Corrosion detection method and device for pipeline under thermal insulation layer, storage medium and electronic equipment
Through the detection method of low-frequency electromagnetic field scanner, the problem of strong corrosion concealment under the insulation layer of the pipeline in nuclear power plant is solved, real-time monitoring of the pipeline status is realized, and pipeline corrosion defects are quickly positioned and quantitatively analyzed, ensuring the safe and stable operation of the pipeline.
Patent Information
- Application Number
- CN202411273210.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-11-22
AI Technical Summary
The existing technology is difficult to effectively detect and promptly detect corrosion problems under the insulation layer of nuclear power plant pipelines, resulting in strong concealment of pipeline corrosion and difficulty in grasping the status of the pipeline in a timely manner, which may lead to perforation and damage to mechanical strength.
The low-frequency electromagnetic field scanner detection method is used to determine the reference curve and scan parameters through the sample tube, scan the measured pipeline, obtain the detection signal and conduct defect analysis, and quantitatively detect the pipeline corrosion defects to achieve real-time monitoring of the pipeline status.
Without magnetizing the pipeline and not interfering with the internal media of the pipeline, it can quickly detect pipeline corrosion defects, effectively discover pipeline corrosion problems under the insulation layer, achieve real-time grasp of the pipeline status, reduce the rate of error judgment, and is suitable for large-scale on-site Range detection.
Smart Images

Figure CN119000853A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of nuclear power plant pipeline corrosion detection, and more specifically, to a pipeline corrosion detection method, device, storage medium and electronic equipment under an insulation layer. Background Art
[0002] The main function of the chilled water system is to regulate the temperature of other systems of the unit to ensure that the unit operates in a stable environment. The function of the steam system is to transport the main steam generated by the steam generator to ensure power production. The chilled water system and the steam system play an important role in the safe operation and daily production of nuclear power plants. The related systems of the two need to operate in low or high temperature environments, so they are often covered with insulation. However, due to improper installation or the performance degradation of the outer protective layer of the insulation layer during service, it is possible that moisture will penetrate and contact the surface of the pipeline.
[0003] When the surface coating of the pipeline is damaged due to the effect of stretching under the humid surface environment, or fails due to improper construction and mechanical wear, it will cause moisture to contact the pipeline matrix, thus causing pipeline corrosion. And due to the existence of the insulation layer, the corrosion under the insulation layer is extremely hidden and difficult to detect in time. When the corrosion is serious, it will cause pipeline perforation and damage the mechanical strength and integrity of the pipeline.
[0004] Nuclear power plants currently deal with the problem of pipeline corrosion under the insulation layer mainly through daily inspections and overhaul inspections to ensure stable system operation. Daily inspections are mainly visual inspections, while overhaul inspections mainly involve removing some pipeline insulation layers for inspection. It is difficult to effectively detect the problem of pipeline corrosion under the insulation layer and it is impossible to grasp the pipeline status in a timely manner. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a method, device, storage medium and electronic equipment for detecting corrosion of pipelines under an insulation layer in view of the problems existing in the prior art.
[0006] The technical solution adopted by the present invention to solve the technical problem is: constructing a pipeline corrosion detection method under the insulation layer, comprising the following steps:
[0007] Determine a reference curve and scanning parameters based on the sample tube; the reference curve is: a wall thickness reduction degree-amplitude curve;
[0008] Perform pre-test preparations;
[0009] After the preparation before the test is completed, a low-frequency electromagnetic field is used to scan each scanning interval of the pipeline to be tested by a scanner according to the scanning parameters to obtain a detection signal;
[0010] Defect analysis is performed on the tested pipeline according to the detection signal and the reference curve.
[0011] In the method for detecting corrosion of pipelines under the insulation layer of the present invention, the determination of the reference curve and scanning parameters based on the sample pipe includes:
[0012] Scanning the sample tube by a scanner to obtain a sample tube detection signal;
[0013] Drawing the reference curve based on the sample tube detection signal;
[0014] During the scanning process of the scanner on the sample tube, the scanning parameters are recorded; the scanning parameters include: lift-off, scanning speed and scanning frequency.
[0015] In the method for detecting corrosion of pipelines under the insulation layer of the present invention, the preparation before performing the detection includes:
[0016] Obtaining the pipe size of the measured pipe and the scanning range of the scanner;
[0017] Dividing scanning intervals along the circumference of the measured pipeline according to the scanning range of the scanner and the pipeline size of the measured pipeline;
[0018] According to the scanning frequency setting, the scanning frequency of the detection setting is set and the basic information of the detected pipeline and the detection file number are recorded;
[0019] The scanner is placed at an initial position of the pipeline to be tested and the gain of the scanner is adjusted.
[0020] In the pipeline corrosion detection method under the insulation layer of the present invention, scanning each scanning interval of the pipeline under test by using a scanner with a low-frequency electromagnetic field according to the scanning parameters to obtain a detection signal includes:
[0021] The scanner scans each scanning interval of the detected pipeline according to the determined scanning speed to obtain the detection signal.
[0022] In the method for detecting corrosion of pipelines under the insulation layer of the present invention, the scanner scans each scanning interval of the pipeline to be tested according to the determined scanning speed, and obtaining the detection signal includes:
[0023] The scanning is performed on each scanning interval of the pipeline under test according to the determined scanning speed;
[0024] Determine whether there are abnormal signals during the scanning process;
[0025] If yes, repeat scanning the pipeline under test;
[0026] Determine whether there is a defect signal based on repeated scanning results;
[0027] If there is a defect signal, the defect position of the tested pipeline is marked and the detection signal is recorded at the same time.
[0028] In the method for detecting corrosion of pipelines under the insulation layer of the present invention, the defect analysis of the pipeline under test according to the detection signal and the reference curve comprises:
[0029] Analyzing the waveform and phase of the detection signal to identify defects in the tested pipeline;
[0030] An amplitude analysis is performed on the defect signal in the detection signal, and the signal is compared with the reference curve to quantitatively analyze the defects of the detected pipeline.
[0031] In the method for detecting corrosion of pipelines under the insulation layer of the present invention, the method further comprises:
[0032] Based on the marked position defects and the scanning distance, the defects of the measured pipeline are located.
[0033] The present invention also provides a device for detecting corrosion of pipelines under an insulation layer, comprising:
[0034] A reference data determination unit, used to determine a reference curve and scanning parameters based on a sample tube; the reference curve is: a wall thickness reduction degree-amplitude curve;
[0035] A pre-test preparation unit, used for performing pre-test preparation;
[0036] A scanner, which is used to scan each scanning interval of the pipeline under test using a low-frequency electromagnetic field according to the scanning parameters after completing the pre-test preparation, to obtain a test signal;
[0037] The detection device is used to perform defect analysis on the detected pipeline according to the detection signal and the reference curve.
[0038] The present invention also provides a storage medium storing a computer program, wherein the computer program is suitable for being loaded by a processor to execute the steps of the method for detecting corrosion of pipelines under the insulation layer as described above.
[0039] The present invention also provides an electronic device, comprising a memory and a processor, wherein the memory stores a computer program, and the processor executes the steps of the above-mentioned method for detecting corrosion of pipelines under the insulation layer by calling the computer program stored in the memory.
[0040] The method, device, storage medium and electronic device for detecting corrosion of pipelines under the insulation layer of the present invention have the following beneficial effects: including the following steps: determining the reference curve and scanning parameters based on the sample pipe; the reference curve is: the wall thickness thinning degree-amplitude curve; performing pre-detection preparation; after completing the pre-detection preparation, scanning each scanning interval of the pipeline under test by using a low-frequency electromagnetic field through a scanner according to the scanning parameters to obtain a detection signal; performing defect analysis on the pipeline under test according to the detection signal and the reference curve. Through the present invention, under the premise that the pipeline does not need to be magnetized, does not interfere with the pipeline, and the medium inside the pipeline has no effect on the detection, the pipeline corrosion defects can be quickly detected according to the detection signal, the pipeline corrosion problem under the insulation layer can be effectively discovered, and the real-time grasp of the pipeline status can be achieved. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] The present invention will be further described below with reference to the accompanying drawings and embodiments, in which:
[0042] Figure 1 It is a schematic flow chart of a method for detecting corrosion of pipelines under an insulation layer provided by the present invention;
[0043] Figure 2 It is a principle block diagram of the pipeline corrosion detection device under the insulation layer provided by the present invention;
[0044] Figure 3 is a schematic diagram of defect dimensions of the tested pipeline in Example 1 of the present invention;
[0045] Figure 4 is a scanning result diagram of the tested pipeline in Example 1 of the present invention;
[0046] Figure 5 is the wall thickness reduction degree-amplitude curve of Example 1 of the present invention;
[0047] Figure 6 is a schematic diagram of defect dimensions of a tested pipeline in Example 2 of the present invention;
[0048] Figure 7 is a scanning result diagram of the tested pipeline in Example 2 of the present invention;
[0049] Figure 8 It is a schematic diagram of the quantitative analysis result of the defect size of the tested pipeline in Example 2 of the present invention. DETAILED DESCRIPTION
[0050] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0051] refer to Figure 1 , Figure 1 A schematic flow chart of a preferred embodiment of a method for detecting corrosion of pipelines under insulation layer provided by the present invention.
[0052] Specifically, Figure 1 As shown, the method for detecting corrosion of pipelines under the insulation layer comprises the following steps:
[0053] Step S101: Determine a reference curve and scanning parameters based on the sample tube, wherein the reference curve is a wall thickness reduction degree-amplitude curve.
[0054] Optionally, in an embodiment of the present invention, determining the reference curve and scanning parameters based on the sample tube includes: scanning the sample tube by a scanner to obtain a sample tube detection signal; drawing a reference curve based on the sample tube detection signal; and recording the scanning parameters during the scanning process of the sample tube by the scanner. The scanning parameters include: lift-off, scanning speed, and scanning frequency. When scanning the sample tube, it can be seen that the absolute value signal and the differential signal at the good part of the pipeline are horizontal straight lines, and the absolute value signal and the differential signal at the defective part are clear and independent sine waveforms.
[0055] Specifically, a sample tube needs to be made first. After the sample tube is made, the sample tube is scanned by a scanner and a wall thickness reduction degree-amplitude curve is drawn. The scanning speed and scanning frequency are determined in combination with the scanning results of the sample tube. It should be noted that the material, diameter, insulation material and thickness of the sample tube should be as consistent as possible with the tested pipeline. Among them, the defects of the sample tube are shown in Table 1.
[0056] Table 1 Defects of prefabricated comparison sample pipes
[0057]
[0058] Step S102: Perform pre-detection preparation.
[0059] In an embodiment of the present invention, the preparation before performing the detection includes: obtaining the pipeline size of the pipeline to be detected and the scanning range of the scanner; dividing the scanning interval along the circumference of the pipeline to be detected according to the scanning range of the scanner and the pipeline size of the pipeline to be detected; setting the scanning frequency of the detection setting according to the scanning frequency and recording the basic information of the pipeline to be detected and the detection file number; placing the scanner at the initial position of the pipeline to be detected and adjusting the gain of the scanner. Among them, scanning each scanning interval of the pipeline to be detected by the scanner using a low-frequency electromagnetic field according to the scanning parameters, and obtaining the detection signal includes: the scanner scans each scanning interval of the pipeline to be detected according to the determined scanning speed to obtain the detection signal.
[0060] Specifically, before performing pipeline corrosion defect detection, first adjust the roller spacing of the scanner to ensure that the rollers are at the same level, rotate the scanner on the pipeline to be tested, and ensure that the rollers and the pipeline to be tested fit well. After completing the above prerequisites, perform defect detection on the pipeline to be tested according to the following steps:
[0061] a. Confirm the surface condition of the insulation layer of the pipeline to be tested, and avoid uneven areas and metal cover overlaps as much as possible during scanning; b. Divide the scanning interval along the circumference of the pipeline to be tested according to the coverage range of the scanner and the length of the pipeline to be tested to ensure that the pipeline to be tested is 100% covered; c. Connect the detection equipment, set the scanning frequency, and record the basic information of the scanned pipeline and the detection file number; d. Place the adjusted scanner at the initial position of the pipeline scanning, adjust the gain, and ensure that the absolute value channel signal level and the differential channel signal level are equivalent; e. Scan the pipeline at the determined scanning speed. Keep the scanner and scanning speed stable during the scanning process, and pay attention to the changes in the signal. If a suspected defect signal is detected, the pipeline should be scanned repeatedly to eliminate the interference of accidental factors, and the defect position should be marked on the pipeline according to the displayed scanning distance; f. Analyze the defect amplitude and compare it with the wall thickness thinning degree-amplitude curve drawn by scanning the sample pipe of the tested pipeline to quantitatively analyze the defects; g. After scanning one interval in this way, perform the scan of the next interval until the scanning work is completed.
[0062] Step S103: After the preparation before the test is completed, a low-frequency electromagnetic field is used by a scanner to scan each scanning interval of the pipeline to be tested according to the scanning parameters to obtain a detection signal.
[0063] In an embodiment of the present invention, the scanner scans each scanning interval of the measured pipeline according to the determined scanning speed, and obtaining the detection signal includes: scanning each scanning interval of the measured pipeline according to the determined scanning speed; determining whether there is an abnormal signal during the scanning process; if so, repeatedly scanning the measured pipeline; determining whether there is a defect signal based on the repeated scanning results; if there is a defect signal, marking the defect position of the measured pipeline and recording the detection signal at the same time.
[0064] Step S104: performing defect analysis on the tested pipeline according to the detection signal and the reference curve.
[0065] In an embodiment of the present invention, defect analysis of the tested pipeline based on the detection signal and the reference curve includes: analyzing the waveform and phase of the detection signal to identify defects of the tested pipeline; performing amplitude analysis on the defect signal in the detection signal and comparing it with the reference curve to quantitatively analyze the defects of the tested pipeline.
[0066] Furthermore, in an embodiment of the present invention, the method for detecting corrosion of pipelines under the insulation layer further includes: locating defects of the pipeline under test based on the marked position defects and the scanning distance.
[0067] Specifically, the detection signal is analyzed to analyze the waveform and phase of the detection signal to identify pipeline defects. For example, by changing the phase angle of the detection signal, corrosion defects can be identified and distinguished from welds and binding wires. By analyzing the amplitude of the detection signal, the defect size can be determined. By verifying the scanning distance, the defect can be located.
[0068] Specifically, the general structure of the insulation layer pipeline of a nuclear power plant is: the coating pipeline is covered with an insulation layer, and the insulation layer includes an insulating layer, a moisture-proof layer and a metal protective cover. In particular, part of the insulation layer and the moisture-proof layer are reinforced by wire tying. This structure perfectly isolates the pipeline from external moisture, thereby effectively reducing the risk of corrosion of the pipeline. For pipeline corrosion that occurs after the failure of the insulation layer, the implementation requirements of X-ray detection are relatively high. The pulse eddy current detection technology is insensitive to smaller corrosion defects. The ultrasonic guided wave detection technology has serious signal attenuation when detecting large-area thinning, and is not suitable for large-scale on-site detection. The present invention uses a low-frequency, high-power excitation coil to excite a low-frequency electromagnetic field, and the low-frequency electromagnetic field penetrates the insulation layer, is transmitted to the pipe wall and then reflects, and the receiving coil detects the reflected signal to achieve pipeline corrosion detection under the insulation layer, providing a convenient pipeline corrosion detection method under the insulation layer for nuclear power plants.
[0069] Among them, when corrosion occurs in the pipeline, the thickness of the defective part is different from that of the normal part, and the waveform, phase and amplitude of the reflected signal will change. Therefore, by analyzing the waveform and phase, the pipeline defects can be qualitatively analyzed (such as distinguishing corrosion defects from welds and binding wires); by analyzing the amplitude of the detection signal, the defect size can be determined. The present invention performs detection without removing the insulation condition, and can adapt to different pipe diameters by replacing rollers of different sizes. The core of the present invention is that there is no need to magnetize the pipeline, no interference is generated to the pipeline, and the medium inside the pipeline has no effect on the detection. A low-frequency electromagnetic field is used to detect the surface of the pipeline. According to the waveform and phase of the reflected signal (i.e., the detection signal), the pipeline defects are quickly located, and the amplitude of the detection signal is analyzed to achieve quantitative analysis of the defects. It should be noted that in the embodiment of the present invention, the low-frequency high-power excitation coil and the receiving coil are both internal components of the scanner.
[0070] Optionally, in an embodiment of the present invention, the detection frequency range is 5 to 40 Hz, and the detection signal output by the detection device includes: a high-frequency differential signal, a high-frequency absolute value signal, a low-frequency differential signal, and a low-frequency absolute value signal. Among them, by analyzing the absolute value signal (high-frequency absolute value signal or low-frequency absolute value signal), the overall thinning of the pipeline can be detected; by analyzing the differential signal (high-frequency differential signal or low-frequency differential signal), local thinning defects can be identified, and the minimum defect that can be detected is 6 mm in diameter and 10% wall thickness thinning.
[0071] refer to Figure 2 , Figure 2 The present invention provides a device for detecting corrosion of pipelines under the insulation layer. Specifically, Figure 2 As shown, the pipeline corrosion detection device under the insulation layer includes:
[0072] The reference data determination unit 201 is used to determine a reference curve and scanning parameters based on the sample tube; the reference curve is: a wall thickness reduction degree-amplitude curve.
[0073] The pre-detection preparation unit 202 is used to perform pre-detection preparation.
[0074] The scanner 203 is used to scan each scanning interval of the pipeline under test using a low-frequency electromagnetic field according to scanning parameters after completing the pre-test preparation to obtain a test signal.
[0075] The detection device 204 is used to perform defect analysis on the detected pipeline according to the detection signal and the reference curve.
[0076] Specifically, the specific coordination operation process between the units in the device for detecting corrosion of pipelines under thermal insulation layer here can refer to the above-mentioned method for detecting corrosion of pipelines under thermal insulation layer, which will not be repeated here.
[0077] The present invention is described below with reference to specific embodiments.
[0078] Example 1: The tested pipeline is a 2.5m long, 168*5mm insulated pipeline, the metal protective cover is 0.8mm aluminum, the insulation layer is 50mm asbestos, and the insulation layer is tied with a plastic binding tape.
[0079] Through machining, Φ20, depths of 20%, 50%, 70% and 100% wall thickness defects are prefabricated on the pipe, such as Figure 3 As shown in the figure, starting from the left end of the pipeline, scan along the pipeline axial direction, passing through 20%, 50%, 70% and 100% wall thickness depth defects in turn, and observe the signal characteristics.
[0080] Detection results of the tested pipeline: The scanning results based on electromagnetic principles are as follows: Figure 4 As shown. Figure 4It can be seen that Figure 4 In the figure, the left picture shows the high-frequency channel signal, and the right picture shows the low-frequency channel signal. It can be seen that the absolute value signals of the high-frequency and low-frequency signals are normal, and the differential channel signal shows 4 sine function waveform signals with different amplitudes. After analyzing the signal phase and comparing the scanning distance, and scanning and verifying multiple times, it is confirmed that the signal distortion is caused by defects.
[0081] According to the low-frequency differential signal (or high-frequency differential signal, selected according to the actual test results) in the scan results of the tested pipeline, a wall thickness reduction degree-amplitude curve is drawn, such as Figure 5 shown.
[0082] Example 2: The tested pipeline is a 2.5m long, 168*5mm insulated pipeline, the metal protective cover is 0.8mm aluminum, the insulation layer is 50mm asbestos, and the insulation layer is tied with a plastic binding tape.
[0083] Through machining, Φ20, 10%, 30% and 60% wall thickness defects are prefabricated on the pipe. Figure 6 As shown in the figure, starting from the left end of the pipeline, scan along the pipeline axial direction, passing through 10%, 30% and 60% wall thickness depth defects in turn, and observe the signal characteristics.
[0084] Detection results of the tested pipeline: The scanning results based on electromagnetic principles are as follows: Figure 7 As shown in the figure, the left figure is the high-frequency channel signal, and the right figure is the low-frequency channel signal. It can be seen that there is no abnormality in the absolute value signals of high and low frequencies, and the differential channel signal shows three sine function waveform signals with different amplitudes. After analyzing the signal phase and checking the scanning distance, and verifying it through multiple scanning, it is confirmed that the signal distortion is caused by defects.
[0085] The defects of the tested pipeline are quantitatively analyzed as follows:
[0086] Based on the wall thickness reduction degree-amplitude curve drawn according to the test results of the tested pipeline, the amplitude of the tested pipeline is plotted in the figure (such as Figure 8 As shown in the figure, the corresponding wall thickness reduction degrees are read, which are 9.05%, 30.57% and 59.8% respectively, thus achieving quantitative analysis of the defects.
[0087] The measurement error analysis is shown in Table 2. From the analysis, it can be seen that the smaller the wall thickness reduction, the larger the measurement error; the larger the wall thickness reduction, the smaller the measurement error.
[0088]
[0089] The present invention uses an electromagnetic detection method to quickly scan the pipeline without removing the insulation layer, determine the defect characteristics according to the distortion of the electromagnetic signal (i.e., the detection signal), and locate the defect position by scanning distance.
[0090] Specifically, the present invention detects magnetic field deformation caused by defects in the pipe wall by exciting a low-frequency electromagnetic field to penetrate the insulation layer and the insulating layer, analyzes the distorted signal, and characterizes the defect. The insulation material and the flat protective cover have no effect on the detection result, and the detection method can pass through common metal protective covers, such as stainless steel, aluminum and galvanized steel. The detection method can identify pipeline welds and metal binding tapes of insulation materials, distinguish defect signals, and reduce the misjudgment rate. The host and probe structure of the detection method are simple, reducing the requirements for scanning operations and pipeline layout space. After the scanning is completed, the detection results are compared and analyzed with the test results of the comparison test piece to improve the detection efficiency and detection accuracy, and the defect position is located by recording the scanning distance. The detection method is suitable for pipelines with insulation layers, and the insulation layer does not need to be removed during detection. The detection method is a pipeline outer wall detection method. For pipelines of different diameters, different sizes of probe rollers are replaced to complete the scanning of pipelines of different diameters. When the detection method is implemented, the scanning track is divided along the circumference of the pipeline to achieve 360° coverage scanning of the pipeline. This method does not require the magnetization of the pipeline, does not interfere with the pipeline, and the medium inside the pipeline has no effect on the detection. This method does not require the unit to be shut down for detection, and the medium inside the pipeline has no effect on the detection results. It can be performed during the daily operation of the unit, saving overhaul time. This method has low requirements for detection personnel, and at least 2 people can complete the on-site detection work, and no external AC power supply is required.
[0091] In addition, an electronic device of the present invention includes a memory and a processor; the memory is used to store a computer program; the processor is used to execute the computer program to implement a method for detecting corrosion of pipelines under insulation layers as described in any one of the above. Specifically, according to an embodiment of the present invention, the process described with reference to the flowchart above can be implemented as a computer software program. For example, an embodiment of the present invention includes a computer program product, which includes a computer program carried on a computer-readable medium, and the computer program contains program code for executing the method shown in the flowchart. In such an embodiment, the computer program can be downloaded and installed by an electronic device and when executed, it executes the above functions defined in the method of the embodiment of the present invention. The electronic device in the present invention can be a terminal such as a notebook, a desktop, a tablet computer, a smart phone, or a server.
[0092] In addition, a storage medium of the present invention stores a computer program thereon, and when the computer program is executed by a processor, any of the above methods for detecting corrosion of pipelines under the insulation layer is implemented. Specifically, it should be noted that the above storage medium of the present invention may be a computer-readable signal medium or a computer-readable storage medium or any combination of the above two. The computer-readable storage medium may be, for example, but not limited to, an electrical, magnetic, optical, electromagnetic, infrared, or semiconductor system, device or device, or any combination of the above. More specific examples of computer-readable storage media may include, but are not limited to: an electrical connection with one or more wires, a portable computer disk, a hard disk, a random access memory (RAM), a read-only memory (ROM), an erasable programmable read-only memory (EPROM or flash memory), an optical fiber, a portable compact disk read-only memory (CD-ROM), an optical storage device, a magnetic storage device, or any suitable combination of the above. In the present invention, a computer-readable storage medium may be any tangible medium containing or storing a program, which may be used by or in combination with an instruction execution system, device or device. In the present invention, a computer-readable signal medium may include a data signal propagated in a baseband or as part of a carrier wave, which carries a computer-readable program code. Such propagated data signals may take a variety of forms, including but not limited to electromagnetic signals, optical signals, or any suitable combination of the above. Computer readable signal media may also be any computer readable medium other than computer readable storage media, which may send, propagate, or transmit programs for use by or in conjunction with an instruction execution system, apparatus, or device. The program code contained on the computer readable medium may be transmitted using any suitable medium, including but not limited to: wires, optical cables, RF (radio frequency), etc., or any suitable combination of the above.
[0093] The computer-readable medium may be included in the electronic device, or may exist independently without being incorporated into the electronic device.
[0094] In this specification, each embodiment is described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the embodiments can be referred to each other. For the device disclosed in the embodiment, since it corresponds to the method disclosed in the embodiment, the description is relatively simple, and the relevant parts can be referred to the method part.
[0095] Professionals may further appreciate that the units and algorithm steps of each example described in conjunction with the embodiments disclosed herein can be implemented in electronic hardware, computer software, or a combination of the two. In order to clearly illustrate the interchangeability of hardware and software, the composition and steps of each example have been generally described in the above description according to function. Whether these functions are performed in hardware or software depends on the specific application and design constraints of the technical solution. Professionals and technicians may use different methods to implement the described functions for each specific application, but such implementation should not be considered to be beyond the scope of the present invention.
[0096] The steps of the method or algorithm described in conjunction with the embodiments disclosed herein may be implemented directly using hardware, a software module executed by a processor, or a combination of the two. The software module may be placed in a random access memory (RAM), a memory, a read-only memory (ROM), an electrically programmable ROM, an electrically erasable programmable ROM, a register, a hard disk, a removable disk, a CD-ROM, or any other form of storage medium known in the art.
[0097] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot limit the scope of protection of the present invention. All equivalent changes and modifications made to the scope of the claims of the present invention should fall within the scope of the claims of the present invention.
Claims
1. A method for detecting corrosion of pipelines under insulation layer, characterized in that: The following steps are involved: Determine a reference curve and scanning parameters based on the sample tube; the reference curve is: a wall thickness reduction degree-amplitude curve; Perform pre-test preparations; After the preparation before the test is completed, a low-frequency electromagnetic field is used to scan each scanning interval of the pipeline to be tested by a scanner according to the scanning parameters to obtain a detection signal; Defect analysis is performed on the tested pipeline according to the detection signal and the reference curve.
2. The method for detecting corrosion of pipelines under insulation layer according to claim 1, characterized in that: Determining the reference curve and scanning parameters based on the sample tube includes: Scanning the sample tube by a scanner to obtain a sample tube detection signal; Drawing the reference curve based on the sample tube detection signal; During the scanning process of the scanner on the sample tube, the scanning parameters are recorded; the scanning parameters include: lift-off, scanning speed and scanning frequency.
3. The method for detecting corrosion of pipelines under insulation layer according to claim 2, characterized in that: The preparation before performing the detection includes: Obtaining the pipe size of the measured pipe and the scanning range of the scanner; Dividing scanning intervals along the circumference of the measured pipeline according to the scanning range of the scanner and the pipeline size of the measured pipeline; According to the scanning frequency setting, the scanning frequency of the detection setting is set and the basic information of the detected pipeline and the detection file number are recorded; The scanner is placed at an initial position of the pipeline to be tested and the gain of the scanner is adjusted.
4. The method for detecting corrosion of pipelines under insulation layer according to claim 1, characterized in that: The step of scanning each scanning interval of the pipeline to be tested by using a scanner with a low-frequency electromagnetic field according to the scanning parameters to obtain a detection signal includes: The scanner scans each scanning interval of the detected pipeline according to the determined scanning speed to obtain the detection signal.
5. The method for detecting corrosion of pipelines under insulation layer according to claim 4, characterized in that: The scanner scans each scanning interval of the pipeline to be tested according to the determined scanning speed, and obtaining the detection signal includes: The scanning is performed on each scanning interval of the pipeline under test according to the determined scanning speed; Determine whether there are abnormal signals during the scanning process; If yes, repeat scanning the pipeline under test; Determine whether there is a defect signal based on repeated scanning results; If there is a defect signal, the defect position of the tested pipeline is marked and the detection signal is recorded at the same time.
6. The method for detecting corrosion of pipelines under insulation layer according to claim 5, characterized in that: The performing defect analysis on the tested pipeline according to the detection signal and the reference curve comprises: Analyzing the waveform and phase of the detection signal to identify defects in the tested pipeline; An amplitude analysis is performed on the defect signal in the detection signal, and the signal is compared with the reference curve to quantitatively analyze the defects of the detected pipeline.
7. The method for detecting corrosion of pipelines under insulation layer according to claim 5, characterized in that: The method further comprises: Based on the marked position defects and the scanning distance, the defects of the measured pipeline are located.
8. A device for detecting corrosion of pipelines under insulation layer, characterized in that: include: A reference data determination unit, used for determining a reference curve and scanning parameters based on the sample tube; The reference curve is: wall thickness reduction degree-amplitude curve; A pre-test preparation unit, used for performing pre-test preparation; A scanner, which is used to scan each scanning interval of the pipeline under test using a low-frequency electromagnetic field according to the scanning parameters after completing the pre-test preparation, to obtain a test signal; The detection device is used to perform defect analysis on the detected pipeline according to the detection signal and the reference curve.
9. A storage medium, characterized in that: The storage medium stores a computer program, and the computer program is suitable for being loaded by a processor to execute the steps of the method for detecting corrosion of pipelines under insulation layer as described in any one of claims 1 to 7.
10. An electronic device, characterized in that: It comprises a memory and a processor, wherein the memory stores a computer program, and the processor executes the steps of the method for detecting corrosion of pipelines under the insulation layer as claimed in any one of claims 1 to 7 by calling the computer program stored in the memory.
Citation Information
Cited By
System and method for evaluating corrosion state of nuclear power pipeline
CN119804284A