the acid value of the carboxyl-terminated polylactic acid is 5.6-168.3 mgKOH / g, preferably 8.0-100.0 mgKOH / g.

4. A method for preparing carboxyl-terminated polylactic acid as claimed in any one of claims 1 to 3, The following steps are involved: In the presence of a first catalyst, a cyclic acid anhydride and a hydroxy-terminated polylactic acid are mixed and reacted to generate the carboxyl-terminated polylactic acid; wherein the hydroxy-terminated polylactic acid has a structure shown in the following formula I-1 or formula II-1: Among them, in formula (I-1), R 1 The definitions of a, b are the same as those in Formula I; in Formula (II-1), R 1 , a, b and c are as defined in Formula II.

5. The preparation method according to claim 4, It is characterized in that The structure of the cyclic anhydride is as follows: Among them, R 2 The meaning is the same as that in any one of claims 1 to 2; Preferably, the cyclic acid anhydride is selected from one or more of phthalic anhydride, trimellitic anhydride, maleic anhydride, glutaric anhydride, succinic anhydride, methylsuccinic anhydride, and decenylsuccinic anhydride.

6. The preparation method according to claim 4 or 5, It is characterized in that The hydroxy-terminated polylactic acid is prepared by a method comprising the following steps: Polymerizing the polyol and lactide under the action of a second catalyst to generate the hydroxy-terminated polylactic acid; Preferably, the polyol is selected from one or more of ethylene glycol, diethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, glycerol, 1,4-butylene glycol, neopentyl glycol, 1,5-pentanediol, 1,6-hexanediol, trimethylolpropane, and 3-methyl-1,5-pentanediol; Preferably, the lactide is selected from one or more of L-lactide, D-lactide, and Meso-lactide; Preferably, the mass ratio of the polyol to lactide is 1:(5-350), preferably 1:(5-300); Preferably, the polymerization temperature is 130-180°C, preferably 140-170°C; Preferably, the polymerization reaction is carried out in an inert atmosphere such as nitrogen; Preferably, the polymerization reaction is a melt polymerization reaction.

7. The preparation method according to claim 4 or 6, It is characterized in that The first catalyst and the second catalyst are the same or different and are independently selected from zinc catalysts and / or tin catalysts; and / or, the added mass of the first catalyst is 0.005%-0.1% of the total mass of the hydroxy-terminated polylactic acid and the cyclic anhydride, preferably 0.01%-0.1%; and / or, the added mass of the second catalyst is 0.005%-0.1% of the total mass of the lactide and the polyol, preferably 0.01%-0.1%; Preferably, the first catalyst and the second catalyst are the same; Preferably, the zinc catalyst is selected from zinc oxide and zinc chloride; Preferably, the tin catalyst is selected from one or more of stannous chloride, stannous octoate and dibutyltin dilaurate.

8. The preparation method according to any one of claims 4 to 7, It is characterized in that The molar ratio of the cyclic anhydride to the hydroxyl group of the hydroxy-terminated polylactic acid is (1.0-1.2):1; and / or the cyclic anhydride and the hydroxy-terminated polylactic acid are reacted in an inert atmosphere such as nitrogen; and / or the temperature of the mixed reaction of the cyclic anhydride and the hydroxy-terminated polylactic acid is 130-180°C, preferably 140-170°C; and / or the time of the mixed reaction of the cyclic anhydride and the hydroxy-terminated polylactic acid is 3-15h, preferably 5-8h.

9. The preparation method according to any one of claims 4 to 8, It is characterized in that The preparation method comprises the following steps: (1) polymerizing lactide and a polyol in the presence of a second catalyst to obtain a reaction solution containing the hydroxy-terminated polylactic acid; (2) mixing the cyclic acid anhydride with the reaction solution containing the hydroxyl-terminated polylactic acid obtained in step (1) to generate the carboxyl-terminated polylactic acid.

10. Use of the carboxyl-terminated polylactic acid according to any one of claims 1 to 3 or the carboxyl-terminated polylactic acid prepared by the preparation method according to any one of claims 4 to 9 in degradable protective coatings; Preferably, the degradable protective coating is a metal shell degradable protective coating or a plastic shell degradable protective coating.

Citation Information

Patent Citations

  • Crosslinking polylactic acid and preparation method thereof

    CN102120817A

  • Degradable light-cured resin and preparation method and application thereof

    CN111499856A

  • Preparation method and application of macromonomer stabilizer

    CN113185683A

  • Thermosensitive block copolymer hydrogel as well as preparation method and application thereof

    CN114634632A

  • Biodegradable branched polylactide derivatives capable of forming polymeric micelles, and their preparation method and use

    US20070003625A1