High-temperature-resistant polyamide film and preparation method thereof
Through the combination of homopolypolyamide, chain extender, nucleating agent and heat stabilizer, the melt extrusion and film blowing process are used to solve the problems of decreasing melt strength and degrading gas barrier properties during processing. A polyamide film with high temperature resistance and excellent gas barrier properties has been achieved.
Patent Information
- Application Number
- CN202310573949.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-19
- Publication Date
- 2024-11-22
AI Technical Summary
During the processing process, the existing polyamide films have large melt viscosity due to intermolecular hydrogen bonding, which requires increasing the processing temperature, but the melt strength decreases, which cannot meet the blow molding requirements, and the blending method affects the gas barrier performance.
The combination of homopolypolyamide, chain extender, nucleating agent and heat stabilizer is adopted to adjust the extrusion and film blowing parameters through the melt extrusion and film blowing process to improve the high temperature resistance and gas barrier properties of the polyamide film.
The high temperature resistance and excellent gas barrier properties of polyamide films are achieved, and the film rupture caused by insufficient melt strength is avoided, the film blowing process is ensured smoothly, and the high temperature resistance performance needs in aerospace and other fields are met.
Smart Images

Figure CN118994896A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polyamide films, and in particular relates to a high-temperature resistant polyamide film and a preparation method thereof. Background Art
[0002] Due to its excellent gas barrier properties, polyamide film is widely used in food packaging, composite material vacuum auxiliary materials and other fields. For food packaging, composite materials and vacuum auxiliary materials, high temperature resistance, mechanical properties and gas barrier properties are the main factors for evaluating their comprehensive performance.
[0003] The melt viscosity of polyamide materials is high due to the effect of intermolecular hydrogen bonds, which increases the temperature required for processing and molding, especially for polyamide 66 materials, where the processing temperature exceeds 270°C. During the processing of polyamide materials, when the temperature exceeds its melting point, the intermolecular hydrogen bonds weaken, and its melt strength drops significantly, making it unsuitable for blow molding. It is necessary to regulate its molecular structure or improve its melt strength through blending to meet the requirements of blow molding.
[0004] For example, the Chinese invention patent with application number CN201610537238.7 discloses a high-temperature resistant vacuum bag film LVF215R and a preparation method thereof, which specifically comprises the following steps: calculating by mass fraction, 50 to 75 parts of homonylon; 15 to 35 parts of copolymer nylon; 2 to 10 parts of elastomer; 1 to 4 parts of heat stabilizer; and 0.2 to 2 parts of masterbatch, mixing and loading into an extruder for extrusion and conveying to the die head of a film blowing machine, and obtaining a vacuum film by extrusion; the above scheme realizes the regulation of the molecular structure by blending homonylon and copolymer nylon, thereby meeting the requirements of blow molding; however, the above scheme neutralizes the temperature resistance of copolymer nylon and homonylon by blending, and cannot give full play to the temperature resistance of the raw materials, and the mixing of copolymer nylon and homonylon affects the crystallization performance of homonylon itself, thereby reducing the gas barrier performance of the polyamide film.
[0005] In view of this, the present invention is proposed. Summary of the invention
[0006] One of the purposes of the present invention is to provide a high temperature resistant polyamide film to address the problems in the above-mentioned prior art. The film is prepared by mixing homopolyamide, a chain extender, a nucleating agent and a stabilizer and then subjecting the mixture to melt extrusion and film blowing. The production process is relatively simple. Since homopolyamide is used as the raw material, the polyamide film can have better high temperature resistance while also having excellent gas barrier properties.
[0007] Another object of the present invention is to provide a method for preparing a high-temperature resistant polyamide film, wherein a homopolymer polyamide and an additive are mixed and then melt-extruded and blown to obtain a high-temperature resistant polyamide film, and by adjusting the extrusion and blowing parameters, the high-temperature resistance and gas barrier properties of the polyamide film are further improved.
[0008] In order to achieve the above object, the first aspect of the present invention provides a high temperature resistant polyamide film, comprising the following components in parts by weight:
[0009] Homopolymer polyamide: 92.2-99.79 parts;
[0010] Chain extender: 0.1-2 parts;
[0011] Nucleating agent: 0.01-5 parts;
[0012] Heat stabilizer: 0.1-0.8 parts;
[0013] The molecular weight of the homopolyamide is 50,000-80,000, and the DPI is 1.8-3.5.
[0014] In the above scheme, the molecular weight of the selected homopolymer polyamide is Mn=50000-80000, and the molecular weight distribution PDI=1.8-3.5; if the molecular weight is too low, the number of intermolecular entanglement points is small, the melt strength is low, and the molecular weight is further reduced after thermal processing, and the mechanical properties of the final product are greatly reduced. In addition, the reduction in molecular weight leads to a decrease in the viscosity of the polyamide, which may cause it to fail to successfully complete the film blowing process and fail to produce a polyamide film; if the molecular weight is too high, the production cost increases, and the increased viscosity of the polyamide leads to processing difficulties; in addition, the polyamide is subjected to thermal shear during the processing, resulting in a significant reduction in the molecular weight. If the molecular weight distribution is too low, the proportion of high molecular weight is too high, and processing and molding are difficult, and if the molecular weight distribution is too wide, the mechanical properties of the product are difficult to meet actual needs.
[0015] First of all, the present invention uses homopolyamide as raw material and makes full use of the relatively excellent crystallization performance of homopolyamide, which can significantly improve the gas barrier properties of polyamide film; the addition of heat stabilizer reduces the thermal degradation of polyamide during heating; at the same time, by adding chain extender to maintain the molecular weight of polyamide during processing, the process requirements for homopolyamide film blowing are met, and the mechanical properties of polyamide film are improved; by adding nucleating agent to increase the nucleation density during polyamide molding, the crystal size is reduced, the crystallization density is increased, and the gas barrier properties of polyamide film are effectively improved.
[0016] Furthermore, the homopolyamide is polyamide 66.
[0017] Furthermore, the chain extender is selected from one or more of epoxy compounds, bisoxazoline chain extenders, carbonate chain extenders, and maleic anhydride chain extenders.
[0018] Preferably, the epoxy chain extender is styrene-methyl methacrylate-glycidyl methacrylate (KL-E4370B); the maleic anhydride chain extender is ethylene maleic anhydride copolymer or propylene maleic anhydride copolymer.
[0019] Furthermore, the nucleating agent is selected from one or more of an inorganic nucleating agent, an organic nucleating agent and a polymer nucleating agent.
[0020] Preferably, the organic nucleating agent is calcium montanate; the inorganic nucleating agent is nano-silicon dioxide; and the polymer nucleating agent is polyvinyl siloxane.
[0021] Further, the heat stabilizer is selected from one or more of phosphate esters, metal copper salts, hindered phenols, and hindered amine heat stabilizers;
[0022] Furthermore, the phosphate ester heat stabilizer is bis(2,4-di-tert-butylphenol) pentaerythritol diphosphite (thermal stabilizer 626); the metal copper salt heat stabilizer is CuI complex; the hindered phenol heat stabilizer is N,N'-1,6-hexylene-bis-[3,5-di-tert-butyl-4-hydroxyphenylpropionamide] (thermal stabilizer 1098); and the hindered amine heat stabilizer is pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate (thermal stabilizer 1010).
[0023] A second aspect of the present invention provides a method for preparing a high temperature resistant polyamide film, comprising the following steps:
[0024] S1, mixing a heat stabilizer with a portion of homopolymerized polyamide and then melt-extruding the mixture to obtain a heat-stable masterbatch;
[0025] S2, mixing the heat-stabilizing masterbatch with the remaining homopolymer polyamide, the chain extender and the nucleating agent, and then drying the mixture, and then melt-extruding and blowing the mixture to obtain a high-temperature resistant polyamide film.
[0026] Furthermore, in step S1, the mass ratio of the heat stabilizer to part of the homopolymerized polyamide is 0.1-0.5:1.
[0027] In the above scheme, the heat stabilizer is first mixed with part of the homopolymer polyamide and then melt-extruded and pelletized to obtain a heat-stable masterbatch, and then the heat-stable masterbatch is mixed with other components and melt-extruded, thereby improving the uniformity of the heat stabilizer dispersion; the mass ratio of the heat stabilizer and part of the polyamide when mixed is 0.1-0.5:1, which avoids the problem that too little polyamide cannot achieve initial uniform mixing with the heat stabilizer, and also avoids the problem that the first step is time-consuming due to excessive use of polyamide, thereby improving the production efficiency and the quality of the polyamide film obtained.
[0028] Furthermore, in step S2, a screw extruder is used for melt extrusion, the temperature of the melt extrusion is 240-300°C, and the speed of the screw is 20-60rpm.
[0029] Since the melting point of polyamide 66 is around 260°C and the complete melting point is above 280°C, the screw heating zone temperature is set to 240-300°C to meet the complete melting of polyamide 66. Higher temperatures will increase the degradation of polyamide 66 and increase energy consumption. If the screw speed is too low, polyamide 66 will melt unevenly in the screw and the resistance will increase. If the speed is too high, it will cause excessive shear heat, increase the degradation of polyamide 66, and cause unstable melt and uneven film thickness. Therefore, it is advisable to set the screw speed at 20-60rpm.
[0030] Furthermore, in step S2, a film blowing machine is used for the film blowing step, the film blowing temperature is 260-300° C.; the temperature of the air ring of the film blowing machine is 5-20° C.; the distance between the air ring and the die of the film blowing machine is 0-50 cm.
[0031] The homopolyamide melt is sent to the film blowing die through a twin-screw extruder, and a tubular film is formed through the die, and then the air ring is blown and cooled to form the required film. Therefore, the temperature of the die needs to be higher than the melting point of the homopolyamide. Below this temperature, the melt will cool rapidly and block the die. Above 300°C, the degradation of homopolyamide is accelerated, the cooling efficiency of the air ring decreases, and the performance of the product decreases. The processing temperature of homopolyamide is relatively high. After the film tube leaves the die, the air ring needs to take away a large amount of heat for molding. Too low an air ring temperature will cause the frost line to be too low, and it will be difficult to increase the blowing ratio. Too high an air ring temperature will cause the crystallization rate of homopolyamide to slow down, the crystal size to increase, and the performance to decrease. The distance between the air ring and the die can be adjusted to achieve the control of the frost line height to meet the control of the crystallization rate of homopolyamide. The adjustment range is preferably 0-50cm. After it is higher than 50cm, the control effect decreases. The beneficial effects of adopting this scheme are:
[0032] 1. Using homopolymer polyamide, chain extender, nucleating agent and heat stabilizer as raw materials, high temperature resistant polyamide film is obtained through melt extrusion and film blowing. The chain extender improves the melt strength of homopolymer polyamide, avoids the film rupture during the film blowing process due to insufficient melt strength, and ensures the smooth progress of homopolymer polyamide film blowing.
[0033] 2. Using homopolyamide 66 as raw material can give full play to the advantage of high melting point of homopolyamide, thereby producing products with better high temperature resistance. Since other polyamides are not blended with homopolyamide 66, the crystallization performance of polyamide 66 will not be affected, thereby ensuring that the polyamide film has excellent gas barrier properties while producing high temperature resistant polyamide film.
[0034] 3. This scheme uses homopolyamide, chain extender, nucleating agent and thermal stabilizer as raw materials, and realizes the chain extension of homopolyamide in a twin-screw, reduces the molecular weight decrease of polyamide materials caused by the melt processing, and ensures that the film has a low gas permeability; at the same time, due to the micro-cross-linking effect of the chain extender, the melt strength of homopolyamide can also be improved, making it suitable for blown film processing. In addition, due to the effect of the nucleating agent, the homopolyamide film formed has a small spherulite size and high transparency of the product. The processing technology of the polyamide material with the above formula is a screw extrusion temperature of 240-300°C, a die temperature of 260-300°C, an air ring temperature of 5-20°C, and the air ring is 0-50cm away from the die. The melting temperature T m Homopolymer polyamide film with high transparency of ≥250℃ and uniform thickness can meet the needs of aerospace, wind power generation and other fields for polyamide film with higher temperature resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 The DSC curve of the polyamide film prepared according to the ratio and preparation method described in Example 1 is shown in FIG.
[0036] Figure 2 This is an AFM image of the polyamide film prepared according to the ratio and preparation method described in Example 1.
[0037] Figure 3 This is an AFM image of the polyamide film prepared according to the ratio and preparation method described in Comparative Example 1.
[0038] Figure 4 It is a melt strength curve diagram of the polyamide film described in Example 1 and Comparative Example 1. DETAILED DESCRIPTION
[0039] The exemplary embodiments of the present invention will be described in more detail below using examples. Those skilled in the art will appreciate that the following embodiments are only used to explain the technical principles of the present invention and are not intended to limit the scope of protection of the present invention.
[0040] It should be noted that the test methods corresponding to the test items of the film performance provided in the embodiments of the present invention are as follows:
[0041] The specific test process of melting temperature is as follows: The test of melting temperature is carried out in accordance with the provisions of GB / T 19466.3-2004 Plastics Differential Scanning Calorimetry (DSC) Part 3: Determination of Melting and Crystallization Temperature and Thermal Enthalpy, as follows: The melting temperature of the film is tested by DSC method. Weigh 2mg to 5mg of the film sample and seal it in a DSC crucible. Under nitrogen protection, heat the sample to 300℃ at a heating rate of 10℃ / min. The peak temperature of the melting peak is taken as the melting temperature T of the sample. m .
[0042] The specific test process of tensile strength is as follows: The test is carried out in accordance with GB / T 1040.3-2006 Determination of tensile properties of plastics Part 3: Test conditions for films and sheets. The specific conditions are as follows. Each sample should be conditioned for at least 48 hours at a temperature of 23±2°C and a humidity of 50%±5% before the experiment. The sample is prepared by XBM-II plastic film cutting machine, preferably a long strip sample with a width of 10mm and a length of not less than 150mm. The edge of the sample is required to be smooth and free of defects (it is recommended to use a low-power magnifying glass for inspection). The gauge length is 100mm, the tensile speed is 100mm / min, and the number of samples in each test direction is not less than 5.
[0043] The specific test process of wetting tension is as follows: according to GB / T 14216-2008, the determination of wetting tension of plastic film and sheet, the sample size is 10cm×10cm, and mixed solutions with different wetting tensions are prepared according to the standard requirements before the test. The sample is conditioned for 4 hours at a temperature of 23±2℃ and a humidity of 50%±5%. The sample is placed horizontally on a smooth test bench, and the mixed solution is applied to the sample to be tested with a cotton swab, so that the mixed solution immediately spreads to at least 20cm 2 The wetting tension of the mixed solution that covers an area of the sample surface without breaking the liquid film and can maintain a continuous liquid film for 2S is the wetting tension of the sample.
[0044] The specific test process of haze is: use the reflection mode of SHIMADZU UV-2600 ultraviolet spectrophotometer and carry out the test with the integrating sphere accessory. The incident light, the total light transmittance through the sample and the light scattering can be measured by the ultraviolet spectrophotometer to calculate the haze value H. The total flux of direct light and diffuse reflection of the integrating sphere is T1, the integrating sphere accessory is removed, and the projection accessory is used to directly measure the pass rate, and T2 is measured. The haze can be calculated by the following formula:
[0045]
[0046] The specific test process of gas permeability is as follows: According to the provisions of GBT1038-2000 Plastic Film Gas Permeability Test Method Pressure Difference Method. The test sample is conditioned in a dryer at 23±2℃ for 48 hours, and the test sample is placed between the high pressure chamber and the low pressure chamber. The test gas is O2, and the pressure change is measured for 24 hours to obtain the gas permeability of the test sample.
[0047] The following is a detailed description with specific examples. The sources of raw materials used in the following specific examples are shown in the following table:
[0048]
[0049]
[0050] Embodiment 1
[0051] As an embodiment of the present invention, this embodiment provides a high temperature resistant polyamide film, including the following components:
[0052] PA66: 99.0 parts;
[0053] KL-E4370B: 0.5 parts;
[0054] Calcium montanate: 0.3 parts;
[0055] Heat stabilizer 1010+626: 0.2 parts;
[0056] Among them, the molecular weight of PA66 is Mn=70000 and PDI=2.3.
[0057] The specific preparation method comprises the following steps:
[0058] S1. Mix the heat stabilizer and part of PA66 in a mass ratio of 0.1:1 and then melt extrude to obtain a heat-stable masterbatch;
[0059] S2. After mixing the heat-stabilizing masterbatch with the remaining PA66, chain extender and nucleating agent, the mixture is sent to a drying tower for drying. After completion, the mixture is added to a screw extruder for melt extrusion. The temperatures in each temperature zone of the screw extruder are: 240°C, 260°C, 270°C, 280°C, 280°C, 275°C, 275°C, 270°C, and the screw speed is 42rpm; the extruded melt is then sent to the die head of a film blowing machine, and a high-temperature resistant polyamide film is obtained by film blowing; wherein, the temperatures in each temperature zone of the die head are: 270°C, 275°C, 275°C, 270°C, the blowing ratio is 1.4, the air ring temperature is 15°C, and the distance between the air ring and the die is 20cm.
[0060] Embodiment 2
[0061] As another embodiment of the present invention, this embodiment provides a high temperature resistant polyamide film, including the following components:
[0062] PA66: 98.7 parts;
[0063] Ethylene maleic anhydride copolymer: 0.5 parts;
[0064] Polyvinylsiloxane: 0.3 parts;
[0065] CuI complex: 0.5 parts;
[0066] Among them, the molecular weight of PA66 is Mn=60000 and PDI=2.7.
[0067] The specific preparation method comprises the following steps:
[0068] S1. Mix the heat stabilizer and part of PA66 in a mass ratio of 0.1:1 and then melt extrude to obtain a heat-stable masterbatch;
[0069] S2. After mixing the heat-stabilizing masterbatch with the remaining PA66, chain extender and nucleating agent, the mixture is sent to a drying tower for drying. After completion, the mixture is added to a screw extruder for melt extrusion. The temperatures in each temperature zone of the screw extruder are: 240°C, 270°C, 280°C, 280°C, 290°C, 290°C, 280°C, 270°C, and the screw speed is 35rpm. The extruded melt is then sent to the die head of a film blowing machine, and a high-temperature resistant polyamide film is obtained by film blowing. Among them, the temperatures in each temperature zone of the die head are: 270°C, 280°C, 280°C, 270°C, the blowing ratio is 1.6, the air ring temperature is 10°C, and the distance between the air ring and the die is 10cm.
[0070] Embodiment 3
[0071] As another embodiment of the present invention, this embodiment provides a high temperature resistant polyamide film, including the following components:
[0072] PA66: 96.1 parts;
[0073] KL-E4370B: 0.5 parts;
[0074] Nano silicon dioxide: 3 parts;
[0075] CuI complex: 0.4 parts;
[0076] Among them, the molecular weight of PA66 is Mn=55000 and PDI=3.1.
[0077] The specific preparation method comprises the following steps:
[0078] S1. Mix the heat stabilizer and part of PA66 in a mass ratio of 0.1:1 and then melt extrude to obtain a heat-stable masterbatch;
[0079] S2. After mixing the heat-stabilizing masterbatch with the remaining PA66, chain extender and nucleating agent, the mixture is sent to a drying tower for drying. After completion, the mixture is added to a screw extruder for melt extrusion. The temperatures in each temperature zone of the screw extruder are: 240°C, 260°C, 270°C, 280°C, 280°C, 280°C, 270°C, and the screw speed is 48rpm. The extruded melt is then sent to the die head of a film blowing machine, and a high-temperature resistant polyamide film is obtained by film blowing. Among them, the temperatures in each temperature zone of the die head are: 270°C, 280°C, 280°C, 270°C, the blowing ratio is 1.5, the air ring temperature is 16°C, and the distance between the air ring and the die is 30cm.
[0080] Embodiment 4
[0081] As another embodiment of the present invention, this embodiment provides a high temperature resistant polyamide film, including the following components:
[0082] PA66: 97.7 parts;
[0083] Ethylene maleic anhydride copolymer: 1.0 part;
[0084] Calcium montanate: 1.0 part;
[0085] Heat stabilizer 1098+626: 0.3 parts;
[0086] Among them, the molecular weight of PA66 is Mn=55000 and PDI=3.2.
[0087] The specific preparation method comprises the following steps:
[0088] S1. Mix the heat stabilizer and part of PA66 in a mass ratio of 0.1:1 and then melt extrude to obtain a heat-stable masterbatch;
[0089] S2. After mixing the heat-stabilizing masterbatch with the remaining PA66, chain extender and nucleating agent, the mixture is sent to a drying tower for drying. After completion, the mixture is added to a screw extruder for melt extrusion. The temperatures in each temperature zone of the screw extruder are: 240°C, 270°C, 270°C, 280°C, 280°C, 280°C, 280°C, 275°C, and the screw speed is 45rpm. The extruded melt is then sent to the die head of a film blowing machine, and a high-temperature resistant polyamide film is obtained by film blowing. Among them, the temperatures in each temperature zone of the die head are: 275°C, 280°C, 280°C, 275°C, the blowing ratio is 1.5, the air ring temperature is 15°C, and the distance between the air ring and the die is 35cm.
[0090] The properties of the high temperature resistant polyamide films obtained in the above embodiments were tested, and the results are shown in the following table:
[0091]
[0092] It can be seen that the polyamide films prepared by the preparation method of the present invention all have a very high melting point, giving full play to the high melting point characteristics of polyamide 66, and the prepared polyamide films have excellent temperature resistance; and the haze of the polyamide films prepared in each embodiment is very low, indicating that the polyamide films have high transparency; it can also be seen that the polyamide films prepared by the present invention also have excellent mechanical properties and gas barrier properties.
[0093] Furthermore, by comparing the above embodiments, it can be seen that the polyamide 66 film prepared in Embodiment 1 has more excellent gas barrier properties, the largest wetting tension, the lowest haze, and a higher melting point of 261°C.
[0094] Experimental Example 1
[0095] In this experimental example, the performance of the high temperature resistant polyamide film prepared by the method described in Example 1 with the same raw materials in different ratios was tested and compared. The specific ratios and the corresponding test results are shown in the following table:
[0096]
[0097]
[0098] It can be seen from the table above that the polyamide film prepared according to the ratio described in Example 1 has a polyamide crystal area of 1-3 μm due to the synergistic effect between the chain extender, nucleating agent and thermal stabilizer. 2 The AFM results are as follows Figure 2 As shown; it can be seen that the crystal density of the polyamide film prepared according to the ratio described in Example 1 is large, and it can also be seen from the table that the obtained polyamide film has excellent gas permeability; at the same time, it has the characteristics of large wetting tension, low haze, and high melting point.
[0099] In comparative example 1, no additive was added, and the area of the formed polyamide crystals was 13-19 μm. 2 The AFM results are as follows Figure 3As shown; it can be seen that the crystal density of the polyamide film prepared according to the ratio described in comparative example 1 is reduced, and due to the decrease in molecular weight, the tensile strength and elongation at break of the prepared polyamide film are greatly reduced, the melting point is the lowest, and the gas permeability is also significantly increased; in comparative example 2, the amount of chain extender added is higher than 2%, and due to the transitional crosslinking, the elongation at break of the prepared polyamide film is significantly reduced, and its melting point is also significantly lower than the melting point of the bulk material polyamide 66; in comparative example 3, no nucleating agent is added, and the haze of the prepared film is significantly increased. In comparative example 4, too much nucleating agent is added, and the melting point of the film is reduced. The heat stabilizer content of comparative example 5 is 0. Due to the intensified degradation during the processing process, the mechanical properties of the film are significantly reduced, and the melting point of the film is also significantly lower than the melting point of the raw material.
[0100] Further, combined with Figure 4 It can be seen that compared with Example 1, the melt strength of Example 1 is significantly improved. The melt strength of Example 1 reaches 4 cN, while the melt strength of Comparative Example 1 is only 0.5 cN, which indicates that the melt stability of the polyamide film prepared in Example 1 is significantly improved, and has a wider processing window, which is beneficial to production, processing and practical use.
[0101] Experimental Example 2
[0102] This experimental example adopts the formula and preparation method as described in Example 1, without changing the ratio of each component, only changing the type of one of the chain extender, nucleating agent or thermal stabilizer, to prepare different high temperature resistant polyamide films, and test and compare their properties. The specific formula is shown in the following table:
[0103]
[0104] The corresponding test results are shown in the following table:
[0105]
[0106]
[0107] From the above comparison, it can be seen that: Comparative Examples 7 to 10 show the performance of different polyamide films obtained by only changing the type of auxiliary agent; in Example 1, the chain extender is KL-E4370B, and due to the high content of epoxy groups in its composition, it can significantly improve the degradation problem in the polyamide processing process, ensure the molecular weight stability, and thus obtain a polyamide film with lower gas permeability, while in Comparative Example 7, ethylene maleic anhydride copolymer is used as the chain extender. Due to its low epoxy equivalent, the chain extension effect is not as good as KL-E4370B, and the performance of the obtained film is not as good as the polyamide film prepared in Example 1.
[0108] Secondly, the nucleating agent used in Example 1 is calcium montanate, which has a better dispersion effect in polyamide than the polyethylene siloxane used in Comparative Example 8, and can improve the gas barrier properties of the film while ensuring that its haze and melting temperature are better.
[0109] The heat stabilizer used in the present application is a composite heat stabilizer obtained by mixing heat stabilizer 1010 and heat stabilizer 626. Its thermal stability is better than that of a single-component heat stabilizer. The heat stabilizers used in Comparative Examples 9 and 10 are CuI and heat stabilizer 1098, respectively. The melting temperatures of the polyamide films obtained with the single-component heat stabilizers show a downward trend, and due to the decrease in molecular weight during the processing, the gas permeability and haze of the obtained films are not as good as those of the polyamide 66 film prepared with the composite heat stabilizer.
[0110] Secondly, when the main components are PA6, PA66-co-PA6, and PA66+PA6+PA66-co-PA6, due to the decrease in intermolecular forces, the melting points of the resulting film products are lower than the melting temperature of the film prepared from homopolymerized polyamide 66.
[0111] Comparative Example 3
[0112] This experimental example adopts the formula as described in Example 1, and only changes the temperature of melt extrusion and the speed of the screw in the preparation method to prepare different high temperature resistant polyamide films, and test and compare their properties. The test results are shown in the following table:
[0113]
[0114] From the above comparison, it can be seen that: when the screw temperature increases and the speed remains unchanged, the decrease in molecular weight of polyamide 66 caused by temperature is dominant, the tensile strength and elongation at break of the prepared film decrease, the gas permeability increases, and the wetting tension, haze and melting point all decrease. When the screw temperature remains unchanged and the speed changes, too low a speed leads to uneven heating and poor plasticization, and too high a speed leads to the dominant decrease in molecular weight caused by shear. As a result, the tensile strength and elongation at break of the prepared film decrease at too low a speed, the gas permeability increases, the wetting tension decreases, the haze decreases, and the melting point decreases. When the screw processing temperature is 310°C and the screw speed is 65rpm, the mechanical properties of the film decrease significantly, the gas permeability increases, and the melting point decreases.
[0115] Comparative Example 4
[0116] This experimental example adopts the formula as described in Example 1, and only changes the temperature of the air ring and the distance between the air ring and the die in the preparation method, and prepares different high temperature resistant polyamide films, and tests and compares their properties. The test results are shown in the following table:
[0117]
[0118] From the above comparison, it can be seen that increasing the air ring temperature and keeping the air ring distance unchanged can slow down the crystallization rate of the polyamide film, resulting in an increase in the tensile strength of the prepared polyamide film while decreasing the elongation at break, decreasing the gas permeability, decreasing the wetting tension, and increasing the haze. While maintaining the air ring temperature unchanged and increasing the distance between the air ring and the die head, the tensile strength decreases, the elongation at break decreases, the gas permeability increases, the wetting tension decreases, and the haze increases. When the air ring temperature is 0°C, due to the accelerated cooling rate, the prepared film exhibits anisotropy, and the mechanical properties in the MD and TD directions differ significantly. In addition, due to the imperfect polyamide crystals, the melting point decreases.
[0119] The above description is only a preferred embodiment of the present invention, and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technician familiar with this patent can make some changes or modifications to equivalent embodiments of equivalent changes by using the technical content suggested above without departing from the scope of the technical solution of the present invention. The implementation scheme in the above embodiment can also be further combined or replaced. However, any simple modification, equivalent change and modification made to the above embodiment based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the scope of the solution of the present invention.
Claims
1. A high temperature resistant polyamide film, characterized in that: The components include the following by weight: Homopolymer polyamide: 92.2-99.79 parts; Chain extender: 0.1-2 parts; Nucleating agent: 0.01-5 parts; Heat stabilizer: 0.1-0.8 parts; The molecular weight of the homopolyamide is 50,000-80,000 and the PDI is 1.8-3.
5.
2. The high temperature resistant polyamide film according to claim 1, characterized in that: The homopolyamide is selected from polyamide 66.
3. The high temperature resistant polyamide film according to claim 1 or 2, characterized in that: The chain extender is selected from one or more of epoxy compounds, bisoxazoline chain extenders, carbonate chain extenders, and maleic anhydride chain extenders; Preferably, the epoxy chain extender is styrene-methyl methacrylate-glycidyl methacrylate; and the maleic anhydride chain extender is ethylene maleic anhydride copolymer or propylene maleic anhydride copolymer.
4. The high temperature resistant polyamide film according to any one of claims 1 to 3, characterized in that: The nucleating agent is selected from one or more of an inorganic nucleating agent, an organic nucleating agent and a polymer nucleating agent; Preferably, the organic nucleating agent is calcium montanate; the inorganic nucleating agent is nano-silicon dioxide; and the polymer nucleating agent is polyvinyl siloxane.
5. The high temperature resistant polyamide film according to any one of claims 1 to 4, characterized in that: The heat stabilizer is selected from one or more of phosphate esters, metal copper salts, hindered phenols and hindered amine heat stabilizers.
6. The high temperature resistant polyamide film according to claim 5, characterized in that: The phosphate ester heat stabilizer is bis(2,4-di-tert-butylphenol)pentaerythritol diphosphite; the metal copper salt heat stabilizer is CuI complex; the hindered phenol heat stabilizer is N,N'-1,6-hexylidene-bis-[3,5-di-tert-butyl-4-hydroxyphenylpropionamide]; and the hindered amine heat stabilizer is pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate].
7. A method for preparing a high temperature resistant polyamide film according to any one of claims 1 to 6, characterized in that: The steps include: S1, mixing a heat stabilizer with a portion of homopolymerized polyamide and then melt-extruding the mixture to obtain a heat-stable masterbatch; S2, mixing the heat-stabilizing masterbatch with the remaining homopolymer polyamide, the chain extender and the nucleating agent, and then drying the mixture, and then melt-extruding and blowing the mixture to obtain a high-temperature resistant polyamide film.
8. The method for preparing a high temperature resistant polyamide film according to claim 7, characterized in that: In step S1, the mass ratio of the heat stabilizer to the homopolymer polyamide is 0.1-0.5:
1.
9. The method for preparing a high temperature resistant polyamide film according to claim 7, characterized in that: In step S2, a screw extruder is used for melt extrusion, the temperature of the melt extrusion is 240-300°C, and the speed of the screw is 20-60rpm.
10. The method for preparing a high temperature resistant polyamide film according to claim 9, characterized in that: In step S2, a film blowing machine is used to perform the film blowing step, and the film blowing temperature is 260-300° C.; The temperature of the air ring of the film blowing machine is 5-20°C; the distance between the air ring and the die of the film blowing machine is 0-50cm.
Citation Information
Cited By
High-strength and high-toughness hydrogen-resistant lining material for hydrogen storage container and preparation method of high-strength and high-toughness hydrogen-resistant lining material
CN120737597A