Preparation method of base tackifying polylipoic acid-based adhesive

By introducing 9-(2-hydroxyethyl)adenine monomer into polylipoic acid, a base-adhesive polylipoic acid adhesive is formed, and a variety of adhesion effects are used to improve the underwater bond strength and maintain stability. The problem of low bonding strength of existing adhesives underwater is solved, and high-strength, long-term stable underwater bonding effect is achieved.

CN118995124APending Publication Date: 2024-11-22CHANGCHUN UNIV OF TECH
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411221972.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing adhesives have low bonding strength in underwater environments, and cannot achieve long-term stable bonding effect, and are greatly affected by the erosion and swelling of water molecules.

Method used

By introducing 9-(2-hydroxyethyl)adenine monomer into the polylipoic acid backbone, a base-adhesive polylipoic acid binder is formed, and hydrogen bonds are formed with the substrate using the nitrogen heterocyclic structure of the base molecule to form a hydrogen bond with the substrate. , metal complexing and ππ stacking and other adhesion effects to improve adhesion strength and ensure stability underwater through the hydrophobicity of polylipoic acid.

Benefits of technology

High-strength underwater bonding with metals, wood, plastics and other materials is achieved, ensuring long-term adhesion performance in the underwater environment, and providing the design and preparation ideas of a new generation of underwater adhesives.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a base tackifying polylipoic acid-based adhesive and a preparation method thereof, and belongs to the field of adhesives. The preparation method comprises the following steps: firstly, modifying a lipoic acid molecule by using 9-(2-hydroxyethyl) adenine, and then carrying out melt polymerization on a basic group modified lipoic acid monomer and the traditional lipoic acid molecule to prepare the basic group tackified polylipoic acid adhesive. The adhesive depends on basic groups as viscosity factors and the good hydrophobicity of a main chain of the polylipoic acid polymer, construction of a high-strength, durable and stable underwater bonding interface is achieved, the adhesive shows excellent adhesion performance on various solid materials, and the underwater bonding strength of the adhesive can reach 1.1 MPa. The preparation method provided by the invention provides a brand new thought and method for design and preparation of a new generation of underwater adhesive.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of adhesives, and in particular relates to a method for preparing a polylipoic acid-based adhesive based on base thickening. Background Art

[0002] Adhesives are widely used in biomedicine, industrial manufacturing, electronic equipment, aerospace and other fields. Today, adhesives with different characteristics are designed for different application environments. However, for existing adhesives, achieving high-strength and stable underwater bonding is still a big challenge. Because the surface hydration layer of underwater materials will limit the occurrence of adhesion, and water molecules have corrosive and plasticizing effects. During long-term underwater use, the underwater bonding interface will be damaged by the swelling and erosion of water molecules, resulting in a decrease in the performance of the bonding interface or even failure. Therefore, the development of an underwater adhesive with high strength and underwater stability is of great significance for long-term application in humid environments.

[0003] Lipoic acid exists in the human body as a coenzyme of aerobic metabolism and is a naturally occurring biological small molecule. Due to its structural characteristics of disulfide bonds, lipoic acid polymers usually exhibit dynamic properties, such as reversible adhesion, self-healing, recyclability, and adaptability. As a dynamic primitive of the polymer, lipoic acid enables a multi-level synergistic dynamic response in the polymer network. In addition, the terminal carboxyl structure of the lipoic acid molecule can be obtained through a series of chemical reactions to obtain the corresponding lipoic acid derivatives. At present, adhesives with polylipoic acid as the main raw material are widely developed, but most of the current polylipoic acid-based adhesives rely on the side groups on the polymer chain to produce a single hydrogen bond with the substrate to achieve the construction of the bonding interface, which results in the low adhesion strength of the existing adhesives, limiting their application in the field of adhesives.

[0004] Bases are codons for biological evolution and growth in nature, and play an important role in genetic inheritance and protein synthesis. In recent years, based on their unique structure, base molecules have been widely used in the development of materials such as gels, adhesives, and elastomers. However, most of the base-based adhesives developed in recent years are prepared based on hydrophilic polymers, so high-strength underwater bonding has not been achieved so far. 9-(2-hydroxyethyl)adenine is a derivative of traditional adenine base molecules, containing functional groups such as amino, hydroxyl, and nitrogen heterocycles. Its hydroxyl group can undergo esterification reaction with the carboxyl group of lipoic acid, thereby modifying the lipoic acid side group. Therefore, the present invention intends to introduce 9-(2-hydroxyethyl)adenine monomers into the polylipoic acid main chain, so that it can be used as a viscosity factor to give the polymer material good adhesion properties. Summary of the invention

[0005] Purpose of the invention: In order to solve the problem that traditional adhesives have low bonding strength and cannot be used underwater for a long time, the purpose of the present invention is to provide a base-thickened polylipoic acid-based adhesive and a preparation method thereof, which provides a new idea for the development and preparation of high-strength, long-lasting and stable underwater adhesives.

[0006] Technical solution: 1. A method for preparing a base thickening polylipoic acid adhesive, characterized in that the steps and conditions are as follows: (1) Add lipoic acid, 9-(2-hydroxyethyl)adenine, 4-dimethylaminopyridine and dichloromethane to a single-necked round-bottom flask, stir at room temperature until completely dissolved, place in an ice-water bath to cool to 0 °C, add (1-ethyl 3-(3-dimethylaminopropyl)) carbodiimide, stir for 15 minutes and then remove the ice-water bath, wrap the round-bottom flask with aluminum foil and stir at room temperature for 12 hours, concentrate in a vacuum to obtain a 9-(2-hydroxyethyl)adenine-modified lipoic acid precursor solution, and precipitate a base-modified lipoic acid monomer using an ethyl acetate solution; the molar ratio of the 9-(2-hydroxyethyl)adenine monomer to the lipoic acid monomer and the 4-dimethylaminopyridine monomer is 1:1-1.3:1.1-1.4; (2) Melting lipoic acid monomer and base-modified lipoic acid monomer at 90°C, melt-polymerizing at 90°C for 6-8 hours, cooling to room temperature, and finally preparing a base-thickening polylipoic acid adhesive. The mass ratio of lipoic acid monomer to base-modified lipoic acid monomer is 0.25-4.

[0007] Innovation: The innovation of the present invention is to introduce bases as viscosity factors into the polylipoic acid polymer network, relying on the inherent nitrogen heterocyclic structure and amino and other characteristic groups of the base molecules to form hydrogen bonding, metal complexation, ππ stacking and other adhesion effects with various substrates to achieve high-strength adhesion between the adhesive and the surface of the substrate; on the other hand, the polylipoic acid polymer main chain has good hydrophobicity, which can ensure the long-term stability of the adhesive in underwater applications.

[0008] Beneficial effects: The present invention introduces base molecules into the main chain of polylipoic acid polymer to make it a viscosity factor, and prepares a base-thickening polylipoic acid-based adhesive, which achieves high-strength underwater adhesion with various solid materials including metal, wood, plastic, etc.; compared with traditional adhesives, it achieves long-term underwater adhesion, and provides a new idea and method for the design and preparation of a new generation of underwater adhesives. Specific embodiments

[0009] Example 1 (1) 1.15 g of lipoic acid, 1 g of 9-(2-hydroxyethyl)adenine, 0.75 g of 4-dimethylaminopyridine and dichloromethane were added to a single-necked round-bottom flask, stirred at room temperature until completely dissolved, placed in an ice-water bath and cooled to 0 °C, (1-ethyl 3-(3-dimethylaminopropyl))carbodiimide was added, stirred for 15 minutes and then the ice-water bath was removed, the round-bottom flask was wrapped with aluminum foil and stirred at room temperature for 12 hours, and concentrated in a vacuum to obtain a 9-(2-hydroxyethyl)adenine-modified lipoic acid precursor solution, and the base-modified lipoic acid monomer was precipitated using an ethyl acetate solution; the molar ratio of the 9-(2-hydroxyethyl)adenine monomer to the lipoic acid monomer and the 4-dimethylaminopyridine monomer was 1:1:1.1.

[0010] (2) 4 g of lipoic acid monomer and 1 g of base-modified lipoic acid monomer were melted at 90°C, melt-polymerized at 90°C for 6 hours, and cooled to room temperature to finally prepare a base-thickening polylipoic acid adhesive, wherein the mass ratio of lipoic acid monomer to base-modified lipoic acid monomer was 4:1.

[0011] The test method for the underwater adhesion performance of the prepared base-thickening polylipoic acid-based adhesive is as follows: 1 mL of the prepared adhesive fluid is applied on the surface of the substrate, and the adhesion of the joint is tested in an underwater environment. The bonding area is fixed to 2.5 cm×2.0 cm. A shear test is performed using a Shimadzu universal tensile testing machine (model: SHIMADZU AGS-X 10KN) with a test speed of 50 mm / min. Using the above test method, the underwater shear adhesion strength of the base-thickening polylipoic acid-based adhesive prepared in Example 1 is 0.75 MPa.

[0012] Example 2 (1) 1.26 g of lipoic acid, 1 g of 9-(2-hydroxyethyl)adenine, 0.82 g of 4-dimethylaminopyridine and dichloromethane were added to a single-necked round-bottom flask, stirred at room temperature until completely dissolved, placed in an ice-water bath and cooled to 0 °C, (1-ethyl 3-(3-dimethylaminopropyl))carbodiimide was added, stirred for 15 minutes and then the ice-water bath was removed, the round-bottom flask was wrapped with aluminum foil and stirred at room temperature for 12 hours, and concentrated in a vacuum to obtain a 9-(2-hydroxyethyl)adenine-modified lipoic acid precursor solution, and the base-modified lipoic acid monomer was precipitated using an ethyl acetate solution; the molar ratio of the 9-(2-hydroxyethyl)adenine monomer to the lipoic acid monomer and the 4-dimethylaminopyridine monomer was 1:1.1:1.2.

[0013] (2) 3 g of lipoic acid monomer and 2 g of base-modified lipoic acid monomer were melted at 90°C, melt-polymerized at 90°C for 6 hours, and cooled to room temperature to finally prepare a base-thickening polylipoic acid adhesive, wherein the mass ratio of lipoic acid monomer to base-modified lipoic acid monomer was 3:2.

[0014] Using the test method in Example 1, the underwater shear adhesion strength of the base thickening polylipoic acid-based adhesive prepared in Example 2 was 0.83 MPa.

[0015] Example 3 (1) 1.38 g of lipoic acid, 1 g of 9-(2-hydroxyethyl)adenine, 1.8 g of 4-dimethylaminopyridine and dichloromethane were added to a single-necked round-bottom flask, stirred at room temperature until completely dissolved, placed in an ice-water bath and cooled to 0 °C, (1-ethyl 3-(3-dimethylaminopropyl))carbodiimide was added, stirred for 15 minutes and then the ice-water bath was removed, the round-bottom flask was wrapped with aluminum foil and stirred at room temperature for 12 hours, and concentrated in a vacuum to obtain a 9-(2-hydroxyethyl)adenine-modified lipoic acid precursor solution, and the base-modified lipoic acid monomer was precipitated using an ethyl acetate solution; the molar ratio of the 9-(2-hydroxyethyl)adenine monomer to the lipoic acid monomer and the 4-dimethylaminopyridine monomer was 1:1.2:1.3.

[0016] (2) 2 g of lipoic acid monomer and 3 g of base-modified lipoic acid monomer were melted at 90°C, melt-polymerized at 90°C for 7 hours, and cooled to room temperature to finally prepare a base-thickening polylipoic acid adhesive, wherein the mass ratio of lipoic acid monomer to base-modified lipoic acid monomer was 2:3.

[0017] Using the test method in Example 1, the underwater shear adhesion strength of the base thickening polylipoic acid-based adhesive prepared in Example 3 was 0.95 MPa.

[0018] Example 4 (1) 1.49 g of lipoic acid, 1 g of 9-(2-hydroxyethyl)adenine, 0.95 g of 4-dimethylaminopyridine and dichloromethane were added to a single-necked round-bottom flask, stirred at room temperature until completely dissolved, placed in an ice-water bath and cooled to 0 °C, (1-ethyl 3-(3-dimethylaminopropyl))carbodiimide was added, stirred for 15 minutes and then the ice-water bath was removed, the round-bottom flask was wrapped with aluminum foil and stirred at room temperature for 12 hours, and concentrated in a vacuum to obtain a 9-(2-hydroxyethyl)adenine-modified lipoic acid precursor solution, and the base-modified lipoic acid monomer was precipitated using an ethyl acetate solution; the molar ratio of the 9-(2-hydroxyethyl)adenine monomer to the lipoic acid monomer and the 4-dimethylaminopyridine monomer was 1:1.3:1.4.

[0019] (2) 1 g of lipoic acid monomer and 4 g of base-modified lipoic acid monomer were melted at 90°C, melt-polymerized at 90°C for 8 hours, and cooled to room temperature to finally prepare a base-thickening polylipoic acid adhesive, wherein the mass ratio of lipoic acid monomer to base-modified lipoic acid monomer was 1:4.

[0020] Using the test method in Example 1, the underwater shear adhesion strength of the base thickening polylipoic acid-based adhesive prepared in Example 4 was 1.1 MPa.

Claims

1. A method for preparing a base thickening polylipoic acid adhesive, characterized in that: The steps and conditions are as follows: (1) Add lipoic acid, 9-(2-hydroxyethyl)adenine, 4-dimethylaminopyridine and dichloromethane to a single-necked round-bottom flask, stir at room temperature until completely dissolved, place in an ice-water bath to cool to 0 °C, add (1-ethyl 3-(3-dimethylaminopropyl)) carbodiimide, stir for 15 minutes and then remove the ice-water bath, wrap the round-bottom flask with aluminum foil and stir at room temperature for 12 hours, concentrate in a vacuum to obtain a 9-(2-hydroxyethyl)adenine-modified lipoic acid precursor solution, and precipitate a base-modified lipoic acid monomer using an ethyl acetate solution; the molar ratio of the 9-(2-hydroxyethyl)adenine monomer to the lipoic acid monomer and the 4-dimethylaminopyridine monomer is 1:1-1.3:1.1-1.4; (2) Melting lipoic acid monomer and base-modified lipoic acid monomer at 90°C, melt-polymerizing at 90°C for 6-8 hours, cooling to room temperature, and finally preparing a base-thickening polylipoic acid adhesive. The mass ratio of lipoic acid monomer to base-modified lipoic acid monomer is 0.25-4.

2. The method for preparing a base thickening polylipoic acid adhesive as claimed in claim 1, wherein: The steps and conditions are as follows: (1) 1.15 g of lipoic acid, 1 g of 9-(2-hydroxyethyl)adenine, 0.75 g of 4-dimethylaminopyridine and dichloromethane were added to a single-necked round-bottom flask, stirred at room temperature until completely dissolved, placed in an ice-water bath and cooled to 0 °C, (1-ethyl 3-(3-dimethylaminopropyl))carbodiimide was added, stirred for 15 minutes and then the ice-water bath was removed, the round-bottom flask was wrapped with aluminum foil and stirred at room temperature for 12 hours, and concentrated in a vacuum to obtain a 9-(2-hydroxyethyl)adenine-modified lipoic acid precursor solution, and the base-modified lipoic acid monomer was precipitated using an ethyl acetate solution; the molar ratio of the 9-(2-hydroxyethyl)adenine monomer to the lipoic acid monomer and the 4-dimethylaminopyridine monomer was 1:1:1.1; (2) 4 g of lipoic acid monomer and 1 g of base-modified lipoic acid monomer were melted at 90 °C, melt-polymerized at 90 °C for 6 hours, and cooled to room temperature to finally prepare a base-thickening polylipoic acid adhesive. The mass ratio of lipoic acid monomer to base-modified lipoic acid monomer was 4:

1.

3. The method for preparing a base thickening polylipoic acid adhesive as claimed in claim 1, characterized in that, The steps and conditions are as follows: (1) 1.26 g of lipoic acid, 1 g of 9-(2-hydroxyethyl)adenine, 0.82 g of 4-dimethylaminopyridine and dichloromethane were added to a single-necked round-bottom flask, stirred at room temperature until completely dissolved, placed in an ice-water bath and cooled to 0 °C, (1-ethyl 3-(3-dimethylaminopropyl))carbodiimide was added, stirred for 15 minutes and then the ice-water bath was removed, the round-bottom flask was wrapped with aluminum foil and stirred at room temperature for 12 hours, and concentrated in a vacuum to obtain a 9-(2-hydroxyethyl)adenine-modified lipoic acid precursor solution, and the base-modified lipoic acid monomer was precipitated using an ethyl acetate solution; the molar ratio of the 9-(2-hydroxyethyl)adenine monomer to the lipoic acid monomer and the 4-dimethylaminopyridine monomer was 1:1.1:1.2; (2) 3 g of lipoic acid monomer and 2 g of base-modified lipoic acid monomer were melted at 90 °C, melt-polymerized at 90 °C for 6 hours, and cooled to room temperature to finally prepare a base-thickening polylipoic acid adhesive. The mass ratio of lipoic acid monomer to base-modified lipoic acid monomer was 3:

2.

4. The method for preparing a base thickening polylipoic acid adhesive as claimed in claim 1, characterized in that: The steps and conditions are as follows: (1) 1.38 g of lipoic acid, 1 g of 9-(2-hydroxyethyl)adenine, 0.89 g of 4-dimethylaminopyridine and dichloromethane were added to a single-necked round-bottom flask, stirred at room temperature until completely dissolved, placed in an ice-water bath and cooled to 0 °C, (1-ethyl 3-(3-dimethylaminopropyl))carbodiimide was added, stirred for 15 minutes and then the ice-water bath was removed, the round-bottom flask was wrapped with aluminum foil and stirred at room temperature for 12 hours, and concentrated in a vacuum to obtain a 9-(2-hydroxyethyl)adenine-modified lipoic acid precursor solution, and the base-modified lipoic acid monomer was precipitated using an ethyl acetate solution; the molar ratio of the 9-(2-hydroxyethyl)adenine monomer to the lipoic acid monomer and the 4-dimethylaminopyridine monomer was 1:1.2:1.3; (2) 2 g of lipoic acid monomer and 3 g of base-modified lipoic acid monomer were melted at 90 °C, melt-polymerized at 90 °C for 7 hours, and cooled to room temperature to finally prepare a base-thickening polylipoic acid adhesive. The mass ratio of lipoic acid monomer to base-modified lipoic acid monomer was 2:

3.

5. The method for preparing a base thickening polylipoic acid adhesive as claimed in claim 1, characterized in that: The steps and conditions are as follows: (1) 1.49 g lipoic acid, 1 g 9-(2-hydroxyethyl)adenine, 0.95 g 4-dimethylaminopyridine and dichloromethane were added to a single-necked round-bottom flask, stirred at room temperature until completely dissolved, placed in an ice-water bath and cooled to 0 °C, (1-ethyl 3-(3-dimethylaminopropyl))carbodiimide was added, stirred for 15 minutes and then the ice-water bath was removed, the round-bottom flask was wrapped with aluminum foil and stirred at room temperature for 12 hours, and concentrated in a vacuum to obtain a 9-(2-hydroxyethyl)adenine-modified lipoic acid precursor solution, and the base-modified lipoic acid monomer was precipitated using an ethyl acetate solution; the molar ratio of the 9-(2-hydroxyethyl)adenine monomer to the lipoic acid monomer and the 4-dimethylaminopyridine monomer was 1:1.3:1.4; (2) 1 g of lipoic acid monomer and 4 g of base-modified lipoic acid monomer were melted at 90 °C, melt-polymerized at 90 °C for 8 hours, and cooled to room temperature to finally prepare a base-thickening polylipoic acid adhesive. The mass ratio of lipoic acid monomer to base-modified lipoic acid monomer was 1:4.

Citation Information

Cited By

  • Hot-melt injectable adhesive as well as preparation method and application thereof

    CN119823707A

  • A luting agent based on lipoic acid compounds and nitrogen heterocyclic compounds, and a preparation method and application thereof

    CN120574556B

  • Composite green adhesive based on lipoic acid and antibacterial air filter paper and preparation method thereof

    CN121344961A