Intermediate film for laminated glass, and laminated glass
By using an intermediate film with obvious thickness differences in laminated glass and adjusting the distribution of thermal insulation compounds in its thickness direction, the problem of uneven visibility and thermal insulation of laminated glass in the prior art is solved, and more uniformity is achieved visibility and thermal insulation.
Patent Information
- Application Number
- CN202411080881.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2015-09-30
- Filing Date
- 2016-09-29
- Publication Date
- 2024-11-22
AI Technical Summary
The thickness of one end of the wedge-shaped intermediate film in existing laminated glass is different from the other end, resulting in uneven visibility of laminated glass using the intermediate film. Especially when the HUD display area is large, the driver may observe a difference in visibility. And it is difficult to effectively shield infrared rays to improve thermal insulation.
An intermediate film containing thermoplastic resin and thermally insulating compounds is used. The absolute difference between the thickness of the thickest part and the thinnest part is more than 0.1mm, and the content of thermally insulating compounds in different areas is set in the thickest part to ensure the intermediate film. The visible light transmittance difference is less than 4%. By adjusting the thermal insulation compound distribution and layer structure in the thickness direction, the wedge-shaped cross-sectional shape of the intermediate film is optimized to improve visibility uniformity and thermal insulation.
The overall visibility and thermal insulation uniformity of laminated glass are achieved, the clarity of the HUD display area and infrared shielding effect are ensured, and the overall performance of laminated glass is improved.
Smart Images

Figure CN118994824A_ABST
Abstract
Description
[0001] This application is a divisional application based on a patent application with an application date of September 29, 2016, a priority date of September 30, 2015, an application number of 201680056469.4, and an invention name of “Intermediate film for laminated glass and laminated glass”. Technical Field
[0002] The present invention relates to an interlayer film for laminated glass for obtaining laminated glass. In addition, the present invention relates to laminated glass using the interlayer film for laminated glass. Background Art
[0003] Generally, even if laminated glass is damaged by external impact, the amount of scattered glass fragments is small, and the safety is excellent. Therefore, the laminated glass is widely used in automobiles, rail vehicles, aircraft, ships, buildings, etc. The laminated glass is manufactured by sandwiching an interlayer film for laminated glass between two glass plates.
[0004] In addition, as the laminated glass used for automobiles, a head-up display (HUD) is known. The HUD can display measurement information such as the speed of the automobile as driving data on the windshield of the automobile.
[0005] The HUD has a problem in which the measurement information displayed on the windshield appears double.
[0006] In order to suppress the ghost image, a wedge-shaped interlayer film is used. The following Patent Document 1 discloses a laminated glass in which a wedge-shaped interlayer film having a specific wedge angle is sandwiched between a pair of glass plates. In this laminated glass, by adjusting the wedge angle of the interlayer film, the measurement information reflected and displayed by one glass plate and the measurement information reflected and displayed by the other glass plate can be combined into one point in the driver's field of vision. Therefore, the displayed measurement information is not easily seen as a ghost image, and the driver's field of vision is not obstructed.
[0007] Furthermore, laminated glass used in openings of vehicles and buildings is required to have high heat-shielding properties.
[0008] Infrared rays with wavelengths longer than visible light, 780nm or longer, have less energy than ultraviolet rays. However, infrared rays have a greater thermal effect, and when they are absorbed by a substance, they are released as heat. Therefore, infrared rays are often called heat rays. Therefore, in order to improve the heat insulation of laminated glass, infrared rays must be fully shielded.
[0009] In order to effectively shield the infrared rays (heat rays), Patent Document 2 below discloses an interlayer film for laminated glass containing heat shielding particles such as tin-doped indium oxide particles (ITO particles) or antimony-doped tin oxide particles (ATO particles).
[0010] Patent Document 3 listed below discloses an intermediate film including tungsten oxide particles (CWO particles).
[0011] Patent Document 4 below discloses a heat shielding material having two or more layers containing at least one of a phthalocyanine infrared absorber and an ultraviolet absorber. The heat shielding material is arranged such that the layer containing the ultraviolet absorber is located closer to the heat incident side than the other layers. The phthalocyanine infrared absorber is a phthalocyanine heat-insulating compound.
[0012] Prior art literature
[0013] Patent Literature
[0014] Patent Document 1: Japanese Patent Publication No. 4-502525
[0015] Patent Document 2: WO2001 / 025162A1
[0016] Patent Document 3: WO2005 / 087680A1
[0017] Patent Document 4: Japanese Patent Application Laid-Open No. 10-77360 Summary of the invention
[0018] Technical problem solved by the invention
[0019] In the wedge-shaped intermediate film, the thickness at one end is different from that at the other end.
[0020] According to the research results of the inventors, it was found that when heat-insulating particles such as ITO particles, ATO particles, and CWO particles, as well as heat-insulating compounds of the phthalocyanine type, are added to an intermediate film with different thicknesses at one end and the other end, there is a problem of different visibility depending on the part of the laminated glass using the intermediate film. If the display area of the HUD is of normal size, the driver will hardly notice the difference in visibility of the part of the laminated glass. However, the larger the display area of the HUD, the more likely the driver will observe the difference in visibility in the part of the laminated glass. In addition, there is a possibility that the display area of the HUD will be larger in the future.
[0021] An object of the present invention is to provide an interlayer film for laminated glass which can make the visibility of the entire laminated glass uniform. Another object of the present invention is to provide a laminated glass using the interlayer film for laminated glass.
[0022] Technical means of solving problems
[0023] According to a broad aspect of the present invention, there is provided an interlayer film for laminated glass (sometimes referred to simply as "interlayer film" in this specification), which comprises a thermoplastic resin and a heat-insulating compound, the interlayer film for laminated glass having one end and another end located on the opposite side of the one end, the thickness of the other end being greater than the thickness of the one end, the absolute value of the difference between the thickness of the thickest portion and the thickness of the thinnest portion of the interlayer film for laminated glass being greater than 0.1 mm, and in a laminated glass obtained by sandwiching the interlayer film between two heat-absorbing flat glass plates having a thickness of 2.1 mm, the absolute value of the difference between the visible light transmittance of the interlayer film at the thickest portion and the visible light transmittance of the interlayer film at the thinnest portion is less than 4%.
[0024] In a specific aspect of the intermediate film of the present invention, in a laminated glass obtained by sandwiching the intermediate film between two heat-absorbing flat glass plates with a thickness of 2.1 mm, the absolute value of the difference between the visible light transmittance of the intermediate film at the thickest part and the visible light transmittance of the intermediate film at the thinnest part is less than 5.5%.
[0025] In a specific aspect of the intermediate film of the present invention, a first region and a second region exist in the thickness direction of the thickest portion of the intermediate film, and the content of the heat-shielding compound in the second region is smaller than that in the first region.
[0026] In a specific aspect of the interlayer film of the present invention, an absolute value of a difference between a content of the heat shielding compound in the first region of the interlayer film and a content of the heat shielding compound in the second region of the interlayer film is 0.0001 wt % or more.
[0027] In a specific aspect of the interlayer film of the present invention, the second region of the interlayer film does not contain the heat-shielding compound, or the second region of the interlayer film contains 0.5 wt % or less of the heat-shielding compound.
[0028] In a specific aspect of the interlayer film of the present invention, when the absolute value of the difference between the thickness of the thickest portion and the thickness of the thinnest portion is X mm, X mm exceeds 0.28, and the thickness of the second region at the thickest portion is not less than (X-0.28) and not more than X.
[0029] In a specific aspect of the interlayer film of the present invention, the heat shielding compound includes at least one component selected from the group consisting of a phthalocyanine compound, a naphthalocyanine compound, and an anthracyanine compound, or the heat shielding compound includes heat shielding particles.
[0030] In a specific aspect of the interlayer film of the present invention, the heat shielding compound includes the heat shielding particles.
[0031] In a specific aspect of the interlayer film of the present invention, the heat shielding compound includes tin-doped indium oxide particles or tungsten oxide particles as the heat shielding particles.
[0032] In a specific aspect of the interlayer film of the present invention, the heat-shielding compound includes at least one component selected from the group consisting of a phthalocyanine compound, a naphthalocyanine compound, and an anthracyanine compound.
[0033] In a specific aspect of the intermediate film of the present invention, the thermoplastic resin is a polyvinyl acetal resin.
[0034] In a specific aspect of the intermediate film of the present invention, the intermediate film contains a plasticizer.
[0035] In a specific aspect of the intermediate film of the present invention, the intermediate film has a portion having a wedge-shaped cross-sectional shape in the thickness direction.
[0036] According to a broad aspect of the present invention, there is provided a laminated glass including a first laminated glass component, a second laminated glass component, and the interlayer film for laminated glass, wherein the interlayer film for laminated glass is disposed between the first laminated glass component and the second laminated glass component.
[0037] According to a broad aspect of the present invention, there is provided a laminated glass comprising a first laminated glass component, a second laminated glass component and an interlayer film for laminated glass, the interlayer film for laminated glass being arranged between the first laminated glass component and the second laminated glass component, the interlayer film comprising a thermoplastic resin and a heat-insulating compound, the interlayer film having one end and another end located on the opposite side of the one end and having a thickness greater than the one end, the absolute value of the difference between the thickness of the thickest part and the thickness of the thinnest part of the interlayer film being 0.1 mm or more, and the absolute value of the difference between the visible light transmittance of the interlayer film in the laminated glass at the thickest part and the visible light transmittance of the interlayer film in the laminated glass at the thinnest part being 4% or less.
[0038] Effects of the Invention
[0039] The interlayer film for laminated glass of the present invention comprises a thermoplastic resin and a heat-insulating compound, has one end and another end located on the opposite side of the one end and having a thickness greater than the one end, the absolute value of the difference between the thickness of the thickest portion and the thickness of the thinnest portion is greater than 0.1 mm, and in a laminated glass obtained by sandwiching the interlayer film between two heat-absorbing flat glass plates with a thickness of 2.1 mm, the absolute value of the difference between the visible light transmittance of the interlayer film at the thickest portion and the visible light transmittance of the interlayer film at the thinnest portion is less than 4%, thereby making the visibility of the entire laminated glass uniform.
[0040] The laminated glass of the present invention comprises a first laminated glass component, a second laminated glass component and an interlayer film for laminated glass, wherein the interlayer film for laminated glass is arranged between the first laminated glass component and the second laminated glass component, wherein the interlayer film comprises a thermoplastic resin and a heat-insulating compound, wherein the interlayer film has one end and another end located on the opposite side of the one end and having a thickness greater than that of the one end, wherein the absolute value of the difference between the thickness of the thickest part and the thickness of the thinnest part of the interlayer film is greater than 0.1 mm, and the absolute value of the difference between the visible light transmittance of the interlayer film in the laminated glass at the thickest part and the visible light transmittance of the interlayer film in the laminated glass at the thinnest part is less than 4%, thereby making the visibility of the entire laminated glass uniform. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] [ Figure 1 ] Figure 1 It is a cross-sectional view schematically showing the interlayer film for laminated glass according to the first embodiment of the present invention.
[0042] [ Figure 2 ] Figure 2 It is a cross-sectional view schematically showing an interlayer film for laminated glass according to a second embodiment of the present invention.
[0043] [ Figure 3 ] Figure 3 A cross-sectional view showing a first variation of the cross-sectional shape of the interlayer film for laminated glass in the thickness direction.
[0044] [ Figure 4 ] Figure 4 A cross-sectional view showing a second variation of the cross-sectional shape of the interlayer film for laminated glass in the thickness direction.
[0045] [ Figure 5 ] Figure 5 A cross-sectional view showing a third variation of the cross-sectional shape of the interlayer film for laminated glass in the thickness direction.
[0046] [ Figure 6 ] Figure 6 A cross-sectional view showing a fourth variation of the cross-sectional shape of the interlayer film for laminated glass in the thickness direction.
[0047] [ Figure 7 ] Figure 7 A cross-sectional view showing a fifth variation of the cross-sectional shape of the interlayer film for laminated glass in the thickness direction.
[0048] [ Figure 8 ] Figure 8 It is a cross-sectional view schematically showing an interlayer film for laminated glass according to a second embodiment of the present invention.
[0049] [ Fig. 9 ] Fig. 9 Indicates the use Figure 1 1 is a cross-sectional view of an example of a laminated glass including the interlayer film for a laminated glass shown. DETAILED DESCRIPTION
[0050] Hereinafter, the present invention will be described in detail.
[0051] The interlayer film for laminated glass of the present invention (may be simply referred to as “interlayer film” in this specification) contains a thermoplastic resin and a heat shielding compound.
[0052] The interlayer film for laminated glass has one end and the other end located on the opposite side of the one end, and the thickness of the other end is greater than the thickness of the one end.
[0053] In the interlayer film for laminated glass, an absolute value of a difference between a thickness of a thickest portion and a thickness of a thinnest portion is 0.1 mm or more.
[0054] In the interlayer film of the present invention, in a laminated glass obtained by sandwiching the interlayer film between two heat absorbing flat glass plates with a thickness of 2.1 mm, the absolute value of the difference between the visible light transmittance of the interlayer film at the thickest part and the visible light transmittance of the interlayer film at the thinnest part is 4% or less. It should be noted that the laminated glass is manufactured to limit the interlayer film. When the interlayer film of the present invention is used to manufacture laminated glass, the interlayer film may be arranged between laminated glass components other than the heat absorbing glass plates.
[0055] Since the interlayer film of the present invention has the above-mentioned technical features, the overall visibility of the laminated glass obtained by using the interlayer film can be made uniform, that is, the uniformity of visibility can be improved.
[0056] The laminated glass of the present invention comprises a first laminated glass component, a second laminated glass component, and an interlayer film for laminated glass. In the laminated glass of the present invention, the interlayer film for laminated glass is arranged between the first laminated glass component and the second laminated glass component, the interlayer film comprises a thermoplastic resin and a heat-insulating compound, the interlayer film has one end and another end located on the opposite side of the one end and having a thickness greater than the one end, the absolute value of the difference between the thickness of the thickest part and the thickness of the thinnest part of the interlayer film is 0.1 mm or more, and the absolute value of the difference between the visible light transmittance of the interlayer film in the laminated glass at the thickest part and the visible light transmittance of the interlayer film in the laminated glass at the thinnest part is 4% or less.
[0057] Since the laminated glass of the present invention has the above-mentioned technical features, the visibility of the laminated glass obtained by using the interlayer film can be made uniform over the entirety, that is, the uniformity of visibility can be improved.
[0058] From the viewpoint of further improving the uniformity of visibility, in the laminated glass obtained by sandwiching an intermediate film between two heat-absorbing flat glass plates with a thickness of 2.1 mm, or in the laminated glass of the present invention, the absolute value of the difference between the visible light transmittance of the intermediate film at the thickest part and the visible light transmittance of the intermediate film at the thinnest part is preferably 3.5% or less, and more preferably 3% or less.
[0059] From the viewpoint of improving visibility, in a laminated glass obtained by sandwiching the interlayer film of the present invention between two heat-absorbing flat glass plates having a thickness of 2.1 mm, or in the laminated glass of the present invention, the lower of the visible light transmittance of the interlayer film at the thickest portion and the visible light transmittance of the interlayer film at the thinnest portion is preferably 65% or more, more preferably 70% or more, and further preferably 73% or more.
[0060] The visible light transmittance is measured in accordance with JIS R3211 (1998).
[0061] In a laminated glass obtained by sandwiching the interlayer film of the present invention between two heat-absorbing flat glass plates having a thickness of 2.1 mm, or in the laminated glass of the present invention, the absolute value of the difference between the solar transmittance Ts2500 of the interlayer film at the thickest portion and the solar transmittance Ts2500 of the interlayer film at the thinnest portion is preferably 5.5% or less, more preferably 5% or less, and further preferably 4% or less. If the absolute value of the difference in solar transmittance Ts2500 is below the upper limit, the heat insulation property can be made uniform over the entire laminated glass obtained using the interlayer film.
[0062] From the viewpoint of improving heat insulation, in the laminated glass obtained by sandwiching the intermediate film of the present invention between two heat-absorbing flat glass plates with a thickness of 2.1 mm, or in the laminated glass of the present invention, the lower solar transmittance Ts2500 of the intermediate film at the thickest part and the solar transmittance Ts2500 of the intermediate film at the thinnest part is preferably 39% or less, more preferably 38% or less, and further preferably 37% or less.
[0063] The solar transmittance is measured in accordance with JIS R 3106 (1998).
[0064] The visible light transmittance and the visible light transmittance were measured at the following positions.
[0065] When the thickest part or the thinnest part is more than 25 mm away from the end, take a square test piece of 50 mm (in the direction connecting one end and the other end) × 50 mm (in the direction perpendicular to the direction connecting one end and the other end) with the thickest part or the thinnest part becoming the center.
[0066] When the thickest part or the thinnest part is less than 25 mm from the end, a square test piece of 50 mm (in the direction connecting one end and the other end) × 50 mm (in the direction perpendicular to the direction connecting one end and the other end) is taken in such a way that the end becomes one side of the test piece.
[0067] In addition, when the thinnest part of the intermediate film is at a certain distance in the direction connecting the one end and the other end, the end on the side of one end of the thinnest part is set as the thinnest part to take the test piece. In the case where the thickest part of the intermediate film is at a certain distance in the direction connecting the one end and the other end (for example, refer to Figure 7 ), and the end portion on the other side of the thickest part is set as the thickest part to take the test piece.
[0068] From the viewpoint of further improving the uniformity of visibility or the uniformity of heat insulation, it is preferred that a first region and a second region exist in the thickness direction of the thickest portion of the intermediate film, wherein the content of the heat insulation compound in the second region is less than that in the first region.
[0069] From the viewpoint of further improving the uniformity of visibility or the uniformity of heat insulation, the absolute value of the difference between the content of the heat-insulating compound in the first region of the interlayer film and the content of the heat-insulating compound in the second region of the interlayer film is preferably 0.0001 wt % or more, more preferably 0.0005 wt % or more. The absolute value of the difference between the content of the heat-insulating compound in the first region of the interlayer film and the content of the heat-insulating compound in the second region of the interlayer film is preferably 0.5 wt % or less, more preferably 0.4 wt % or less.
[0070] From the viewpoint of further improving the uniformity of visibility or the uniformity of heat insulation, it is preferred that the second region of the interlayer film does not contain the heat-insulating compound, or the second region of the interlayer film contains 0.2 wt % or less of the heat-insulating compound. From the viewpoint of further improving the uniformity of visibility or the uniformity of heat insulation, the heat-insulating compound in the second region of the interlayer film is more preferably 0.15 wt % or less.
[0071] The absolute value of the difference between the thickness of the thickest portion and the thickness of the thinnest portion is set to X mm. From the viewpoint of further improving the uniformity of visibility or further improving the uniformity of heat insulation, the thickness Y mm of the thickest portion of the second region is preferably (X-0.28) or more, more preferably (X-0.25) or more, and is preferably less than X, more preferably less than (X-0.05).
[0072] Hereinafter, specific embodiments of the present invention will be described with reference to the accompanying drawings.
[0073] Figure 1 It is a cross-sectional view schematically showing the interlayer film for laminated glass according to the first embodiment of the present invention.
[0074] exist Figure 1 , a cross section of the intermediate film 11 in the thickness direction is shown. Figure 1 In the following drawings, for the convenience of illustration, the thickness of the interlayer film and each layer constituting the interlayer film, and the wedge angle θ are shown to be different from the actual thickness and wedge angle.
[0075] Figure 1 The interlayer film 11 shown includes a first layer 1. The interlayer film 11 has a single-layer structure consisting of only the first layer 1 and is a single-layer interlayer film. The interlayer film 11 is the first layer 1. The interlayer film 11 is used to obtain a laminated glass. The interlayer film 11 is an interlayer film for laminated glass.
[0076] The cross-sectional shape of the intermediate film 11 and the first layer 1 in the thickness direction is wedge-shaped. The intermediate film 11 has one end 11a and the other end 11b located on the opposite side of the one end 11a. The one end 11a and the other end 11b are end portions on both sides facing each other. The thickness of the one end 11a of the intermediate film 11 is smaller than the thickness of the other end 11b. Therefore, the intermediate film 11 and the first layer 1 have a region with a smaller thickness and a region with a larger thickness.
[0077] The second region R2 containing no heat-shielding compound exists on the thicker other end 11b side of the intermediate film 11. The first region R1 containing the heat-shielding compound exists on both sides of the second region R2 in the thickness direction. The second region R2 of the intermediate film 11 may also contain the heat-shielding compound.
[0078] The second region R2 is preferably a region where the thickness of one end (corresponding to one end of the intermediate film) is smaller than the thickness of the other end (corresponding to the other end of the intermediate film), and the cross-sectional shape in the thickness direction is a wedge-shaped region. At this time, the direction from one end 11a toward the other end 11b of the intermediate film 11 is preferably the same as the direction from one end toward the other end of the second region R2.
[0079] When the distance from one end 11a to the other end 11b of the intermediate film 11 is defined as Z, one end is defined as 0Z, and the other end is defined as Z, the second region R2 is preferably located between 0Z and 0.5Z.
[0080] Figure 2 It is a cross-sectional view schematically showing an interlayer film for laminated glass according to a second embodiment of the present invention.
[0081] Figure 2The intermediate film 11A shown includes a first layer 1A (intermediate layer), a second layer 2A (surface layer), and a third layer 3A (surface layer). The second layer 2A is arranged in a laminated manner on the first surface side of the first layer 1A. The third layer 3A is arranged in a laminated manner on the second surface side of the first layer 1A opposite to the first surface. The first layer 1A is arranged between the second layer 2A and the third layer 3A in a sandwiched manner. The intermediate film 11A is used to obtain laminated glass. The intermediate film 11A is an intermediate film for laminated glass. The intermediate film 11A is a multilayer intermediate film. Laminated glass components are laminated on the surface layer.
[0082] The intermediate film 11A has one end 11a and the other end 11b located on the opposite side of the one end 11a. The one end 11a and the other end 11b are end portions on both sides facing each other. The cross-sectional shape of the second layer 2A and the third layer 3A in the thickness direction is a wedge shape. The cross-sectional shape of the first layer 1A in the thickness direction is a rectangle. The thickness of the second layer 2A and the third layer 3A on the one end 11a side is smaller than that on the other end 11b side. Therefore, the thickness of the one end 11a of the intermediate film 11A is smaller than the thickness of the other end 11b. Therefore, the intermediate film 11A has a region with a smaller thickness and a region with a larger thickness.
[0083] The difference between the maximum and minimum thicknesses of the first layer 1A is smaller than the difference between the maximum and minimum thicknesses of the second layer 2A. The difference between the maximum and minimum thicknesses of the first layer 1A is smaller than the difference between the maximum and minimum thicknesses of the third layer 3A.
[0084] The intermediate film 11A is not particularly limited. For example, a heat-insulating compound may be added to the first layer 1A, and no heat-insulating compound may be added to the second layer 2A and the third layer 3A. Alternatively, a heat-insulating compound may be added to the second layer 2A and the third layer 3A, and no heat-insulating compound may be added to the first layer 1A. As in the intermediate film 11A, each layer may correspond to a first region and a second region having a smaller content of the heat-insulating compound than the first region.
[0085] Figure 2 The intermediate film 11A shown has a structure in which a rectangular first layer 1A is sandwiched between a wedge-shaped second layer 2A and a third layer 3A. Figures 3 to 7 1 to 5 variations in which the shapes of the layers of the intermediate film are changed are shown.
[0086] Figure 3 The intermediate film 11B of the first variation shown includes a first layer 1B having a wedge-shaped cross section in the thickness direction, a second layer 2B having a wedge-shaped cross section in the thickness direction, and a third layer 3B having a wedge-shaped cross section in the thickness direction. The first layer 1B is disposed and sandwiched between the second layer 2B and the third layer 3B.
[0087] The thickness of the first layer 1B, the second layer 2B, and the third layer 3B on one end 11a side is smaller than that on the other end 11b side. Therefore, the intermediate film 11B has a region with a smaller thickness and a region with a larger thickness.
[0088] In the intermediate film 11B, the thickness variation of the first layer 1B is smaller than the thickness variation of the second layer 2B and the third layer 3B.
[0089] The intermediate film 11B is not particularly limited. For example, a heat shielding compound may be added to the first layer 1B, while no heat shielding compound may be added to the second layer 2B and the third layer 3B.
[0090] Figure 4 The intermediate film 11C of the second variation shown includes a first layer 1C having a rectangular cross-sectional shape in the thickness direction, a second layer 2C having a wedge-shaped cross-sectional shape in the thickness direction, and a third layer 3C having a rectangular cross-sectional shape in the thickness direction. The first layer 1C is sandwiched between the second layer 2C and the third layer 3C. The thickness of the second layer 2C on the side of one end 11a is smaller than that on the side of the other end 11b. Therefore, the intermediate film 11C has a region with a smaller thickness and a region with a larger thickness. In terms of the shape of the intermediate film 11C, the intermediate film may also be a single layer.
[0091] Figure 5 The intermediate film 11D of the third variation shown has a first layer 1D having a rectangular cross-sectional shape in the thickness direction, a second layer 2D having a wedge-shaped cross-sectional shape in the thickness direction, and a third layer 3D having a rectangular cross-sectional shape in the thickness direction. The second layer 2D is sandwiched between the first layer 1D and the third layer 3D. The thickness of the second layer 2D on one end 11a side is smaller than that on the other end 11b side. Therefore, the intermediate film 11D has a region with a smaller thickness and a region with a larger thickness.
[0092] The intermediate film 11D is not particularly limited. For example, a heat-shielding compound may be added to the second layer 2D and the third layer 3D, but not to the first layer 1D. Alternatively, a heat-shielding compound may be added to the first layer 1D, but not to the second layer 2D and the third layer 3D.
[0093] Figure 6 The intermediate film 11E of the fourth variation shown includes a first layer 1E having a rectangular cross-sectional shape in the thickness direction, and a second layer 2E having a wedge-shaped cross-sectional shape in the thickness direction. The second layer 2E is stacked on the first surface side of the first layer 1E. The thickness of the second layer 2E on the side of one end 11a is smaller than that on the side of the other end 11b. Therefore, the intermediate film 11E has a region with a smaller thickness and a region with a larger thickness.
[0094] Figure 7The intermediate film 11F of the fifth variation shown includes a first layer 1F having a rectangular cross-sectional shape in the thickness direction, and a second layer 2F having a rectangular cross-sectional shape in the thickness direction and a wedge-shaped cross-sectional shape in the thickness direction. The second layer 2F is stacked on the first surface side of the first layer 1F. The thickness of the second layer 2F on the side of one end 11a is smaller than that on the side of the other end 11b. Therefore, the intermediate film 11F has a region with a smaller thickness and a region with a larger thickness. In terms of the shape of the intermediate film 11F, the intermediate film may be a single layer.
[0095] The intermediate film preferably has a portion whose cross-sectional shape in the thickness direction is a wedge shape. The intermediate film preferably has a portion whose thickness gradually increases from one end toward the other end. The cross-sectional shape of the intermediate film in the thickness direction is preferably a wedge shape. Examples of the cross-sectional shape of the intermediate film in the thickness direction include a trapezoid, a triangle, and a pentagon.
[0096] Figure 8 It is a cross-sectional view schematically showing an interlayer film for laminated glass according to a second embodiment of the present invention.
[0097] Figure 8 The intermediate film 11G shown includes a first layer 1G having a rectangular cross-sectional shape in the thickness direction, a second layer 2G having a wedge-shaped cross-sectional shape in the thickness direction, and a third layer GD having a rectangular cross-sectional shape in the thickness direction. The second layer 2G is sandwiched between the first layer 1G and the third layer 3G. The thickness of the second layer 2G on one end 11a side is smaller than that on the other end 11b side. Therefore, the intermediate film 11G has a region with a smaller thickness and a region with a larger thickness. The intermediate film 11G has a second region R2 in the second layer 2G.
[0098] In order to suppress ghost images, the wedge angle θ of the interlayer film can be appropriately set according to the installation angle of the laminated glass. From the viewpoint of further suppressing ghost images, the wedge angle θ of the interlayer film is preferably 0.01 mrad (0.0006 degrees) or more, more preferably 0.2 mrad (0.0115 degrees) or more, and preferably 2 mrad (0.1146 degrees) or less, more preferably 0.7 mrad (0.0401 degrees) or less. The wedge angle θ of the interlayer film is the inner angle at the intersection of the following two straight lines: a straight line connecting the first surface portion of the interlayer film with the maximum thickness portion and the minimum thickness portion, and a straight line connecting the second surface portion of the interlayer film with the maximum thickness portion and the minimum thickness portion.
[0099] The intermediate film may also have a colored band in a part of the region. The intermediate film may also have a colored region in a part of the region. In the case where the multilayer intermediate film has a colored band or a colored region, it is preferred that the surface layer has a colored band or a colored region. However, the intermediate layer may also have a colored band or a colored region. The colored band or the colored region may be formed, for example, by adding a colorant to a specific region when the intermediate film is extruded or when each layer of the intermediate film is extruded.
[0100] The thickness of the intermediate film is not particularly limited. The thickness of the intermediate film refers to the total thickness of the layers constituting the intermediate film. Therefore, in the case of a multilayer intermediate film 11A, the thickness of the intermediate film 11A refers to the total thickness of the first layer 1A, the second layer 2A, and the third layer 3A.
[0101] The maximum thickness of the intermediate film is preferably 0.1 mm or more, more preferably 0.25 mm or more, further preferably 0.5 mm or more, particularly preferably 0.8 mm or more, and is preferably 3 mm or less, more preferably 2 mm, further preferably 1.5 mm or less.
[0102] When the distance between one end and the other end is defined as Z, the intermediate film preferably has a minimum thickness in a region of 0Z to 0.2Z from one end toward the inside, and has a maximum thickness in a region of 0Z to 0.2Z from the other end toward the inside, and more preferably has a minimum thickness in a region of 0X to 0.1X from one end toward the inside, and has a maximum thickness in a region of 0Z to 0.1Z from the other end toward the inside. Preferably, one end of the intermediate film has the minimum thickness, and the other end of the intermediate film has the maximum thickness.
[0103] The intermediate film 11 , 11A, 11B, 11C, 11D, 11E, 11F, 1G has the smallest thickness at one end 11 a and the largest thickness at the other end 11 b .
[0104] From a practical point of view and from the viewpoint of sufficiently improving adhesion and penetration resistance, the maximum thickness of the surface layer is preferably 0.001 mm or more, more preferably 0.2 mm or more, further preferably 0.3 mm or more, and preferably 1 mm or less, more preferably 0.8 mm or less.
[0105] From a practical point of view and from the perspective of fully improving penetration resistance, the maximum thickness of the layer (intermediate layer) disposed between the two surface layers is preferably greater than 0.001 mm, more preferably greater than 0.1 mm, further preferably greater than 0.2 mm, and preferably less than 0.8 mm, more preferably less than 0.6 mm, further preferably less than 0.3 mm.
[0106] The distance Z between one end and the other end of the intermediate film is preferably 3 m or less, more preferably 2 m or less, particularly preferably 1.5 m or less, and is preferably 0.5 m or more, more preferably 0.8 m or more, particularly preferably 1 m or more.
[0107] The intermediate film of the present invention has a one-layer structure or a structure of two or more layers. The intermediate film of the present invention may have a one-layer structure, may have a structure of two or more layers, or may have a structure of three or more layers. The intermediate film of the present invention includes a first layer. The intermediate film of the present invention may be a single-layer intermediate film including only the first layer, or may be a multilayer intermediate film including the first layer and other layers.
[0108] The intermediate film may also have a structure of more than two layers, and may also include a second layer in addition to the first layer. The intermediate film preferably includes the second layer as a surface layer in the intermediate film. In the case where the intermediate film includes the second layer, the second layer is arranged on the first surface side of the first layer. In this case, the first layer and the second layer may be directly laminated, or another layer may be arranged between the first layer and the second layer.
[0109] The intermediate film may also have a structure of more than three layers, and may include a third layer in addition to the first layer and the second layer. The intermediate film preferably includes the third layer as a surface layer in the intermediate film. In the case where the intermediate film includes the third layer, the third layer is arranged on the second surface side of the first layer opposite to the first surface. In the case where the intermediate film includes the third layer, the first layer is arranged between the second layer and the third layer. In this case, the first layer and the third layer may be directly laminated, or another layer may be arranged between the first layer and the third layer.
[0110] Hereinafter, the materials of each layer constituting the multilayer interlayer film and the single-layer interlayer film will be described in detail.
[0111] (Polyvinyl acetal resin or thermoplastic resin)
[0112] The intermediate film preferably contains a thermoplastic resin, and preferably contains a polyvinyl acetal resin as the thermoplastic resin. The first layer (comprising a single-layer intermediate film) preferably contains a thermoplastic resin (hereinafter, sometimes referred to as thermoplastic resin (1)), and preferably contains a polyvinyl acetal resin (hereinafter, sometimes referred to as polyvinyl acetal resin (1)) as the thermoplastic resin (1). The second layer preferably contains a thermoplastic resin (hereinafter, sometimes referred to as thermoplastic resin (2)), and preferably contains a polyvinyl acetal resin (hereinafter, sometimes referred to as polyvinyl acetal resin (2)) as the thermoplastic resin (2). The third layer preferably contains a thermoplastic resin (hereinafter, sometimes referred to as thermoplastic resin (3)), and preferably contains a polyvinyl acetal resin (hereinafter, sometimes referred to as polyvinyl acetal resin (3)) as the thermoplastic resin (3). The thermoplastic resin (1), the thermoplastic resin (2) and the thermoplastic resin (3) may be the same or different. The thermoplastic resin (1), the thermoplastic resin (2) and the thermoplastic resin (3) may be used alone or in combination of two or more. The polyvinyl acetal resin (1), the polyvinyl acetal resin (2) and the polyvinyl acetal resin (3) may be the same or different. The polyvinyl acetal resin (1), the polyvinyl acetal resin (2) and the polyvinyl acetal resin (3) may be used alone or in combination of two or more.
[0113] Examples of the thermoplastic resin include polyvinyl acetal resin, ethylene-vinyl acetate copolymer resin, ethylene-acrylic acid copolymer resin, polyurethane resin, and polyvinyl alcohol resin. Thermoplastic resins other than these may also be used.
[0114] The thermoplastic resin is preferably a polyvinyl acetal resin. By using the polyvinyl acetal resin and the plasticizer in combination, the adhesion of the interlayer film for laminated glass of the present invention to the laminated glass component or other interlayer films is further improved.
[0115] The polyvinyl acetal resin can be produced, for example, by acetalizing polyvinyl alcohol (PVA) with aldehyde. The polyvinyl acetal resin is preferably an acetalized product of polyvinyl alcohol. The polyvinyl alcohol can be obtained, for example, by saponifying polyvinyl acetate. The degree of saponification of the polyvinyl alcohol is generally 70 to 99.9 mol%.
[0116] The average degree of polymerization of the polyvinyl alcohol (PVA) is preferably 200 or more, more preferably 500 or more, further preferably 1500 or more, further preferably 1600 or more, particularly preferably 2600 or more, most preferably 2700 or more, and preferably 5000 or less, more preferably 4000 or less, further preferably 3500 or less. If the average degree of polymerization is above the lower limit, the penetration resistance of the laminated glass is further improved. If the average degree of polymerization is below the upper limit, the formation of the interlayer film becomes easy.
[0117] The average degree of polymerization of the polyvinyl alcohol is determined according to the method of JIS K6726 "Testing methods for polyvinyl alcohol".
[0118] The number of carbon atoms in the acetal group contained in the polyvinyl acetal resin is not particularly limited. The aldehyde used when producing the polyvinyl acetal resin is not particularly limited. The number of carbon atoms in the acetal group in the polyvinyl acetal resin is preferably 3 to 5, more preferably 3 or 4. When the number of carbon atoms in the acetal group in the polyvinyl acetal resin is 3 or more, the glass transition temperature of the interlayer film becomes sufficiently low.
[0119] The aldehyde is not particularly limited. Generally, aldehydes having 1 to 10 carbon atoms are preferably used. Examples of the aldehyde having 1 to 10 carbon atoms include propionaldehyde, n-butyraldehyde, isobutyraldehyde, n-valeraldehyde, 2-ethylbutyraldehyde, n-hexanal, n-octanal, n-nonanal, n-decanal, formaldehyde, acetaldehyde, and benzaldehyde. Preferred are propionaldehyde, n-butyraldehyde, isobutyraldehyde, n-hexanal, or n-valeraldehyde, more preferably propionaldehyde, n-butyraldehyde, or isobutyraldehyde, and even more preferably n-butyraldehyde. The aldehyde may be used alone or in combination of two or more.
[0120] The hydroxyl content (hydroxyl amount) of the polyvinyl acetal resin (1) is preferably 17 mol% or more, more preferably 20 mol% or more, further preferably 22 mol% or more, and preferably 35 mol% or less, more preferably 30 mol% or less, further preferably less than 27 mol%, and particularly preferably less than 25 mol%. If the hydroxyl content is greater than or equal to the lower limit, the adhesive force of the interlayer film is further improved. In particular, if the hydroxyl content of the polyvinyl acetal resin (1) is greater than or equal to 20 mol%, the reaction efficiency is improved and the productivity is excellent. In addition, if it is less than 27 mol%, the sound insulation of the laminated glass is further improved. In addition, if the hydroxyl content is less than or equal to the upper limit, the flexibility of the interlayer film is improved, and the handling of the interlayer film becomes easy.
[0121] The hydroxyl content of the polyvinyl acetal resin (2) and the polyvinyl acetal resin (3) is preferably 25 mol% or more, more preferably 28 mol% or more, and preferably 35 mol% or less, more preferably 32 mol% or less. If the hydroxyl content is above the lower limit, the adhesive force of the interlayer film is further improved. If the hydroxyl content is below the upper limit, the flexibility of the interlayer film is improved, and the handling of the interlayer film becomes easy.
[0122] From the viewpoint of further improving the sound insulation, the hydroxyl content of the polyvinyl acetal resin (1) is preferably lower than the hydroxyl content of the polyvinyl acetal resin (2). From the viewpoint of further improving the sound insulation, the hydroxyl content of the polyvinyl acetal resin (1) is preferably lower than the hydroxyl content of the polyvinyl acetal resin (3). From the viewpoint of further improving the sound insulation, the absolute value of the difference between the hydroxyl content of the polyvinyl acetal resin (1) and the hydroxyl content of the polyvinyl acetal resin (2), and the absolute value of the difference between the hydroxyl content of the polyvinyl acetal resin (1) and the hydroxyl content of the polyvinyl acetal resin (3) are preferably 1 mol% or more, more preferably 5 mol% or more, further preferably 9 mol% or more, particularly preferably 10 mol% or more, and most preferably 12 mol% or more. The absolute value of the difference between the hydroxyl content of the polyvinyl acetal resin (1) and the hydroxyl content of the polyvinyl acetal resin (2), and the absolute value of the difference between the hydroxyl content of the polyvinyl acetal resin (1) and the hydroxyl content of the polyvinyl acetal resin (3) are preferably 20 mol% or less.
[0123] The hydroxyl content of the polyvinyl acetal resin is a value expressed as a percentage, which is a molar fraction obtained by dividing the amount of ethylene groups bonded with hydroxyl groups by the amount of all ethylene groups in the main chain. The amount of ethylene groups bonded with hydroxyl groups can be measured, for example, in accordance with JIS K6728 "Testing methods for polyvinyl butyral".
[0124] The degree of acetylation (acetyl group content) of the polyvinyl acetal resin (1) is preferably 0.01 mol% or more, more preferably 0.1 mol% or more, further more preferably 7 mol% or more, further preferably 9 mol% or more, and preferably 30 mol% or less, more preferably 25 mol% or less, further preferably 15 mol% or less. If the degree of acetylation is above the lower limit, the compatibility of the polyvinyl acetal resin with the plasticizer is improved. If the degree of acetylation is below the upper limit, the moisture resistance of the interlayer film and the laminated glass is improved. In particular, if the degree of acetylation of the polyvinyl acetal resin (1) is 0.1 mol% or more and 25 mol% or less, the penetration resistance is excellent.
[0125] The acetylation degree of each of the polyvinyl acetal resin (2) and the polyvinyl acetal resin (3) is preferably 0.01 mol% or more, more preferably 0.5 mol% or more, and preferably 10 mol% or less, more preferably 2 mol% or less. If the acetylation degree is above the lower limit, the compatibility of the polyvinyl acetal resin with the plasticizer is improved. If the acetylation degree is below the upper limit, the moisture resistance of the interlayer film and the laminated glass is improved.
[0126] The acetylation degree is a value expressed as a percentage, which is a molar fraction obtained by dividing the amount of ethylene groups bonded with acetyl groups by the total amount of ethylene groups in the main chain. The amount of ethylene groups bonded with acetyl groups can be measured, for example, in accordance with JIS K6728 "Testing methods for polyvinyl butyral".
[0127] The degree of acetalization of the polyvinyl acetal resin (1) (the degree of butyralization in the case of a polyvinyl butyral resin) is preferably 47 mol% or more, more preferably 60 mol% or more, and preferably 80 mol% or less, more preferably 70 mol% or less. If the degree of acetalization is above the lower limit, the compatibility of the polyvinyl acetal resin with the plasticizer is improved. If the degree of acetalization is below the upper limit, the reaction time required for producing the polyvinyl acetal resin is shortened.
[0128] The acetalization degree of each of the polyvinyl acetal resin (2) and the polyvinyl acetal resin (3) (the butyralization degree in the case of the polyvinyl butyral resin) is preferably 55 mol% or more, more preferably 67 mol% or more, and preferably 75 mol% or less, more preferably 71 mol% or less. If the acetalization degree is above the lower limit, the compatibility of the polyvinyl acetal resin with the plasticizer is improved. If the acetalization degree is below the upper limit, the reaction time required for producing the polyvinyl acetal resin is shortened.
[0129] The degree of acetalization is a value expressed as a percentage, which is the molar fraction obtained by subtracting the amount of ethylene groups bonded with hydroxyl groups and the amount of ethylene groups bonded with acetyl groups from the total amount of ethylene groups in the main chain and dividing the result by the total amount of ethylene groups in the main chain.
[0130] It should be noted that the hydroxyl content (hydroxyl amount), acetalization degree (butyralization degree) and acetylation degree are preferably calculated based on the results of measurement according to JIS K6728 "Testing methods for polyvinyl butyral". However, it can also be measured according to ASTM D1396-92. When the polyvinyl acetal resin is a polyvinyl butyral resin, the hydroxyl content (hydroxyl amount), acetalization degree (butyralization degree) and acetylation degree can be calculated based on the results of measurement according to JIS K6728 "Testing methods for polyvinyl butyral".
[0131] From the viewpoint of further improving the penetration resistance of laminated glass, the polyvinyl acetal resin (1) is preferably a polyvinyl acetal resin (A) having an acetylation degree (a) of 8 mol% or less and 66 mol% or more, or a polyvinyl acetal resin (B) having an acetylation degree (b) exceeding 8 mol%. The polyvinyl acetal resin (1) may be the polyvinyl acetal resin (A) or the polyvinyl acetal resin (B).
[0132] The degree of acetylation (a) of the polyvinyl acetal resin (A) is 8 mol% or less, preferably 7.5 mol% or less, more preferably 7 mol% or less, further preferably 6.5 mol% or less, particularly preferably 5 mol% or less, preferably 0.1 mol% or more, more preferably 0.5 mol% or more, further preferably 0.8 mol% or more, particularly preferably 1 mol% or more. When the degree of acetylation (a) is below the upper limit and above the lower limit, the migration of the plasticizer can be easily controlled, and the sound insulation of the laminated glass can be further improved.
[0133] The degree of acetalization (a) of the polyvinyl acetal resin (A) is 66 mol% or more, preferably 67.5 mol% or more, more preferably 70.5 mol% or more, particularly preferably 71 mol% or more, further preferably 71.5 mol% or more, particularly preferably 72 mol% or more, and preferably 85 mol% or less, more preferably 83 mol% or less, further preferably 81 mol% or less, particularly preferably 79 mol% or less. If the degree of acetalization (a) is above the lower limit, the sound insulation of the laminated glass is further improved. If the degree of acetalization (a) is below the upper limit, the reaction time required for producing the polyvinyl acetal resin (A) can be shortened.
[0134] The hydroxyl content (a) of the polyvinyl acetal resin (A) is preferably 18 mol% or more, more preferably 19 mol% or more, further preferably 20 mol% or more, particularly preferably 21 mol% or more, and preferably 31 mol% or less, more preferably 30 mol% or less, further preferably 29 mol% or less, particularly preferably 28 mol% or less. If the hydroxyl content (a) is above the lower limit, the adhesive force of the first layer is further improved. If the hydroxyl content (a) is below the upper limit, the sound insulation of the laminated glass is further improved.
[0135] The degree of acetylation (b) of the polyvinyl acetal resin (B) exceeds 8 mol%, preferably 9 mol% or more, more preferably 9.5 mol% or more, further preferably 10 mol% or more, particularly preferably 10.5 mol% or more, and preferably 30 mol% or less, more preferably 28 mol% or less, further preferably 26 mol% or less, particularly preferably 24 mol% or less. If the degree of acetylation (b) is above the lower limit, the sound insulation of the laminated glass is further improved. If the degree of acetylation (b) is below the upper limit, the reaction time required for producing the polyvinyl acetal resin (B) can be shortened.
[0136] The degree of acetalization (b) of the polyvinyl acetal resin (B) is preferably 50 mol% or more, more preferably 53 mol% or more, further preferably 55 mol% or more, particularly preferably 60 mol% or more, and preferably 80 mol% or less, more preferably 78 mol% or less, further preferably 76 mol% or less, and particularly preferably 74 mol% or less. If the degree of acetalization (b) is above the lower limit, the sound insulation of the laminated glass is further improved. If the degree of acetalization (b) is below the upper limit, the reaction time required for producing the polyvinyl acetal resin (B) can be shortened.
[0137] The hydroxyl content (b) of the polyvinyl acetal resin (B) is preferably 18 mol% or more, more preferably 19 mol% or more, further preferably 20 mol% or more, particularly preferably 21 mol% or more, and preferably 31 mol% or less, more preferably 30 mol% or less, further preferably 29 mol% or less, particularly preferably 28 mol% or less. If the hydroxyl content (b) is above the lower limit, the adhesive force of the first layer is further improved. If the hydroxyl content (b) is below the upper limit, the sound insulation of the laminated glass is further improved.
[0138] The polyvinyl acetal resin (A) and the polyvinyl acetal resin (B) are each preferably a polyvinyl butyral resin.
[0139] (Plasticizer)
[0140] The intermediate film preferably contains a plasticizer. The first layer (comprising a single-layer intermediate film) preferably contains a plasticizer (hereinafter, sometimes referred to as plasticizer (1)). The second layer preferably contains a plasticizer (hereinafter, sometimes referred to as plasticizer (2)). The third layer preferably contains a plasticizer (hereinafter, sometimes referred to as plasticizer (3)). By using a polyvinyl acetal resin and a plasticizer in combination, the adhesion of the layer containing the polyvinyl acetal resin and the plasticizer to the laminated glass component or other layers can be appropriately improved. The plasticizer is not particularly limited. The plasticizer (1), the plasticizer (2), and the plasticizer (3) may be the same or different. Only one type of the plasticizer may be used, or two or more types may be used in combination.
[0141] Examples of the plasticizer include organic ester plasticizers such as monobasic organic acid esters and polybasic organic acid esters, and organic phosphoric acid plasticizers such as organic phosphoric acid plasticizers and organic phosphorous acid plasticizers. Organic ester plasticizers are preferred. The plasticizer is preferably a liquid plasticizer.
[0142] Examples of the monobasic organic acid ester include glycol esters obtained by reacting glycols with monobasic organic acids. Examples of the glycol include triethylene glycol, tetraethylene glycol, and tripropylene glycol. Examples of the monobasic organic acid include butyric acid, isobutyric acid, hexanoic acid, 2-ethylbutyric acid, heptanoic acid, n-octanoic acid, 2-ethylhexanoic acid, n-nonanoic acid, and decanoic acid.
[0143] Examples of the polybasic organic acid ester include ester compounds of polybasic organic acids and alcohols having a linear or branched structure having 4 to 8 carbon atoms. Examples of the polybasic organic acid include adipic acid, sebacic acid, and azelaic acid.
[0144] Examples of the organic ester plasticizer include triethylene glycol di-2-ethyl propionate, triethylene glycol di-2-ethyl butyrate, triethylene glycol di-2-ethyl hexanoate, triethylene glycol dioctanoate, triethylene glycol di-n-octanoate, triethylene glycol di-n-heptanoate, tetraethylene glycol di-n-heptanoate, dibutyl sebacate, dioctyl azelate, dibutyl carbitol adipate, ethylene glycol di-2-ethyl butyrate, 1,3-propylene glycol di-2-ethyl butyrate, 1,4-butylene glycol di-2-ethyl butyrate, diethylene glycol di-2-ethyl butyrate, and the like. Di-2-ethylbutyrate, diethylene glycol di-2-ethylhexanoate, dipropylene glycol di-2-ethylbutyrate, triethylene glycol di-2-ethylvalerate, tetraethylene glycol di-2-ethylbutyrate, diethylene glycol dicaprylate, dihexyl adipate, dioctyl adipate, hexyl cyclohexyl adipate, a mixture of heptyl adipate and nonyl adipate, diisononyl adipate, diisodecyl adipate, heptyl nonyl adipate, dibutyl sebacate, oil-modified sebacic acid alcohol acid, and a mixture of phosphoric acid ester and adipic acid ester, etc. Organic ester plasticizers other than these can also be used. Other adipic acid esters other than the adipic acid esters can also be used.
[0145] Examples of the organic phosphoric acid plasticizer include tris(butoxyethyl) phosphate, isodecyl phenyl phosphate, and triisopropyl phosphate.
[0146] The plasticizer is preferably a diester plasticizer represented by the following formula (1).
[0147] [Chemical formula 1]
[0148]
[0149] In the formula (1), R1 and R2 each represent an organic group having 2 to 10 carbon atoms, R3 represents an ethylene group, an isopropylene group or an n-propylene group, and p represents an integer from 3 to 10. R1 and R2 in the formula (1) each preferably represent an organic group having 5 to 10 carbon atoms, and more preferably represent an organic group having 6 to 10 carbon atoms.
[0150] The plasticizer is preferably triethylene glycol di-2-ethylhexanoate (3GO), triethylene glycol di-2-ethylbutyrate (3GH) or triethylene glycol di-2-ethylpropionate, more preferably triethylene glycol di-2-ethylhexanoate or triethylene glycol di-2-ethylbutyrate, and further preferably triethylene glycol di-2-ethylhexanoate.
[0151] The content of the plasticizer (1) relative to 100 parts by weight of the thermoplastic resin (1) (when the thermoplastic resin (1) is the polyvinyl acetal resin (1), 100 parts by weight of the polyvinyl acetal resin (1)) (hereinafter, sometimes referred to as content (1)) is preferably 35 parts by weight or more, more preferably 50 parts by weight or more, further preferably 55 parts by weight or more, particularly preferably 60 parts by weight or more, and is preferably 100 parts by weight or less, more preferably 90 parts by weight or less, further preferably 85 parts by weight or less, particularly preferably 80 parts by weight or less. When the content (1) is at least the lower limit, the flexibility of the interlayer film is improved, and the handling of the interlayer film becomes easy. When the content (1) is at most the upper limit, the penetration resistance of the laminated glass is further improved.
[0152] The content of the plasticizer (2) relative to 100 parts by weight of the thermoplastic resin (2) (when the thermoplastic resin (2) is a polyvinyl acetal resin (2), 100 parts by weight of the polyvinyl acetal resin (2)) (hereinafter, sometimes referred to as content (2)), and the content of the plasticizer (3) relative to 100 parts by weight of the thermoplastic resin (3) (when the thermoplastic resin (3) is a polyvinyl acetal resin (3), 100 parts by weight of the polyvinyl acetal resin (3)) (hereinafter, sometimes referred to as content (3)) are preferably 10 parts by weight or more, more preferably 15 parts by weight or more, and preferably 45 parts by weight or less, more preferably 40 parts by weight or less, further preferably 35 parts by weight or less, and particularly preferably 32 parts by weight or less. When the content (2) and the content (3) are at least the lower limit, the flexibility of the interlayer film is improved, and the handling of the interlayer film is facilitated. When the content (2) and the content (3) are at most the upper limit, the flexural rigidity is further improved.
[0153] In order to improve the sound insulation of the laminated glass, the content (1) is preferably greater than the content (2), and the content (1) is preferably greater than the content (3).
[0154] From the viewpoint of further improving the sound insulation of laminated glass, the absolute value of the difference between the content (2) and the content (1), and the absolute value of the difference between the content (3) and the content (1) are each preferably 10 parts by weight or more, more preferably 15 parts by weight or more, and even more preferably 20 parts by weight or more. The absolute value of the difference between the content (2) and the content (1), and the absolute value of the difference between the content (3) and the content (1) are each preferably 80 parts by weight or less, more preferably 75 parts by weight or less, and even more preferably 70 parts by weight or less.
[0155] (Thermal insulation compound)
[0156] The intermediate film contains a heat-insulating compound. The first layer preferably contains a heat-insulating compound. The second layer preferably contains a heat-insulating compound. The third layer preferably contains a heat-insulating compound. The heat-insulating compound may be used alone or in combination of two or more.
[0157] The heat shielding compound preferably includes at least one component X selected from the group consisting of phthalocyanine compounds, naphthalocyanine compounds, and anthraphthalocyanine compounds, or the heat shielding compound includes heat shielding particles. In this case, both the component X and the heat shielding particles may be included.
[0158] The content of the thermal insulating compound in 100% by weight of the entire region containing the thermal insulating compound (excluding the region not containing the thermal insulating compound) is preferably 0.0001% by weight or more, more preferably 0.05% by weight or more, further preferably 0.1% by weight or more, and preferably 0.5% by weight or less, more preferably 0.4% by weight or less, and further preferably 0.35% by weight or less. If the content of the thermal insulating compound is above the lower limit and below the upper limit, the thermal insulating property is sufficiently improved, and the visible light transmittance is sufficiently improved. For example, the visible light transmittance can be 70% or more.
[0159] Ingredient X:
[0160] The intermediate film preferably contains at least one component X selected from phthalocyanine compounds, naphthalocyanine compounds, and anthraphthalocyanine compounds. The first layer preferably contains the component X. The second layer preferably contains the component X. The third layer preferably contains the component X. The first region preferably contains the component X. The second region may also contain the component X. The component X is a heat-insulating compound. The component X may be used alone or in combination of two or more.
[0161] The component X is not particularly limited. As the component X, conventionally known phthalocyanine compounds, naphthalocyanine compounds, and anthraphthalocyanine compounds can be used.
[0162] As the component X, phthalocyanine, phthalocyanine derivatives, naphthalocyanine, naphthalocyanine derivatives, anthraphthalocyanine and anthraphthalocyanine derivatives can be listed. The phthalocyanine compound and the phthalocyanine derivative preferably have a phthalocyanine skeleton. The naphthalocyanine compound and the naphthalocyanine derivative preferably have a naphthalocyanine skeleton. The anthraphthalocyanine compound and the anthraphthalocyanine derivative preferably have an anthraphthalocyanine skeleton.
[0163] From the viewpoint of further improving the heat shielding properties of the interlayer film and laminated glass, the component X is preferably at least one selected from phthalocyanine, phthalocyanine derivatives, naphthalocyanine and naphthalocyanine derivatives, and more preferably at least one selected from phthalocyanine and phthalocyanine derivatives.
[0164] From the viewpoint of effectively improving the heat insulation and maintaining the visible light transmittance at a higher level for a long time, it is preferred that the component X contains a vanadium atom or a copper atom. It is preferred that the component X contains a vanadium atom, and it is also preferred that it contains a copper atom. It is more preferred that the component X contains at least one of phthalocyanine containing a vanadium atom or a copper atom and a derivative of phthalocyanine containing a vanadium atom or a copper atom. From the viewpoint of further improving the heat insulation of the interlayer film and the laminated glass, it is preferred that the component X has a structural unit in which an oxygen atom is bonded to a vanadium atom.
[0165] The content of the component X in the entire region containing the component X (excluding the region not containing the component X) is preferably 0.001% by weight or more, more preferably 0.005% by weight or more, further preferably 0.01% by weight or more, particularly preferably 0.02% by weight or more, and preferably 0.2% by weight or less, more preferably 0.1% by weight or less, further preferably 0.05% by weight or less, and particularly preferably 0.04% by weight or less. If the content of the component X is above the lower limit and below the upper limit, the heat insulation is sufficiently improved and the visible light transmittance is sufficiently improved. For example, the visible light transmittance can be 70% or more.
[0166] Thermal insulation particles:
[0167] The intermediate film preferably contains thermal insulation particles. The first layer preferably contains thermal insulation particles. The second layer preferably contains thermal insulation particles. The third layer preferably contains thermal insulation particles. The first region preferably contains thermal insulation particles. The second region may also contain the thermal insulation particles. The thermal insulation particles are thermal insulation compounds. By using thermal insulation particles, infrared rays (heat rays) can be effectively shielded. Only one type of the thermal insulation particles may be used, or two or more types may be used in combination.
[0168] From the viewpoint of further improving the heat shielding property of laminated glass, the heat shielding particles are more preferably metal oxide particles. The heat shielding particles are preferably particles formed of metal oxides (metal oxide particles).
[0169] Infrared rays with wavelengths longer than visible light, above 780nm, have less energy than ultraviolet rays. However, infrared rays have a greater thermal effect, and when they are absorbed by a substance, they are released in the form of heat. Therefore, infrared rays are generally referred to as heat rays. By using the heat-insulating particles, infrared rays (heat rays) can be effectively blocked. It should be noted that heat-insulating particles refer to particles that can absorb infrared rays.
[0170] As specific examples of the heat-insulating particles, aluminum-doped tin oxide particles, indium-doped tin oxide particles, antimony-doped tin oxide particles (ATO particles), gallium-doped zinc oxide particles (GZO particles), indium-doped zinc oxide particles (IZO particles), aluminum-doped zinc oxide particles (AZO particles), niobium-doped titanium oxide particles, sodium-doped tungsten oxide particles, cesium-doped tungsten oxide particles, thallium-doped tungsten oxide particles, rubidium-doped tungsten oxide particles, tin-doped indium oxide particles (ITO particles), tin-doped zinc oxide particles, silicon-doped zinc oxide particles and other metal oxide particles, or lanthanum hexaboride (LaB6) particles, etc. can be listed. Heat-insulating particles other than these can also be used. In terms of the higher shielding function of the heat line, metal oxide particles are preferred, and ATO particles, GZO particles, IZO particles, ITO particles or tungsten oxide particles are more preferred, and ITO particles or tungsten oxide particles are particularly preferred. In particular, in terms of the higher shielding function of the heat line and easy to obtain, tin-doped indium oxide particles (ITO particles) are preferred, and tungsten oxide particles are also preferred.
[0171] The tungsten oxide particles are generally represented by the following formula (X1) or the following formula (X2). In the intermediate film, the tungsten oxide particles represented by the following formula (X1) or the following formula (X2) are preferably used.
[0172] Wy Oz···Formula (X1)
[0173] In the above formula (X1), W represents tungsten, O represents oxygen, and y and z satisfy 2.0<z / y<3.0.
[0174] Mx Wy Oz···Formula (X2)
[0175] In the formula (X2), M represents at least one element selected from H, He, alkali metals, alkaline earth metals, rare earth elements, Mg, Zr, Cr, Mn, Fe, Ru, Co, Rh, Ir, Ni, Pd, Pt, Cu, Ag, Au, Zn, Cd, Al, Ga, In, Tl, Si, Ge, Sn, Pb, Sb, B, F, P, S, Se, Br, Te, Ti, Nb, V, Mo, Ta and Re, W represents tungsten, O represents oxygen, and x, y and z satisfy 0.001≤x / y≤1, and 2.0<z / y≤3.0.
[0176] From the viewpoint of further improving the heat insulation of the interlayer film and the laminated glass, the tungsten oxide particles are preferably metal-doped tungsten oxide particles. The "tungsten oxide particles" include metal-doped tungsten oxide particles. As the metal-doped tungsten oxide particles, specifically, sodium-doped tungsten oxide particles, cesium-doped tungsten oxide particles, thallium-doped tungsten oxide particles, and rubidium-doped tungsten oxide particles can be cited.
[0177] In terms of further improving the heat shielding properties of the interlayer film and the laminated glass, cesium-doped tungsten oxide particles are particularly preferred. In terms of further improving the heat shielding properties of the interlayer film and the laminated glass, the cesium-doped tungsten oxide particles are preferably of the formula: Cs 0.33 Tungsten oxide particles represented by WO3.
[0178] The average particle size of the heat shielding particles is preferably 0.01 μm or more, more preferably 0.02 μm or more, and preferably 0.1 μm or less, more preferably 0.05 μm or less. If the average particle size is above the lower limit, the heat shielding property is sufficiently improved. If the average particle size is below the upper limit, the dispersibility of the heat shielding particles is improved.
[0179] The “average particle size” refers to a volume average particle size. The average particle size can be measured using a particle size distribution measuring device (“UPA-EX150” manufactured by Nikkiso Co., Ltd.) or the like.
[0180] In 100 wt% of the entire region containing the heat-insulating particles (excluding the region not containing the heat-insulating particles), the content of each heat-insulating particle is preferably 0.01 wt% or more, more preferably 0.1 wt% or more, further preferably 1 wt% or more, particularly preferably 1.5 wt% or more, and preferably 6 wt% or less, more preferably 5.5 wt% or less, further preferably 4 wt% or less, particularly preferably 3.5 wt% or less, and most preferably 3.0 wt% or less. If the content of the heat-insulating particles is above the lower limit and below the upper limit, the heat-insulating property is sufficiently improved, and the visible light transmittance is sufficiently improved.
[0181] The layer (first layer, second layer or third layer) containing the heat shielding particles preferably has a density of 0.1 g / m 2 Above and 12g / m 2 The heat shielding particles are contained in the following ratios. When the ratio of the heat shielding particles is within the above range, the heat shielding property is sufficiently improved and the visible light transmittance is sufficiently improved. The ratio of the heat shielding particles is preferably 0.5 g / m 2 More preferably 0.8 g / m 2 More preferably 1.5 g / m 2 Above, especially preferably 3g / m 2 Above, and preferably 11g / m 2Below, more preferably 10g / m 2 Below, more preferably 9g / m 2 Below, especially preferably 7g / m 2 If the ratio is greater than or equal to the lower limit, the heat insulation property is further improved. If the ratio is less than or equal to the upper limit, the visible light transmittance is further improved.
[0182] (Metal Salt)
[0183] The intermediate film preferably contains at least one metal salt selected from alkali metal salts, alkaline earth metal salts and magnesium salts (hereinafter, sometimes referred to as metal salt M). The first layer preferably contains the metal salt M. The second layer preferably contains the metal salt M. The third layer preferably contains the metal salt M. By using the metal salt M, it is easy to control the adhesion between the intermediate film and laminated glass components such as glass plates or the adhesion between the layers of the intermediate film. The metal salt M may be used alone or in combination of two or more.
[0184] The metal salt M preferably includes at least one metal selected from the group consisting of Li, Na, K, Rb, Cs, Mg, Ca, Sr, and Ba. The metal salt included in the intermediate film preferably includes at least one metal selected from the group consisting of K and Mg.
[0185] In addition, the metal salt M is more preferably an alkali metal salt of an organic acid having 2 to 16 carbon atoms, an alkaline earth metal salt of an organic acid having 2 to 16 carbon atoms, or a magnesium salt of an organic acid having 2 to 16 carbon atoms, and is further preferably a magnesium salt of a carboxylate having 2 to 16 carbon atoms or a potassium salt of a carboxylate having 2 to 16 carbon atoms.
[0186] The magnesium salt of the carboxylate having 2 to 16 carbon atoms and the potassium salt of the carboxylate having 2 to 16 carbon atoms are not particularly limited, and examples thereof include magnesium acetate, potassium acetate, magnesium propionate, potassium propionate, magnesium 2-ethylbutyrate, potassium 2-ethylbutyrate, magnesium 2-ethylhexanoate, and potassium 2-ethylhexanoate.
[0187] The total content of Mg and K in the layer (first layer, second layer or third layer) containing the metal salt M is preferably 5 ppm or more, more preferably 10 ppm or more, further preferably 20 ppm or more, and preferably 300 ppm or less, more preferably 250 ppm or less, further preferably 200 ppm or less. When the total content of Mg and K is above the lower limit and below the upper limit, the adhesion between the interlayer film and the laminated glass component or the adhesion between the layers in the interlayer film can be more well controlled.
[0188] (UV shielding agent)
[0189] The intermediate film preferably contains an ultraviolet shielding agent. The first layer preferably contains an ultraviolet shielding agent. The second layer preferably contains an ultraviolet shielding agent. The third layer preferably contains an ultraviolet shielding agent. By using an ultraviolet shielding agent, the visible light transmittance is less likely to decrease even if the intermediate film and the laminated glass are used for a long time. The ultraviolet shielding agent can be used alone or in combination of two or more.
[0190] The ultraviolet shielding agent includes an ultraviolet absorber. The ultraviolet shielding agent is preferably an ultraviolet absorber.
[0191] Examples of the ultraviolet shielding agent include ultraviolet shielding agents containing metal atoms, ultraviolet shielding agents containing metal oxides, ultraviolet shielding agents having a benzotriazole structure (benzotriazole compounds), ultraviolet shielding agents having a benzophenone structure (benzophenone compounds), ultraviolet shielding agents having a triazine structure (triazine compounds), ultraviolet shielding agents having a malonic ester structure (malonic ester compounds), ultraviolet shielding agents having an oxalylanilide structure (oxalylanilide compounds), and ultraviolet shielding agents having a benzoate structure (benzoate compounds).
[0192] Examples of the ultraviolet shielding agent containing a metal atom include platinum particles, particles in which the surface of platinum particles is coated with silicon dioxide, palladium particles, and particles in which the surface of palladium particles is coated with silicon dioxide, etc. The ultraviolet shielding agent is preferably not a heat shielding particle.
[0193] The ultraviolet shielding agent is preferably an ultraviolet shielding agent with a benzotriazole structure, an ultraviolet shielding agent with a benzophenone structure, an ultraviolet shielding agent with a triazine structure, or an ultraviolet shielding agent with a benzoate structure, more preferably an ultraviolet shielding agent with a benzotriazole structure or an ultraviolet shielding agent with a benzophenone structure, and further preferably an ultraviolet shielding agent with a benzotriazole structure.
[0194] Examples of the ultraviolet shielding agent comprising a metal oxide include zinc oxide, titanium oxide, cerium oxide, and the like. Furthermore, the surface of the ultraviolet shielding agent comprising a metal oxide may also be coated. Examples of the coating material on the surface of the ultraviolet shielding agent comprising a metal oxide include insulating metal oxides, hydrolyzable organic silicon compounds, and polysilicone compounds.
[0195] As the ultraviolet shielding agent having a benzotriazole structure, there can be cited: 2-(2'-hydroxy-5'-methylphenyl)benzotriazole ("Tinuvin P" manufactured by BASF), 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)benzotriazole ("Tinuvin320" manufactured by BASF), 2-(2'-hydroxy-3'-tert-butyl-5-methylphenyl)-5-chlorobenzotriazole ("Tinuvin326" manufactured by BASF), and 2-(2'-hydroxy-3',5'-dipentylphenyl)benzotriazole ("Tinuvin328" manufactured by BASF), etc. In terms of excellent performance in absorbing ultraviolet rays, the ultraviolet shielding agent preferably has a benzotriazole structure containing a halogen atom, and more preferably has a benzotriazole structure containing a chlorine atom.
[0196] Examples of the ultraviolet shielding agent having a benzophenone structure include octabenzone ("Chimassorb 81" manufactured by BASF Corporation).
[0197] Examples of the ultraviolet shielding agent having a triazine structure include "LA-F70" manufactured by ADEKA Corporation and 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-[(hexyl)oxy]-phenol ("Tinuvin 1577FF" manufactured by BASF Corporation).
[0198] Examples of the ultraviolet shielding agent having a malonate structure include dimethyl 2-(p-methoxybenzylidene)malonate, tetraethyl 2,2-(1,4-phenylenedimethylene)bismalonate, and 2-(p-methoxybenzylidene)-bis(1,2,2,6,6-pentamethyl-4-piperidinyl)malonate.
[0199] Examples of commercially available products of the ultraviolet shielding agent having a malonic acid ester structure include Hostavin B-CAP, Hostavin PR-25, and Hostavin PR-31 (all manufactured by Clariant).
[0200] Examples of the ultraviolet shielding agent having an oxalic acid anilide structure include oxalic acid anilides having an aromatic group substituted on a nitrogen atom, such as N-(2-ethylphenyl)-N\'-(2-ethoxy-5-tert-butylphenyl) oxalic acid diamide, N-(2-ethylphenyl)-N'-(2-ethoxy-phenyl) oxalic acid diamide, and 2-ethyl-2'-ethoxy-oxalic acid anilide ("Sanduvor VSU" manufactured by Clariant).
[0201] Examples of the ultraviolet shielding agent having a benzoate structure include 2,4-di(tert-butylphenyl)-3,5-di-tert-butyl-4-hydroxybenzoate ("Tinuvin 120" manufactured by BASF Corporation).
[0202] With regard to the viewpoint of further suppressing the reduction of the visible light transmittance after time, in the layer (first layer, second layer or third layer) 100% by weight of the ultraviolet shielding agent, the content of the ultraviolet shielding agent is preferably 0.1% by weight or more, more preferably 0.2% by weight or more, further preferably 0.3% by weight or more, especially preferably 0.5% by weight or more, and preferably 2.5% by weight or less, more preferably 2% by weight or less, further preferably 1% by weight or less, especially preferably 0.8% by weight or less. In particular, by making the content of the ultraviolet shielding agent in the layer 100% by weight containing the ultraviolet shielding agent be 0.2% by weight or more, the reduction of the visible light transmittance after time of the intermediate film and the laminated glass can be significantly suppressed.
[0203] (Antioxidant)
[0204] The intermediate film preferably contains an antioxidant. The first layer preferably contains an antioxidant. The second layer preferably contains an antioxidant. The third layer preferably contains an antioxidant. The antioxidant may be used alone or in combination of two or more.
[0205] As the antioxidant, there can be cited phenolic antioxidants, sulfur antioxidants, phosphorus antioxidants, etc. The phenolic antioxidant is an antioxidant having a phenol skeleton. The sulfur antioxidant is an antioxidant containing a sulfur atom. The phosphorus antioxidant is an antioxidant containing a phosphorus atom.
[0206] The antioxidant is preferably a phenolic antioxidant or a phosphorus antioxidant.
[0207] Examples of the phenolic antioxidant include 2,6-di-tert-butyl-p-cresol (BHT), butylated hydroxyanisole (BHA), 2,6-di-tert-butyl-4-ethylphenol, stearyl β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, 2,2'-methylenebis-(4-methyl-6-butylphenol), 2,2'-methylenebis-(4-ethyl-6-tert-butylphenol), 4,4'-butylene-bis-(3-methyl-6-tert-butylphenol), 1,1,3-tri-(2 1,3,3-tris-(2-methyl-4-hydroxy-5-tert-butylphenol)butane, 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, bis(3,3'-tert-butylphenol)butyrate and bis(3-tert-butyl-4-hydroxy-5-methylphenylpropionate)ethylenebis(oxyethylene)ester, etc. One or more of these antioxidants are preferably used.
[0208] As the phosphorus antioxidant, tridecyl phosphite, tri(tridecyl) phosphite, triphenyl phosphite, tri(nonylphenyl) phosphite, ditridecyl pentaerythritol diphosphite, didecyl pentaerythritol diphosphite, tris(2,4-di-tert-butylphenyl) phosphite, bis(2,4-di-tert-butyl-6-methylphenyl) ethyl phosphite, tris(2,4-di-tert-butylphenyl) phosphite, and 2,2'-methylenebis(4,6-di-tert-butyl-1-phenoxy)(2-ethylhexyloxy)phosphite, etc. One or more of these antioxidants are preferably used.
[0209] Examples of commercially available antioxidants include "IRGANOX 245" manufactured by BASF, "IRGAFOS 168" manufactured by BASF, "IRGAFOS 38" manufactured by BASF, "Sumilizer BHT" manufactured by Sumitomo Chemical Industries, Ltd., and "IRGANOX 1010" manufactured by BASF.
[0210] In order to maintain a high visible light transmittance of the interlayer film and the laminated glass for a long time, the content of the antioxidant in 100 wt % of the interlayer film or in 100 wt % of the layer (first layer, second layer or third layer) containing the antioxidant is preferably 0.1 wt % or more. In addition, since the effect of adding the antioxidant will be saturated, the content of the antioxidant in 100 wt % of the interlayer film or in 100 wt % of the layer containing the antioxidant is preferably 2 wt % or less.
[0211] (Other ingredients)
[0212] The first layer, the second layer and the third layer may also contain coupling agents, dispersants, surfactants, flame retardants, antistatic agents, pigments, dyes, adhesion modifiers other than metal salts, moisture resistance agents, fluorescent whitening agents and infrared absorbers as needed. These additives may be used alone or in combination of two or more.
[0213] (Laminated glass)
[0214] Fig. 9 It means use Figure 1 1 is a cross-sectional view of an example of a laminated glass including the interlayer film for a laminated glass shown.
[0215] Fig. 9 The laminated glass 21 shown includes an intermediate film 11, a first laminated glass component 22, and a second laminated glass component 23. The intermediate film 11 is sandwiched between the first laminated glass component 22 and the second laminated glass component 23. The first laminated glass component 22 is arranged on a first surface of the intermediate film 11. The second laminated glass component 23 is arranged on a second surface of the intermediate film 11 opposite to the first surface.
[0216] As the laminated glass component, glass plates and PET (polyethylene terephthalate) films can be cited. The laminated glass includes not only a laminated glass formed by sandwiching an intermediate film between two glass plates, but also a laminated glass formed by sandwiching an intermediate film between a glass plate and a PET film. The laminated glass preferably has a laminated body of glass plates, and at least one glass plate is used. It is preferred that the first laminated glass component and the second laminated glass component are glass plates or PET (polyethylene terephthalate) films, respectively, and the intermediate film includes at least one glass plate as the first laminated glass component and the second laminated glass component. It is particularly preferred that both the first laminated glass component and the second laminated glass component are glass plates.
[0217] Examples of the glass plate include inorganic glass and organic glass. Examples of the inorganic glass include float glass, heat absorbing glass, heat reflecting glass, ground glass, patterned glass, wired glass, and green glass. Organic glass is a synthetic resin glass used in place of inorganic glass. Examples of the organic glass include polycarbonate and poly(meth)acrylic resin plates. Examples of the poly(meth)acrylic resin plates include poly(methyl)acrylate plates.
[0218] The thickness of each of the first laminated glass component and the second laminated glass component is not particularly limited, but is preferably 1 mm or more and preferably 5 mm or less. When the laminated glass component is a glass plate, the thickness of the glass plate is preferably 1 mm or more and preferably 5 mm or less. When the laminated glass component is a PET film, the thickness of the PET film is preferably 0.03 mm or more and preferably 0.5 mm or less.
[0219] The manufacturing method of the laminated glass is not particularly limited. For example, the intermediate film is sandwiched between the first and second laminated glass components, and passed through a pressing roller, or placed in a rubber bag for decompression and suction. In this way, the air remaining between the first laminated glass component and the intermediate film and the second laminated glass component and the intermediate film is removed. Thereafter, pre-bonding is performed at about 70 to 110°C to obtain a laminate. Next, the laminate is placed in an autoclave, or pressed, and pressed at about 120 to 150°C and a pressure of 1 to 1.5 MPa. In this way, laminated glass can be obtained.
[0220] The laminated glass can be used in automobiles, rail vehicles, airplanes, ships, buildings, etc. The laminated glass is preferably laminated glass for construction or vehicles, and more preferably laminated glass for vehicles. The laminated glass can also be used for purposes other than these. The laminated glass can be used for windshields, side windows, rear windows, or skylights of automobiles, etc. The laminated glass is preferably used in automobiles because of its high heat insulation and high visible light transmittance.
[0221] Since the interlayer film and the laminated glass can suppress ghost images, they are suitable for use in automobile windshields. The interlayer film is preferably used in laminated glass as a head-up display (HUD). The laminated glass is preferably a head-up display (HUD).
[0222] In the laminated glass, the speed and other measurement information sent from the control unit can be projected from the display unit of the instrument panel onto the windshield, so that the driver of the car can simultaneously observe the forward field of view and the measurement information without lowering his or her field of vision.
[0223] The present invention will be described in further detail below with reference to the following examples, but the present invention is not limited to these examples.
[0224] Prepare the following materials.
[0225] (Thermoplastic resin)
[0226] PVB1 (polyvinyl acetal resin: polyvinyl butyral resin acetalized with n-butyraldehyde, average degree of polymerization 1700, hydroxyl content 30.5 mol%, acetylation degree 1 mol%, butyralization degree 68.5 mol%)
[0227] PVB2 (polyvinyl acetal resin: polyvinyl butyral resin acetalized with n-butyraldehyde, average degree of polymerization 3000, hydroxyl content 22 mol%, acetylation degree 13 mol%, butyralization degree 65 mol%)
[0228] The hydroxyl content, acetylation degree, and acetalization degree (butyralization degree) were measured by a method in accordance with JIS K6728 "Testing methods for polyvinyl butyral". When measured in accordance with ASTM D1396-92, the same values as those in accordance with JIS K6728 "Testing methods for polyvinyl butyral" were shown.
[0229] (Plasticizer)
[0230] Triethylene glycol di-2-ethylhexanoate (3GO)
[0231] (Thermal insulation compound)
[0232] ITO particles
[0233] NIR-43V (vanadium phthalocyanine compound, "NIR-43V" manufactured by Yamada Chemical Co., Ltd.)
[0234] (UV shielding agent)
[0235] Tinuvin 326 (2-(2'-hydroxy-3'-tert-butyl-5-methylphenyl)-5-chlorobenzotriazole, "Tinuvin 326" manufactured by BASF)
[0236] (Antioxidant)
[0237] H-BHT (2,6-di-tert-butyl-4-methylphenol, "H-BHT" manufactured by Sakai Chemical Industry Co., Ltd.)
[0238] (Example 1)
[0239] Preparation of a composition for forming a portion other than the second region (including the first region):
[0240] By means of a mixing roller, 100 parts by weight of a polyvinyl acetal resin (PVB1), 40 parts by weight of a plasticizer (3GO), a heat-insulating compound (ITO particles) in an amount of 0.15% by weight in the resulting intermediate film, a heat-insulating compound (NIR-43V) in an amount of 0.0085% by weight in the resulting intermediate film, 0.2 parts by weight of a UV shielding agent (Tinuvin326), and 0.2 parts by weight of an antioxidant (H-BHT) are thoroughly mixed to obtain a composition for forming a portion other than the second region.
[0241] Preparation of the composition for forming the second region:
[0242] 100 parts by weight of polyvinyl acetal resin (PVB1), 40 parts by weight of plasticizer (3GO), 0.2 parts by weight of ultraviolet shielding agent (Tinuvin 326), and 0.2 parts by weight of antioxidant (H-BHT) were fully mixed with a mixing roller to obtain a composition for forming the second region.
[0243] Production of intermediate film:
[0244] Production Figure 1 The intermediate film shown.
[0245] An extruder is used to extrude a composition for forming a portion other than the second region and a composition for forming the second region to produce an intermediate film having a wedge-shaped cross-sectional shape in the thickness direction. The first region and the second region are formed in the thickest part of the intermediate film. The thickness Tmax of the thickest part of the intermediate film, the thickness Tmin of the thinnest part of the intermediate film, the absolute value X (|Tmax-Tmin|) of the thickness difference, and the thickness Y of the thickest part of the second region are shown in Table 1 below. It should be noted that the second region is a region in which the thickness at one end is less than the thickness at the other end, and the cross-sectional shape in the thickness direction is a wedge-shaped region, and the direction from one end to the other end of the intermediate film is the same as the direction from one end to the other end of the second region R2. In addition, the other end of the second region is in the same position as the other end of the intermediate film, and the distance from one end to the other end of the second region is 0.25Z relative to the distance Z from one end to the other end of the intermediate film.
[0246] Laminated glass production:
[0247] According to the above sampling method, test pieces (intermediate film) of 50 mm (direction connecting one end and the other end) × 50 mm (direction perpendicular to the direction connecting one end and the other end) are sampled at the thickest part and the thinnest part of the intermediate film.
[0248] Next, two sheets of heat absorbing flat glass (50 mm×50 mm×thickness 2.1 mm) conforming to JIS R3208 were prepared. The obtained interlayer film was sandwiched between the two sheets of heat absorbing glass plates, and vacuum pressed by a vacuum laminator at 90°C for 30 minutes to obtain a laminate. The interlayer film portion that protruded from the glass plates was cut off from the laminate to obtain a laminated glass.
[0249] (Examples 2 to 11)
[0250] An interlayer film was obtained in the same manner as in Example 1 except that the types and contents of the additive components in the first region and the second region of the interlayer film were set as shown in Tables 1 and 2 below, and the thickness Tmax of the thickest portion of the interlayer film, the thickness Tmin of the thinnest portion of the interlayer film, the absolute value X (|Tmax-Tmin|) of the thickness difference, and the thickness Y of the thickest portion of the second region were set as shown in Tables 1 and 2 below. Using the obtained interlayer film, a laminated glass was obtained in the same manner as in Example 1.
[0251] (Comparative Example 1)
[0252] Preparation of the composition for forming the intermediate film:
[0253] By means of a mixing roller, 100 parts by weight of a polyvinyl acetal resin (PVB1), 40 parts by weight of a plasticizer (3GO), a heat-insulating compound (ITO particles) in an amount of 0.15% by weight in the resulting interlayer film, a heat-insulating compound (NIR-43V) in an amount of 0.0085% by weight in the resulting interlayer film, 0.2 parts by weight of a UV shielding agent (Tinuvin326), and 0.2 parts by weight of an antioxidant (H-BHT) are fully mixed to obtain a composition for forming an interlayer film.
[0254] Production of intermediate film:
[0255] Made in Figure 1 The intermediate film shown does not form the intermediate film of the second region.
[0256] Only the composition for forming the intermediate film was extruded using an extruder to produce an intermediate film having a wedge-shaped cross-sectional shape in the thickness direction. The thickness Tmax of the thickest part of the intermediate film, the thickness Tmin of the thinnest part of the intermediate film, and the absolute value X (|Tmax-Tmin|) of the thickness difference are shown in the following Table 1. The second region was not formed in the thickest part of the intermediate film.
[0257] Using the obtained interlayer film, a laminated glass was obtained in the same manner as in Example 1.
[0258] (Comparative Examples 2 and 3)
[0259] An interlayer film was obtained in the same manner as in Example 1 except that the type and content of the additive component in the first region of the interlayer film were set as shown in Table 2 below, and the thickness Tmax of the thickest portion of the interlayer film, the thickness Tmin of the thinnest portion of the interlayer film, the absolute value X (|Tmax-Tmin|) of the thickness difference, and the thickness Y of the thickest portion of the second region were set as shown in Table 2 below. Using the obtained interlayer film, a laminated glass was obtained in the same manner as in Example 1.
[0260] (Example 12)
[0261] Preparation of the composition (1) for forming the portion other than the second region (including the first region):
[0262] By means of a mixing roller, 100 parts by weight of a polyvinyl acetal resin (PVB1), 40 parts by weight of a plasticizer (3GO), a heat-insulating compound (ITO particles) in an amount of 0.17% by weight in the resulting intermediate film, a heat-insulating compound (NIR-43V) in an amount of 0.0098% by weight in the resulting intermediate film, 0.2 parts by weight of a UV shielding agent (Tinuvin326), and 0.2 parts by weight of an antioxidant (H-BHT) are fully mixed to obtain a composition for forming a portion other than the second region.
[0263] Preparation of the composition (2) for forming the portion other than the second region:
[0264] 100 parts by weight of polyvinyl acetal resin (PVB2), 60 parts by weight of plasticizer (3GO), 0.2 parts by weight of ultraviolet shielding agent (Tinuvin 326), and 0.2 parts by weight of antioxidant (H-BHT) were fully mixed with a mixing roller to obtain a composition for forming a portion other than the second region.
[0265] Preparation of the composition for forming the second region:
[0266] 100 parts by weight of polyvinyl acetal resin (PVB1), 40 parts by weight of plasticizer (3GO), 0.2 parts by weight of ultraviolet shielding agent (Tinuvin 326), and 0.2 parts by weight of antioxidant (H-BHT) were fully mixed by a mixing roller to obtain a composition for forming the second region.
[0267] Production of intermediate film:
[0268] Production Figure 8 The intermediate film shown. It should be noted that the composition (1) for forming the portion other than the second region is used as the second and third layers 2G and 3G, the composition (2) for forming the portion other than the second region is used as the first layer 1G, and the composition for forming the second region is used as the second region R2 in the second layer 2G. The thickness of 1G is 0.1 mm.
[0269] Using an extruder, a composition (1) for forming a portion other than the second region, a composition (2) for forming a portion other than the second region, and a composition for forming the second region are extruded to produce an intermediate film having a wedge-shaped cross-sectional shape in the thickness direction. In the thickest part of the intermediate film, a first region (2G, 3G), a second region (R2), and other regions (1G) are formed. The thickness Tmax of the thickest part of the intermediate film, the thickness Tmin of the thinnest part of the intermediate film, the absolute value X (|Tmax-Tmin|) of the thickness difference, and the thickness Y of the thickest part of the second region are shown in Table 1 below. It should be noted that in the second region, the thickness at one end is less than the thickness at the other end, the cross-sectional shape in the thickness direction is a wedge, and the direction from one end to the other end of the intermediate film is the same as the direction from one end to the other end of the second region R2. In addition, the other end of the second region is in the same position as the other end of the intermediate film, and the distance from one end to the other end of the second region is 0.25Z relative to the distance Z from one end to the other end of the intermediate film.
[0270] Laminated glass production:
[0271] Using the obtained interlayer film, a laminated glass was obtained in the same manner as in Example 1.
[0272] (Examples 13 to 22)
[0273] An interlayer film was obtained in the same manner as in Example 12 except that the types and contents of the additive components in the first region and the second region of the interlayer film were set as shown in Table 3 below, and the thickness Tmax of the thickest portion of the interlayer film, the thickness Tmin of the thinnest portion of the interlayer film, the absolute value X (|Tmax-Tmin|) of the thickness difference, and the thickness Y of the thickest portion of the second region were set as shown in Table 3 below. Using the obtained interlayer film, a laminated glass was obtained in the same manner as in Example 1.
[0274] (Comparative Example 4)
[0275] Preparation of the composition (1) for forming an intermediate film:
[0276] By means of a mixing roller, 100 parts by weight of a polyvinyl acetal resin (PVB1), 40 parts by weight of a plasticizer (3GO), a heat-insulating compound (ITO particles) in an amount of 0.17% by weight in the resulting intermediate film, a heat-insulating compound (NIR-43V) in an amount of 0.0098% by weight in the resulting intermediate film, 0.2 parts by weight of a UV shielding agent (Tinuvin326), and 0.2 parts by weight of an antioxidant (H-BHT) are fully mixed to obtain a composition for forming a portion other than the second region.
[0277] Preparation of the composition (2) for forming an intermediate film:
[0278] 100 parts by weight of polyvinyl acetal resin (PVB2), 60 parts by weight of plasticizer (3GO), 0.2 parts by weight of ultraviolet shielding agent (Tinuvin 326), and 0.2 parts by weight of antioxidant (H-BHT) were fully mixed by a mixing roller to obtain a composition for forming the third region.
[0279] Production of intermediate film:
[0280] Made in Figure 8 The intermediate film shown does not have the second region formed therein. It should be noted that the composition (1) used to form the portion other than the second region was used as 2G and 3G, and the composition (2) used to form the portion other than the second region was used as 1G. The thickness of 1G was 0.1 mm.
[0281] Only the composition (1) for forming an intermediate film and the composition (2) for forming an intermediate film were extruded using an extruder to produce an intermediate film having a wedge-shaped cross-sectional shape in the thickness direction. The thickness Tmax of the thickest part of the intermediate film, the thickness Tmin of the thinnest part of the intermediate film, and the absolute value X (|Tmax-Tmin|) of the thickness difference are shown in the following Table 3. The second region was not formed in the thickest part of the intermediate film.
[0282] Laminated glass production:
[0283] Using the obtained interlayer film, a laminated glass was obtained in the same manner as in Example 1.
[0284] (Comparative Examples 5 and 6)
[0285] An interlayer film was obtained in the same manner as in Example 1 except that the type and content of the additive component in the first region of the interlayer film were set as shown in Table 3 below, and the thickness Tmax of the thickest portion of the interlayer film, the thickness Tmin of the thinnest portion of the interlayer film, the absolute value X (|Tmax-Tmin|) of the thickness difference, and the thickness Y of the thickest portion of the second region were set as shown in Table 3 below. Using the obtained interlayer film, a laminated glass was obtained in the same manner as in Example 1.
[0286] (evaluate)
[0287] (1) Thickness of the interlayer
[0288] The thickness Tmax of the thickest portion of the intermediate film, the thickness Tmin of the thinnest portion of the intermediate film, the absolute value X (|Tmax−Tmin|) of the thickness difference, and the thickness Y of the thickest portion of the second region were evaluated.
[0289] (2) Measurement of visible light transmittance (A light Y value, initial Α-Y (380 to 780 nm))
[0290] The visible light transmittance of the obtained laminated glass at a wavelength of 380 to 780 nm was measured using a spectrophotometer ("U-4100" manufactured by Hitachi High-Tech Corporation) in accordance with JIS R3211 (1998).
[0291] (3) Measurement of solar transmittance (initial Ts2500 (300-2500 nm))
[0292] The solar transmittance Ts (Ts2500) of the obtained laminated glass at a wavelength of 300 to 2500 nm was determined using a spectrophotometer ("U-4100" manufactured by Hitachi High-Tech Corporation) in accordance with JIS R3106 (1998).
[0293] The details and results of the interlayer are shown in the following Tables 1 to 3. It should be noted that in the following Tables 1 to 3, only the content of the heat-insulating compound is recorded, and the content of the polyvinyl acetal resin, the plasticizer, the ultraviolet shielding agent, and the antioxidant is omitted. In all the examples and comparative examples, 40 parts by weight of the plasticizer, 0.2 parts by weight of the ultraviolet shielding agent (Tinuvin 326), and 0.2 parts by weight of the antioxidant (H-BHT) were used relative to 100 parts by weight of the polyvinyl acetal resin.
[0294]
[0295]
[0296]
[0297] It should be noted that since the laminated glass using the interlayer film obtained in the example has a small difference in visible light transmittance, it is excellent in uniformity of visibility. The uniformity of visibility was confirmed by visual observation.
[0298] Explanation of symbols
[0299] 1, 1A, 1B, 1C, 1D, 1E, 1F, 1G...First floor
[0300] 2A, 2B, 2C, 2D, 2E, 2F, 2G... Second floor
[0301] 2Fa···Part with a rectangular cross-section in the thickness direction
[0302] 2Fb···Part with a wedge-shaped cross section in the thickness direction
[0303] 3A, 3B, 3C, 3D...Third floor
[0304] 11, 11A, 11B, 11C, 11D, 11E, 11F, 11G...Intermediate film
[0305] 11a···One end
[0306] 11b···The other end
[0307] 21···Laminated glass
[0308] 22···Laminated glass components
[0309] 23···Laminated glass components
Claims
1. An interlayer film for laminated glass, comprising a thermoplastic resin and a heat-insulating compound, The interlayer film for laminated glass has one end and another end located on the opposite side of the one end, and the thickness of the other end is greater than the thickness of the one end. In the interlayer film for laminated glass, the absolute value of the difference between the thickness of the thickest part and the thickness of the thinnest part is 0.1 mm or more, In a laminated glass obtained by sandwiching an interlayer between two heat absorbing flat glass plates with a thickness of 2.1 mm, the absolute value of the difference between the visible light transmittance of the thickest part of the interlayer and the visible light transmittance of the thinnest part of the interlayer is 4% or less.
2. The interlayer film for laminated glass according to claim 1, wherein In a laminated glass obtained by sandwiching an interlayer between two heat absorbing glass plates having a thickness of 2.1 mm, the absolute value of the difference between the solar transmittance of the thickest portion of the interlayer and the solar transmittance of the thinnest portion of the interlayer is 5.5% or less.
3. The interlayer film for laminated glass according to claim 1 or 2, wherein: In the thickness direction of the thickest portion of the intermediate film, there are a first region and a second region, and the content of the heat-shielding compound in the second region is smaller than that in the first region.
4. The interlayer film for laminated glass according to claim 3, wherein An absolute value of a difference between a content of the heat-shielding compound in the first region of the interlayer film and a content of the heat-shielding compound in the second region of the interlayer film is 0.0001% by weight or more.
5. The interlayer film for laminated glass according to claim 3 or 4, wherein The second region of the interlayer film does not contain the heat-shielding compound, or the second region of the interlayer film contains 0.5 wt % or less of the heat-shielding compound.
6. The interlayer film for laminated glass according to any one of claims 3 to 5, wherein When the absolute value of the difference between the thickness of the thickest part and the thickness of the thinnest part is set to X mm, Xmm exceeds 0.28, The thickness of the thickest portion of the second region is greater than or equal to (X-0.28) and less than or equal to X.
7. The interlayer film for laminated glass according to any one of claims 1 to 6, wherein The heat-shielding compound includes at least one component selected from the group consisting of a phthalocyanine compound, a naphthalocyanine compound, and an anthracyanine compound; or the heat-shielding compound includes heat-shielding particles.
8. The interlayer film for laminated glass according to claim 7, wherein The thermal insulation compound includes thermal insulation particles.
9. The interlayer film for laminated glass according to claim 7 or 8, wherein The heat shielding compound contains tin-doped indium oxide or tungsten oxide particles as the heat shielding particles.
10. The interlayer film for laminated glass according to any one of claims 7 to 9, wherein The heat-shielding compound includes at least one component selected from the group consisting of a phthalocyanine compound, a naphthalocyanine compound, and an anthracyanine compound.
11. The interlayer film for laminated glass according to any one of claims 1 to 10, wherein The thermoplastic resin is polyvinyl acetal resin. 12 . The interlayer film for laminated glass according to claim 1 , comprising a plasticizer. 13 . The interlayer film for laminated glass according to claim 1 , which has a portion having a wedge-shaped cross-sectional shape in the thickness direction.
14. A laminated glass comprising: The first laminated glass component, a second laminated glass component, and The interlayer film for laminated glass according to any one of claims 1 to 13, The interlayer film for laminated glass is arranged between the first laminated glass component and the second laminated glass component.
15. A laminated glass comprising: The first laminated glass component, a second laminated glass component, and Interlayer film for laminated glass, The interlayer film for laminated glass is arranged between the first laminated glass component and the second laminated glass component. The intermediate film contains a thermoplastic resin and a heat-insulating compound. The intermediate film has one end and another end located on the opposite side of the one end, and the thickness of the other end is greater than the thickness of the one end. In the intermediate film, the absolute value of the difference between the thickness of the thickest part and the thickness of the thinnest part is 0.1 mm or more, An absolute value of a difference between a visible light transmittance of the thickest portion of the interlayer film in the laminated glass and a visible light transmittance of the thinnest portion of the interlayer film in the laminated glass is 4% or less.